Powder compact
A silane coupling agent and silicone resin coating on soft magnetic powder in powder compacts addresses weak binding issues, preventing chipping and cracking while maintaining magnetic properties and density.
Patent Information
- Application Number
- JP2023045147
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
In pressure molding of powder compacts, weak binding forces between soft magnetic powders lead to chipping and cracking, making it difficult to form the desired shape.
A powder compact comprising soft magnetic powder coated with an insulating coating layer containing a silane coupling agent and silicone resin, with a molecular weight of 244.4 to 260.4, and an optimal addition of 0.3 to 1.5 wt% silane coupling agent, enhances binding and prevents chipping and cracking.
The solution effectively reduces chipping and cracking, maintains stable core loss, and improves the density and magnetic properties of the powder compact.
Smart Images

Figure 2024134785000006 
Figure 2024134785000007 
Figure 2024134785000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder compact. [Background technology]
[0002] Coil components such as reactors are used in a variety of applications, including office equipment, solar power generation systems, automobiles, and uninterruptible power supplies. For example, a reactor is an electromagnetic component that converts electrical energy into magnetic energy and stores and releases it. A reactor mainly comprises a core and a coil. The coil is wound around the core. When power is supplied to the coil, it generates magnetic flux. The core is ring-shaped. The core becomes a magnetic path through which the magnetic flux generated by the coil flows.
[0003] Powder magnetic cores are sometimes used as reactor cores. Powder magnetic cores are produced by heat treating a powder compact. Powder compacts are produced, for example, by compacting soft magnetic powder with an insulating coating formed on the surface. In this compacting, a pressure of 10 to 20 ton / cm is generally used. 2 This is done under high pressure. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-125622 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the case of high pressure compaction, if the binding strength between the soft magnetic powder particles is weak, chips and cracks will occur in the compact. In some cases, the legs of the compact may come off, making it impossible to form the compact into the desired shape.
[0006] The present invention has been made to solve the above problems, and an object of the present invention is to provide a powder molded body that can prevent chipping and cracks from occurring in the powder molded body. [Means for solving the problem]
[0007] The powder compact of the present invention comprises a soft magnetic powder and an insulating coating layer covering the soft magnetic powder, the insulating coating layer containing a silicone resin and a silane coupling agent, and the molecular weight of the silane coupling agent is 244.4 or more and 260.4 or less. Effect of the Invention
[0008] According to the present invention, it is possible to obtain a powder compact that is capable of preventing chipping and cracks from occurring in the powder compact. [Brief description of the drawings]
[0009] [Figure 1] 1 is a graph showing the relationship between the Rattra value and the molecular weight of the silane coupling agent when the amount of the silane coupling agent added is 0.5 wt %. [Diagram 2] 1 is a graph showing the relationship between the Rattra value and the molecular weight of the silane coupling agent when the amount of the silane coupling agent added is 1.0 wt %. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The configuration of the powder molded body of this embodiment will be described below. Note that the present invention is not limited to the embodiment described below.
[0011] Coil components such as reactors have a core containing a magnetic material. Powder magnetic cores are used as the core. Powder magnetic cores are produced by compressing soft magnetic powder into a powder compact and then subjecting the powder compact to a heat treatment called annealing.
[0012] The powder compact of the present embodiment includes a soft magnetic powder and an insulating coating layer. The insulating coating layer covers the surface of the soft magnetic powder. The insulating coating layer contains a silane coupling agent and a silicone resin.
[0013] The soft magnetic powder is mainly composed of iron. As the soft magnetic powder, pure iron powder, permalloy (Fe-Ni alloy) mainly composed of iron, Si-containing iron alloy (Fe-Si alloy), sendust alloy (Fe-Si-Al alloy), or a mixture of two or more of these powders can be used. In addition, amorphous alloy and nanocrystalline alloy powder can be used as the soft magnetic powder. The particle size (median size D50) of the soft magnetic powder is preferably 1 μm or more and 200 μm or less.
[0014] The Fe-Si-Al alloy powder contains, for example, about 7 wt% to 11 wt% of Si and about 4 wt% to 8 wt% of Al relative to Fe. The Fe-Si-Al alloy powder may contain, for example, about 1 wt% to 3 wt% of Ni relative to Fe. Furthermore, the Fe-Si-Al alloy powder may contain Co, Cr, or Mn.
[0015] The Si-containing iron alloy may contain Co, Al, Cr, or Mn. When using permalloy (Fe-Ni alloy), the ratio of Ni to Fe is preferably 50:50 or 25:75, but may be other ratios. For example, Fe-80Ni, Fe-36Ni, Fe-78Ni, or Fe-47Ni may be used. In addition to Fe and Ni, Si, Cr, Mo, Cu, Nb, Ta, etc. may be contained. Examples of Fe-Si alloy powder include Fe-3.5%Si alloy powder and Fe-6.5%Si alloy powder, but the ratio of Si to Fe may be other than 3.5% or 6.5%. Pure iron powder contains Fe at 99% or more.
[0016] The soft magnetic powder may be produced by a pulverization method or an atomization method, which may be any of water atomization, gas atomization, and water gas atomization.
[0017] However, since the pulverized powder produced by the pulverization method is non-circular, the soft magnetic powder particles tend to bond together, and chips and cracks are unlikely to occur in the green compact. On the other hand, the gas atomized powder produced by the atomization method, particularly the gas atomization method, is circular, and therefore has weak binding properties, making the green compact brittle. For this reason, the soft magnetic powder is preferably a gas atomized powder, which significantly exhibits the effect of the present invention of preventing chips and cracks from occurring in the green compact.
[0018] The circularity of the soft magnetic powder is preferably 0.8 or more in terms of the powder with an average particle size (median diameter D50). When the circularity is 0.8 or more, the binding between the soft magnetic powder particles is weak, and the powder compact is easily brittle. Therefore, when the circularity of the soft magnetic powder is 0.8 or more, the effect of the present invention is remarkable. In addition, the Vickers hardness of the soft magnetic powder is preferably 400HV or more. In the case of a hard soft magnetic powder with a Vickers hardness of 400HV or more, the binding between the soft magnetic powder particles is weak, and the powder compact is easily brittle, so the effect of the present invention is remarkable.
[0019] An insulating coating layer is formed on the surface of the soft magnetic powder. The insulating coating layer contains a silane coupling agent and a silicone resin. The insulating coating layer can be applied to the surface of each individual particle of the soft magnetic powder, or to a surface of a bonded particle formed by bonding several particles. It can also be applied to the entire surface or a part of the surface of a particle. In other words, the insulating coating layer does not need to completely cover the surface of the soft magnetic powder, and can be applied to a part of the surface of the soft magnetic powder.
[0020] The silane coupling agent may have a molecular weight of 244.4 or more and 260.4 or less. Examples of the silane coupling agent that may be used include dimethoxydiphenylsilane, 3-glycidoxypropylmethyldiethoxysilane, hexyltriethoxysilane, and 3-methacryloxypropylmethyldiethoxysilane. By setting the molecular weight of the silane coupling agent to 244.4 or more and 260.4 or less, chipping and cracking of the powder compact can be prevented. In particular, it is preferable to set the molecular weight of the silane coupling agent to 244.4 or more and 248.4 or less. By setting the molecular weight within this range, chipping and cracking of the powder compact can be prevented, and the iron loss can be stably low.
[0021] The amount of the silane coupling agent added is preferably 0.3 wt% or more, more preferably 0.5 wt% or more, relative to the soft magnetic powder. When the amount of the silane coupling agent added is 0.3 wt% or more, the effect of preventing chipping and cracks from occurring in the powder compact is exhibited, and when the amount is 0.5 wt% or more, the effect becomes more remarkable.
[0022] In particular, it is preferable that the molecular weight of the silane coupling agent is 244.4 or more and 248.4 or less, and the amount of the silane coupling agent added is 1.0 wt% or more. By setting the molecular weight and amount of the silane coupling agent within this range, the effect of preventing chipping and cracks from occurring in the powder compact becomes more remarkable.
[0023] The upper limit of the amount of the silane coupling agent added is preferably 1.5wt% relative to the soft magnetic powder. When the amount of the silane coupling agent added is 1.5wt%, the iron loss tends to worsen slightly compared to when the silane coupling agent is added at 1.0wt%. Therefore, when the amount of the silane coupling agent added exceeds 1.5wt%, there is a risk that the iron loss will worsen further, so it is preferable to set the upper limit at 1.5wt%.
[0024] Examples of the silicone resin that can be used include silicone resin and silicone oligomer. Silicone resin is a resin that has a siloxane bond (Si-O-Si) as its main structure. By using silicone resin, an insulating coating layer with excellent flexibility can be formed. Examples of the silicone resin that can be used include methyl-based, methylphenyl-based, propylphenyl-based, epoxy resin-modified, alkyd resin-modified, polyester resin-modified, and rubber-based silicone resins.
[0025] Examples of silicone oligomers that can be used include methyl-based and methylphenyl-based ones that have an alkoxysilyl group but no reactive functional group, epoxy-based, epoxymethyl-based, mercapto-based, mercaptomethyl-based, acrylmethyl-based, methacrylmethyl-based, and vinylphenyl-based ones that have an alkoxysilyl group and a reactive functional group, and alicyclic epoxy-based ones that have a reactive functional group instead of an alkoxysilyl group.
[0026] As the silicone resin, it is preferable to use a methylphenyl-based resin. Specifically, it is preferable to use a methylphenyl-based silicone resin or a silicone oligomer. When a methylphenyl-based silicone resin is used, it is possible to form an insulating coating layer with little loss in weight upon heating and excellent heat resistance. Also, when a methylphenyl-based silicone oligomer is used, it is possible to form a thick and hard insulating coating layer.
[0027] The amount of silicone resin added is preferably 0.3 wt% or more and 2.0 wt% or less relative to the soft magnetic powder. If the amount added is less than 0.3 wt%, it will not function as an insulating coating layer, and eddy current loss will increase, resulting in reduced magnetic properties. If the amount added is more than 2.0 wt%, it will result in a reduced density of the powder compact.
[0028] After adding and mixing the silane coupling agent and silicone resin to the soft magnetic powder, the powder is heated and dried to form an insulating coating layer on the surface of the soft magnetic powder. The heating and drying conditions are not limited to the above, but are preferably at a temperature of 25°C or higher and 350°C or lower for about 2 hours.
[0029] The insulating coating layer may be a mixed layer of a silane coupling agent and a silicone resin, or a layer of a silane coupling agent and a layer of a silicone resin may be laminated. For example, when the insulating coating layer is laminated in the order of a layer of a silane coupling agent and a layer of a silicone resin, first, a silane coupling agent is added to and mixed with a soft magnetic powder, and then the soft magnetic powder on which the layer of the silane coupling agent has been formed is heated and dried. Then, a silicone resin is added to and mixed with the soft magnetic powder on which the layer of the silane coupling agent has been formed, and the soft magnetic powder is heated and dried to form a layer of the silicone resin on the surface of the layer of the silane coupling agent.
[0030] A lubricant may be added to the soft magnetic powder on which the insulating coating layer is formed. Examples of the lubricant include, but are not limited to, stearic acid, calcium stearate, lithium stearate, aluminum stearate, zinc stearate, ethylene bisstearamide, ethylene bisstearamide, and ethylene bisstearamide. By mixing the lubricant, the soft magnetic powder can slide easily, so that the density of the green compact can be increased. Furthermore, it is possible to reduce the upper punch pressure during compaction and prevent the occurrence of vertical streaks on the core wall surface due to contact between the die and the soft magnetic powder.
[0031] The amount of lubricant added is preferably about 0.2wt% to 0.8wt% of the soft magnetic powder. By setting the amount in this range, the sliding between the soft magnetic powder particles can be further improved. The lubricant may be added twice, before and after the insulating coating layer is formed. That is, the lubricant may be added to the soft magnetic powder before the silane coupling agent and silicone resin are added, and then the lubricant may be added to the soft magnetic powder on which the insulating coating layer has been formed.
[0032] After adding the lubricant, the soft magnetic powder is poured into a die and pressure-molded. This pressure molding produces a green compact. In the pressure molding, the soft magnetic powder is subjected to a pressure of 10 to 20 ton / cm 2 A pressure of about 12 to 15 ton / cm is applied to produce a green compact.2 degree is more preferable.
[0033] Thereafter, the powder compact produced by the pressure molding is heat-treated in a non-oxidizing atmosphere such as nitrogen gas or a mixed gas of nitrogen and hydrogen, or in air at a temperature of 600°C or higher and lower than the temperature at which the insulating coating layer covering the soft magnetic powder is destroyed (for example, 900°C). Through this heat treatment, a powder magnetic core is produced.
[0034] (Example) The present invention will be described in more detail with reference to the following examples. However, the present invention is not limited to the following examples. Powder compacts of Examples 1 to 18 and Comparative Examples 1 to 14 were produced. The powder compacts of Examples 1 to 18 and Comparative Examples 1 to 14 differ only in the type and amount of the silane coupling agent added.
[0035] First, a powder compact was produced in Example 1. Fe-Si-Al alloy powder produced by gas atomization was used as the soft magnetic powder. The particle size and circularity of the Fe-Si-Al alloy powder are shown in Table 1 below.
[0036] [Table 1]
[0037] First, a lubricant was added to the Fe-Si-Al alloy powder. Stearic acid (D50=100 μm, melting point 57° C.) was used as the lubricant. 0.3 wt % of stearic acid was added to the Fe-Si-Al alloy powder and mixed.
[0038] After adding and mixing stearic acid, the silane coupling agent was added and mixed. Then, silicone resin was added and mixed. As the silane coupling agent, "C dimethoxydiphenylsilane" (product name: KBM202SS) shown in Table 2 below was used. Dimethoxydiphenylsilane was added at 0.3 wt% to the Fe-Si-Al alloy powder.
[0039] [Table 2]
[0040] Methylphenyl silicone resin was used as the silicone resin. 1.2wt% of silicone resin was added to the Fe-Si-Al alloy powder. After adding and mixing the silicone resin, the mixture was dried by heating. The drying temperature was 130℃, and the drying time was 2 hours.
[0041] After heating and drying, the Fe-Si-Al alloy powder was passed through a sieve with 850 μm openings to break up the agglomerates. Then, a lubricant was added again and mixed. The lubricant used in this case was aluminum stearate (D50=21 μm, melting point 110°C). Aluminum stearate was added at 0.2 wt% to the Fe-Si-Al alloy powder.
[0042] After adding and mixing the lubricant, the Fe-Si-Al alloy powder with the lubricant was filled into a die and pressed to produce a cylindrical green compact with an outer diameter of 11.3 mm and a height of 10.0 mm (height dimensional tolerance ±0.1 mm). The pressure for the press molding was 12.0 ton / cm. 2 Five powder compacts of Example 1 were produced.
[0043] Examples 2 to 5 differ from Example 1 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same materials, the same manufacturing method, and the same conditions as Example 1. The amount of silane coupling agent added is 0.5 wt% in Example 2, 0.7 wt% in Example 3, 1.0 wt% in Example 4, and 1.5 wt% in Example 5.
[0044] Example 6 differs from Example 1 only in the type of silane coupling agent, and the rest, including the amount of silane coupling agent added, are the same materials, the same manufacturing method, and the same conditions as Example 1. The silane coupling agent used in Example 6 was "D 3-glycidoxypropylmethyldiethoxysilane" (product name: KBE-402) shown in Table 2 above.
[0045] Examples 7 to 10 differ from Example 6 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same materials, the same manufacturing method, and the same conditions as Example 6. The amount of silane coupling agent added is 0.5 wt% in Example 7, 0.7 wt% in Example 8, 1.0 wt% in Example 9, and 1.5 wt% in Example 10.
[0046] Example 11 differs from Example 1 only in the type of silane coupling agent, and the rest, including the amount of silane coupling agent added, are the same materials, the same manufacturing method, and the same conditions as Example 1. The silane coupling agent in Example 11 was "E hexyltriethoxysilane" (product name: KBE-3063) shown in Table 2 above.
[0047] Examples 12 to 14 differ from Example 11 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same as those in Example 11, using the same materials, manufacturing method, and conditions. The amount of silane coupling agent added is 0.5 wt% in Example 12, 1.0 wt% in Example 13, and 1.5 wt% in Example 14.
[0048] Example 15 differs from Example 1 only in the type of silane coupling agent, and the rest, including the amount of silane coupling agent added, are the same materials, the same manufacturing method, and the same conditions as Example 1. The silane coupling agent in Example 15 was "F 3-methacryloxypropylmethyldiethoxysilane" (product name: KBE-502) shown in Table 2 above.
[0049] Examples 16 to 18 differ from Example 15 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same as those in Example 15, using the same materials, manufacturing method, and conditions. The amount of silane coupling agent added is 0.5 wt% in Example 16, 1.0 wt% in Example 17, and 1.5 wt% in Example 18.
[0050] Next, the preparation of the powder compacts of Comparative Examples 1 to 14 will be described. Comparative Example 1 differs from Example 1 only in that a silane coupling agent was not added. That is, the insulating coating layer of Comparative Example 1 contains only silicone resin, and does not contain a silane coupling agent. In Comparative Example 1, the materials, manufacturing method, and conditions are otherwise the same as those of Example 1.
[0051] Comparative Example 2 differs from Example 1 only in the type and amount of silane coupling agent, and the rest of the materials, manufacturing method, and conditions are the same as those of Example 1. The silane coupling agent used in Comparative Example 2 was "A Tetraethoxysilane" (product name: TES28) shown in Table 2 above. The amount of silane coupling agent added was 0.5 wt%.
[0052] Comparative Example 3 differs from Example 1 only in the type of silane coupling agent, and the rest, including the amount of silane coupling agent added, are the same materials, the same manufacturing method, and the same conditions as Example 1. The silane coupling agent in Comparative Example 3 was "B Phenyltriethoxysilane" (product name: KBE-103) shown in Table 2 above.
[0053] Comparative Examples 4 to 6 differ from Comparative Example 3 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same as those in Comparative Example 3, using the same materials, manufacturing method, and conditions. The amount of silane coupling agent added is 0.5 wt% in Comparative Example 4, 1.0 wt% in Comparative Example 5, and 1.5 wt% in Comparative Example 6.
[0054] Comparative Example 7 differs from Example 1 only in the type of silane coupling agent, and the rest, including the amount of silane coupling agent added, are the same materials, the same manufacturing method, and the same conditions as Example 1. The silane coupling agent in Comparative Example 7 was "G 3-methacryloxypropyltriethoxysilane" (product name: KBE-503) shown in Table 2 above.
[0055] Comparative Examples 8 to 10 differ only in the amount of silane coupling agent added from Comparative Example 7, and the rest, including the type of silane coupling agent, are the same as those in Comparative Example 7, using the same materials, manufacturing method, and conditions. The amount of silane coupling agent added is 0.5 wt% in Comparative Example 8, 1.0 wt% in Comparative Example 9, and 1.5 wt% in Comparative Example 10.
[0056] Comparative Example 11 differs from Example 1 only in the type of silane coupling agent, and the rest, including the amount of silane coupling agent added, are the same materials, the same manufacturing method, and the same conditions as Example 1. The silane coupling agent in Comparative Example 11 was "H 1,6-bis(trimethoxysilyl)hexane" (product name: KBM-3066) shown in Table 2 above.
[0057] Comparative Examples 12 to 14 differ from Comparative Example 11 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same as those of Comparative Example 11, using the same materials, manufacturing method, and conditions. The amount of silane coupling agent added is 0.5 wt% in Comparative Example 12, 1.0 wt% in Comparative Example 13, and 1.5 wt% in Comparative Example 14.
[0058] The rattle values of the green compacts of Examples 1 to 18 and Comparative Examples 1 to 14 prepared as described above were measured. A rattle tester (manufactured by Intesco Co., Ltd.) was used to measure the rattle values. The rattle values were measured based on the Japan Powder Metallurgy Association (JPMA) standard method for measuring the rattle values of metal green compacts (JPMA P11 1992).
[0059] First, the total weight of five powder compacts of Examples 1 to 18 and Comparative Examples 1 to 14 was measured before being put into the Rattler tester. Then, the five powder compacts were put into a cylindrical cage covered with a 14 mesh stainless steel wire mesh and rotated 100 times at a rotation speed of 87 rpm. Finally, the total weight of the five powder compacts taken out of the Rattler tester was measured. Then, the total weight measured after rotation was subtracted from the total weight measured before rotation to obtain the weight reduction rate, thereby calculating the Rattler value. That is, the Rattler value was calculated from the following calculation formula (1). S = ((AB) / A) × 100 (1) S: Rattler value (%) A: Total weight of the five green compacts before testing (g) B: Total weight of the five compacts after testing (g)
[0060] The calculation results are shown in Table 3 below. Figure 1 shows a graph showing the relationship between the Rattra value and the molecular weight of the silane coupling agent when the amount of the silane coupling agent added is 0.5 wt%. Figure 2 shows a graph showing the relationship between the Rattra value and the molecular weight of the silane coupling agent when the amount of the silane coupling agent added is 1.0 wt%.
[0061] [Table 3]
[0062] As shown in Table 3, in Examples 1 to 18 in which the molecular weight of the silane coupling agent was 244.4 or more and 260.4 or less, even the highest rattle value was lower than 35%, which was lower than the values in Comparative Examples 1 to 14. Therefore, it was confirmed that by setting the molecular weight of the silane coupling agent in the range of 244.4 or more and 260.4 or less, the rattle value was reduced, and chipping and cracking in the powder compact could be prevented.
[0063] It was confirmed that the rattle value decreased when the amount of the silane coupling agent added was 0.3 wt% or more. In addition, as shown in Fig. 1, it was confirmed that the rattle value decreased further to less than 30% in Examples 2 to 5, 7 to 10, 12 to 14, and 16 to 18, in which the amount of the silane coupling agent added was 0.5 wt% or more.
[0064] In particular, comparing Examples 2, 4 and 5, in which the molecular weight of the silane coupling agent is 244.4, with Comparative Examples 4, 5 and 6, in which the molecular weight of the silane coupling agent is 240.4, the rattle value of the Examples is significantly reduced to about 1 / 4 of that of Comparative Examples at each addition amount.Thus, it was confirmed that, even though the molecular weight of the silane coupling agent is only 4, when the molecular weight of the silane coupling agent is 244.4, the rattle value is dramatically reduced compared to that of the one with a molecular weight lower than 244.4.
[0065] Furthermore, as shown in FIG. 2, in Examples 4, 5, 9, 10, 13, 14, 17, and 18 in which the molecular weight of the silane coupling agent was 244.4 or more and 248.4 or less and the amount of the silane coupling agent added was 1.0 wt % or more, the Rattra value was confirmed to be approximately 15 or less, which is an extremely good value.
[0066] In addition, although the rattle value is slightly different between Examples 6 to 10 and Examples 11 to 14, in which the molecular weight of the silane coupling agent is the same, this is within the range of measurement error. In addition, the rattle value is an index regarding the chipping tendency of the molded body, so it does not correlate with the strength. In other words, it cannot be immediately said that the rattle value decreases as the strength increases.
[0067] Next, the powder compacts of Examples 19 and 20 and Comparative Example 15 were further produced. Example 19 differs from Example 7 only in that the powder of Example 19 was a pulverized powder produced by a pulverization method using Fe-Si-Al alloy powder. Other aspects, including the type and amount of the silane coupling agent, were the same as those of Example 7, using the same materials, manufacturing method, and conditions.
[0068] Example 20 differs from Example 2 only in that the powder of the Fe-Si-Al alloy powder was prepared by a pulverization method. The rest of the materials, manufacturing method, and conditions, including the type and amount of the silane coupling agent, were the same as those of Example 2.
[0069] Comparative Example 15 differs from Comparative Example 2 only in that the powder used is a pulverized powder made by pulverizing Fe-Si-Al alloy powder. The rest of the comparison, including the type and amount of silane coupling agent added, is the same as that of Comparative Example 2, using the same materials, manufacturing method, and conditions.
[0070] Five powder compacts were also prepared for each of Examples 19 and 20 and Comparative Example 15, and the Rattler values were calculated. The Rattler values were calculated using the same apparatus and under the same measurement conditions as above. The calculation results are shown in Table 4 below.
[0071] [Table 4]
[0072] As shown in Table 4, even when the Fe-Si-Al alloy powder is a pulverized powder, it was confirmed that the rattle value is lower in Examples 19 and 20, in which the molecular weight of the silane coupling agent is in the range of 244.4 to 260.4, than in Comparative Example 15. That is, it was confirmed that the type of soft magnetic powder is not limited to gas atomized powder, and the effect is also obtained even in pulverized powder.
[0073] However, looking at Comparative Example 15, the rattler value is 3.9%, which is originally a low value, and it is difficult to say that the rattler values of Examples 19 and 20 are dramatically lower than those of Comparative Example 15. On the other hand, the rattler value of Comparative Example 2, which is a gas atomized powder, is a high value of 58.0%. And the rattler values of Examples 2 and 7 are 16.0% and 29.0%, which are less than half of Comparative Example 2. Therefore, it was confirmed that the effect of lowering the rattler value is more remarkable when a silane coupling agent with a molecular weight of 244.4 or more and 260.4 or less is added to the soft magnetic powder, which is a gas atomized powder.
[0074] Powder magnetic cores of Examples 21 to 38 and Comparative Examples 16 to 27 were produced. The types and amounts of silane coupling agents in Examples 21 to 38 and Comparative Examples 16 to 27 correspond to Examples 1 to 18 and Comparative Examples 1 to 12, respectively. That is, the type and amount of silane coupling agent in Example 21 is the same as that in Example 1, the type and amount of silane coupling agent in Example 22 is the same as that in Example 2, and the type and amount of silane coupling agent in Comparative Example 27 is the same as that in Comparative Example 12. The powder compacts of Examples 21 to 38 and Comparative Examples 16 to 27 were produced using the same materials, the same manufacturing method, and the same conditions as the corresponding Examples or Comparative Examples up to the point where aluminum stearate (D50=21 μm, melting point 110° C.) was added and mixed as a lubricant.
[0075] The manufacturing methods of the powder compacts in Examples 21 to 38 and Comparative Examples 16 to 27 differ in the steps after pressure molding. After adding and mixing aluminum stearate as a lubricant, the Fe-Si-Al alloy powder was filled into a die and pressure molding was performed to produce a toroidal powder compact with an outer diameter of 16.5 mm, an inner diameter of 11.0 mm, and a height of 5.0 mm. The pressure for the press molding was 12.0 ton / cm. 2 In addition, in each of Examples 21 to 38 and Comparative Examples 16 to 27, only one powder compact was produced.
[0076] Thereafter, the powder compact was heat-treated to remove distortion caused by compaction. This heat treatment was performed in a nitrogen atmosphere at a temperature of 700°C. The heat treatment time was 2 hours. In this manner, each of the powder cores of Examples 21 to 38 and Comparative Examples 16 to 27 was produced. Then, the iron loss of each of the powder cores of Examples 21 to 38 and Comparative Examples 16 to 27 was measured.
[0077] When measuring the iron loss, 15 turns of φ0.5 mm copper wire were wound around the powder magnetic core as the primary winding and 15 turns as the secondary winding. Then, using a BH analyzer (Iwatsu Measurement Corporation: SY-8219), which is a magnetic measuring device, the iron loss Pcv (kW / m 3 The measurement results are shown in Table 5.
[0078] [Table 5]
[0079] As shown in Table 5, in Examples 21 to 38 in which the molecular weight of the silane coupling agent is in the range of 244.4 to 260.4, the iron loss is 300 kW / m 3 In particular, in Examples 21 to 34, in which the molecular weight of the silane coupling agent is in the range of 244.4 to 248.4, the iron loss is always 300 kW / m 3 It was confirmed that the iron loss was stably reduced as shown below.
[0080] In addition, the iron loss of Examples 25, 30, 34 and 38, which contain 1.5wt% silane coupling agent, is higher than that of the other examples containing the same type of silane coupling agent. In other words, if the amount of silane coupling agent is further increased, the iron loss may worsen. Therefore, it is presumed that the amount of silane coupling agent added is 1.5wt%, which results in a good rattler value, prevents chipping and cracking of the powder compact, and improves the magnetic properties.
[0081] (Other embodiments) In this specification, an embodiment of the present invention has been described, but this embodiment is presented as an example and is not intended to limit the scope of the invention. The above-mentioned embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the scope of the invention. The embodiment and its modifications are included in the scope of the invention and its equivalents described in the claims, as well as in the scope and gist of the invention.
Claims
1. A soft magnetic powder; An insulating coating layer that covers the periphery of the soft magnetic powder; Equipped with the insulating coating layer contains a silicone resin and a silane coupling agent, The molecular weight of the silane coupling agent is 244.4 or more and 260.4 or less; A powder compact characterized by the above.
2. The amount of the silane coupling agent added is 0.5 wt % or more based on the soft magnetic powder; The powder compact according to claim 1 ,
3. The molecular weight of the silane coupling agent is 244.4 or more and 248.4 or less, The amount of the silane coupling agent added is 1.0 wt % or more based on the soft magnetic powder; The powder compact according to claim 2 ,
4. The soft magnetic powder is a gas atomized powder; 4. The powder molded body according to claim 1, wherein
5. The silicone resin is a methylphenyl-based resin; 4. The powder molded body according to claim 1, wherein
6. The upper limit of the amount of the silane coupling agent added is 1.5 wt % or less with respect to the soft magnetic powder; 4. The powder molded body according to claim 1, wherein
Citation Information
Patent Citations
Forming method of display device barrier rib and paint for display device barrier rib formation used for it
JP2005322590A
Dust core and method for manufacturing the same
JP2011018822A
Dust core, coated metal powder for dust core, and methods for producing them
JP2013243268A
Powder for dust core, and dust core
JP2014019929A
Low-noise reactor, powder-compact magnetic core, and method for manufacturing the same
JP2015015364A
Cited By
Component hybridizing system allowing for defective planarity
US6399895B1