Artificial leather and manufacturing method thereof and laminate, vehicular interior material, clothing, miscellaneous goods

A discontinuous resin pattern on artificial leather addresses the flexibility and abrasion resistance challenge by forming resin portions A and B with specific ratios, achieving a thick design and wear resistance while maintaining flexibility.

JP2024134605APending Publication Date: 2024-10-04TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023044877
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing artificial leathers face challenges in achieving both flexibility and abrasion resistance, as methods that enhance design through surface resin application either result in hardness or poor wear resistance.

Method used

A discontinuous resin pattern is formed on the surface of artificial leather, with resin portions A and B, where resin portion A covers raised naps and is laminated on discontinuous resin portion B, adhering to specific area and length ratios, ensuring resin does not penetrate deeply into the base material.

Benefits of technology

The solution results in artificial leather with a thick design, excellent wear resistance, and flexibility, suitable for applications requiring both properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134605000001_ABST
    Figure 2024134605000001_ABST
Patent Text Reader

Abstract

To provide an artificial leather excellent in flexibility by giving excellent abrasion resistance and designability to the artificial leather coated with resin.SOLUTION: At least one surface of an artificial leather has naps. A resin portion A and a noncontinuous resin portion B are formed on the surface having naps. At least a part of the resin portion A is laminated on the noncontinuous resin portion B. The resin portion A is resin such as polyurethane resin. The noncontinuous resin portion B is resin such as polyurethane resin. Area ratio of the resin portion A and the noncontinuous resin portion B on the surface having naps is 50% or more and 95% or less. Length a (mm) of the resin portion A and length b (mm) of the noncontinuous resin portion B satisfy following formula 1. At least a part of the resin portion A directly comes in contact with the surface having naps of the artificial leather. 1<a / b≤50...(Formula 1)SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an artificial leather and a method for producing the same, as well as interior materials for vehicles, clothing and miscellaneous goods, at least a part of which is made of the artificial leather. [Background technology]

[0002] Suede-like artificial leather generally has high abrasion resistance and a soft texture, and is used in a wide range of fields such as automobile interior materials, furniture, miscellaneous goods, clothing, etc. When applying designs such as logos or patterns to the artificial leather, the most common methods are to apply a resin to the surface, to print the design, or to create a textured pattern by embossing.

[0003] In the case of artificial leather in which a design is applied to the surface by coating the surface with resin, there has long been a need for a means to achieve both the flexibility characteristic of artificial leather and the abrasion resistance of the applied design.

[0004] As an example of such a technique, Patent Document 1 proposes a grain-finished artificial leather in which three polymer elastomer coating layers, each having a specific structure and characteristics, are laminated in sequence on the surface of a base layer made of a fiber-entangled nonwoven fabric containing a polymer elastomer. It is described that this invention has excellent surface smoothness and design formability, is lightweight, and has high peel strength.

[0005] Patent Document 2 proposes a grain-finished artificial leather in which a skin material made of a polymer elastomer is present on the surface of a fabric substrate, and the polymer elastomer forming the skin material permeates from the surface of the substrate into the substrate in the thickness direction within a specific range. It is described that this invention can provide a grain-finished artificial leather that combines a sense of fullness and flexibility without reducing peel strength.

[0006] Patent Document 3 proposes a leather-like sheet having transparency, in which a concealing layer B, made of a resin solution containing a specific amount of a specific colorant relative to the resin solid weight and having a certain thickness, is laminated on the surface of a base layer A made of a fiber assembly impregnated with a polymer mainly composed of a specific polyurethane elastomer, and a colored layer C, made of a resin solution containing a specific amount of a specific colorant and having a specific thickness, is laminated on the surface of the concealing layer B. It is described that the leather-like sheet obtained according to this invention has excellent transparency and vivid hue.

[0007] Patent Document 4 proposes an artificial leather comprising a fiber substrate, a smoothing layer, and a resin surface layer, the smoothing layer being a layer of a specific thickness formed through a coating process and containing a polymeric elastomer and a filler in a specific ratio. It also describes that this invention provides an artificial leather with excellent flexibility and grain finish, which is provided with a resin layer that does not sink deeply into the fiber substrate. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2013-177713 A [Patent Document 2] JP 2014-1463 A [Patent Document 3] Japanese Patent Application Publication No. 11-1878 [Patent Document 4] JP 2015-158030 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, although the artificial leathers obtained by the methods proposed in Patent Documents 1, 2, etc. can provide artificial leathers excellent in design and abrasion resistance, the methods involve causing a resin applied to the surface of the substrate to soak into the substrate to a certain extent, which makes it difficult to form a thick design on the surface of the substrate, and when an attempt is made to apply resin, the artificial leather becomes hard and loses flexibility, which is a problem.

[0010] Conversely, in the case of artificial leathers obtained by the methods disclosed in Patent Documents 3, 4, etc., the resin that imparts the design does not penetrate into the substrate, so that a relatively flexible artificial leather can be provided; however, when an attempt is made to form a thick design on the surface of the substrate, there is a problem that the abrasion resistance is poor.

[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an artificial leather having excellent flexibility and which is provided with a resin-coated artificial leather having excellent abrasion resistance and design properties. [Means for solving the problem]

[0012] As a result of intensive research by the inventors to achieve the above object, it was discovered that by forming discontinuous resin parts on the napped surface of an artificial leather, and then forming further discontinuous resin parts in a specific shape on the discontinuous resin parts, resin part A penetrates into the napped parts between discontinuous resin parts B, thereby imparting a surface state that combines a thick design and abrasion resistance. It was also found that this artificial leather can be made into an artificial leather with excellent flexibility because the resin parts do not penetrate too much into the substrate.

[0013] The present invention has been completed based on these findings, and provides the following inventions.

[0014] [1] An artificial leather comprising: a fiber-entangled body containing, as a component, a nonwoven fabric composed of ultrafine fibers whose main component is a thermoplastic resin and whose average single fiber diameter is 1.0 μm or more and 10.0 μm or less; and a polymer elastomer; wherein one surface of the artificial leather has nap, and a resin portion A and a discontinuous resin portion B are formed on the napped surface, and at least a part of the resin portion A is laminated on the discontinuous resin portion B; and further, the artificial leather satisfies the following requirements (1) to (4): (1) The resin portion A is a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin, and the discontinuous resin portion B is a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin. (2) The area ratio of the resin portion A and the discontinuous resin portion B to the surface having nap is 50% or more and 95% or less. (3) The length a (mm) of the resin portion A and the length b (mm) of the discontinuous resin portion B satisfy the following formula 1.

[0015] 1 (4) At least a part of the resin portion A is in direct contact with the surface having the nap, and in that part, the resin portion A covers the nap.

[0016] [2] The thickness T of the resin portion A at a position where the resin portion A is on the discontinuous resin portion B. A The artificial leather according to the above [1], wherein the thickness of the surface roughness layer is 5 μm or more and 200 μm or less.

[0017] [3] The artificial leather according to [1] or [2], wherein the length b (mm) of the discontinuous resin portion B is 0.05 mm or more and 2.00 mm or less.

[0018] ​[4] The artificial leather according to any one of [1] to [3], wherein the resin portion A has a resin filling rate of 95% or more and less than 100%.

[0019] [5] A step of forming a sheet-like material including a fiber-entangled body containing, as a component, a nonwoven fabric composed of ultrafine fibers having an average single fiber diameter of 1.0 μm or more and 10.0 μm or less, and a polymer elastomer; A step of grinding at least one surface of the sheet-like material to form a napped sheet; a step of discontinuously placing a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin on the napped surface of the napped sheet to form a discontinuous resin portion B, and further placing a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, and natural resin and having a viscosity of 1000 mPa·s or more and 4000 mPa or less to form a resin portion A; The method for producing the artificial leather according to any one of the above [1] to [4],

[0020] [6] A laminate comprising the artificial leather according to any one of [1] to [4] above and a fabric layer and / or a foamed resin layer on the other surface of the artificial leather.

[0021] [7] A vehicle interior material, at least a part of which is the artificial leather according to any one of [1] to [4] above or the laminate according to [6] above.

[0022] [8] Clothing, at least a part of which is the artificial leather according to any one of [1] to [4] above or the laminate according to [6] above.

[0023] [9] Miscellaneous goods, at least a part of which is the artificial leather according to any one of [1] to [4] above or the laminate according to [6] above. Effect of the Invention

[0024] According to the present invention, an artificial leather having a surface state that combines a thick design with abrasion resistance and excellent flexibility can be obtained. In particular, the artificial leather of the present invention, which has the characteristics of being able to combine a thick design with flexibility, can be suitably used for automobile interior materials, miscellaneous goods and small items, clothing, CE (Consumer Electronics) applications, etc. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating and explaining the positional relationship between a resin portion A, a discontinuous resin portion B, and a napped portion of an artificial leather according to the present invention. [Diagram 2] FIG. 2 is a schematic top view illustrating and explaining an embodiment of the arrangement of discontinuous resin portions B. As shown in FIG. [Diagram 3] FIG. 3 is a schematic top view illustrating a formation pattern of the resin portion A of the artificial leather according to the first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The artificial leather of the present invention comprises a fiber-entangled body containing, as a component, a nonwoven fabric composed of ultrafine fibers whose main component is a thermoplastic resin and whose average single fiber diameter is 1.0 μm or more and 10.0 μm or less, and a polymer elastomer, one surface of the artificial leather having nap, a resin portion A and a discontinuous resin portion B are formed on the napped surface, at least a portion of the resin portion A is laminated on the discontinuous resin portion B, and further satisfies the following requirements (1) to (4). (1) The resin portion A is a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin, and the discontinuous resin portion B is a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin. (2) The area ratio of the resin portion A and the discontinuous resin portion B to the surface having nap is 50% or more and 95% or less. (3) The length a (mm) of the resin portion A and the length b (mm) of the discontinuous resin portion B satisfy the following formula 1. 1 (4) At least a part of the resin portion A is in direct contact with the surface having the nap, and in that part, the resin portion A covers the nap.

[0027] The components are described in detail below, but the present invention is not limited to the scope described below as long as it does not exceed the gist of the present invention, and various modifications are possible without departing from the gist of the present invention.

[0028] [Fiber entanglement] First, the fiber-entangled body according to the present invention contains, as a constituent element, a nonwoven fabric composed of ultrafine fibers having an average single fiber diameter of 1.0 μm or more and 10.0 μm or less, and whose main component is a thermoplastic resin. Note that, in the present invention, "composed mainly of a thermoplastic resin" refers to a state in which the mass ratio of the thermoplastic resin is 90 mass% or more.

[0029] The thermoplastic resin is preferably a polyester-based resin from the viewpoints of abrasion resistance, particularly mechanical strength, heat resistance, etc. In the present invention, the term "polyester-based resin" refers to a resin in which the molar fraction of the polyester unit in the repeating unit is 80 mol % to 100 mol %. Unless otherwise specified, the term "...-based resin" has the same meaning.

[0030] ​Examples of the polyester resin include polyethylene terephthalate, polytrimethylene terephthalate, polytetramethylene terephthalate, polycyclohexylene dimethylene terephthalate, polyethylene-2,6-naphthalenedicarboxylate, and polyethylene-1,2-bis(2-chlorophenoxy)ethane-4,4'-dicarboxylate. Among them, polyethylene terephthalate, which is the most widely used, or a polyester copolymer mainly containing ethylene terephthalate units, i.e., the molar fraction of the ethylene terephthalate units in the repeating units is 50 mol% to 99 mol% is preferably used.

[0031] As the polyester-based resin, a single polyester or two or more different polyesters may be used. When two or more different polyesters are used, the difference in intrinsic viscosity (IV value) of the polyesters used is preferably 0.50 or less, and more preferably 0.30 or less, from the viewpoint of compatibility of the two or more components.

[0032] In the present invention, the intrinsic viscosity is calculated by the following method. (1) Dissolve 0.8 g of the sample polymer in 10 mL of orthochlorophenol. (2) Relative viscosity η measured using an Ostwald viscometer at a temperature of 25°C r Calculate using the formula below and round off to the third decimal place. η r =η / η0=(t×d) / (t0×d0) Intrinsic viscosity (IV value) = 0.0242 η r +0.2634 (Here, η is the viscosity of the polymer solution, η0 is the viscosity of orthochlorophenol, t is the drop time of the solution (sec), and d is the density of the solution (g / cm 3 ), t0 is the fall time of orthochlorophenol (sec), and d0 is the density of orthochlorophenol (g / cm 3 ) respectively.

[0033] In the present invention, the thermoplastic resin may contain carbon black. Carbon black is easy to obtain a black pigment with a fine particle size and has excellent dispersibility in polymers. Therefore, by containing carbon black, an artificial leather having excellent deep and uniform color development, as well as excellent color fastness, abrasion resistance, and strength can be obtained.

[0034] In addition to carbon black, inorganic particles such as titanium oxide particles, lubricants, heat stabilizers, ultraviolet absorbers, conductive agents, heat storage agents, antibacterial agents, and the like can be added to the polyester resin according to various purposes, within the scope of not impairing the object of the present invention.

[0035] Next, the ultrafine fibers according to the present invention are mainly composed of the above-mentioned thermoplastic resin and have an average single fiber diameter of 1.0 μm to 10.0 μm. From the viewpoint of processing operability, the cross-sectional shape of the ultrafine fibers is preferably a round cross-section, but cross-sectional shapes of irregular cross-sections such as an ellipse, a flattened or triangular shape, a sector shape, a cross shape, a hollow shape, a Y shape, a T shape, or a U shape can also be adopted.

[0036] The average single fiber diameter of the ultrafine fibers is 1.0 μm or more and 10.0 μm or less. By setting the average single fiber diameter of the ultrafine fibers to 1.0 μm or more, preferably 1.5 μm or more, the artificial leather has excellent color development after dyeing, light fastness and friction fastness, and stability during spinning. On the other hand, by setting the average single fiber diameter of the ultrafine fibers to 10.0 μm or less, preferably 6.0 μm or less, more preferably 4.5 μm or less, the artificial leather has a dense feel, is soft, and has excellent surface quality.

[0037] In the present invention, the average single fiber diameter of ultrafine fibers is calculated by taking a scanning electron microscope (SEM) photograph of the cross section of the artificial leather, randomly selecting 10 ultrafine fibers that are circular or elliptical and close to circular, measuring the single fiber diameter, calculating the arithmetic average value of the 10 fibers, and rounding off to one decimal place. However, when ultrafine fibers with a modified cross section are used, the diameter of the single fiber is calculated by first measuring the cross-sectional area of ​​the single fiber and calculating the diameter (circle equivalent diameter) when the cross section is regarded as a circle.

[0038] The fiber-entangled body according to the present invention contains, as a component, a nonwoven fabric made of the ultrafine fibers. In the present invention, the term "fiber-entangled body containing a nonwoven fabric as a component" refers to an embodiment in which the fiber-entangled body is a nonwoven fabric, or an embodiment in which a nonwoven fabric and a woven or knitted fabric are entangled and integrated, as described below. The fiber-entangled body containing a nonwoven fabric as a component can provide a uniform and elegant appearance and texture when the surface is raised.

[0039] The nonwoven fabric generally has a long fiber nonwoven fabric mainly composed of filaments and a short fiber nonwoven fabric mainly composed of fibers having a fiber length of 100 mm or less. When the fibrous substrate is a long fiber nonwoven fabric, it is preferable because it produces an artificial leather with excellent strength. On the other hand, when the fibrous substrate is a short fiber nonwoven fabric, it is possible to increase the fibers oriented in the thickness direction of the artificial leather compared to the case of a long fiber nonwoven fabric, and therefore, when the surface is raised, it produces an artificial leather with a high density on the surface.

[0040] In the artificial leather of the present invention, it is also preferable that the fiber-entangled body further includes a woven or knitted fabric, and the woven or knitted fabric is integrated and entangled with the nonwoven fabric. In this way, the artificial leather has improved strength and shape stability. Examples of the "further including a woven or knitted fabric" include those in which the layers are laminated in the order of nonwoven fabric / woven or knitted fabric, those in which the layers are laminated in the order of nonwoven fabric / woven or knitted fabric / nonwoven fabric, and those in which the layers are laminated in the order of nonwoven fabric / woven or knitted fabric / woven or knitted fabric / nonwoven fabric. Among these, from the viewpoint of the surface quality and strength of the artificial leather, it is more preferable that the layers are laminated in the order of nonwoven fabric / woven or knitted fabric.

[0041] In the present invention, the woven or knitted fabric is a general term for woven fabrics and knitted fabrics. When the woven or knitted fabric is a woven fabric, examples of the weave structure include plain weave, twill weave, satin weave, etc., and when the woven or knitted fabric is a knitted fabric, examples of the knit structure include weft knits such as "plain knit, rib knit, pearl knit" and warp knits such as "single denbigh knit, single atlas knit, single cord knit, double denbigh knit, double atlas knit, double cord knit, half tricot knit". Among them, when the woven fabric has a plain weave structure, it is particularly preferable because it can be used as an artificial leather with excellent strength.

[0042] As the type of fiber constituting the woven or knitted fabric, it is preferable to use filament yarn, spun yarn, a mixed composite yarn of filament yarn and spun yarn, etc., and from the viewpoint of abrasion resistance, particularly mechanical strength, etc., it is more preferable to use a multifilament made of a polyester-based resin or a polyamide-based resin.

[0043] The average single fiber diameter of the fibers constituting the woven or knitted fabric is preferably 1.0 μm or more and 50 μm or less. By making the average single fiber diameter of the fibers constituting the woven or knitted fabric preferably 50.0 μm or less, more preferably 15.0 μm or less, and even more preferably 13.0 μm or less, not only can the artificial leather have excellent flexibility, but also, even if the fibers of the woven or knitted fabric are exposed on the surface of the artificial leather, the hue difference with the ultrafine fibers containing the pigment after dyeing is small, so that the artificial leather does not lose the uniformity of the hue of the surface. On the other hand, by making the average single fiber diameter preferably 1.0 μm or more, more preferably 8.0 μm or more, and even more preferably 9.0 μm or more, the shape stability of the product, at least a part of which is the artificial leather of the present invention, is improved.

[0044] In the present invention, the average single fiber diameter of the fibers constituting the woven or knitted fabric is calculated by taking a scanning electron microscope (SEM) photograph of the cross section of the artificial leather, randomly selecting 10 fibers constituting the woven or knitted fabric, measuring the single fiber diameter of the selected fibers, calculating the arithmetic average value of the 10 fibers, and rounding off to one decimal place.

[0045] When the fibers constituting the woven or knitted fabric are multifilament, the total fineness of the multifilament is measured according to "8.3.1 Correct fineness b) Method B (simplified method)" of "8.3 Fineness" of JIS L1013:2010 "Testing methods for chemical fiber filament yarns," and the total fineness is preferably 30 dtex or more and 170 dtex or less.

[0046] The total fineness of the multifilaments is 170 dtex or less, which results in an artificial leather with excellent flexibility. On the other hand, the total fineness of the multifilaments is 30 dtex or more, which not only improves the shape stability of the product at least a part of which is the artificial leather of the present invention, but also makes it difficult for the fibers constituting the woven or knitted fabric to be exposed on the surface of the artificial leather when the nonwoven fabric and the woven or knitted fabric are entangled and integrated by needle punching or the like, which results in an artificial leather with excellent design, which is preferable. In this case, it is preferable that the total fineness of the warp and weft multifilaments is the same.

[0047] Furthermore, the twist number of the yarns constituting the woven or knitted fabric is preferably 1000 T / m or more and 4000 T / m or less. By having the twist number of 4000 T / m or less, more preferably 3500 T / m or less, and even more preferably 3000 T / m or less, an artificial leather with excellent flexibility is obtained, and by having the twist number of 1000 T / m or more, more preferably 1500 T / m or more, and even more preferably 2000 T / m or more, damage to the fibers constituting the woven or knitted fabric can be prevented when the nonwoven fabric and the woven or knitted fabric are entangled and integrated by needle punching or the like, and an artificial leather with excellent mechanical strength is obtained, which is preferable.

[0048] [Polymer elastomer] Next, the artificial leather of the present invention contains a polymeric elastomer. Here, in the present invention, "containing a polymeric elastomer" refers to a state in which a polymeric elastomer is contained in the central 40% of the artificial leather, excluding 30% of the thickness direction from both surfaces excluding the napped parts, and can be determined by the following procedures (1) to (7). (1) With the napped surface of the artificial leather laid down using a lint brush or the like, a thin section 1 mm thick is prepared in the cross-sectional direction of the artificial leather from a randomly selected position on the artificial leather. (2) Using a scanning electron microscope (SEM, for example, Keyence Corporation's VHX-D500 / D510), observe the cross section of the thin section of (1), excluding 30% of the cross section from both surfaces in the thickness direction, and the remaining central 40%. (3) In the SEM images taken, the presence or absence of any substances other than the fibers that make up the fiber-entangled structure is confirmed. (4) If there are any substances other than the fibers that make up the fiber-entangled body, remove them by peeling off the resin parts A and B applied to the surface layer of the artificial leather. (5) Remove 30% of the thickness of both surfaces of the artificial leather, excluding the napped portions, by polishing or other means, leaving only the central 40%. (6) The test piece (5) is dissolved in N,N-dimethylformamide (DMF) and hexafluoro-2-propanol (HFIP), and the presence or absence of the polymer elastomer is confirmed by performing a composition analysis of the solute in the DMF solution after dissolution and the insoluble matter in HFIP. In the composition analysis, the presence or absence of the polymer elastomer is confirmed by, for example, infrared spectroscopy (IR) or the like. (7) When the structure of a polymeric elastomer described below is confirmed in either the solute in the DMF solution or the insoluble matter in HFIP, it is deemed to contain a polymeric elastomer.

[0049] Since this polymeric elastomer is a binder that holds the ultrafine fibers that make up the artificial leather, in consideration of the soft feel of the artificial leather of the present invention, it is preferable to use polyurethane as the main component of the polymeric elastomer used. Note that, in the present invention, "main component" means that the mass of polyurethane is more than 50% by mass of the total mass of the polymeric elastomer.

[0050] In the present invention, the polyurethane resin preferably used as the polymeric elastomer can be either an organic solvent-based polyurethane resin used in a state dissolved in an organic solvent, or a water-dispersed polyurethane resin used in a state dispersed in water. Here, in the present invention, the water-dispersed polyurethane resin refers to a polyurethane resin having a hydrophilic group and a solubility in DMF of less than 40g / 100g-DMF (less than 40g of the polyurethane can be dissolved in 100g of DMF). Conversely, a polyurethane resin having a solubility in DMF of 40g / 100g-DMF or more (more than 40g of the polyurethane can be dissolved in 100g of DMF) is considered to be an organic solvent-based polyurethane resin.

[0051] In addition, examples of polyurethane resins that can be preferably used in the present invention include polyurethane resins obtained by reacting a polymer diol, an organic diisocyanate, and a chain extender. Each of these will be described below.

[0052] <1> Polymer Diol As the above-mentioned polymer diol, for example, polycarbonate-based diol, polyester-based diol, polyether-based diol, silicone-based diol and fluorine-based diol can be adopted, and copolymers of these can also be used. Among them, from the viewpoint of hydrolysis resistance and abrasion resistance, it is more preferable to use polycarbonate-based diol.

[0053] When the molecular weight of the polyurethane elastomer is constant, the number average molecular weight of the polymer diol is preferably in the range of 500 to 4000. By setting the number average molecular weight to preferably 500 or more, more preferably 1500 or more, it is possible to prevent the artificial leather from becoming hard. In addition, by setting the number average molecular weight to preferably 4000 or less, more preferably 3000 or less, it is possible to maintain the strength of the polyurethane resin.

[0054] <2> Organic Diisocyanates Examples of organic diisocyanates preferably used in the present invention include aliphatic diisocyanates such as hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, and xylylene diisocyanate, and aromatic diisocyanates such as diphenylmethane diisocyanate and tolylene diisocyanate, and these can also be used in combination.

[0055] <3> Chain extender The chain extender preferably used in the present invention is preferably an amine-based chain extender such as ethylenediamine or methylenebisaniline, or a diol-based chain extender such as ethylene glycol. Also, a polyamine obtained by reacting a polyisocyanate with water can be used as the chain extender.

[0056] <4> Other Ingredients In the present invention, the polyurethane resin preferably used as the polymeric elastomer can be used in combination with a crosslinking agent for the purpose of improving water resistance, abrasion resistance, hydrolysis resistance, etc. The crosslinking agent may be an external crosslinking agent added to the polyurethane resin as a third component, or an internal crosslinking agent that introduces reactive points that will become a crosslinked structure in advance into the molecular structure of the polyurethane resin can also be used. The internal crosslinking agent is more preferable from the viewpoint of reducing the decrease in flexibility because it can form uniform crosslinking points in the molecular structure of the polyurethane resin.

[0057] In addition, the polymer elastomer may contain various additives depending on the purpose, for example, flame retardants such as "phosphorus-based, halogen-based, and inorganic" antioxidants, such as "phenol-based, sulfur-based, and phosphorus-based" antioxidants, ultraviolet absorbers such as "benzotriazole-based, benzophenone-based, salicylate-based, cyanoacrylate-based, and oxalic acid anilide-based" light stabilizers such as "hindered amine-based and benzoate-based" hydrolysis-resistant stabilizers such as polycarbodiimide, plasticizers, antistatic agents, surfactants, coagulation adjusters, carbon black, and dyes.

[0058] In general, the content of the polymer elastomer in the artificial leather can be appropriately adjusted in consideration of the type of polymer elastomer used, the manufacturing method of the polymer elastomer, and the texture and physical properties, but in the present invention, the content of the polymer elastomer is preferably 10% by mass or more and 60% by mass or less with respect to the mass of the fiber-entangled material. By making the content of the polymer elastomer 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, the bond between the fibers by the polymer elastomer can be strengthened, and the abrasion resistance of the artificial leather can be improved. On the other hand, by making the content of the polymer elastomer 60% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less, the artificial leather can be made more flexible and have a soft texture.

[0059] In the present invention, the content (mass %) of the polymer elastomer in the artificial leather is a value measured and calculated by the following procedure. (1) Randomly take three test pieces measuring 10 cm x 10 cm from the artificial leather. (2) The layer consisting of resin portion A and discontinuous resin portion B applied to the surface of the artificial leather is removed by peeling or the like. (3) Remove 30% of the thickness of both surfaces of the artificial leather, excluding the napped portions, by polishing or other methods, leaving only the central 40%. (4) In the method (7) for confirming whether or not the polymer elastomer is contained, if the structure of the polymer elastomer is confirmed on the solute side in the DMF solution, carry out step (5), and if the structure of the polymer elastomer is confirmed on the insoluble side of the HFIP, carry out step (6) to calculate the content of the polymer elastomer. If the structure of the polymer elastomer is confirmed in both DMF and HFIP, the larger of the values ​​calculated in steps (5) and (6) is used as the content of the polymer elastomer. (5) The test piece is immersed in DMF and dried at 25° C. for 24 hours. The mass ratio of the test piece before and after dissolution is calculated using the following formula, and the arithmetic average value (%) of the three test pieces is rounded off to the first decimal place to calculate the content of the polymer elastomer. (Sample mass before dissolution (g) - Sample mass after dissolution and drying (g)) / (Sample mass before dissolution (g)) x 100 (6) The test piece is immersed in HFIP and dried at 25° C. for 24 hours. The mass ratio of the test piece before and after dissolution is calculated using the following formula, and the arithmetic average value (%) of the three test pieces is rounded off to the first decimal place to calculate the content of the polymer elastomer. (Sample mass after dissolution (g)) / (Sample mass before dissolution (g)) x 100.

[0060] [Artificial leather] The artificial leather of the present invention includes the fiber-entangled body and the polymeric elastomer. The artificial leather of the present invention has one surface with nap. Here, in the present invention, whether or not a surface has "napped" is determined by observing the surface as follows. (1) With the napped surface of the artificial leather raised using a lint brush or similar tool, a thin section 1 mm thick is prepared in the cross-sectional direction perpendicular to the longitudinal direction of the artificial leather from a randomly selected position on the artificial leather. (2) Using a scanning electron microscope (SEM, for example, Keyence Corporation's "VHX-D500 / D510 type"), observe the cross section of the artificial leather at 120x magnification in a position where the observation field does not include resin portion A and discontinuous resin portion B described below. (3) In the cross section, a layer consisting only of fibers oriented in the thickness direction is defined as the napped portion, and the length from the intersection of the fibers oriented in the thickness direction and the fibers oriented in the surface direction of the artificial leather to the tip of the nap is measured as the nap length (μm). (4) In a 3,000 μm wide area of ​​the SEM image, standing fibers of 50 μm or more in length are confirmed from the fiber-entangled base material, and if 10 or more are confirmed, it is judged to be "has standing fibers."

[0061] In addition, the artificial leather of the present invention has a napped surface on one surface, but the other surface may also have napped surfaces. In the case where both surfaces have napped surfaces, it goes without saying that the resin part A and the discontinuous resin part B described below may be formed only on one surface or on both surfaces. However, when the resin part A and the discontinuous resin part B described below are formed on the napped surfaces on both surfaces, it is sufficient that at least one surface satisfies the above requirements (1) to (4) that the artificial leather must satisfy.

[0062] Next, the artificial leather of the present invention has a resin portion A and a discontinuous resin portion B formed on the surface having the nap. The formation of these two discontinuous resin portions on the surface having the nap is important for obtaining an artificial leather excellent in design and abrasion resistance. This will be described in more detail below.

[0063] <1> Resin part A First, the resin portion A is formed on the surface having the nap. At least a part of the resin portion A according to the present invention is in direct contact with the surface having the nap, and the resin portion A covers the nap in that part. At least a part of the resin portion A is laminated on the discontinuous resin portion B described later. That is, the resin portion A is in direct contact with the surface having the nap in a certain part, and the resin portion A covers the nap in that part, and is laminated on the discontinuous resin portion B in another part. With this configuration, the resin portion A is in direct contact with the surface having the nap, and the nap is excellent in abrasion resistance, and the resin portion A is less likely to directly penetrate into the fiber substrate, resulting in an artificial leather with excellent flexibility. In the present invention, "the resin portion A covers the nap" refers to a state in which at least 50% or more of the nap from the tip to the base is surrounded (embedded) by the resin portion A.

[0064] The resin portion A is a resin containing at least one selected from the group consisting of styrene butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin. Among them, polyurethane resin is preferable from the viewpoint of flexibility and abrasion resistance. The natural resin referred to here is a resin derived from plants such as rosin, lacquer, amber, and latex, or a resin derived from animals such as glue.

[0065] When the resin portion A is a polyurethane resin, the polyurethane may be an organic solvent-based polyurethane that is used in a dissolved state in an organic solvent, or a water-dispersed polyurethane that is used in a dispersed state in water, and either of these may be used in the present invention.

[0066] As the polyurethane preferably used in the present invention, a polyurethane having a structure obtained by appropriately reacting a polyol, a polyisocyanate, and a chain extender can be used.

[0067] Examples of polyols that can be used include polycarbonate-based diols, polyester-based diols, polyether-based diols, silicone-based diols, and fluorine-based diols, as well as copolymers of combinations thereof. Among them, polycarbonate-based diols and polyester-based diols are preferably used from the viewpoint of light resistance. Furthermore, polycarbonate-based diols are preferably used from the viewpoints of hydrolysis resistance and heat resistance, but in the adhesive layer of the present invention, polyether-based diols or polyester-based diols are preferably used from the viewpoint of adhesion to the surface of the fiber structure.

[0068] In addition, at the position where resin portion A is laminated on discontinuous resin portion B described later, the thickness of said resin portion A is preferably 5 μm or more and 200 μm or less. When the thickness is preferably 5 μm or more, more preferably 10 μm or more, an artificial leather having a clear design is obtained. Moreover, when the thickness is preferably 200 μm or less, more preferably 150 μm or less, an artificial leather having excellent abrasion resistance and flexibility is obtained.

[0069] The thicknesses mentioned above are values ​​measured and calculated by the following method. (1) Using scissors or a cutter, take ten test pieces measuring 3.0 cm x 0.1 cm at random from the artificial leather, making sure to include the area where resin part A is laminated on top of discontinuous resin part B. (2) A scanning electron microscope (SEM) photograph of a cross section at a position where resin portion A is laminated on discontinuous resin portion B is taken. (3) The thickness of resin portion A is measured at 10 points at 10 μm intervals where resin portion A is laminated on discontinuous resin portion B. Specifically, as shown in Figs. 1(A) to (D) as examples, the difference between the highest position in discontinuous resin portion B in the SEM photograph and the highest position in resin portion A is measured. The arithmetic mean value of the thicknesses measured at the 10 points is regarded as the representative value of resin portion A in that image. (4) (2) and (3) are performed on all 10 test pieces, and the arithmetic mean value of the thicknesses of resin part A measured and calculated from them, rounded off to two decimal places, shall be the thickness of resin part A at the position where resin part A is located above discontinuous resin part B.

[0070] Furthermore, it is preferable that the resin filling rate of the resin portion A is 95% or more and less than 100%. When the resin filling rate of the resin portion A is 95% or more, the abrasion resistance of the resin portion A can be ensured. Also, when the resin filling rate of the resin portion A is less than 100%, an artificial leather that combines flexibility and texture while ensuring the abrasion resistance of the resin portion can be formed.

[0071] The resin filling rate is a value measured and calculated by the following method. (1) Using scissors or a cutter, take ten test pieces measuring 3.0 cm x 0.1 cm at random from the artificial leather, making sure to include the area where resin part A is laminated on top of discontinuous resin part B. (2) A scanning electron microscope (SEM) photograph of a cross section at a position where resin portion A is laminated on discontinuous resin portion B is taken. (3) Calculate the ratio of the total area of ​​resin part A using image analysis software (for example, "ImageJ", an image analysis software developed by the National Institutes of Health (NIH) in the United States). In this case, when using the above-mentioned "ImageJ", set the threshold value between the filled part and the void part of resin part A to 100 (set so that pixel values ​​0 to 99 are white and 100 to 255 are black), and when using other software, set the threshold value to the same value and perform the calculation by binarization. In addition, in calculating the area ratio of the resin filling rate, if a part that is clearly not a void part is judged from the SEM image and binarized as if it were a void part, edit the image of that part manually so that that part is calculated as resin part A. (4) The arithmetic mean value of the resin filling rate of resin part A measured from the SEM images taken at 10 locations is rounded off to two decimal places to determine the resin filling rate of resin part A.

[0072] In the present invention, the resin used in the resin portion A may contain, to the extent that the effects of the present invention are not impaired, elastomer resins such as polyester, polyamide and polyolefin, acrylic resins and ethylene-vinyl acetate resins, etc. Furthermore, these resins may contain various additives, for example, pigments such as carbon black, phosphorus-, halogen- and inorganic-based flame retardants, phenol-, sulfur- and phosphorus-based antioxidants, hindered amine and benzoate-based light stabilizers, hydrolysis-resistant stabilizers such as polycarbodiimide, plasticizers, antistatic agents, surfactants, coagulation regulators, dyes, etc.

[0073] <2> Discontinuous resin part B First, the discontinuous resin part B is formed on the surface having the nap. In the present invention, this "discontinuous resin part B is formed on the surface having the nap" refers to the surface having the nap being formed so that there are parts where the resin part B does not exist, and refers to a state in which each resin part B is formed independently, such as a checkered pattern as shown in FIG. 2(A), a pattern in which random circles are arranged as shown in FIG. 2(B), a logo as shown in FIG. 2(C), and a random island pattern as shown in FIG. 2(D), or a state in which only the vertices of the constituent units are connected and most of the constituent units are not in contact with each other, such as a checkered pattern as shown in FIG. 2(E) and a houndstooth check as shown in FIG. 2(F). Note that in FIG. 2, the resin part A is not shown in order to explain the discontinuous resin part B.

[0074] The discontinuous resin portion B is a resin containing at least one selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin. Among them, polyurethane resin is preferable from the viewpoints of flexibility and abrasion resistance.

[0075] When the discontinuous resin portion B is a polyurethane resin, the polyurethane may be an organic solvent-based polyurethane that is used in a dissolved state in an organic solvent, or a water-dispersed polyurethane that is used in a dispersed state in water, and either of these may be used in the present invention.

[0076] As the polyurethane preferably used in the present invention, a polyurethane having a structure obtained by appropriately reacting a polyol, a polyisocyanate, and a chain extender can be used.

[0077] Examples of polyols that can be used include polycarbonate-based diols, polyester-based diols, polyether-based diols, silicone-based diols, and fluorine-based diols, as well as copolymers of combinations thereof. Among them, polycarbonate-based diols and polyester-based diols are preferably used from the viewpoint of light resistance. Furthermore, polycarbonate-based diols are preferably used from the viewpoints of hydrolysis resistance and heat resistance, but in the adhesive layer of the present invention, polyether-based diols or polyester-based diols are preferably used from the viewpoint of adhesion to the surface of the fiber structure.

[0078] In the present invention, the resin used in the discontinuous resin portion B may contain, to the extent that the effects of the present invention are not impaired, elastomer resins such as polyester, polyamide and polyolefin, acrylic resins and ethylene-vinyl acetate resins, etc. Furthermore, these resins may contain various additives, for example, pigments such as carbon black, phosphorus-, halogen- and inorganic-based flame retardants, phenol-, sulfur- and phosphorus-based antioxidants, hindered amine and benzoate-based light stabilizers, hydrolysis-resistant stabilizers such as polycarbodiimide, plasticizers, antistatic agents, surfactants, coagulation regulators, dyes, etc.

[0079] <3> Relationship between resin part A and discontinuous resin part B In the artificial leather of the present invention, the area ratio of the resin part A and the discontinuous resin part B to the surface having nap is 50% or more and 95% or less. By making the above area ratio 50% or more, preferably 60% or more, it is possible to obtain a design that is excellent in design and abrasion resistance and is resistant to friction. In addition, by making the above area ratio 95% or less, preferably 90% or less, it is possible to maintain the flexibility unique to artificial leather.

[0080] The above area ratio is to be measured and calculated by the following method. (1) Using scissors or a cutter, take ten test pieces measuring 2.0 cm x 2.0 cm at random from the artificial leather, making sure to include the area where resin part A is laminated on top of discontinuous resin part B. (2) A scanning electron microscope (SEM) photograph is taken of the surface at the position where resin portion A is laminated on discontinuous resin portion B. (3) Calculate the ratio of the total area of ​​resin parts A and B using image analysis software (for example, "ImageJ", an image analysis software developed by the National Institutes of Health (NIH) in the United States). In this case, when using the above-mentioned "ImageJ", set the threshold value between the resin part and the non-plume part to 100 (set so that pixel values ​​0 to 99 are white and 100 to 255 are black), and when using other software, set the threshold value to the same value and perform the calculation by binarization. In addition, in calculating the area ratio, if a material that is not resin parts A and B is judged from the SEM image to have been binarized as a resin part, manually edit the image for that part and calculate that part as something other than a resin part.

[0081] Next, in the artificial leather of the present invention, the length a (mm) of the resin portion A and the length b (mm) of the discontinuous resin portion B satisfy the following formula 1. 1 By making a / b larger than 1, preferably 5 or more, resin portion A embeds resin portion B and also embeds nap, resulting in an artificial leather having wear resistance even with a thick resin portion A. On the other hand, by making a / b 50 or less, preferably 40 or less, flexibility characteristic of artificial leather can be ensured.

[0082] ​As long as the above formula 1 is satisfied, first, the length a (mm) of the resin portion A is preferably 0.10 mm or more and 50.00 mm or less. When the length a of the resin portion A is preferably 0.10 mm or more, more preferably 0.20 mm or more, the artificial leather has a resin portion with excellent abrasion resistance and a thickness. When the length a of the resin portion A is preferably 50.00 mm or less, more preferably 40.00 mm, the artificial leather has both the abrasion resistance of the resin portion A and the flexibility peculiar to artificial leather.

[0083] Next, the length b (mm) of the discontinuous resin portion B is preferably 0.05 mm or more and 2.00 mm or less. By making the length b of the resin portion B preferably 0.05 mm or more, more preferably 0.08 mm or more, even if a thick resin layer is placed as the resin portion A, the nap is not exposed from the resin portion, and a uniform surface can be obtained. Furthermore, by making the length b of the resin portion B 2.00 mm or less, preferably 1.50 mm, it is possible to obtain an artificial leather that combines the abrasion resistance of the resin portion A with the flexibility peculiar to artificial leather.

[0084] The length a (mm) of the resin portion A, the length b (mm) of the discontinuous resin portion B, and the ratio a / b of the length a (mm) of the resin portion A to the length b (mm) of the discontinuous resin portion B shall be values ​​measured and calculated by the following method. (1) While making sure to include the position where resin part A is laminated on discontinuous resin part B, set one arbitrary direction as 0°, and randomly take 10 cross-sectional samples of 7.0 cm x 0.1 cm from each direction using scissors or a cutter at 4 directions of 0°, 30°, 60°, and 90°. However, if there is a continuous resin part in one direction as in Figure 2(G), take the test pieces so that the short side (width of the line) that can be considered discontinuous can be observed. (2) A scanning electron microscope (SEM) photograph of a cross section at a position where resin portion A is laminated on discontinuous resin portion B is taken. (3) Measure the length a (mm) of resin portion A and b (mm) of discontinuous resin portion B from the SEM image. This length is the left-right distance of each individual resin portion A or discontinuous resin portion B in the SEM image, as exemplified in Figure 1, and if there is variation in this length, that is, if multiple resin portions A or discontinuous resin portions B are identified and their lengths differ, measure the lengths a and b that can be identified from the image at several points, and use the arithmetic average value as the representative value for that image. (4) The arithmetic mean values ​​of lengths a and b measured from the 10 SEM images taken, rounded off to two decimal places, shall be the length a (mm) of resin part A and the length b (mm) of resin part B. (5) The value of a / b is calculated from the lengths a and b measured in the SEM images taken at 10 points, and the average value is rounded off to two decimal places.

[0085] In the artificial leather of the present invention, the weight of the artificial leather is 150 g / m 2 More than 600g / m 2 The weight of the artificial leather is preferably 150 g / m 2 More preferably, 200 g / m 2 This makes it possible to produce an artificial leather that combines a thick design, abrasion resistance, and strength as a fabric. 2 Less than 550 g / m 2 This results in an artificial leather with excellent flexibility.

[0086] In the artificial leather of the present invention, the abrasion loss after a Martindale abrasion test (12.0 kPa x 10,000 times) on the napped surface (hereinafter, sometimes simply referred to as "abrasion loss") is preferably 15 mg or less. By keeping the abrasion loss at 15 mg or less, more preferably at 13 mg or less, the design of the resin portion A can be maintained clear without being torn even after long-term use.

[0087] The wear loss shall be measured and calculated by the following method. (1) Using scissors or a cutter, randomly select four test pieces with a diameter of 3.8 cm from the test cloth, making sure to include the area where resin part A is laminated on top of discontinuous resin part B. (2) Measure the mass (mg) of each test cloth before the abrasion test. (3) Conduct an abrasion test in accordance with "8.19.5 E Method (Martindale Method)" of "8.19 Abrasion resistance and discoloration due to friction" of JIS L1096:2010 "Test methods for woven and knitted fabrics" with a pressure load of 12.0 kPa and a number of frictions of 10,000. (4) After the abrasion test, the mass (mg) of the test cloth is measured, and the difference in mass of the test cloth before and after the abrasion test is regarded as the abrasion loss of the test cloth. (5) Repeat (2) to (4) for each test piece to calculate the abrasion loss of the test piece, and calculate the arithmetic mean value (mg) of the calculated loss, rounded off to the first decimal place.

[0088] The artificial leather of the present invention preferably has a bending resistance of 10 mm or more and 60 mm or less. When the bending resistance is 10 mm or more, preferably 15 mm or more, the artificial leather has high shape stability during sewing or lamination. When the bending resistance is 60 mm or less, more preferably 55 mm or less, the artificial leather has both a soft feel and designability.

[0089] The bending resistance of the artificial leather is measured and calculated by the following method. (1) Using scissors or a cutter, randomly select three test pieces measuring 2 cm x 15 cm, making sure to include the area where resin part A is laminated on top of discontinuous resin part B. (2) For each test cloth, a cantilever with an inclination of 41.5° is used to measure the bending resistance of the surface coated with resin parts A and B as the front surface. If both surfaces are coated with resin parts A and B, both the front and back surfaces are measured, and the average value of both surfaces is regarded as the bending resistance of the test cloth. (3) Calculate the arithmetic mean value of the stiffness (cm) measured for each test cloth, rounded off to the first decimal place.

[0090] [Manufacturing method of artificial leather] A preferred embodiment of the method for producing the artificial leather of the present invention is (a) forming a sheet-like material including a fiber-entangled body containing, as a component, a nonwoven fabric composed of ultrafine fibers having an average single fiber diameter of 1.0 μm or more and 10.0 μm or less, and a polymeric elastomer; (b) grinding one surface of the sheet-like material to form a napped sheet; (c) discontinuously placing a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin on the napped surface of the napped sheet to form a discontinuous resin portion B, and further placing a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, and natural resin and having a viscosity of 1000 mPa·s or more and 4000 mPa or less to form a resin portion A; Each of the above steps will be described in more detail below.

[0091] (a) forming a sheet-like material First, in this process, a sheet-like material is formed, which includes a fiber-entangled body containing, as a component, a nonwoven fabric composed of ultrafine fibers having an average single fiber diameter of 1.0 μm or more and 10.0 μm or less, and a polymer elastomer.

[0092] In order to form a nonwoven fabric composed of ultrafine fibers having an average single fiber diameter of 1.0 μm or more and 10.0 μm or less, which is one of the components of this fiber-entangled body, there can be mentioned a method of directly spinning ultrafine fibers having the above-mentioned average single fiber diameter into a nonwoven fabric, a method of first forming a nonwoven fabric from ultrafine fiber-developing fibers, and then developing ultrafine fibers from the nonwoven fabric, etc. Among them, from the viewpoint of excellent operability and ability to obtain uniform ultrafine fibers, it is preferable to adopt the method of first forming a nonwoven fabric using ultrafine fiber-developing fibers.

[0093] As the ultrafine fiber-producing fiber, an islands-in-sea type composite fiber is used in which thermoplastic resins having different solvent solubilities are used as a sea part (easily soluble polymer) and an island part (slightly soluble polymer), and the sea part is dissolved and removed using a solvent or the like to convert the island parts into ultrafine fibers. The use of islands-in-sea type composite fiber is preferred from the viewpoint of the soft feel and surface quality of the artificial leather, since it is possible to provide appropriate gaps between the island parts, i.e., between the ultrafine fibers inside the fiber bundle, when removing the sea part.

[0094] As a method for spinning ultrafine fiber-producing fibers having an islands-in-sea type composite structure, a method using a polymer mutual alignment body in which the sea part and the island part are mutually aligned and spun using a spinneret for islands-in-sea type composite fibers is preferred from the viewpoint of obtaining ultrafine fibers with uniform single fiber fineness.

[0095] As the sea component of the islands-in-sea type composite fiber, polyethylene, polypropylene, polystyrene, copolymer polyesters copolymerized with sodium sulfoisophthalic acid or polyethylene glycol, and polylactic acid can be used, but from the viewpoints of spinnability, ease of elution, etc., polystyrene and copolymer polyesters are preferably used.

[0096] In the method for producing the artificial leather of the present invention, it is preferable to use islands-in-sea type composite fibers in which the strength of the island components is 2.0 cN / dtex or more. By making the strength of the island components 2.0 cN / dtex or more, more preferably 2.3 cN / dtex or more, and further preferably 2.8 cN / dtex or more, the abrasion resistance of the artificial leather can be improved and the decrease in friction fastness due to the falling off of fibers can be suppressed.

[0097] In the present invention, the strength of the island components of the islands-in-sea type composite fiber is calculated by the following method. (1) Ten islands-in-the-sea composite fibers, each 20 cm long, are bundled together. (2) After dissolving and removing the sea component from the sample (1), air-dry it. (3) In accordance with JIS L1013:2010 "Test methods for chemical fiber filament yarn", "8.5 Tensile strength and elongation", "8.5.1 Standard time test", the test shall be carried out 10 times under the conditions of a grip length of 5 cm, a pulling speed of 5 cm / min, and a load of 2 N (N=10). (4) The arithmetic mean value (cN / dtex) of the test results obtained in (3) above, rounded off to one decimal place, shall be the strength of the island components of the islands-in-sea type composite fiber.

[0098] The spun ultrafine fiber-developing fibers are then opened and formed into a fiber web by a cross wrapper or the like, and entangled to obtain a fiber-entangled body containing a nonwoven fabric as a constituent element. Methods that can be used to obtain a fiber-entangled body containing a nonwoven fabric as a constituent element by entangling the fiber web include needle punching and water jet punching.

[0099] As for the form of the nonwoven fabric, either a short fiber nonwoven fabric or a long fiber nonwoven fabric can be used as described above. In the case of a short fiber nonwoven fabric, the number of fibers oriented in the thickness direction of the artificial leather is greater than in the case of a long fiber nonwoven fabric, and it is possible to obtain a high degree of density and a soft texture on the surface of the artificial leather when it is raised.

[0100] When the nonwoven fabric is a staple fiber nonwoven fabric, the islands-in-sea type composite fibers obtained in the step of forming the islands-in-sea type composite fibers are preferably subjected to a crimping process, cut to a predetermined length to obtain raw cotton, and then opened, laminated, and entangled to obtain a staple fiber nonwoven fabric. The crimping process and cutting process can be performed by known methods.

[0101] When using a short fiber nonwoven fabric, the average fiber length of the ultrafine fibers is preferably 25 mm or more and 90 mm or less. By making the fiber length 90 mm or less, more preferably 80 mm or less, and even more preferably 70 mm or less, good quality and soft feel can be obtained. On the other hand, by making the fiber length 25 mm or more, more preferably 35 mm or more, and even more preferably 40 mm or more, an artificial leather with excellent abrasion resistance can be obtained.

[0102] Furthermore, when the fiber-entangled body includes a woven or knitted fabric, the nonwoven fabric obtained by the above-mentioned method and the woven or knitted fabric are laminated and integrated. The nonwoven fabric and the woven or knitted fabric can be integrated by laminating the woven or knitted fabric on one or both sides of the nonwoven fabric, or by sandwiching the woven or knitted fabric between a plurality of nonwoven fabric webs and then entangling the fibers of the nonwoven fabric and the woven or knitted fabric by needle punching, water jet punching, or the like.

[0103] The basis weight of the nonwoven fabric constituting the artificial leather of the present invention is 50 g / m2, as measured according to "6.2 Mass per unit area (ISO method)" of JIS L1913:2010 "General nonwoven fabric testing method". 2 More than 600g / m 2 The weight of the nonwoven fabric is preferably 50 g / m or less. 2 More preferably, 80 g / m 2 By satisfying the above requirements, an artificial leather having a good texture and a sense of fullness can be obtained. 2 Less than 500g / m 2 The above conditions result in a flexible artificial leather with excellent shaping design.

[0104] The apparent density of the nonwoven fabric made of islands-in-the-sea type composite fibers after needle punching or water jet punching is 0.15 g / cm 3 More than 0.45g / cm 3 The apparent density is preferably 0.15 g / cm or less. 3 By setting the density to 0.45 g / cm or more, the artificial leather can have sufficient shape stability and dimensional stability. 3 By setting the thickness to the range below, a sufficient space for imparting the polymeric elastomer can be maintained, and voids in the cross section can be maintained, thereby achieving a soft feel.

[0105] It is also a preferred embodiment that the fiber entanglement is subjected to a heat shrinkage treatment with hot water or steam in order to improve the denseness of the fibers.

[0106] Next, the fiber-entangled body can be impregnated with an aqueous solution of a water-soluble resin and dried to impart the water-soluble resin to the fiber-entangled body. By imparting the water-soluble resin to the fiber-entangled body, the fibers are fixed and the dimensional stability is improved.

[0107] The resulting fibrous base material is then treated with a solvent or solution to form ultrafine fibers having an average single fiber diameter of 1.0 μm or more and 10.0 μm or less.

[0108] The ultrafine fibers can be formed by immersing the above-mentioned fiber entanglement in a solvent or solution to dissolve and remove the sea component of the islands-in-sea type composite fiber.

[0109] As a solvent for dissolving and removing the sea component, when the sea component is polyethylene, polypropylene or polystyrene, an organic solvent such as toluene or trichloroethylene can be used. When the sea component is a copolymer polyester or polylactic acid, an alkaline aqueous solution such as sodium hydroxide can be used. When the sea component is a water-soluble thermoplastic polyvinyl alcohol resin, hot water can be used.

[0110] Then, the fiber-entangled body, which is mainly composed of ultrafine fibers or islands-in-the-sea type composite fibers, is impregnated with a solution of the polymer elastomer and the polymer elastomer is solidified to form a sheet-like material containing the fiber-entangled body and the polymer elastomer. As a method for solidifying the polymer elastomer, there is a method in which the fiber-entangled body is impregnated with a solution of the polymer elastomer, and then the solution is wet-coagulated or dry-coagulated, and these methods can be appropriately selected depending on the type of polymer elastomer used.

[0111] When polyurethane is selected as the polymeric elastomer, the solvent preferably used is N,N'-dimethylformamide, dimethylsulfoxide, etc. Also, a water-dispersed polyurethane liquid in which polyurethane is dispersed in water as an emulsion may be used.

[0112] The polymer elastomer may be applied to the fiber-entangled body before or after ultrafine fibers are generated from the islands-in-sea type composite fibers.

[0113] (b) Step of forming napped sheet Next, one surface of the obtained sheet-like material is ground to form a napped sheet. From the viewpoint of production efficiency, it is also a preferred embodiment to cut the sheet-like material in half in the thickness direction into two sheet-like materials before grinding the surface of the sheet-like material.

[0114] Then, one surface of the sheet-like material (including a half-cut sheet-like material) is ground with sandpaper, a roll sander, etc. to form a napped sheet. As described above, it goes without saying that both surfaces may be ground to form napped surfaces on both sides.

[0115] Before grinding, a lubricant such as a silicone emulsion can be applied to the surface of the artificial leather. Also, by applying an antistatic agent before grinding, grinding powder generated from the sheet-like material during grinding is less likely to accumulate on the sandpaper.

[0116] Furthermore, at this stage of the process, the napped sheet can be dyed, for example, by a flow dyeing process using a jigger dyeing machine or a flow dyeing machine, a dip dyeing process such as a thermosol dyeing process using a continuous dyeing machine, or a printing process on the napped surface using roller printing, screen printing, inkjet printing, sublimation printing, vacuum sublimation printing, etc. Among them, it is preferable to use a flow dyeing machine from the viewpoint of quality and grade, since a soft texture can be obtained. In addition, if necessary, a finishing process can be performed by adding a finishing agent such as a softener or an antistatic agent after dyeing.

[0117] (c) A process for forming discontinuous resin portion B and resin portion A Further, a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin is discontinuously placed on the napped surface of the obtained napped sheet to form a discontinuous resin portion B, and further a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, and natural resin and having a viscosity of 1000 mPa·s or more and 4000 mPa or less is placed on the napped surface to form a resin portion A.

[0118] In the present invention, the method for forming resin portion A and resin portion B is not particularly limited as long as it is a method that can form a resin portion on the surface of a fiber structure, and examples of the method include a screen method using a flat screen or a rotary screen, a gravure coating method, a method of applying a coating such as hand printing and then drying to form a resin layer, and a method of forming a discontinuous resin film on the fiber of a supporting substrate such as release paper, applying an adhesive to the surface of the resin film and bonding it to the surface that will become the fiber structure, and then peeling off the release paper to form a resin layer.

[0119] In the above, the viscosity of the resin when forming resin portion A is 1000 mPa·s or more and 4000 mPa·s or less. By setting the viscosity of resin portion A to preferably 1000 mPa·s or more, more preferably 1100 mPa·s, resin portion A can maintain its texture without soaking into the fiber base material, and an artificial leather with excellent flexibility can be obtained. Furthermore, by setting the viscosity of resin portion B to preferably 4000 mPa·s or less, more preferably 3900 mPa·s, resin portion A can easily assume a structure that allows it to embed the napped portion, and the abrasion resistance of resin portion A can be further improved.

[0120] (d) Other processes Furthermore, in the method for producing an artificial leather of the present invention, if necessary, the artificial leather can be subjected to post-processing such as hole-making such as perforation, embossing, laser processing, Pinsonic processing, and printing.

[0121] [Laminates, interior materials for vehicles, clothing, miscellaneous goods] The artificial leather of the present invention has a soft touch similar to that of natural leather, and excellent strength, quality and denseness, and can be used in a wide range of applications, from furniture, chairs and vehicle interior materials to clothing.

[0122] For example, it is also preferable to form a laminate comprising a fabric layer and / or a foamed resin layer on the surface of the side of the artificial leather where the resin portion A and the discontinuous resin portion B are not formed. The fabric layer referred to here means a layer composed of a nonwoven fabric, a woven fabric, a knitted fabric, etc., and the foamed resin layer means a layer composed of a resin having a porous structure, which is composed of a resin obtained by foaming a general polyurethane-based or olefin-based resin according to desired characteristics, more specifically, a layer composed of a soft polyurethane foam, etc. For example, a laminate comprising a fabric layer is strong and easy to mold. Also, a laminate comprising a foamed resin layer is soft and has excellent cushioning properties.

[0123] The fabric layer and the foamed resin layer may be laminated, for example, by adhering them to the artificial leather with an adhesive or the like, or they may be laminated by melting and fusing at least a portion of the surface of the fabric layer and the foamed resin layer.

[0124] The artificial leather or the laminate is particularly excellent in durability, moldability, designability, and abrasion resistance of the resin portion, and further has a soft texture. Therefore, it is preferable to use the artificial leather or the laminate at least in part for vehicle interior materials, clothing, and miscellaneous goods.

[0125] It should be noted that the "vehicle interior material" referred to here refers to, for example, steering wheels, horn switches, shift knobs, dashboards, instrument panels, glove boxes, floor carpets, floor mats, ceiling linings, sun visors, assist grips, and the like, and the "vehicle" in this invention includes automobiles, aircraft, railway cars, ships, as well as carriages, baskets, rickshaws, and other vehicles, and further includes some industrial, construction, and agricultural machinery capable of carrying humans or animals, such as excavators, cranes, tractors, and combine harvesters.

[0126] Moreover, "clothing" here refers to jackets, pants, coats, etc., and "miscellaneous goods" refers to bags, shoes, hats, wallets, pouches, etc. Note that clothing and miscellaneous goods are not limited to those for humans, but may be worn or used by pet animals such as dogs and cats, or may be worn or used by character costumes. EXAMPLES

[0127] The present invention will now be described in detail with reference to examples, although the present invention is not limited to these examples.

[0128] [Measurement method] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements of each physical property were performed according to the above-mentioned methods.

[0129] (1) Average single fiber diameter of ultrafine fibers (μm): The scanning electron microscope used was a VHX-D500 / D510 model manufactured by Keyence Corporation, and measurements and calculations were performed according to the above-mentioned methods.

[0130] (2) Area ratio (%) of resin part A and discontinuous resin part B on the surface having nap: The scanning electron microscope used was a Keyence VHX-D500 / D510 model, and the image analysis software was ImageJ (National Institutes of Health, USA), and measurements and calculations were performed using the above-mentioned method. In Tables 1 and 2, this is abbreviated to simply "area ratio of resin portion."

[0131] (3) Length a (mm) of resin part A, length b (mm) of discontinuous resin part B, and ratio a / b(-): The scanning electron microscope used was a VHX-D500 / D510 model manufactured by Keyence Corporation, and measurements and calculations were performed according to the above-mentioned methods.

[0132] (4) Thickness T of resin part A at a position where resin part A is on discontinuous resin part B A (μm): The scanning electron microscope used was a VHX-D500 / D510 model manufactured by Keyence Corporation, and measurements and calculations were performed according to the above-mentioned methods.

[0133] (5) Resin filling rate of resin part A (%): The scanning electron microscope used was a VHX-D500 / D510 model manufactured by Keyence Corporation, and measurements and calculations were performed according to the above-mentioned methods.

[0134] (6) Abrasion resistance (wear loss): The abrasion resistance of the resin portion A in the artificial leather was evaluated by measuring and calculating the abrasion loss (mg) after the Martindale abrasion test (12.0 kPa x 10,000 times) of the artificial leather according to the above procedure.

[0135] (7)Flexibility: The flexibility of the artificial leather was evaluated by measuring and calculating the bending resistance of the artificial leather according to the above-mentioned procedure.

[0136] (8) Design of artificial leather: The design of the artificial leather was visually and tactilely evaluated by a total of 20 healthy adult males and females, 10 of each. Specifically, the surface condition of the resin part A was judged from the viewpoints of visual and tactile sense on the following 5-level evaluation, and the most common evaluation was determined as the design of the artificial leather. However, in the case of a tie in the number of evaluations, the higher evaluation was determined as the appearance quality of the composite artificial leather. The good level of the present invention was determined as "A or B". A: The design of the resin part A is very clear and uniform. B: The design of resin part A is clear and uniform. C: The design of resin part A is unclear and uneven. D: The design of the resin part A is very unclear and uneven. E: The resin part A is thin or has no thickness and lacks design appeal.

[0137] [Example 1] (a) forming a sheet-like material An islands-in-sea type composite fiber having an islands-in-sea type composite structure consisting of island parts and sea parts was melt spun under the following conditions. Island component: Polyethylene terephthalate A with an intrinsic viscosity (IV value) of 0.73 Sea component: Polystyrene with MFR (Melt Flow Rate, measured according to the test method specified in ISO 1133:1997) of 65g / 10min Spinneret: Spinneret for islands-in-sea composite fiber with 16 islands / hole Spinning temperature: 285℃ ·Island component / sea component mass ratio: 80 / 20 Discharge rate: 1.2g / min. / whole Spinning speed: 1100m / min The islands-in-the-sea composite fibers were then stretched 2.7 times in a steam box at 150°C.

[0138] The islands-in-sea type composite fiber obtained above was subjected to a crimping process using a push-in type crimper, and then cut to a length of 51 mm to form an islands-in-sea type composite fiber web having a single fiber fineness of 4.2 dtex. The average single fiber diameter of the ultrafine fibers obtained from this islands-in-sea type composite fiber was 4.4 μm.

[0139] The islands-in-the-sea composite fiber web obtained as described above was used to form a laminated web (nonwoven fabric) through carding and cross-wrapping processes, and then a plain weave fabric (weight 75 g / m2) was produced using a multifilament (average single fiber diameter: 11.0 μm, total fineness: 84 dtex, 72 filaments) made of polyethylene terephthalate with an intrinsic viscosity (IV value) of 0.65 twisted at 2500 T / m as both the weft and warp yarns with a weave density of 95 warp threads / 2.54 cm and 76 weft threads / 2.54 cm. 2 ) (woven or knitted fabric (a)) was laminated on the top and bottom of the laminated web (nonwoven fabric). 2 The fabric is needle punched with the number of punches, and the weight is 700g / m 2 Thus, a fiber-entangled body having a thickness of 3.0 mm was obtained.

[0140] The fiber-entangled body obtained as described above was shrunk with hot water at 96°C. Then, the fiber-entangled body shrunk with hot water was impregnated with an aqueous solution of polyvinyl alcohol (hereinafter sometimes abbreviated as PVA) with a saponification degree of 88% and adjusted to a concentration of 5% by mass. The fiber-entangled body was further squeezed with a roll and dried with hot air at a temperature of 125°C for 10 minutes while migrating the PVA, to obtain a sheet with PVA such that the mass of PVA relative to the mass of the sheet was 45% by mass. The sheet with PVA thus obtained was immersed in trichloroethylene, and the process of squeezing the liquid with a mangle and compressing was performed 10 times. In this way, the sea component was dissolved and removed (sea removal) and the sheet with PVA was compressed, to obtain a sheet with PVA in which ultrafine fiber bundles were entangled.

[0141] The PVA-attached sheet obtained by entangling the ultrafine fiber bundles as described above was immersed in a dimethylformamide (hereinafter sometimes abbreviated as DMF) solution of polyurethane, which was adjusted so that the concentration of solids mainly composed of polyurethane was 11.3% by mass. After that, the PVA-attached sheet immersed in the DMF solution of polyurethane was squeezed with a roll. Next, this sheet was immersed in an aqueous DMF solution with a concentration of 30% by mass to coagulate the polyurethane. After that, the PVA and DMF were removed with hot water, and the sheet was impregnated with a silicone oil emulsion liquid adjusted to a concentration of 1% by mass, and a silicone-based lubricant was applied so that the amount applied was 0.5% by mass relative to the total mass of the mass of the fiber entanglement body and the mass of the polyurethane, and the sheet was dried for 10 minutes with hot air at a temperature of 120°C. As a result, a sheet-like product was obtained with a thickness of 2.1 mm and a polyurethane mass of 28% by mass relative to the mass of the fiber entanglement body.

[0142] (b) Step of forming napped sheet The sheet-like material obtained as described above was cut in half so that each half had a thickness of 1 / 2. Next, the surface layer of the cut surface (the surface formed when cut in half) of the cut sheet was ground by 0.15 mm using endless sandpaper with a sandpaper size of 240 to obtain a napped sheet with a thickness of 0.9 mm.

[0143] The napped sheet obtained as described above was dyed using a jet dyeing machine. After that, it was dried at 100°C for 7 minutes to obtain a sheet having an average single fiber diameter of 4.4 μm and a basis weight of 375 g / m. 2 A dyed napped sheet having a thickness of 1.1 mm and a nap length of 330 μm was obtained.

[0144] (c) A process for forming discontinuous resin portion B and resin portion A A DMF (dimethylformamide) solution (referred to as DMF solution-B1) of polyurethane (hereinafter sometimes abbreviated as PU) adjusted to a solid content concentration of 30% was applied to the napped surface of the dyed napped sheet by gravure coating method, and dried to form discontinuous random island-like (island size is approximately 100 μm × 100 μm to 1000 μm × 1200 μm) discontinuous resin part B (length b of discontinuous resin part B is 0.20 mm).

[0145] Furthermore, a PU DMF (dimethylformamide) solution (referred to as DMF solution-A1) with a viscosity adjusted to 2000 mPa s was applied on top of the lattice pattern (a pattern with staggered squares) using a mold, and then dried to obtain resin part A (length a of resin part A is 6.00 mm, thickness T A A resin layer having a thickness of 130 μm was formed. This resulted in an artificial leather having a napped surface on which resin portion A and discontinuous resin portion B were formed, with at least a portion of resin portion A laminated on discontinuous resin portion B. The results are shown in Table 1. The artificial leather obtained had excellent design and abrasion resistance, as well as excellent flexibility. In particular, in the evaluation of abrasion resistance, no pattern breaks or noticeable abrasion were observed after the test, and a uniform surface was maintained.

[0146] [Example 2] (c) In the process of forming discontinuous resin portion B and resin portion A, the DMF solution-A1 was replaced with a DMF solution of foamable PU (referred to as DMF solution-A2) whose viscosity was adjusted to 1050 mPa s. Furthermore, the length a of resin portion A was adjusted to 5.80 mm and the thickness T A An artificial leather was obtained in the same manner as in Example 1, except that the thickness was 120 μm. The results are shown in Table 1. The artificial leather obtained had good design properties, a certain degree of abrasion resistance, and excellent flexibility.

[0147] [Example 3] In the step (c) of forming the discontinuous resin portion B and the resin portion A in Example 1, the discontinuous DMF solution-A1 was replaced with a DMF solution of PU (referred to as DMF solution-A3) whose viscosity was adjusted to 3,500 mPa s, and the length a of the resin portion A was adjusted to 6.60 mm and the thickness T A An artificial leather was obtained in the same manner as in Example 1, except that the thickness was 210 μm. The results are shown in Table 1. The artificial leather obtained had a certain degree of abrasion resistance and excellent design properties.

[0148] [Example 4] In the step of forming discontinuous resin portions B and A in Example 1 (c), the DMF solution-A1 was replaced with a DMF solution of PU with a viscosity adjusted to 1300 mPa s (referred to as DMF solution-A4), and the pattern of resin portion A was changed to a different lattice pattern (a pattern in which squares with sizes of 1 mm × 1 mm to 3 mm × 3 mm are randomly staggered on a square lattice with a lattice spacing D = 10 mm, as shown in the conceptual top view of FIG. 3) of resin portion A (the length a of resin portion A is 2.00 mm, the thickness T A An artificial leather was obtained in the same manner as in Example 1, except that a fine grained layer (5 μm) was formed. The results are shown in Table 1. The artificial leather obtained had excellent abrasion resistance, flexibility, and a clear design.

[0149] [Example 5] In the step of forming the discontinuous resin portion B and the resin portion A in Example 1 (c), the mesh of the gravure roll for the discontinuous resin portion B was made smaller, the size of the islands of the discontinuous resin portion B was changed from about 100 μm×200 μm to 1100 μm×1300 μm to about 10 μm×20 μm to 150 μm×200 μm, and the length b of the discontinuous resin portion B was changed from 0.20 mm to 0.04 mm. Furthermore, the pattern of the resin portion A was changed to a different lattice pattern (a pattern in which squares of 1 mm×1 mm to 3 mm×3 mm are randomly arranged in a staggered pattern on a square lattice with a lattice spacing D=10 mm as shown in the conceptual top view of FIG. 3) to form the resin portion A (the length a of the resin portion A is 2.00 mm, the thickness T A An artificial leather was obtained in the same manner as in Example 1, except that a thickness of 30 μm was formed on the surface of the layer. The results are shown in Table 1. The artificial leather obtained had excellent abrasion resistance, flexibility, and a clear design.

[0150] [Example 6] In the step (c) of forming the discontinuous resin portion B and the resin portion A in Example 1, the mesh of the gravure roll for the discontinuous resin portion B was enlarged to change the size of the islands of the discontinuous resin portion B from about 100 μm×200 μm to 1100 μm×1300 μm to about 1500 μm×1800 μm to 2500 μm×2500 μm, the length b of the discontinuous resin portion B was changed from 0.20 mm to 2.20 mm, and further, the length a of the resin portion A was changed to 6.60 mm, but other than that, an artificial leather was obtained in the same manner as in Example 1. The results are shown in Table 1. The obtained artificial leather had excellent design properties.

[0151] [Example 7] An artificial leather was obtained in the same manner as in Example 1, except that in the step (c) of forming discontinuous resin portion B and resin portion A in Example 1, the DMF solution-A1 was changed to a natural resin (lacquer) whose viscosity had been adjusted to 2500 mPa s, and further, the length a of resin portion A was changed to 5.60 mm. The results are shown in Table 1. The obtained artificial leather had excellent design properties and abrasion resistance, as well as excellent flexibility.

[0152] [Table 1]

[0153] [Comparative Example 1] An artificial leather was obtained in the same manner as in Example 1, except that in the step (c) of forming discontinuous resin portion B and resin portion A in Example 1, no resin portion A was applied at all. The results are shown in Table 2. The artificial leather obtained had excellent flexibility, but its abrasion resistance was equivalent to that of general nubuck-like artificial leather, and since it did not have resin portion A, it was inferior in design.

[0154] [Comparative Example 2] In the step of forming the discontinuous resin portion B and the resin portion A in Example 1 (c), the discontinuous resin portion B was not applied at all, and only the resin portion A was applied as it was. The length a of the resin portion A was 5.80 mm and the thickness T AAn artificial leather was obtained in the same manner as in Example 1, except that the thickness was 80 μm. The results are shown in Table 2. The artificial leather obtained was poor in abrasion resistance and flexibility, and in addition, the resin portion A penetrated between the raised naps, and the design was poor.

[0155] [Comparative Example 3] In the step of forming the napped sheet (b) of Example 1, the surface was not napped, and the DMF solution-A1 was applied to the surface without nap, and the length a of the resin portion A was 5.60 mm and the thickness T A An artificial leather was obtained in the same manner as in Example 1, except that the thickness was 120 μm. The results are shown in Table 2. The artificial leather obtained had a certain degree of flexibility and a fairly clear design, but was poor in abrasion resistance.

[0156] [Comparative Example 4] In the step of forming the discontinuous resin portion B and the resin portion A in Example 1 (c), the resin portion B is applied to the entire surface of the dyed napped sheet having nap without any gaps, and the thickness T of the resin portion A is A An artificial leather was obtained in the same manner as in Example 1, except that the thickness was 100 μm. The results are shown in Table 2. The artificial leather obtained had a certain degree of flexibility and a clear design, but was poor in abrasion resistance.

[0157] [Comparative Example 5] In the step (c) of forming the discontinuous resin portion B and the resin portion A in Example 1, the DMF solution A1 was replaced with a DMF solution of PU (DMF solution A6) whose viscosity was adjusted to 900 mPa s, and the length a of the resin portion A was adjusted to 8.30 mm and the thickness T A An artificial leather was obtained in the same manner as in Example 1, except that the thickness was 3 μm. The results are shown in Table 2. The artificial leather obtained was inferior in abrasion resistance, and the resin portion A penetrated into the substrate, resulting in poor flexibility. In addition, the resin filling rate of the resin portion A could not be measured.

[0158] [Comparative Example 6] In the step (c) of forming the discontinuous resin portion B and the resin portion A in Example 1, the DMF solution A1 was replaced with a DMF solution of PU (DMF solution A7) adjusted to 4200 mPa·s, and the length a of the resin portion A was set to 6.40 mm and the thickness T A An artificial leather was obtained in the same manner as in Example 1, except that the thickness was 250 μm. The results are shown in Table 2. The artificial leather obtained was poor in abrasion resistance, and the resin portion A was hard and lacked in flexibility.

[0159] [Table 2]

[0160] As shown in Table 1, the artificial leathers of Examples 1 to 7 have a specific range of sizes for the resin part A and the discontinuous resin part B that make up the artificial leather, and the resin part A is in contact with the raised nap, thereby achieving a clear design and excellent abrasion resistance, and further achieving the soft texture unique to artificial leather.

[0161] On the other hand, as shown in Table 2, when the artificial leathers of Comparative Examples 1 to 6 had a structure that did not satisfy the length ratio (a / b) of the resin part A to the discontinuous resin part B, a structure in which the resin part A was not in contact with the raised nap, or a structure that did not include the resin part B, the design was thin and unclear, and the abrasion resistance and the texture unique to artificial leather were impaired, resulting in artificial leathers that were inferior in touch and appearance quality. [Explanation of symbols]

[0162] 1:Artificial leather 2: Base part 3: Hair standing 4, 12: Discontinuous resin part B 5, 22: Resin part A 11, 21: Pierrection part D: Lattice spacing

Claims

1. An artificial leather comprising: a fiber-entangled body containing, as a component, a nonwoven fabric composed of ultrafine fibers whose main component is a thermoplastic resin and whose average single fiber diameter is 1.0 μm or more and 10.0 μm or less; and a polymer elastomer; one surface of the artificial leather has nap, and a resin portion A and a discontinuous resin portion B are formed on the napped surface, and at least a part of the resin portion A is laminated on the discontinuous resin portion B; and the artificial leather further satisfies the following requirements (1) to (4): (1) The resin portion A is a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin, and the discontinuous resin portion B is a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin. (2) The area ratio of the resin portion A and the discontinuous resin portion B to the surface having nap is 50% or more and 95% or less. (3) The length a (mm) of the resin portion A and the length b (mm) of the discontinuous resin portion B satisfy the following formula 1. 1<a / b≦50 (Formula 1) (4) At least a part of the resin portion A is in direct contact with the surface having the nap, and in that part, the resin portion A covers the nap.

2. A thickness T of the resin portion A at a position where the resin portion A is on the discontinuous resin portion B A The artificial leather according to claim 1, wherein the thickness of the surface roughness layer is 5 μm or more and 200 μm or less.

3. 3. The artificial leather according to claim 1, wherein the length b (mm) of the discontinuous resin portion B is 0.05 mm or more and 2.00 mm or less.

4. 3. The artificial leather according to claim 1, wherein the resin portion A has a resin filling rate of 95% or more and less than 100%.

5. A step of forming a sheet-like article including a fiber-entangled body containing, as a component, a nonwoven fabric composed of ultrafine fibers having an average single fiber diameter of 1.0 μm or more and 10.0 μm or less, and a polymer elastomer; A step of grinding one surface of the sheet-like material to form a napped sheet; A step of discontinuously placing a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, polyurethane resin, and natural resin on the napped surface of the napped sheet to form a discontinuous resin portion B, and further placing a resin containing one or more selected from the group consisting of styrene-butadiene rubber, nitrile rubber, acrylic resin, epoxy resin, and natural resin and having a viscosity of 1000 mPa·s to 4000 mPa to form a resin portion A; The method for producing the artificial leather according to claim 1 or 2, comprising:

6. A laminate comprising the artificial leather according to claim 1 and a fabric layer and / or a foamed resin layer on the other surface of the artificial leather.

7. 7. A vehicle interior material, at least a part of which is the artificial leather according to claim 1 or the laminate according to claim 6.

8. 7. A garment, at least a part of which is the artificial leather according to claim 1 or the laminate according to claim 6.

9. 7. Miscellaneous goods, at least a part of which is the artificial leather according to claim 1 or the laminate according to claim 6.

Citation Information

Patent Citations

  • Transparent leather like sheet

    JP1999001878A

  • Grained artificial leather, and method of manufacturing the same

    JP2013177713A

  • Grained artificial leather and method for producing the same

    JP2014001463A

  • Artificial leather and method for producing artificial leather

    JP2015158030A