Method for repairing crack

The method repairs metal structure cracks by forming bolt insertion holes and using thermal contraction to apply compressive stress, addressing the limitations of existing methods and ensuring robust front-side repair.

JP2024134641AInactive Publication Date: 2024-10-04NAN SEIKO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023044938
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for repairing cracks in metal structures, such as welding and using fiber-reinforced resin sheets, are inadequate as they do not increase strength and require access to the back side of the wall, limiting their applicability.

Method used

A method involving forming bolt insertion holes straddling the crack, inserting a bolt with a nut, and utilizing thermal contraction to draw the crack sides together, applying compressive stress for reinforcement.

Benefits of technology

The method allows for robust crack repair from the front side without back access, providing stronger reinforcement than welding and adjustable compressive stress for optimal repair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134641000001_ABST
    Figure 2024134641000001_ABST
Patent Text Reader

Abstract

To provide a method for repairing a crack capable of firmly repairing a crack generated on a wall surface of a metal structure only by processing from a front surface.SOLUTION: The present invention relates to a method for repairing a crack 11 generated in a wall surface 10 of a metal structure. The wall surface 10 in which the crack 11 is generated is scraped by a tool, thereby forming a bolt insertion hole 12 in which both end portions 14 are widened so as to straddle the crack 11. Next, a bolt 17 in which a nut is screwed to one end or both ends of a shaft portion 15 is heated and inserted into the inside of the bolt insertion hole 12 after adjusting distance between the nuts, and then both sides of the crack are drawn to each other by utilizing thermal contraction caused by subsequent temperature drop to repair the crack 11.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for repairing a crack occurring in the wall surface of a metal structure. [Background technology]

[0002] Cracks may occur on the walls of metal structures such as rolling mills and forging machines, which are large machines that are repeatedly loaded over a long period of time. Generally, the cracks are repaired by welding or by riveting a cover plate to close the cracks.

[0003] However, welding the cracked area does not increase the strength of that area, so there is a possibility that a crack will appear again. Also, the method of fixing the cover plate with rivets requires the rivets to penetrate the wall, so it cannot be used if there is no space behind the wall.

[0004] Patent Document 1 describes a method for repairing a steel structure in which the back of the steel structure is sealed with a sheet, resin is injected into the crack from the front, and a fiber-reinforced resin sheet is applied to the front. However, since the strength of the repaired area depends on the fiber-reinforced resin sheet, there is a possibility that the crack will appear again. In addition, this method cannot be used when there is no space to work on the back. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-255195 A Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, the object of the present invention is to provide a method for repairing cracks that are caused by the above-mentioned problems of the conventional technology and that can reliably repair cracks that have occurred in the wall surface of a metal structure by processing only from the front side. [Means for solving the problem]

[0007] The present invention, made to solve the above-mentioned problems, is a method for repairing a crack that has occurred in the wall of a metal structure, which is characterized in that the wall surface in which the crack has occurred is scraped with a tool to form a bolt insertion hole that is wider at both ends than in the middle so as to span the crack, and a bolt having nuts screwed onto one or both ends of the shaft is heated and inserted into the bolt insertion hole after adjusting the distance between the nuts, and then the thermal contraction caused by the subsequent temperature drop is used to draw both sides of the crack together.

[0008] The nut may be a nut having a circular or spherical outer circumferential surface and a plurality of radial tool insertion holes. It is also preferable that the nut contact surfaces at both ends of the bolt insertion hole have a curved shape. Effect of the Invention

[0009] According to the present invention, cracks occurring on the wall surface of a metal structure can be repaired only from the front surface without inserting hands into the back surface of the wall surface, so that repairs can be made even when there is no work space on the back surface. In addition, since the repair method of the present invention utilizes the thermal contraction of the bolts, a compressive stress that prevents the crack from expanding can be applied to the cracked portion, making it possible to perform a more solid repair than a simple welding method.

[0010] Furthermore, since the crack repair method of the present invention is carried out using a bolt with a nut screwed onto one or both ends of the shank, by rotating the nut, the length between the nuts can be precisely and freely adjusted to match the distance between the nut contact surfaces of the bolt insertion hole, thereby always generating optimal compressive stress. [Brief description of the drawings]

[0011] [Figure 1] FIG. 13 is a front view showing a state in which a crack has occurred on a wall surface. [Diagram 2] FIG. 11 is a front view showing a state in which a bolt insertion hole has been formed. [Diagram 3] FIG. 4 is a front view showing a state in which a bolt is inserted into a bolt insertion hole. [Figure 4] FIG. 2 is an explanatory diagram of a bolt and a bolt insertion hole according to the first embodiment. [Diagram 5] FIG. 11 is an explanatory diagram of a bolt and a bolt insertion hole according to the second embodiment. [Figure 6] 13 is an explanatory diagram of a bolt and a bolt insertion hole according to the third embodiment. FIG. [Figure 7] 13 is an explanatory diagram of a bolt and a bolt insertion hole according to the fourth embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Preferred embodiments of the present invention will now be described. As shown in Fig. 1, a crack 11 may occur on a wall surface 10 of a metal structure. The metal structure may be, for example, a large machine such as a forging machine, but the type of the metal structure is not particularly limited, and may be a metal building. However, the wall surface 10 must be several tens of millimeters thick, and the repair method of the present invention cannot be applied to a thin wall surface 10.

[0013] Next, as shown in Figure 2, a bolt insertion hole 12 is formed at a position spanning the crack 11. The bolt insertion hole 12 is formed by scraping the wall surface 10 of the metal structure from the surface with a tool. The bolt insertion hole 12 consists of a central portion 13 corresponding to the bolt and wide portions 14 at both ends, with the central portion 13 crossing the crack 11 and the wide portions 14 on both ends being positioned on both sides of the crack 11. Although two parallel bolt insertion holes 12 are shown in Figure 2, the number can be one or more depending on the occurrence of the crack 11.

[0014] 3, a bolt 17 with a nut screwed onto one or both ends of the shaft 15 is inserted into the bolt insertion hole 12 in a heated, high-temperature state, and the thermal contraction of the bolt 17 caused by the subsequent cooling is utilized to draw together both sides of the crack. The specific shape of the bolt 17 and the details of the bolt insertion hole 12 are described below.

[0015] FIG. 4 shows the first embodiment, where (A) is an external view of bolt 17, (B) is a front view of bolt insertion hole 12, and (C) is a front view of bolt 17 inserted into bolt insertion hole 12. In this first embodiment, a bolt 17 having male threads 18 cut at both ends of a shaft portion 15 and two nuts screwed together is used. The nut in the first embodiment is a commercially available hexagonal nut 19, and the bolt 17 can also be a stud bolt or a double-threaded bolt that is commercially available. In the present invention, the strength of shaft portion 15 is important, and in this embodiment, a steel double-threaded bolt with a nominal thread diameter of 20 mm is used.

[0016] The seating surface 20 of the hexagonal nut 19 is a plane perpendicular to the axis. Therefore, the inner surface of the wide portion 14 of the bolt insertion hole 12 on the side of the central portion 13 into which the shaft portion 15 is inserted, i.e., the nut contact surface 21 that comes into contact with the seating surface 20 of the hexagonal nut 19, is a plane. The width of the wide portion 14 is formed to be sufficiently larger than the outer diameter of the hexagonal nut 19 so that the hexagonal nut 19 can be rotated therein with a wrench. The depth of the bolt insertion hole 12 is preferably set to a depth such that the hexagonal nut 19 does not protrude from the wall surface 10 even when the bolt 17 to which the hexagonal nut 19 is screwed is inserted.

[0017] 5 is a diagram showing a second embodiment. In this second embodiment, a circular nut 22 is used as a nut to be screwed onto a bolt 17 having male threads 18 cut at both ends of a shaft portion 15. A plurality of radial tool insertion holes 23 are formed on the outer circumferential surface of the circular nut 22, so that a rod-shaped tool can be inserted and rotated. Therefore, in the second embodiment, the wide portion 14 of the bolt insertion hole 12 can be made smaller than in the first embodiment. The bearing surface 24 of the circular nut 22 is also flat, and the nut contact surface 25 of the bolt insertion hole 12 with the circular nut 22 is also flat.

[0018] 6 is a diagram showing a third embodiment, and (A) shows the bolt and nut separated. In the third embodiment, a spherical nut 26 with a spherical outer circumferential surface is used as the nut. A plurality of radial tool insertion holes 27 are formed on the outer circumferential surface in a direction perpendicular to the axis. When the spherical nut 26 is used in this manner, the nut contact surface 28 between the wide portion 14 of the bolt insertion hole 12 and the spherical nut 26 is also spherical, which has the advantage of mitigating stress concentration at the contact portion.

[0019] 7 shows the fourth embodiment, in which a general bolt 17 is used, with a male thread 18 cut on one side of the shaft portion 15 and a bolt head 28. The nut is a commercially available hexagonal nut 19. The shape of the bolt insertion hole 12 is the same as in the first embodiment, but one side of the wide portion 14 becomes a nut contact surface 25, and the other side becomes a bolt head contact surface 29. In this way, a structure in which the nut is screwed onto only one side of the shaft portion 15 may be used. It is also possible to replace the hexagonal nut 19 with a circular nut 22 or a spherical nut 26.

[0020] Next, the procedure of the crack repair method of the present invention will be described. Here, the description will be based on the first embodiment, but the procedure is the same in the other embodiments.

[0021] First, as shown in Figure 2, a bolt insertion hole 12 is formed with a tool at a position spanning a crack 11 in a wall surface 10. Next, a bolt 17 with a hexagonal nut 19 screwed onto both ends of a shaft 15 is inserted into the bolt insertion hole 12, and the hexagonal nut 19 on either side or both sides is rotated so that the nut seating surface 20 is in close contact with the nut contact surface 21 of the bolt insertion hole 12. Because the bolt insertion hole 12 is machined manually, there is an unavoidable machining error in the spacing between the nut contact surfaces 21, 21 on both sides, but by rotating the hexagonal nut 19, the effect of the machining error can be cancelled out.

[0022] Next, the bolt with hexagonal nuts 19 screwed onto both ends of the shaft 15 is removed from the bolt insertion hole 12, and the hexagonal nuts 19 are further rotated slightly to make the distance between the bearing surfaces 20, 20 of the hexagonal nuts 19 on both sides slightly narrower than the distance between the nut contact surfaces 21, 21 on both sides of the bolt insertion hole 12. For this reason, it becomes impossible to insert the bolt into the bolt insertion hole 12 in this state, but the bolt is heated to thermally expand the shaft 15, thereby increasing the distance between the bearing surfaces 20, 20, and the bolt can be inserted into the bolt insertion hole 12.

[0023] Since the thermal expansion coefficient α of the steel material constituting the bolt is known, it is possible to accurately calculate how much the bolt will expand when heated to a certain degree. In addition, since the pitch of the male thread 18 cut into the shank 15 is known, the relationship between the rotation angle of the nut and the distance between the bearing surfaces 20, 20 can also be accurately calculated. Therefore, the nut is rotated to a position where it can be inserted into the bolt insertion hole 12 in a heated state but cannot be inserted into the bolt insertion hole 12 at room temperature. As a result, the shank 15 thermally contracts as the temperature drops, and the nut tightly adheres to the nut contact surface 21 of the bolt insertion hole 12, drawing in both sides of the crack 11.

[0024] At this time, compressive stress is generated in the crack 11, so the tensile stress that propagates the crack 11 can be relaxed or reduced to zero, enabling a strong crack repair. As a reaction to this, a strong tensile stress is applied to the shaft 15 of the bolt 17, so it is necessary to adjust the rotation angle of the nut so that the bolt 17 does not break afterwards. However, since the strength of the bolt is also known, the optimal rotation angle of the nut can be found by calculation.

[0025] As described above, the method of repairing cracks of the present invention strongly attracts the nut contact surfaces 21, 21 of the bolt insertion hole 12 formed in the wall surface 10, and if excessive stress concentration occurs in that area, another crack may occur in the wall surface 10 near the nut contact surface 21. The ball nut 26 shown in the third embodiment is optimal for alleviating this stress concentration. However, since the manufacturing cost of such a specially shaped ball nut 26 is high, it is necessary to appropriately select whether to use the inexpensive hexagonal nut 19 of the first or fourth embodiment or the circular nut 22 of the second embodiment depending on the situation.

[0026] As described above, according to the method for repairing a crack of the present invention, a crack 11 occurring in a wall surface 10 of a metal structure can be firmly repaired only by processing from the front surface. [Explanation of symbols]

[0027] 10 Wall 11. Crack 12 Bolt insertion holes 13 Central part 14 Wide section 15 Shaft 17 Volts 18 Male thread 19 Hexagon Nut 20 Seat 21 Nut contact surface 22 Circular Nut 23 Tool insertion hole 24 Seat 25 Nut contact surface 26 Ball Nut 27 Tool insertion hole 28 Bolt head 29 Bolt head contact surface

Claims

1. A method for repairing a crack that has occurred on a wall surface of a metal structure, comprising the steps of: By cutting the wall where the crack occurred with a tool, a bolt insertion hole that is wider at both ends than in the center is formed so that it spans the crack. A bolt with nuts screwed onto one or both ends of the shaft is heated and inserted into the bolt insertion hole after adjusting the distance between the nuts. A method for repairing a crack, characterized by using the thermal contraction caused by the subsequent temperature drop to pull both sides of the crack together.

2. 2. The method for repairing a crack according to claim 1, wherein the nut used is a circular or spherical nut having a plurality of radial tool insertion holes on its outer circumferential surface.

3. 2. The method for repairing a crack according to claim 1, wherein the shape of the nut contact surfaces at both ends of the bolt insertion hole is curved.

Citation Information

Patent Citations

  • Method for repairing steel structure

    JP2010255195A