Method for producing recycled polyethylene terephthalate and recycled polyethylene terephthalate
By controlling antimony, titanium, and sodium contents and employing solid phase polymerization, the method produces recycled PET with improved hue and minimal color variation, addressing the hue issues in existing PET recycling methods.
Patent Information
- Application Number
- JP2023045258
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing methods for producing recycled polyethylene terephthalate (PET) do not adequately control the L and b values, leading to undesirable changes in hue after recycling.
The method involves using recovered PET flakes, controlling the content of antimony, titanium, and sodium within specific ranges, followed by solid phase polymerization to produce recycled PET with an L value of 78 or more, minimizing differences in hue from the raw material flakes.
The method results in recycled PET with excellent hue, maintaining a small difference in L and b values from the raw material flakes, suitable for a wide range of applications.
Smart Images

Figure 2024134850000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing recycled polyethylene terephthalate having an L value in a specific range using recovered polyethylene terephthalate. The present invention also relates to recycled polyethylene terephthalate containing specific elements in specific amounts and having an L value in a specific range. [Background technology]
[0002] Polyethylene terephthalate (hereinafter sometimes referred to as PET) is excellent in transparency, mechanical strength, and chemical properties, and is therefore widely used in clothing and industrial fibers, PET bottles and various functional films, and containers such as bottles made using the blow molding method. In recent years, interest in environmental issues has increased, and beverage manufacturers are trying to increase the proportion of PET bottles and clothing made from recycled polyethylene terephthalate, as typified by mechanical recycling. For example, the recovery and reuse of PET bottles has progressed at a high rate thanks to the development of infrastructure and social systems. Representative examples include the bottle-to-bottle method used in bottle manufacturing and the bottle-to-film method used in film manufacturing.
[0003] Patent Document 1 discloses that a polyester resin containing an aluminum compound or a phosphorus compound has excellent recyclability.
[0004] Patent Document 2 discloses a recycled polyester raw material that preferably contains antimony and has a relaxation time determined by a pulse NMR method that is equal to or longer than a specific time. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2022 / 234749 [Patent Document 2] JP 2023-006803 A Summary of the Invention [Problem to be solved by the invention]
[0006] The polyethylene terephthalate disclosed in Patent Documents 1 and 2 does not disclose the L value or b value after recycling, or the b value is high, and therefore it is considered that the recycled polyethylene terephthalate has room for improvement, for example, in terms of hue.
[0007] Therefore, an object of the present invention is to provide a method for providing recycled polyethylene terephthalate having improved color, and to provide recycled polyethylene terephthalate. [Means for solving the problem]
[0008] As a result of intensive research conducted by the present inventors to achieve the above object, they discovered that recycled polyethylene terephthalate can be obtained by, for example, melt extrusion molding recovered polyethylene terephthalate as raw material flakes to obtain pellets having a specific range of titanium, sodium, etc., and then subjecting the pellets to solid-phase polymerization, thereby obtaining recycled polyethylene terephthalate having small changes in a and b values compared to the raw material flakes, and thus completed the present invention. The present invention is specified by the following requirements.
[0009] [1] Using recycled polyethylene terephthalate flakes, After preparing polyethylene terephthalate pellets satisfying the following requirements (a), (b), and (c), solid-state polymerization is carried out; A method for producing recycled polyethylene terephthalate having an L value of 78 or more. (a) The antimony content is 50 to 400 ppm; (b) The sum of the titanium and sodium content is 10 ppm or less; (c) Titanium content is 0.1 ppm or more [2] A method for producing recycled polyethylene terephthalate according to [1], wherein the total content of titanium and sodium in the requirement (b) is 7 ppm or less. [3] The method for producing recycled polyethylene terephthalate according to [1] or [2], wherein the sodium content in the pellets is 0.3 ppm or more. [4] The method for producing recycled polyethylene terephthalate according to any one of [1] to [3], wherein in the requirement (c), the total content of titanium and sodium is 0.4 ppm or more. [5] Recycled polyethylene terephthalate that meets the following requirements (a), (b), and (c) and has an L value of 78 or more. (a) The antimony content is 50 to 400 ppm; (b) The sum of the titanium and sodium content is 10 ppm or less; (c) Titanium content is 0.1 ppm or more Effect of the Invention
[0010] According to the present invention, the recycled polyethylene terephthalate obtained by using recovered polyethylene terephthalate as raw material flakes has a small difference in a value and b value from the raw material flakes, i.e., it is a recycled polyethylene terephthalate with excellent hue. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. [Manufacturing method of recycled polyethylene terephthalate] The present invention is a method for producing recycled polyethylene terephthalate, which can produce recycled polyethylene terephthalate having a hue that is less different from that of the flakes of recovered polyethylene terephthalate, which is the raw material. The recycled polyethylene terephthalate also has an excellent hue. The recovered polyethylene terephthalate flakes that are the raw material and the production method will be described below in order.
[0012] <Recycled polyethylene terephthalate flakes> The recycled polyethylene terephthalate flakes used in the present invention can be obtained by washing PET bottles obtained by a domestic recycling system or the like in a known manner, cutting them, etc. The method for producing the flakes is not particularly limited.
[0013] The intrinsic viscosity (IV) of the recovered polyethylene terephthalate flakes is preferably 0.60 to 0.90 (dL / g). If the IV is outside the above range, it may be difficult to adjust the IV to a suitable range in the solid-phase polymerization step described below.
[0014] The hue of the recycled polyethylene terephthalate used in the present invention is not particularly limited, but one with excellent hue is preferred because the recycled polyethylene terephthalate has a wide range of uses, etc. Specifically, it is preferred that the L value is in the range of 60 to 90, the a value is in the range of -1 to 0.5, and the b value is in the range of -3 to 3.
[0015] The hue of the recovered polyethylene terephthalate can be measured by preparing a sample from the recovered polyethylene terephthalate and subjecting it to the method described in the Examples below.
[0016] <Pelletization of recycled polyethylene terephthalate> The present invention includes a step of pelletizing the above-mentioned recovered polyethylene terephthalate flakes by a known method.
[0017] The conditions of such a pelletizing process can be adopted from known suitable conditions without any restrictions. For example, when pelletizing by melt extrusion, specifically, the flakes are melted at a temperature of 190°C to 290°C, a twin-screw extruder or a single-screw extruder is used to obtain strands, and the strands are cooled with cooling water, and then cut with a cutter device to obtain pellets. In addition, a method such as underwater cutting can be adopted in the process after cooling. Usually, at this stage, a decrease in molecular weight occurs due to hydrolysis, etc. For example, the intrinsic viscosity (IV) value of the pellets tends to be 0.1 to 0.3 dL / g lower than that of the raw material flakes.
[0018] In the present invention, the pellets are (a) The antimony content is 50 to 400 ppm; (b) The sum of the titanium and sodium content is 10 ppm or less; (c) Titanium content is 0.1 ppm or more It is characterized by satisfying the requirements.
[0019] There is no limit to the method for controlling the content within such a range. For example, the method includes selecting flakes that satisfy the above requirements (a) to (c) as the raw material, mixing components containing various elements in the pelletizing process, and reducing the amount of specific elements contained in the flakes by setting up a contact (washing) process with water or the like. Of course, it is also possible to combine the above methods.
[0020] The lower limit of the antimony content is preferably 70 ppm, more preferably 80 ppm, even more preferably 90 ppm, and particularly preferably 100 ppm, while the upper limit is preferably 350 ppm, more preferably 330 ppm, even more preferably 310 ppm, and particularly preferably 300 ppm. If the antimony content is outside the above range, it may be difficult to control the a-value in particular, and the b-value may also be affected.
[0021] The upper limit of the total content of titanium and sodium is preferably 9 ppm, more preferably 8 ppm, even more preferably 7 ppm, particularly preferably 6.5 ppm, and especially preferably 6.0 ppm, while the lower limit is preferably 0.4 ppm, more preferably 1.0 ppm, even more preferably 2.0 ppm, and especially preferably 2.5 ppm. If the total content of titanium and sodium is outside the above range, it may be difficult to control the a-value and b-value in particular.
[0022] The lower limit of the sodium content of the pellets used in the present invention is preferably 0.3 ppm, more preferably 1.0 ppm, even more preferably 2.0 ppm, and particularly preferably 2.5 ppm, while the upper limit is preferably 8 ppm, more preferably 7.0 ppm, even more preferably 6.5 ppm, and particularly preferably 6.0 ppm. If the sodium content is outside the above range, it may be difficult to control the a value in particular.
[0023] The upper limit of the titanium content is preferably 7 ppm, more preferably 6 ppm, further preferably 5.5 ppm, and particularly preferably 5.0 ppm. If the total titanium content is outside the above range, it may be difficult to control the b-value in particular.
[0024] <Solid-state polymerization step using the pellets> In the present invention, pellets of recovered polyethylene terephthalate obtained by the above-mentioned method or the like are used to carry out solid-phase polymerization.
[0025] In the present invention, the pellets are subjected to solid-phase polymerization, thereby making it possible to obtain recycled polyethylene terephthalate having a higher intrinsic viscosity (IV) than the pellets.
[0026] In the above-mentioned production method, the method for crystallizing the pellets is not particularly limited. For example, the pellets can be crystallized by charging the pellets into a tower reactor and heating them under an inert gas flow.
[0027] In the above-mentioned manufacturing method, the type of inert gas used in crystallization is not particularly limited as long as it is a gas that does not react with the polyethylene terephthalate obtained in the liquid phase polymerization step.Specific examples include rare gases such as helium, neon, argon, krypton, and xenon, and nitrogen.From the viewpoint of availability and cost, nitrogen is preferred.
[0028] The temperature at which crystallization is carried out in the above-mentioned production method (crystallization temperature) is preferably 120 to 200° C., and more preferably 130 to 180° C. The time for which crystallization is carried out (crystallization time) is preferably 1 minute to 8 hours, and more preferably 1 to 4 hours.
[0029] The crystallization temperature may be constant or increased stepwise. When crystallization is performed at a high temperature (for example, about 170°C), if the temperature is increased suddenly, the granular liquid phase polymerized product may fuse together, so it is preferable to increase the temperature stepwise.
[0030] In the above-mentioned production method, the method of solid-phase polymerization of the crystallized granular liquid-phase polymerization product is not particularly limited. For example, the crystallized granular liquid-phase polymerization product is charged into a tower reactor and heated under an inert gas flow to increase the intrinsic viscosity (IV) to a value higher than that before the solid-phase polymerization.
[0031] The solid-state polymerization temperature in the present invention is not particularly limited as long as the intrinsic viscosity (IV) of the crystallized granular liquid-phase polymerized product is higher than the IV before the solid-state polymerization, but is preferably 190 to 235° C., more preferably 195 to 232° C. The solid-state polymerization pressure is preferably 1.33 kPa to 0.2 MPa, and the solid-state polymerization is usually carried out at atmospheric pressure.
[0032] The solid-state polymerization time in the present invention is not particularly limited as long as the polyethylene terephthalate reaches the desired physical properties (predetermined intrinsic viscosity, etc.) Usually, the solid-state polymerization is carried out for 5 to 24 hours, preferably 20 hours or less.
[0033] The type of inert gas used in the solid-state polymerization is not particularly limited as long as it is a gas that does not react with polyethylene terephthalate.Specific examples include rare gases such as helium, neon, argon, krypton, and xenon, and nitrogen.From the viewpoints of availability and cost, nitrogen is preferred.
[0034] The solid-phase polymerization can be carried out in the presence of a stabilizer. Specific examples of such stabilizers include phosphoric acid esters such as trimethyl phosphate, triethyl phosphate, tri-n-butyl phosphate, trioctyl phosphate, and triphenyl phosphate; phosphorous acid esters such as triphenyl phosphite, trisdodecyl phosphite, and trisnonylphenyl phosphite; acidic phosphoric acid esters such as methyl acid phosphate, ethyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, dibutyl phosphate, monobutyl phosphate, dioctyl phosphate, and ethyl diethylphosphonoacetate; phosphorus compounds such as phosphoric acid and polyphosphoric acid; hindered phenols; and hindered amines.
[0035] When a phosphorus compound is used as a stabilizer, the amount added is preferably 0.005 to 0.2 mol %, and more preferably 0.01 to 0.1 mol %, calculated as phosphorus atoms in the phosphorus compound, relative to the polyethylene terephthalate to be polymerized.
[0036] Furthermore, in order to reduce the rate of increase in the intrinsic viscosity (IV) of polyethylene terephthalate and the by-product cyclic trimer, etc., the solid-phase polymerization can be carried out by circulating an inert gas containing ethylene glycol.
[0037] The method for recovering the reaction product (liquid-phase polymerized product) after the completion of the solid-phase polymerization reaction is not particularly limited. For example, the reaction product can be withdrawn in the form of a strand from the bottom of the polycondensation reaction tank, cooled with water, and then cut into granules (chips) for recovery.
[0038] The granular product generally has an average particle size of 2.0 to 5.0 mm, preferably 2.2 to 4.0 mm.
[0039] By using such a method, it is possible to obtain recycled polyethylene terephthalate having an L value of at least 78. The lower limit of the L value is preferably 79, more preferably 80.0, and even more preferably 80.5.
[0040] Furthermore, the contents of titanium, sodium, and antimony contained in the recycled polyethylene terephthalate can be considered to be, in principle, equivalent to the contents in the pellets used.
[0041] In the present invention, the pellets used are characterized by containing antimony, titanium, and sodium in specific ranges as described above. If the amounts are within these ranges, the differences in a and b between the raw flakes and the resulting recycled polyethylene terephthalate can be reduced.
[0042] The hue of the recycled polyethylene terephthalate can be measured by preparing a sample from the recovered polyethylene terephthalate and by the method described in the Examples below.
[0043] The reason why such excellent effects are shown is unclear at present, but the inventors speculate as follows.
[0044] The titanium is thought to come mainly from the titanium catalyst contained in the recycled PET. Titanium catalysts are said to have a relatively high tendency to cause depolymerization. This type of depolymerization may decompose PET, but it may also decompose unnecessary components that are mixed in during the process of obtaining recycled PET flakes. It is expected that such decomposition products will be removed to a certain extent in the venting process during solid-state polymerization, and the effect of this is thought to be relatively high compared to the disadvantages of decomposing recycled PET. However, if the titanium content is too high, the disadvantages of PET decomposition will be greater, and the b value may deteriorate.
[0045] As long as the sodium content is within the range of the requirements of the present invention, the higher the sodium content, the smaller the difference in a value between the raw material flakes and the recycled polyethylene terephthalate (recycled PET) tends to be. The reason for this is that, for example, the unnecessary decomposition products generated by the depolymerization react with sodium, making it difficult for them to be incorporated into the recycled PET chain during solid-phase polymerization. The reaction between the unnecessary components and sodium may be promoted in the crystallization process. On the other hand, if the sodium content is too high, for example, the interaction with titanium may occur at the same time, causing coloring.
[0046] Antimony is also thought to come mainly from the antimony catalyst contained in the recycled PET. The higher the value, the greater the possibility of a larger difference in the a-value between the raw flakes and the recycled polyethylene terephthalate. This is presumably because depolymerization caused by the catalytic action of antimony occurs at a higher rate in the PET itself than titanium. On the other hand, the aforementioned sodium may have the effect of suppressing this depolymerization through interaction with antimony, and therefore the presence of a certain amount of sodium may have a favorable effect on the hue, especially the a-value.
[0047] Thus, while the presence of antimony and titanium is unavoidable in recovered PET, the presence of a specific amount of sodium directly or indirectly affects their catalytic action, reducing the difference in hue between the raw flakes and the resulting recycled PET, thereby enabling the production of recycled PET with excellent hue.
[0048] Of course, the above-mentioned effect of sodium can be expected from potassium, which is also an alkali metal, so the pellets may contain potassium in addition to sodium. In that case, the content of potassium is preferably half or less of that of sodium.
[0049] [Recycled polyethylene terephthalate] The recycled polyethylene terephthalate of the present invention is (a) The antimony content is 50 to 400 ppm; (b) The sum of the titanium and sodium content is 10 ppm or less; (c) Titanium content is 0.1 ppm or more It is characterized by an L value of 78 or more. The reason why recycled polyethylene terephthalate that satisfies such requirements is preferable is the same as that described in the above-mentioned production method.
[0050] The recycled PET obtained by the manufacturing method of the present invention can be used in combination with other resins, stabilizers, etc. A representative example of such a resin is PET, which is copolymerized with high-purity terephthalic acid and ethylene glycol, known as virgin PET. Examples of the stabilizer include known heat-resistant stabilizers such as hindered phenols, hindered amines, and phosphorus compounds exemplified in the section "Solid-phase polymerization step."
[0051] There is no restriction on the timing of adding the stabilizer, and it may be added all at once or in several divided portions.
[0052] [Method of manufacturing a molded product containing recycled polyethylene terephthalate] Molded articles containing recycled polyethylene terephthalate can be produced mainly by injection molding of recycled polyethylene terephthalate. As described above, recycled polyethylene terephthalate can be used in combination with other resins, stabilizers, etc., and therefore may be used in the form of a composition.
[0053] <Drying> When the recycled polyethylene terephthalate obtained by the production method of the present invention is subjected to, for example, injection molding, it is preferable to dry it before injection molding in order to suppress a decrease in intrinsic viscosity (IV) during molding. The dryer is not particularly limited as long as it can sufficiently reduce the moisture content in the recycled polyethylene terephthalate, but a dehumidified air dryer or the like is generally used.
[0054] The drying temperature is preferably 130° C. to 160° C. If the temperature is lower than 130° C., the drying time will be longer, and if the temperature is higher than 160° C., the recycled polyethylene terephthalate may become discolored.
[0055] The drying time is not particularly limited as long as the moisture content in the recycled polyethylene terephthalate can be sufficiently reduced, but is preferably 3 to 10 hours. If the drying time is shorter than 3 hours, the drying may be insufficient, which may result in a large decrease in intrinsic viscosity (IV) during injection molding, and if the drying time is longer than 10 hours, coloring may occur.
[0056] The water content of the recycled polyethylene terephthalate after drying is preferably 10 ppm to 100 ppm, more preferably 20 ppm to 50 ppm. If the water content is more than 100 ppm, it is not preferable because the IV decrease during injection molding may become large.
[0057] By providing such a drying step, it is possible to obtain a suitable PET molded product by various molding methods, which are preferable. As such a molding method, known molding methods such as injection molding, blow molding, extrusion molding, etc. can be used without any restrictions.
[0058] <Applications of molded products containing recycled polyethylene terephthalate> The uses of molded articles containing recycled polyethylene terephthalate are not particularly limited, but examples include containers such as PET bottles produced by blow molding, containers produced by injection molding, functional films, food containers thermoformed from sheets, fibers, and the like. EXAMPLES
[0059] The present invention will be described in detail below with reference to examples. Note that the description of the examples in this specification is for the purpose of aiding understanding of the contents of the present invention, and is not intended to provide a basis for narrowly interpreting the technical scope of the present invention. The evaluation methods used in these examples are as follows.
[0060] <Analysis> The various analytical methods are explained below. The various raw material flakes and the recycled PET obtained in Examples 1 to 5 and Comparative Example 1 that were the subject of the analysis are referred to as polyethylene terephthalate samples (PET samples).
[0061] (1) Intrinsic viscosity (IV) 0.1 g of a PET sample was dissolved in 20 mL of a mixed solution of tetrachloroethane / phenol = 50 / 50 (wt% / wt%) by heating, and then cooled and calculated from the solution viscosity measured at 25°C.
[0062] (2) Hue (L value, a value, b value) The hue of the PET samples was measured using a spectrophotometer (SD-6000, manufactured by Nippon Denshoku Industries Co., Ltd.). In Table 1, Δ indicates the difference in hue between the raw material flakes and the hue of the recycled PET.
[0063] (3) Element content The pellets and raw material flakes obtained in Examples 1 to 5 and Comparative Example 1 were used as samples. Sulfuric acid was added to them, and then nitric acid was added dropwise while heating to decompose the organic matter. The element contents in the pellet samples (aqueous solutions) were quantified using pure water. Next, the metals in the pellet sample aqueous solution were quantitatively analyzed by ICP atomic emission spectrometry (ICP-AES method: using Shimadzu Corporation's ICPE-9820 and ICPS-8100 devices).
[0064] <Examples 1 to 5, Comparative Example 1> Various used PET bottles collected from the market were crushed and washed in the usual way to obtain various raw material flakes, which were then pelletized by melt extrusion according to the method described below, and then subjected to solid-phase polymerization according to the method described below to obtain recycled polyethylene terephthalate (recycled PET). The above-mentioned various raw material flakes are PET with different contents of titanium, sodium, antimony, and germanium. The analytical results of the raw flakes and recycled PET are summarized in Table 1.
[0065] (Pelletizing process) The various raw material flakes were extruded in a vented twin-screw extruder at 250° C. by melt extrusion into strands, which were then cooled, cut, and pelletized.
[0066] (Solid-state polymerization) 6.0 kg of each type of pellet obtained by the above method was charged into a crystallizer and subjected to crystallization at 170°C for 2 hours under 45 Nm 3 The mixture was heated under nitrogen flow for 1 hour to cause crystallization, thereby obtaining crystallized pellets. 5.5 kg of the crystallized pellets were charged into a solid-state polymerization apparatus and subjected to polymerization at 220° C. for 5.5 hours under 45 Nm 3 The mixture was heated for 1 hour under nitrogen flow while removing water, alcohols, etc., to carry out solid-state polymerization.
[0067] [Table 1]
[0068] The results in Table 1 show that the recycled polyethylene terephthalates of Examples 1 to 5 which satisfy the requirements of the present invention have a relatively small difference in hue from the raw material flakes and are recycled polyethylene terephthalates whose hue is close to that of the raw material flakes.
Claims
1. Using recycled polyethylene terephthalate flakes, Pellets of polyethylene terephthalate satisfying the following requirements (a), (b), and (c) are prepared, and then solid-state polymerization is carried out. A method for producing recycled polyethylene terephthalate having an L value of 78 or more. (a) the antimony content is 50 to 400 ppm; (b) The sum of the titanium and sodium content is 10 ppm or less; (c) Titanium content is 0.1 ppm or more.
2. 2. The method for producing recycled polyethylene terephthalate according to claim 1, wherein the total content of titanium and sodium in the requirement (b) is 7 ppm or less.
3. The method for producing recycled polyethylene terephthalate according to claim 1, wherein the sodium content in the pellets is 0.3 ppm or more.
4. 2. The method for producing recycled polyethylene terephthalate according to claim 1, wherein the total content of titanium and sodium in the requirement (c) is 0.4 ppm or more.
5. A recycled polyethylene terephthalate which satisfies the following requirements (a), (b), and (c) and has an L value of 78 or more. (a) the antimony content is 50 to 400 ppm; (b) The sum of the titanium and sodium content is 10 ppm or less; (c) Titanium content is 0.1 ppm or more.
Citation Information
Patent Citations
Recycled polyester raw materials and recycled polyester film
JP2023006803A
Method for producing polyester resin composition and method for regenerating collected polyester resin
WO2022234749A1