Polyethylene resin and high purity chemical container composed of the same
A polyethylene resin with tailored properties addresses contaminant elution and surface issues in high-purity chemical containers, ensuring reduced fine particles and enhanced chemical resistance through a two-stage polymerization process.
Patent Information
- Application Number
- JP2023045122
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing polyethylene resins used for high-purity chemical containers face issues with contaminant elution, insufficient chemical resistance, surface smoothness, and high costs due to the use of tetrafluoroethylene copolymers, along with inadequate control of ash content and metal impurities.
A polyethylene resin with specific properties such as melt flow rate, density, molecular weight ratio, and low metal content, produced through a two-stage polymerization process using highly active catalysts, to minimize contaminant elution and enhance chemical resistance and surface smoothness.
The resin results in high-purity chemical containers with reduced fine particles and metal impurities, improved chemical resistance, and excellent surface smoothness, suitable for small containers, maintaining low particulate elution even after long-term storage.
Smart Images

Figure 2024134768000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene resin and a high-purity chemical container made therefrom. [Background technology]
[0002] In recent years, the demand for high-purity chemicals has increased with the remarkable development of the electronics industry. High-purity chemicals are used as essential chemicals for the manufacture of electronic circuits such as large-scale, integrated LSIs. Specifically, sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, ammonium fluoride, hydrogen peroxide, isopropyl alcohol, xylene, TMAH (tetramethylammonium hydroxide), methanol, acetic acid, phosphoric acid, ammonia water, PGMEA (propylene glycol methyl ether acetate), DMSO (dimethyl sulfoxide), NMP (N-methyl-2-pyrrolidone), etc. are used for wafer cleaning and etching, wiring and insulating film etching, jig cleaning, developing solution, resist dilution solution, resist stripping solution, drying, etc. Fluorine-based resins and polyethylene resins are mainly used as container materials for these high-purity chemicals of 20L or less, such as 18L containers, 4L containers, and 1L containers. As the integration density of semiconductor circuits increases, the demands for reducing impurities and particulates in these chemicals are becoming more stringent. To satisfy these demands, the cleanliness requirements for the containers in which these chemicals are filled are also increasing year by year.
[0003] One method for solving this problem is to use a specific tetrafluoroethylene copolymer, but the tetrafluoroethylene copolymer has the problem of being expensive (see Patent Document 1). In addition, there have been proposals for containers that suppress the amount of hydrocarbon solvents extracted from polyethylene resins and the content of low molecular weight components, and limit the amount of antioxidants, neutralizing agents, and light stabilizers added as much as possible, but improvements to the effects of ash from catalyst components remaining in the polyethylene resin are insufficient, and measures to reduce the concentration of metal impurities eluted into chemicals are incomplete. Also, the level of fine particles is insufficient at 0.2 μm or more (see Patent Documents 2 and 3).
[0004] In addition, the density is 0.940 to 0.970 g / cm 3 A polyethylene for high-purity chemical containers and a high-purity chemical container have been proposed, which are characterized by a melt flow rate of 2 to 50 g / 10 min at a temperature of 190°C and a load of 21.6 kg, a ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) determined by gel permeation chromatography (GPC) of 8 to 15, and an ash content of 50 PPM or less in the polyethylene resin; however, improvements to the effects of ash due to catalyst components remaining in the polyethylene resin are insufficient, and measures to reduce the concentration of metal impurities eluted into chemicals have not been completed (see Patent Document 4).
[0005] Furthermore, the density is 0.940 to 0.970 g / cm 3 A polyethylene resin for ultra-high purity chemical containers and a high purity chemical container have been proposed, which have the following properties: a melt flow rate of 2 to 8.5 g / 10 min at a temperature of 190°C and a load of 21.6 kg, a ratio (Mw / Mn) of 8 to 15 of weight average molecular weight (Mw) to number average molecular weight (Mn) determined by gel permeation chromatography (GPC), a molecular weight distribution curve obtained using GPC showing that components having a molecular weight of 1000 or less account for 0.30% by weight or less, and an ESCR of 130 hours or more. However, when made into a small container, the surface smoothness was insufficient (see Patent Document 5). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] WO00 / 17057 publication [Patent Document 2] Japanese Patent Application Publication No. 7-62161 [Patent Document 3] Japanese Patent Application Publication No. 7-257540 [Patent Document 4] Japanese Patent Application Publication No. 11-80257 [Patent Document 5] Patent No. 6705157 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a polyethylene resin which, when used as a high-purity chemical container, minimizes the elution of contaminants such as eluates and deterioration products of the resin and has excellent chemical resistance and surface smoothness, and a high-purity chemical container made of the polyethylene resin. [Means for solving the problem]
[0008] As a result of extensive research to solve the above problems, the inventors discovered that by using polyethylene having specific properties such as density, melt flow rate, molecular weight determined by gel permeation chromatography (GPC), metal content, ESCR, etc., it is possible to obtain high-purity chemical containers which have excellent chemical resistance and surface smoothness with fewer fine particles derived from polyethylene and less metal impurities derived from polymerization catalyst components, and thus developed the present invention.
[0009] That is, the respective aspects of the present invention are [1] to [7] shown below. [1] Melt flow rate (MFR) at 190°C and 2.16 kg load is 20-40g / 10min, density (JIS K6922-1) is 0.960-0.970g / cm 3 and an ethylene polymer having a high melt flow rate (HLMFR) of 0.10 to 10 g / 10 min at a temperature of 190°C and a load of 21.6 kg and a density of 0.920 to 0.940 g / cm 3 The polyethylene resin contains two ethylene polymer components, the weight ratio of which is 40:60 to 60:40, and has the following properties (1) to (7): (1) Density is 0.945 to 0.955 g / cm 3 (2) HLMFR is 21 to 80 g / 10 min at a temperature of 190°C and a load of 21.6 kg. (3) MFR is 0.5 to 1.5 g / 10 min at a temperature of 190°C and a load of 2.16 kg. (4) The ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) determined by gel permeation chromatography (GPC) is 5.0 to 7.9. (5) In the molecular weight distribution curve obtained using GPC, the content of components with a molecular weight of 1,000 or less is 0.30% by weight or less (6) Metal content is 15 ppm or less for polyethylene resin (7) Environmental stress cracking resistance (ESCR) of 100 hours or more [2] The high-purity polyethylene resin for chemical containers according to [1] above, which does not contain any additives. [3] A high-purity chemical container made of the polyethylene resin described in [1] or [2] above. [4] A high-purity chemical container made of the polyethylene resin described in [3] above, in which the developed area ratio of the inner surface of the container is 1.10 or less. [5] A high-purity chemical container made of the polyethylene resin described in [3] or [4] above, in which the maximum roughness Rz of the container's inner surface is 10 μm or less. [6] A container for high-purity chemicals according to any one of the above [3] to [5], wherein the gloss of the inner surface of the container is 40% or more. [7] A container for high-purity chemicals according to any one of [3] to [6] above, in which the number of particles of 0.1 μm or more eluted from the container after filling an unwashed container with ultrapure water and storing it at 40°C for 35 days is 10 particles / mL or less. Effect of the Invention
[0010] When the polyethylene resin for high-purity drug containers according to one embodiment of the present invention is used, a high-purity drug container with excellent chemical resistance and surface smoothness can be molded with less fine particles derived from the polyethylene resin and less metal impurities derived from polymerization catalyst components. In addition, a high-purity drug container suitable for small containers of 20 L or less can be provided, which has less elution of fine particle components from the filled drug and has less elution of fine particles even after long-term storage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The high-purity polyethylene resin for chemicals according to one embodiment of the present invention has a melt flow rate (MFR) of 20 to 40 g / 10 min at 190° C. and a load of 2.16 kg, and a density (JIS K6922-1) of 0.960 to 0.970 g / cm 3 and an ethylene polymer having a high melt flow rate (HLMFR) of 0.10 to 10 g / 10 min at 190 °C and a load of 21.6 kg and a density of 0.920 to 0.940 g / cm 3 The weight ratio of the two components is 40:60 to 60:40, and the polymer has the following properties (1) to (7). (1) Density is 0.945 to 0.955 g / cm 3 (2) HLMFR at 190℃ and 21.6kg load is 21-80g / 10min (3) MFR at 190°C and a load of 2.16 kg is 0.5 to 1.5 g / 10 min. (4) The ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) determined by gel permeation chromatography (GPC) is 5.0 to 7.9. (5) In the molecular weight distribution curve obtained using GPC, the content of components having a molecular weight of 1,000 or less is 0.30% by weight or less. (6) Metal content is 15 ppm or less for polyethylene resin (7) Environmental stress cracking resistance (ESCR) of 100 hours or more The high-purity polyethylene resin for chemicals can be produced by a highly active catalyst such as a Ziegler catalyst or a metallocene catalyst. For example, the resin can be suitably produced by using a highly active Ziegler catalyst consisting of a transition metal compound such as titanium or zirconium, a magnesium compound, and an organoaluminum compound as a polymerization catalyst, and copolymerizing ethylene or ethylene and an α-olefin having 3 to 20 carbon atoms in a ratio that gives a desired density.
[0012] The catalyst may be one described in Japanese Patent No. 3319051.
[0013] Examples of the α-olefin having 3 to 20 carbon atoms include propylene, 1-butene, 4-methyl-1-pentene, 3-methyl-1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene.
[0014] The polymerization method for producing the polyethylene resin is slurry polymerization using a polymerization solvent having a carbon number of 6 to 10, such as normal hexane or normal heptane, in order to keep the concentration of metal impurities eluted in the chemicals low and to limit the incorporation of low molecular weight polymers that cause the generation of fine particles into the resin. The polymerization solvent has an MFR of 20 to 40 g / 10 min and a density of 0.960 to 0.970 g / cm. 3 and a low molecular weight ethylene polymer having an HLMFR of 0.1 to 10 g / 10 min and a density of 0.920 to 0.940 g / cm 3 and a high molecular weight ethylene polymer having a weight ratio of 40:60 to 60:40. The two components, the low molecular weight component and the high molecular weight component, can be produced, for example, by a two-stage polymerization method.
[0015] The polyethylene resin is specified in terms of density, HLMFR, MFR, molecular weight distribution (Mw / Mn), components with a molecular weight of 1000 or less, amount of contained metals and ESCR as shown below.
[0016] That is, the density of the polyethylene resin (JIS K6922-1) is 0.945 to 0.955 g / cm 3 and preferably 0.948 to 0.952 g / cm 3 0.945g / cm 3 If the density is less than 0.955g / cm3, the polymer components eluted into the drug in the container will increase, causing the generation of fine particles. 3 Above this value, the ESCR of the container decreases.
[0017] The HLMFR (JIS K6922-1) of the polyethylene resin is 21 to 80 g / 10 min, preferably 30 to 60 g / 10 min. If it is less than 21 g / 10 min, the surface texture of the container deteriorates. If it exceeds 80 g / 10 min, the drawdown becomes large and moldability deteriorates.
[0018] The polyethylene resin has an MFR (JIS K6922-1) of 0.5 to 1.5 g / 10 min, preferably 0.7 to 1.2 g / 10 min. If it is less than 0.5 g / 10 min, the surface texture of the container deteriorates. If it exceeds 1.5 g / 10 min, the drawdown becomes large and moldability deteriorates.
[0019] The ratio Mw / Mn of the polyethylene resin determined by GPC is 5.0 to 7.9, preferably 6.0 to 7.9. If the Mw / Mn is less than 5.0, the molecular weight distribution is narrow, the surface texture of the container deteriorates, and the ESCR of the container also decreases. If the Mw / Mn is more than 7.9, the molecular weight distribution is broadened, the amount of low molecular weight components increases, and the amount of fine particles in the container increases.
[0020] In the molecular weight distribution curve obtained by using GPC for the polyethylene resin, the content of components having a molecular weight of 1000 or less is 0.30% by weight or less. If the content of components having a molecular weight of 1000 or less exceeds 0.30% by weight, the content of low molecular weight components increases, and the number of fine particles eluted from the container increases.
[0021] The amount of metal contained in the polyethylene resin is 15 PPM or less relative to the polyethylene resin. If the amount of metal contained is 15 PPM or less, the amount of metal eluted into high-purity chemicals is small, so the concentration of metal impurities in the chemicals can be suppressed. The amount of metal contained is the ratio of metal to the total resin in weight ppm. The amount of metal contained is obtained by incinerating the resin and then melting it with alkali, and is the remaining matter such as Mg, Al, and Ti.
[0022] The ESCR of the polyethylene resin is 100 hours or more. If the ESCR is less than 100 hours, for example, when a surfactant or the like is filled and the container is left for six months or more, the container may be damaged by environmental stress cracking.
[0023] Furthermore, the polyethylene resin is preferably free of all additives such as antioxidants, light stabilizers, and neutralizing agents. Here, the neutralizing agents are fatty acid metal salts, typically calcium stearate and zinc stearate, and hydrotalcites, both of which dissolve in chemicals and become metal contaminants, and are therefore preferably free of neutralizing agents.
[0024] The polyethylene resin can be molded into a container shape by direct blow molding, injection molding, injection blow molding, etc. to produce a high-purity chemical container. In particular, a blow molding method using a direct blow molding machine installed in a clean room and using air from which fine particles have been removed by a filter as the blow air is preferable for producing a clean container. The shape of the high-purity chemical container obtained by using the resin is not specified, but in order to reinforce the barrier properties of the contents and the strength of the container, the resin may be used as the inner layer, and a polyethylene resin other than the resin, an ethylene-vinyl alcohol copolymer, a polyvinyl alcohol resin, a polyamide resin, etc. may be used as the intermediate layer, or a polyethylene resin other than the resin, FRP, etc. may be used as the outer layer to reinforce the container.
[0025] The developed area ratio of the inner surface of the container molded using the polyethylene resin is preferably 1.10 or less. If the developed area ratio exceeds 1.10, the contact area with the liquid content increases, causing an increase in fine particles derived from the polyethylene resin. Here, the developed area ratio is the ratio of surface area to area (surface area / area).
[0026] The maximum roughness Rz of the inner surface of a high-purity drug container obtained using the resin is preferably 10 μm or less. If Rz exceeds 10 μm, the molded product will have a poor appearance. Furthermore, air bubbles in the drug will remain in the roughened areas and be detected as fine particles, causing an increase in the number of fine particles. Rz is expressed by calculating the sum of the height of the highest peak and the depth of the deepest valley in the roughness curve over the reference length.
[0027] The gloss of the inner surface of a high-purity drug container obtained using the resin is preferably 40% or more. If the gloss is 40% or more, the container has a glossy appearance and excellent surface smoothness, and therefore has excellent defoaming properties for drugs and can reduce the number of detected fine particles.
[0028] Furthermore, when an unwashed container molded using the polyethylene resin is filled with ultrapure water, the number of particles of 0.1 μm or more eluted from the container is preferably 10 particles / mL or less after storage at 40° C. for 35 days. If the number of particles of 0.1 μm or more is 10 particles / mL or less, the container can be adapted to the miniaturization of LSIs.
[0029] The high-purity chemical container obtained using this polyethylene resin has an inner area of 5000 cm 2 It is preferably used for the following small containers, for example, containers with a capacity of 10 mL to 20 L. EXAMPLES
[0030] The present invention will be described below with reference to examples, but is not limited to these examples. The test methods used in the examples and comparative examples are as follows.
[0031] (1) Density The measurement was performed by the density gradient tube method in accordance with JIS K6922-1.
[0032] (2) HLMFR The measurement was performed in accordance with JIS K6922-1 at 190°C and a load of 21.6 kg.
[0033] (3)MFR The measurement was performed in accordance with JIS K6922-1 at 190°C and a load of 2.16 kg.
[0034] (4) Mw / Mn The molecular weight was measured by GPC using Tosoh HLC-8321GPC / HT (columns: Tosoh TSKgel guardcolumn HHR and TSKgel GMHHR-H) and 1,2,4-trichlorobenzene as the eluent. The molecular weight calibration curve was calibrated using polystyrene samples with known molecular weights.
[0035] (5) Components with a molecular weight of 1,000 or less The ratio of the integral amount of components having a molecular weight of 1000 or less was calculated from the molecular weight distribution curve obtained by GPC measurement.
[0036] (6)Contained metal content The polyethylene resin was incinerated and then fused with an alkali to produce a solution, which was used as the measurement solution. The amount of metal contained in the sample was measured by ICP-AES measurement using an Optima 8300.
[0037] (7) Environmental Stress Cracking Resistance (ESCR) In accordance with JIS K6922-2, the test piece was immersed in a nonionic surfactant (10 wt% aqueous solution) at 50°C, and the time it took for the test piece to break with a 50% probability (F50 value) was measured.
[0038] (8) Blow molding Using a direct blow molding machine MSE-50E / 54M-A (manufactured by Tahara Co., Ltd.) with a 50 mm diameter extrusion screw, the parison was continuously extruded from the tip of the die at a cylinder temperature of 190 to 200 °C and a screw rotation speed of 10 to 18 revolutions, resulting in an average wall thickness of 1 mm and an internal volume of 800 mL (internal area = 560 cm). 2 ) or 500mL (internal area = 420cm 2 ) containers were molded.
[0039] (9) Ratio of the deployed area of the container inner surface Containers with an internal volume of 800 mL or 500 mL obtained by blow molding polyethylene resin were used. The surface area and area of the inner surface of the container body were measured using a shape measuring laser microscope (Keyence Corporation, VK-X200), and the developed area ratio (surface area / area) was calculated.
[0040] (10) Maximum roughness of the container inner surface Rz The maximum roughness Rz value of the inner surface of the container body was measured using a shape measuring laser microscope (Keyence Corporation, VK-X200).
[0041] (11) Gloss of the inner surface of the container The gloss of the inner surface of the container body at an incident angle of 60° was measured using a variable angle glossmeter (300A, manufactured by NIPPON DENSYOKU).
[0042] (12) Number of fine particles In a clean room at 23°C, an unwashed container was filled with ultrapure water to 80% of its internal volume, the container was capped and shaken 15 times, and then left to stand for 35 days in a clean oven (Yamato Scientific Co., Ltd., DE411) set at 40°C. The number of particles of 0.1 μm or more in the filled water was then measured using a particle counter (Rion Co., Ltd., controller: KE-40B1, particle sensor: KS-42A). The number of particles in the water is expressed in particles / mL.
[0043] Example 1 Preparation of Solid Catalyst Component In a 3L glass flask equipped with a stirrer, 30.0g (1.23mol) of metallic magnesium powder and 168.0g (0.494mol) of titanium tetrabutoxide were placed, and 192g (2.59mol) of n-butanol in which 1.5g of iodine had been dissolved was added over a period of 2 hours at 90°C. The mixture was then stirred for 2 hours at 140°C under a nitrogen seal while removing the hydrogen gas that was generated. After this was brought to 110°C, 26g (0.125mol) of tetraethoxysilane and 19g (0.125mol) of tetramethoxysilane were added, and the mixture was further stirred for 2 hours at 140°C. Next, 2.1 liters of hexane was added to obtain a homogeneous solution.
[0044] This homogeneous solution was placed in a 10L stainless steel autoclave equipped with a stirrer, and the internal temperature of the autoclave was kept at 45°C. 800mL of a hexane solution containing 1.0mol of diethylaluminum chloride and 0.5mol of i-butylaluminum dichloride was added over 1 hour, and the mixture was stirred at 60°C for 1 hour to generate particles. After the temperature was returned to 45°C, 1.04kg (3.35mol) of a 50% hexane solution was added over 2 hours. After all the contents were added, the mixture was stirred at 60°C for 1 hour to obtain a solid catalyst component. The obtained solid catalyst component was used to remove remaining unreacted materials and by-products using hexane, and then used as a hexane slurry for the production of polyethylene resin.
[0045] <Production of Polyethylene A> The reactor was operated at a temperature of 85°C and a total pressure of 30 kg / cm while feeding 110 L / hr of dehydrated and purified hexane, 110 mmol of tributylaluminum as an organoaluminum compound, 0.4 g / hr of a solid catalyst component, 25.4 kg / hr of ethylene, and 0.45 mol / mol of hydrogen to the first stage of a 370 L continuous polymerization reactor. 2 The first stage of ethylene polymerization (low molecular weight fraction) was carried out continuously under the conditions of an average residence time of 3.4 hours. The MFR of the low molecular weight fraction was 35 g / 10 min and the density was 0.968 g / cm. 3 It was.
[0046] The hexane slurry containing the first-stage polymer was subjected to removal of unreacted hydrogen and ethylene in a flash tank, and then introduced into a second-stage polymerization reactor having an internal volume of 545 L. While additional hexane was supplied to this polymerization reactor at 45 L / hr, ethylene was supplied at 21.5 kg / hr, 1-butene at 1.9 kg / hr, and hydrogen at a concentration relative to ethylene of 0.016 mol / mol, respectively, and the polymerization was continued at a temperature of 80° C. and a total pressure of 20 kPa / cm. 2 Ethylene polymerization (high molecular weight fraction) was carried out under the conditions of an average residence time of 3.3 hours. The HLMFR of the high molecular weight fraction was 2.2 g / 10 min and the density was 0.930 g / cm 3The discharge from the second-stage polymerization reactor was passed through a flash tank to remove unreacted hydrogen, ethylene, and 1-butene, and was then washed with 50 L / hour of hexane before being dried to obtain a powder mixture of ethylene-based copolymers. The proportion of low molecular weight components was 55% by weight, and the proportion of high molecular weight components was 45% by weight. The powder polymerized in two stages in the above manufacturing process was pelletized without the addition of any additives, to obtain polyethylene A. The results of the physical property measurements are shown in Table 1.
[0047] Polyethylene A was used to mold an 800 mL container, and the above-mentioned evaluation of the container's inner surface and measurement of fine particles were carried out using the resulting container. The results are shown in Table 1.
[0048] Example 2 The same polyethylene A as in Example 1 was used to mold a 500 mL container, and the above-mentioned evaluation of the inner surface of the container and measurement of fine particles were carried out using the resulting container. The results are shown in Table 1.
[0049] Example 3 <Production of Polyethylene B> Ethylene and butene-1 were copolymerized in hexane in the same manner as in Example 1, except that hydrogen was supplied to the first-stage polymerization reactor at a concentration ratio to ethylene of 0.40 mol / mol, and 1-butene was supplied to the second-stage polymerization reactor at 2.5 kg / hr and hydrogen was supplied to the second-stage polymerization reactor at a concentration ratio to ethylene of 0.020 mol / mol. Polymer powder was obtained by a two-stage polymerization method. The MFR of the low molecular weight component in the first-stage polymerization reactor was 27 g / 10 min, and the density was 0.967 g / cm. 3 The HLMFR of the high molecular weight component in the second stage polymerization reactor was 3.2 g / 10 min, and the density was 0.928 g / cm 3 The powder obtained by the two-stage polymerization was pelletized without adding any additives to obtain polyethylene B. The results of the measurement of the physical properties are shown in Table 1.
[0050] Polyethylene B was used to mold an 800 mL container, and the above-mentioned evaluation of the container's inner surface and measurement of fine particles were carried out using the resulting container. The results are shown in Table 1.
[0051] Comparative Example 1 <Production of Polyethylene C> Ethylene and butene-1 were copolymerized in hexane in the same manner as in Example 1, to obtain a polymerized powder by a two-stage polymerization method, except that hydrogen was supplied to the first-stage polymerization reactor at a concentration ratio to ethylene of 0.25 mol / mol and hydrogen was supplied to the second-stage polymerization reactor at a concentration ratio to ethylene of 0.050 mol / mol.
[0052] The MFR of the low molecular weight component in the first stage polymerization reactor was 18 g / 10 min, and the density was 0.967 g / cm 3 The HLMFR of the high molecular weight component in the second stage polymerization reactor was 8.5 g / 10 min, and the density was 0.932 g / cm 3 The powder obtained by the two-stage polymerization was pelletized without adding any additives to obtain polyethylene C. The results of the measurement of the physical properties are shown in Table 1.
[0053] Polyethylene C was used to mold an 800 mL container, and the above-mentioned evaluation of the container's inner surface and measurement of fine particles were carried out using the resulting container. The results are shown in Table 1. Comparative Example 2 <Production of Polyethylene D> Ethylene and butene-1 were copolymerized in hexane in the same manner as in Example 1, to obtain a polymerized powder by a two-stage polymerization method, except that hydrogen was supplied to the first-stage polymerization reactor at a concentration ratio to ethylene of 0.70 mol / mol and hydrogen was supplied to the second-stage polymerization reactor at a concentration ratio to ethylene of 0.010 mol / mol.
[0054] The MFR of the low molecular weight component in the first stage polymerization reactor was 50 g / 10 min, and the density was 0.969 g / cm 3 The HLMFR of the high molecular weight component in the second stage polymerization reactor was 1.4 g / 10 min, and the density was 0.927 g / cm 3 The powder obtained by the two-stage polymerization was pelletized without adding any additives to obtain polyethylene D. The results of the measurement of the physical properties are shown in Table 1.
[0055] Polyethylene D was used to mold an 800 mL container, and the above-mentioned evaluation of the container's inner surface and measurement of fine particles were carried out using the resulting container. The results are shown in Table 1.
[0056] Comparative Example 3 The same polyethylene D as in Comparative Example 2 was used to mold a 500 mL container, and the above-mentioned evaluation of the inner surface of the container and measurement of fine particles were carried out using the resulting container. The results are shown in Table 1.
[0057] Comparative Example 4 As polyethylene E, the following commercially available high-density polyethylene was used.
[0058] Tosoh Corporation, product name: Nipolon Hard 8022 (MFR = 0.35 g / 10 min, density = 0.958 g / cm 3 , no additives added) An 800 mL container was molded using polyethylene E, and the above-mentioned evaluation of the container's inner surface and measurement of the number of fine particles were carried out. The evaluation results of the resin's physical properties and the container are shown in Table 1.
[0059] Comparative Example 5 As polyethylene F, the following commercially available high-density polyethylene was used.
[0060] Tosoh Corporation, (product name) Nipolon Hard 5110 (MFR = 0.9 g / 10 min, density = 0.961 g / cm 3 , with additives) An 800 mL container was molded using polyethylene F, and the above-mentioned evaluation of the inner surface of the container and measurement of the number of fine particles were carried out. The evaluation results of the physical properties of the resin and the container are shown in Table 1.
[0061] Comparative Example 6 As polyethylene G, the following commercially available high-density polyethylene was used.
[0062] Tosoh Corporation, (product name) Nipolon Hard 8D01A (MFR = 0.05 g / 10 min, density = 0.957 g / cm 3 , no additives added) Polyethylene G was used to mold an 800 mL container, and the above-mentioned evaluation of the container's inner surface and measurement of the number of fine particles were carried out. The evaluation results of the resin's physical properties and the container are shown in Table 1.
[0063] [Table 1]
Claims
1. Melt flow rate (MFR) at 190°C and 2.16 kg load is 20 to 40 g / 10 min, density (JIS K6922-1) is 0.960 to 0.970 g / cm 3 and a polymer having a melt flow rate (HLMFR) of 0.10 to 10 g / 10 min at 190 ° C. and a load of 21.6 kg and a density of 0.920 to 0.940 g / cm 3 The polyethylene resin contains two ethylene polymer components, the weight ratio of which is 40:60 to 60:40, and has the following properties (1) to (9): (1) Density is 0.945 to 0.955 g / cm 3 (2) HLMFR at 190°C and a load of 21.6 kg is 21 to 80 g / 10 min. (3) MFR at 190° C. and a load of 2.16 kg is 0.5 to 1.5 g / 10 min. (4) The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) determined by gel permeation chromatography (GPC) is 5.0 to 7.
9. (5) In a molecular weight distribution curve obtained using GPC, the content of components having a molecular weight of 1,000 or less is 0.30% by weight or less. (6) Metal content is 15 ppm or less for polyethylene resin (7) Environmental stress crack resistance (ESCR) of 100 hours or more
2. 10. The polyethylene resin of claim 1 which is additive-free.
3. A high-purity chemical container made of the polyethylene resin according to claim 1 or 2.
4. 4. The container for high-purity chemicals according to claim 3, wherein the developed area ratio of the container inner surface is 1.10 or less.
5. 4. The container for high-purity chemicals according to claim 3, wherein the surface roughness Rz of the inner surface of the container is 10 μm or less.
6. 4. The container for high purity chemicals according to claim 3, wherein the gloss of the inner surface of the container is 40% or more.
7. 4. The high-purity chemical container according to claim 3, wherein the number of particles of 0.1 μm or more eluted from the content liquid container after filling the unwashed container with ultrapure water and storing it at 40° C. for 35 days is 10 particles / mL or less.
Citation Information
Patent Citations
Polyolefin for container for aqueous hydrogen peroxide solution
JP1995062161A
Container for high-purity solvent
JP1995257540A
Polyethylene resin for highly pure reagent container and highly pure reagent container comprising same
JP1999080257A
Polyethylene resin for ultra-high purity chemical containers and high purity chemical containers made therefrom
JP6705157B2
Blow-molded container
WO2000017057A1