Cell growth scaffold material and molded body for cell growth

A polarized vinylidene fluoride (co)polymer scaffolding material with specific surface properties enhances cell proliferation and regeneration by improving cell adhesion and membrane interaction, addressing the lack of effective application methods in existing technologies.

JP2024134962APending Publication Date: 2024-10-04KUREHA CORPORATION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023045433
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for using vinylidene fluoride (co)polymer films to promote cell proliferation and regeneration lack specific application techniques, limiting their effectiveness.

Method used

A scaffolding material comprising a polarized vinylidene fluoride (co)polymer with a surface contact angle of 50° to 85° and zeta potential of -15 mV or less, applied with a negative voltage, is used to enhance cell proliferation and regeneration.

Benefits of technology

The material effectively promotes cell proliferation and regeneration by enhancing cell adhesion and membrane potential interaction, achieving higher proliferation rates and regeneration efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134962000001_ABST
    Figure 2024134962000001_ABST
Patent Text Reader

Abstract

To provide a scaffold material for promoting cell proliferation or regeneration using a film of vinylidene fluoride (co)polymer, which is highly effective in promoting cell proliferation and regeneration.SOLUTION: Provided is a scaffold material for promoting cell proliferation or regeneration, comprising a molded body containing a polarized vinylidene fluoride (co)polymer and a support for supporting the molded body, the support supporting the molded body so that the surface to which a negative voltage is applied when the vinylidene fluoride (co)polymer is polarized comes into contact with the cells.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cell growth scaffold and a molded article for cell growth. [Background technology]

[0002] Attempts have been made to use films of vinylidene fluoride (co)polymers as substrates for in vivo tissue regeneration and wound healing, ex vivo production of organs for transplantation, cell culture for research, etc. For example, Patent Documents 1 and 2 describe medical devices in which vinylidene fluoride (co)polymers, which are piezoelectric bodies, are brought into contact with the heart, blood vessels, etc., and electrical stimulation is imparted to cells by surface charges and electric fields generated by deformation of the film, thereby promoting cell proliferation. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2008-522769 [Patent Document 2] Special Publication No. 2016-505325 Summary of the Invention [Problem to be solved by the invention]

[0004] As described in Patent Documents 1 and 2, applications of vinylidene fluoride (co)polymer films to cell proliferation promotion have been studied. However, studies on specific application methods have not progressed, and there are still many unknowns regarding how to use the film to enhance the cell proliferation promotion effect.

[0005] The present invention aims to provide a scaffold for promoting cell proliferation or regeneration using a molded body of vinylidene fluoride (co)polymer, which is highly effective in promoting cell proliferation and regeneration, and a molded body for promoting cell proliferation or regeneration that can be used for the scaffold. [Means for solving the problem]

[0006] One embodiment of the present invention for solving the above problems relates to the following scaffolding materials [1] to [6]. [1] A molded body containing a polarized vinylidene fluoride (co)polymer; A scaffold for promoting cell proliferation or regeneration, comprising: a support for supporting the molded body; The support supports the molded body so that a surface to which a negative voltage is applied when the vinylidene fluoride (co)polymer is polarized comes into contact with a cell. A scaffolding material for promoting cell growth or regeneration. [2] The surface to which the negative voltage is applied has a contact angle with water of 50° or more and 85° or less. A scaffolding material as described in [1]. [3] The surface to which the negative voltage is applied has a zeta potential of -15 mV or less. A scaffolding material according to [1] or [2]. [4] A cell culture material. A scaffolding material according to any one of [1] to [3]. [5] A cell regenerating or tissue regenerating material. A scaffolding material according to any one of [1] to [3].

[0007] Another embodiment of the present invention for solving the above problem relates to a molded article according to the following item [6]. [6] A molded article of a polarized vinylidene fluoride (co)polymer, When polarized, the surface to which a negative voltage is applied has a contact angle with water of 50° or more and 85° or less, and a zeta potential of -15 mV or less. A molded article for promoting cell proliferation or regeneration. Effect of the Invention

[0008] According to the present invention, there is provided a scaffold for promoting cell proliferation or regeneration using a molded body of vinylidene fluoride (co)polymer, which is highly effective in promoting cell proliferation and regeneration, and a molded body for promoting cell proliferation or regeneration that can be used with the scaffold. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1A is a schematic diagram showing an exemplary embodiment of a scaffold for promoting cell proliferation or regeneration, which has a molded body as a substrate for promoting cell proliferation or regeneration and a support for supporting the molded body, and FIG. 1B is a schematic cross-sectional view thereof. [Diagram 2] FIG. 2 is a schematic diagram showing another exemplary embodiment of a scaffold for promoting cell proliferation or regeneration, which has the above-mentioned molded body as a substrate for promoting cell proliferation or regeneration, and a support for supporting the molded body. [Diagram 3] FIG. 3 is a graph showing the average length of neurites of cells when cells were cultured on the surfaces of test pieces 1-1 and 1-2 to which a negative voltage was applied and when cells were cultured on the surfaces to which a positive voltage was applied in Example Test 1. [Figure 4] FIG. 4 is a graph showing the length of neurites relative to the cell area when cells were cultured on the surfaces of test pieces 1-2 and 1-3 to which a negative voltage was applied in Example Test 1, with and without ultrasound irradiation. [Diagram 5] FIG. 5 is a graph showing the cell proliferation rate when cells were cultured on the surfaces of test pieces 2-1 to 2-4 to which a negative voltage was applied and when cells were cultured on the surfaces to which a positive voltage was applied in Example Test 2. [Figure 6] FIG. 6 is a graph showing the proliferation rate of cells when cells were cultured on the surfaces of Test Specimens 5-1 to 5-8 to which a negative voltage was applied in Test 5 of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] One embodiment of the present invention relates to a scaffold for promoting cell proliferation or regeneration, comprising a substrate (molded body) for promoting cell proliferation or regeneration, and a support for supporting the substrate.

[0011] The substrate is a molded article containing a polarized vinylidene fluoride (co)polymer. The vinylidene fluoride (co)polymer is a fluororesin containing a constituent unit derived from vinylidene fluoride as a main constituent unit. In this specification, the main constituent unit means that the proportion of the constituent unit derived from vinylidene fluoride to all the constituent units constituting the (co)polymer is 50 mol% or more. The proportion of the constituent unit derived from vinylidene fluoride to all the constituent units constituting the (co)polymer is preferably 60 mol% or more and 100 mol% or less, more preferably 70 mol% or more and 100 mol% or less.

[0012] The vinylidene fluoride (co)polymer may be a homopolymer of vinylidene fluoride or a copolymer of vinylidene fluoride and other monomers. Examples of the other monomers include 1-chloro-1-fluoro-ethylene, 1-chloro-2-fluoro-ethylene, trifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, tetrafluoropropene, hexafluoropropylene, and vinyl fluoride. Alternatively, the other monomer may be a monomer having an ethylenically unsaturated group that is copolymerizable with vinylidene fluoride. The ratio of the constituent units derived from these other monomers to all the constituent units constituting the (co)polymer may be less than 50 mol%, preferably 0 mol% to 40 mol%, and more preferably 0 mol% to 30 mol%.

[0013] The inherent viscosity of the vinylidene fluoride (co)polymer is preferably 0.8 dl / g or more. In this specification, the inherent viscosity is a value measured at 30°C using a dimethylformamide solution having a concentration of 0.4 g / dl. The higher the inherent viscosity of the vinylidene fluoride (co)polymer, the more improved the strength and extensibility of the molded body will be, and the less likely the base material will break due to constriction during use of the cell growth scaffold. From the above viewpoint, it is more preferable that the inherent viscosity of the vinylidene fluoride (co)polymer is 0.85 dl / g or more and 3.0 dl / g or less.

[0014] The molded article may contain resins other than vinylidene fluoride (co)polymers, additives, etc. Examples of resins other than vinylidene fluoride (co)polymers include (meth)acrylic resins, cellulose derivative resins, polyester resins, polycarbonate resins, polyolefin resins, polyether resins, polyvinyl alcohol resins, epoxy resins, polyamide resins, polyimide resins, polyurethane resins, polysaccharides, cellulose, polypeptides, and synthetic peptides. The content of resins other than vinylidene fluoride (co)polymers is preferably 0% by mass or more and 30% by mass or less, more preferably 0% by mass or more and 20% by mass or less, and even more preferably 0% by mass or more and 10% by mass or less, based on the total mass of the molded article.

[0015] Examples of additives include substances that can regulate the rate of cell proliferation and regeneration, such as natural or synthetic peptides, such as collagen, poly-L-lysine, and poly-D-lysine, mucopolysaccharides, such as hyaluronic acid, and extracellular matrices containing these, other polysaccharides, cellulose, etc.

[0016] The shape of the molded product is not particularly limited, but is preferably a film or sheet. The thickness of the film or sheet-shaped molded product is preferably 1 μm or more and 300 μm or less, more preferably 5 μm or more and 200 μm or less, and even more preferably 10 μm or more and 100 μm or less.

[0017] The molded article can be produced by molding a resin composition containing vinylidene fluoride (co)polymer and, optionally, the other resins and additives described above, by a known method such as melt extrusion or melt casting, stretching and relaxing the resulting product as necessary, and then subjecting it to a polarization treatment.

[0018] The conditions for stretching and relaxation are not particularly limited. For example, stretching may be performed at a temperature of 70°C to 135°C and at a stretch rate of 2.5 to 6.0 times. Relaxation may be performed at a temperature of 90°C to 140°C and for 20 seconds to 5 minutes. Each of the stretching and relaxation may be performed in multiple stages.

[0019] The polarization treatment can be carried out, for example, by exposing the molded resin composition to a high DC electric field between a non-contact pointed electrode connected to a DC high voltage power supply and a grounded polarizing roll (counter electrode). Specifically, in the polarization treatment, a charge generated by corona discharge at the tip of a pointed electrode (such as a needle-shaped electrode) is held on the surface of the resin composition, and DC electrolysis is carried out between the surface and the polarizing roll. The pointed electrode may be a non-contact type electrode or a contact type electrode, but it is preferable to use a non-contact type electrode in order to prevent the power supply from being shut down due to insulation breakdown of the resin composition.

[0020] The absolute value of the DC voltage applied to the resin composition in the polarization treatment may be greater than 0 kV, and is preferably 2 kV or more, more preferably 4 kV or more, and even more preferably 5 kV or more. The maximum absolute value of the DC voltage is not particularly limited, but can be 100 kV or less. The strength of the electric field during the polarization treatment is preferably 50 MV / m or more, more preferably 100 MV / m or more, and even more preferably 125 MV / m or more. The maximum value of the electric field strength is not particularly limited, but can be 2500 MV / m or less.

[0021] Piezoelectric constant d of the compact after polarization treatment 33is preferably 0.3 pC / N or more, more preferably 1.7 pC / N or more, and even more preferably 2.0 pC / N or more. 33 The maximum value of the strength is not particularly limited, but can be 50 pC / N or less. 33 The higher the piezoelectric constant d 33 Even if the piezoelectricity is between 0.7 pC / N and 2 pC / N, which means that the piezoelectricity hardly acts at all as a piezoelectric material, it has the effect of promoting cell proliferation and regeneration.

[0022] FIG. 1A is a schematic diagram showing an exemplary embodiment of a scaffold for promoting cell proliferation, the scaffold having the above-mentioned molded body as a substrate for promoting cell proliferation and a support for supporting the molded body, and FIG. 1B is a schematic cross-sectional view thereof.

[0023] The scaffold 100 is a scaffold for producing a cell sheet, which has a molded body 110 as the above-mentioned base material and a container-shaped support 120 that supports the molded body 110. As shown in FIG. 1A and FIG. 1B, in the scaffold 100, the sheet-shaped molded body 110 is disposed on a part or the entire surface of the bottom of the container-shaped support 120. The molded body 110 is a sheet-shaped molded body produced by subjecting the above-mentioned resin composition to a polarization treatment. The support 120 supports the molded body 110 so that the surface to which a negative voltage is applied during the polarization treatment comes into contact with the cells. In the example shown in FIG. 1A and FIG. 1B, the surface of the sheet-shaped molded body 110 facing the inside of the container is the surface to which a negative voltage is applied during the polarization treatment. The surface to which a negative voltage is applied during the polarization treatment may be a surface that is positively charged when stress is applied in the surface direction, depending on the molded body 110.

[0024] In addition, if the polarization treatment is performed by the method using a pointed electrode as described above, the surface to which a negative voltage is applied during polarization treatment is the surface of the molded body facing the pointed electrode when the pointed electrode is a positive electrode, and is the surface of the molded body opposite the pointed electrode when the pointed electrode is a negative electrode.

[0025] FIG. 2 is a schematic diagram showing another exemplary embodiment of a scaffold for promoting cell regeneration, which has the above-mentioned molded body as a substrate for promoting cell regeneration and a support for supporting the molded body.

[0026] The scaffold 200 is a scaffold as a nerve cell regeneration material, which includes the molded body 210 as the base material, and the support 220 which is an adhesive tape that fixes the molded body 210 in a tubular shape and supports the nerve cells. As shown in FIG. 2, in the scaffold 200, the sheet-shaped molded body 210 is wound around the axon 230 of the nerve cell, and the end is fixed by the support 220 which is an adhesive tape to form a tube. As a result, the molded body 210 is fixed in position relative to the nerve cell so as to surround the axon. The support 220 supports the molded body 210 so that the surface to which a negative voltage is applied when the molded body is polarized contacts the axon of the nerve cell. In the example shown in FIG. 2, the surface of the sheet-shaped molded body 210 that is shaped like a tube and faces the inside of the tube (axon direction) is the surface to which a negative voltage is applied when the molded body is polarized.

[0027] According to the findings of the present inventors, as described above, when the surface of the molded body to which a negative voltage is applied during polarization treatment comes into contact with cells, the effect of promoting cell proliferation and regeneration is enhanced. Although the reason for this is unclear, it is thought that this is due to the fact that cells are more likely to adhere due to interaction with the surface to which a negative voltage is applied, or due to fluctuations in cell membrane potential and enhancement of intracellular signal transduction caused by the action of the surface to which a negative voltage is applied.

[0028] In this case, from the viewpoint of further enhancing the effect of promoting cell proliferation and regeneration, the surface to which the negative voltage is applied preferably has a contact angle with water of 50° to 85°, more preferably 50° to 80°, even more preferably 50° to 75°, and particularly preferably 60° to 75°. The contact angle with water of the surface to which the negative voltage is applied can be adjusted by the conditions of the polarization treatment, hydrophilization treatment such as surface functional group modification, surface irregularity by die pressing, etc.

[0029] The contact angle can be determined by measuring the contact angle by the sessile drop method (θ / 2 method) using 2 μL of ultrapure water as a droplet. At this time, the test piece is fixed on a slide glass, and the contact angle is measured at 10 points per test piece, and the average value of these is regarded as the contact angle of the test piece.

[0030] In order to further enhance the effect of promoting cell proliferation and regeneration, the surface to which the negative voltage is applied preferably has a zeta potential of -15 mV or less, more preferably -25 mV or less, and even more preferably -30 mV or less. The lower limit of the zeta potential is not particularly limited, but can be -90 mV or more. The zeta potential of the surface to which the negative voltage is applied can be adjusted by the conditions of the polarization treatment and chemical modification of the surface with an acid or alkali.

[0031] The zeta potential can be a value measured using a commercially available zeta potential measuring device, commercially available monitor particles, and a 10 mM NaCl solution (pH 5 to about 6). In this case, the zeta potential is measured three times for each test piece, and the average value of these measurements is regarded as the zeta potential of the test piece.

[0032] Such scaffold materials can be widely used for applications such as cell culture materials for growing cells, cell regeneration materials for promoting cell regeneration, or tissue regeneration materials for promoting tissue regeneration.

[0033] For example, scaffolds as cell culture materials can be used to produce cell sheets as shown in Figures 1A and 1B, as well as to culture various types of cells using well-shaped or other shaped containers, produce organoids (artificial organs) and spheroids, produce artificial meat, etc. In this case, the various containers (supports) can be filled with the cells to be cultured and a culture solution (medium) appropriate for the cells and the purpose of the culture.

[0034] Alternatively, the scaffold material as a cell regeneration material or tissue regeneration material can be used for nerve regeneration as shown in Figure 2, as well as for bone augmentation during implantation, healing of fractures, etc., and as a fixation device that fixes and holds a transplanted organ while regenerating surrounding tissues. In this case, the molded body can be fixed and held at the target site by a support (e.g., bolts, sutures, etc.) appropriate for each application.

[0035] The type of cells to be promoted in proliferation or regeneration is not particularly limited, and may be an animal-derived cell or a plant-derived cell. Examples of animals include mammals such as humans, rats, mice, guinea pigs, rabbits, dogs, cats, cows, sheep, goats, pigs, and monkeys.

[0036] The cells may also be cells derived from various tissues or organs, such as skin, bone, cartilage, vascular tissue, muscle, brain, eye, nerve, lung, thymus, mammary gland, stomach, colon, small intestine, large intestine, heart, pancreas, kidney, spleen, liver, uterus, ovary, testis, bladder, prostate, and oral mucosa.

[0037] The above cells may be undifferentiated or differentiated. The above cells may be somatic cells, germ cells, liver cells (ES cells, iPS cells, etc.), or cancer cells. Examples of somatic cells include fibroblasts, bone marrow cells, immune cells (B lymphocytes, T lymphocytes, neutrophils, macrophages, monocytes, etc.), organ-derived cells (hepatocytes, spleen cells, pancreatic cells, kidney cells, embryonic cells, etc.), muscle tissue cells (skeletal muscle cells, smooth muscle cells, myoblasts, cardiac muscle cells, etc.), nerve cells, glial cells, osteoblasts, osteoblast-like cells, chondrocytes, endothelial cells, epithelial cells, epidermal cells, interstitial cells, adipocytes, and precursor cells thereof.

[0038] When the above scaffold is used to promote cell proliferation or regeneration, ultrasonic waves may be continuously or intermittently irradiated to the molded body in contact with the cells. However, the scaffold of this embodiment has a sufficient effect of promoting cell proliferation or regeneration even when the molded body does not have a high piezoelectric effect or when ultrasonic waves are not irradiated. For this reason, it is considered that the above molded body can promote cell proliferation or regeneration without relying on electrical stimulation generated by the piezoelectric effect.

[0039] [Other embodiments] It should be noted that the above-described embodiment is an exemplary embodiment of the present invention, and it goes without saying that the present invention may include embodiments other than the above-described embodiment within the scope of its core technical concept. EXAMPLES

[0040] The present invention will be described in detail based on examples, but the present invention is not limited to these examples.

[0041] 1. Preparation of Substrate 1-1.Vinylidene fluoride homopolymer Vinylidene fluoride homopolymer (Kureha Corporation, KF#1000) was melt-extruded at 260°C to form a sheet, which was then uniaxially stretched 4.6 times to obtain an unpolarized film. Aluminum foil cut to a size of 4 cm x 4 cm was fixed on a polytetrafluoroethylene plate with insulating tape, and the above film cut to a size of 10 cm x 10 cm was placed on the aluminum foil. In this state, a needle electrode connected to a voltage resistance measuring device (Kikusui Electronics Co., Ltd.) was set on the above film at a position corresponding to the center of the aluminum foil, and corona polarization was performed for 30 seconds with a set voltage of 2 to 10 kV. Then, a 4 cm x 4 cm area (corresponding to the aluminum foil) centered on the needle electrode was cut to a specified size to prepare a test piece, and the following experiment was performed.

[0042] At this time, several test pieces were obtained by changing the corona discharge conditions. These test pieces are called PVDF test pieces.

[0043] 1-2.Vinylidene fluoride-trifluoroethylene copolymer Vinylidene fluoride and trifluoroethylene were polymerized in a molar ratio (vinylidene fluoride:trifluoroethylene) of 75:25 and formed into a sheet by melt extrusion to obtain an unpolarized film with a thickness of 25 μm. This test piece was designated as a P(VDF-TrFE) test piece.

[0044] 2. Measurement The piezoelectric constant, contact angle, and zeta potential of each test piece were measured by the following methods.

[0045] 2-1.Piezoelectric constant The piezoelectric constant was measured using a d33 meter (PIEZOTEST) by the Berlincourt Method. Specifically, the sample was sandwiched between electrodes, vibration was applied from below, and the generated charge was measured and calculated. The values ​​of the piezoelectric constant below are shown as absolute values.

[0046] 2-2.Contact angle A contact angle meter (DM500, manufactured by Kyowa Interface Science Co., Ltd.) was used to measure the contact angle by the sessile drop method (θ / 2 method) using 2 μL of ultrapure water (manufactured by Merck using Milli-Q) as a droplet. At this time, the test piece was fixed on a slide glass, and the contact angle was measured at 10 points per test piece, and the average value of these was taken as the contact angle of the test piece.

[0047] 2-3.Zeta potential Each test piece was cut to 3.5 cm x 1.5 cm. In addition, the stock solution of monitor particles for flat cell (hydroxypropyl cellulose-coated polystyrene latex, manufactured by Otsuka Electronics Co., Ltd.) was adjusted by diluting 200 times with 10 mM NaCl. The cut test piece was washed with 10 mM physiological saline, and then set in the flat cell unit of a zeta potential measuring device (ELS-Z2, manufactured by Otsuka Electronics Co., Ltd.), and the monitor particles for flat cell adjusted as above were injected without generating air bubbles. The zeta potential was measured three times consecutively for one test piece, and the average value was taken as the zeta potential of the test piece.

[0048] 3. Test 1 The following five test pieces were prepared. · Test piece 1-1: PDVF test piece that was not polarized. Specimen 1-2: Polarized PDVF specimen. Piezoelectric constant is 15 pC / N. Specimen 1-3: Polarized PDVF specimen. Piezoelectric constant is 9.7 pC / N.

[0049] These test pieces were cut into 1cm x 1cm pieces and washed in a 24-well plate with disinfectant ethanol and Dulbecco's phosphate buffered saline (D-PBS(-)) in that order. A 0.1mg / mL poly-D-lysine (PDL) solution was added to each well and left to stand overnight to coat it. Then, nerve-like cells (PC12 cells) suspended in medium (Roswell Park Memorial Institute (RPMI) medium supplemented with 1% HS (horse serum), 0.5% FBS (fetal bovine serum), and 1% P / S (penicillin-streptomycin solution)) were seeded on each film and cultured for 11 days in a CO2 incubator (CO2 concentration: 5%, temperature: 37°C). During the culture period, the medium was replaced every 1-3 days. At this time, for the test piece 1-2, multiple test pieces were installed so that the surface to which a positive voltage was applied and the surface to which a negative voltage was applied faced the upper surface of the well, and cells were cultured under both conditions, that is, when cells were cultured on the surface to which a positive voltage was applied and when cells were cultured on the surface to which a negative voltage was applied. In addition, for the test piece 1-2 and the test piece 1-3, cells were cultured under both conditions, that is, when ultrasonic waves were applied to the test piece and when ultrasonic waves were not applied to the test piece. Ultrasound was applied at 120 kHz for 10 minutes intermittently for 7 days.

[0050] After 11 days of culture, the medium was removed and the cells were fixed with neutral buffered formalin (Fujifilm Wako Pure Chemicals). The specimen was then attached to a slide glass, and images were taken from the midpoints of the vertical and horizontal axes of the specimen to the ends of the specimen using a digital microscope (Keyence Corporation), and the length of the neurites and the area of ​​the cells were measured for the nerve-like cells in the images obtained. From the results obtained, the average value (μm) of the neurite length of the cells in the images was calculated. In addition, the neurite length relative to the number of cells and the neurite length relative to the cell area were calculated using the following formula. Length of neurite per cell (μm / cell) = sum of neurite lengths of all cells in the image (μm) / (total area of ​​cells in the image (μm 2) / average area per cell in the image (μm 2 ))

[0051] Figure 3 shows the average neurite lengths of cells in the images when cells were cultured on the surface of test piece 1-1 and test piece 1-2 to which a negative voltage was applied (labeled as test piece 1-2(-)) and when cells were cultured on the surface to which a positive voltage was applied (labeled as test piece 1-2(+)). Note that Figure 3 shows the results without ultrasonic treatment. The neurite length grew longer in the polarized test piece 1-2. Furthermore, the neurite length grew longer when cells were cultured on the surface to which a negative voltage was applied. Furthermore, since the growth of neurites was promoted even without ultrasonic treatment, it can be seen that the piezoelectrically treated vinylidene fluoride (co)polymer promotes the regeneration of nerve cells even without the electrical stimulation caused by the deformation of the film.

[0052] Figure 4 shows the neurite length relative to the cell area when cells were cultured on the surfaces of test pieces 1-2 and 1-3 to which a negative voltage was applied, with and without ultrasound irradiation. It can be seen that test piece 1-2, which has a piezoelectric constant of 15 pC / N, promotes the regeneration of nerve cells more than test piece 1-3, which has a piezoelectric constant of 9.7 pC / N. It can also be seen that the application of ultrasound promotes the regeneration of nerve cells.

[0053] 4. Test 2 The following four test pieces were prepared. Specimen 2-1: PDVF specimen without polarization treatment. The piezoelectric constant is 0.2 pC / N. Specimen 2-2: Polarized PDVF specimen. The piezoelectric constant is 9.7 pC / N. Specimen 2-3: Polarized PDVF specimen. Piezoelectric constant is 15 pC / N. Specimen 2-4: P(VDF-TrFE) specimen without polarization treatment. The piezoelectric constant is 0.4 pC / N.

[0054] These test pieces were cut into pieces measuring 1 cm x 1 cm, and washed with disinfectant ethanol and Dulbecco's phosphate buffered saline (D-PBS(-)) in that order. Each test piece was placed in a well of a 24-well plate, and fibroblasts (L929 cells) suspended in culture medium (MEMα+10% FBS+1% P / S) were seeded on each test piece, followed by culturing for two days in a CO2 incubator (CO2 concentration: 5%, temperature: 37°C). At this time, multiple test pieces were placed so that the surface to which the negative voltage was applied of each test piece faced the top of the well.

[0055] FIG. 5 shows the cell proliferation rate when cells are cultured on the surfaces of test pieces 2-1 to 2-4 to which a negative voltage is applied (denoted as test piece 2-1(-) etc.) and when cells are cultured on the surfaces to which a positive voltage is applied (denoted as test piece 2-2(+) etc.). It can be seen from FIG. 5 that, regardless of which test piece is used, the cell proliferation rate is higher when cells are cultured on the surfaces to which a negative voltage is applied.

[0056] 5. Test 3 The following two test pieces were prepared. The contact angle was measured on the surface with which the cells were in contact. Test piece 3-1: Polarized PVDF test piece. A negatively charged surface (contact angle 86.9°) was used. Specimen 3-2: Polarized PVDF specimen. The surface to which a negative voltage was applied (contact angle was 83.3°) was used.

[0057] These test pieces were cut into 1 cm x 1 cm pieces and washed with disinfectant ethanol and Dulbecco's phosphate buffered saline (D-PBS(-)) in that order. Each test piece was placed in a well of a 24-well plate, and osteoblast-like cells (MC3T3-E1 cells) suspended in culture medium (MEMα+10% FBS+1% P / S) were seeded on each test piece, and cultured for one day in a CO2 incubator (CO2 concentration: 5%, temperature: 37°C).

[0058] A predetermined amount of cell proliferation / cytotoxicity assay kit (Cell Counting Kit-8, Dojindo Laboratories, Inc.) was added to the culture medium after culturing, and after 2.5 hours of incubation, the culture medium was recovered. The recovered culture medium was transferred to a 96-well plate, and the absorbance at 450 nm was measured using a plate reader (BD). As a control, cells were directly seeded in a well of a 24-well plate in which no test piece was placed, and the absorbance obtained was measured in the same manner. The increase rate of absorbance relative to this was calculated and used as the proliferation rate of cells by each test piece.

[0059] The results are shown in Table 1.

[0060] [Table 1]

[0061] From Table 1, it can be seen that when the contact angle is 85° or less, the cell proliferation rate is high.

[0062] 6. Test 4 The following seven test pieces were prepared. Note that the numbers in parentheses indicate the strength of the electric field during polarization treatment. The contact angle indicates the value on the side in contact with the cells. Specimen 4-1: (0MV / m). The piezoelectric constant is 0.2pC / N and the contact angle is 82.8°. Specimen 4-2: (75MV / m). The piezoelectric constant is 0.7pC / N and the contact angle is 81.2°. Specimen 4-3: (100MV / m). The piezoelectric constant is 1.7pC / N and the contact angle is 80.5°. Specimen 4-4: (125MV / m). The piezoelectric constant is 2.0pC / N and the contact angle is 78.8°. Specimen 4-5: (150MV / m). The piezoelectric constant is 2.7pC / N and the contact angle is 75.1°. Specimen 4-6: (175MV / m). The piezoelectric constant is 12.0pC / N and the contact angle is 73.0°. Specimen 4-7: (200MV / m). The piezoelectric constant is 17.3pC / N and the contact angle is 72.8°.

[0063] These test pieces were cut into 1cm x 1cm pieces and washed with disinfectant ethanol and Dulbecco's phosphate buffered saline (D-PBS(-)) in that order. Each test piece was placed in a well of a 24-well plate, and osteoblast-like cells (MC3T3-E1 cells) suspended in culture medium (MEMα+10%FBS+1%P / S) were seeded on each test piece, followed by culturing for 3.5 hours in a CO2 incubator (CO2 concentration: 5%, temperature: 37°C). At this time, multiple test pieces were placed so that the surface to which the negative voltage was applied of each test piece faced the top of the well.

[0064] A predetermined amount of cell proliferation / cytotoxicity assay kit (Cell Counting Kit-8, Dojindo Laboratories, Inc.) was added to the culture medium after culturing, and after 2.5 hours of incubation, the culture medium was recovered. The recovered culture medium was transferred to a 96-well plate, and the absorbance at 450 nm was measured using a plate reader (BD). As a control, cells were directly seeded in a well of a 24-well plate in which no test piece was placed, and the absorbance obtained was measured in the same manner. The increase rate of absorbance relative to this was calculated and used as the proliferation rate of cells by each test piece.

[0065] The results are shown in Table 2.

[0066] [Table 2]

[0067] From Table 2, it can be seen that the smaller the contact angle, the higher the cell proliferation rate.

[0068] 6. Test 5 The following seven test pieces were prepared. Note that the numbers in parentheses indicate the strength of the electric field during polarization treatment. The contact angle indicates the value on the side in contact with the cells. Specimen 5-1: (75MV / m). Zeta potential is -28.6mV, contact angle is 81.2°. Specimen 5-2: (150MV / m). Zeta potential is -28.9mV, contact angle is 75.1°. Specimen 5-3: (175MV / m). Zeta potential is -29.4mV, contact angle is 73.0°. Specimen 5-4: (200MV / m). Zeta potential is -33.6mV, contact angle is 72.8°. Specimen 5-5: (75MV / m). Zeta potential is -23.8mV, contact angle is 82.2°. Specimen 5-6: (150MV / m). Zeta potential is -19.7mV, contact angle is 73.6°. Specimen 5-7: (175MV / m). Zeta potential is -25.6mV, contact angle is 73.1°. Specimen 5-8: (200MV / m). Zeta potential is -28.5mV, contact angle is 72.3°.

[0069] These test pieces were cut into 1cm x 1cm pieces and washed with disinfectant ethanol and Dulbecco's phosphate buffered saline (D-PBS(-)) in that order. Each test piece was placed in a well of a 24-well plate, and osteoblast-like cells (MC3T3-E1 cells) suspended in culture medium (MEMα+10%FBS+1%P / S) were seeded on each test piece, and cultured for 2 days in a CO2 incubator (CO2 concentration: 5%, temperature: 37°C). At this time, multiple test pieces were placed so that the surface to which the negative voltage was applied of each test piece faced the top of the well.

[0070] A predetermined amount of cell proliferation / cytotoxicity assay kit (Cell Counting Kit-8, Dojindo Laboratories, Inc.) was added to the culture medium after culturing, and after 2.5 hours of incubation, the culture medium was recovered. The recovered culture medium was transferred to a 96-well plate, and the absorbance at 450 nm was measured using a plate reader (BD). As a control, cells were directly seeded in a well of a 24-well plate in which no test piece was placed, and the absorbance obtained was measured in the same manner. The increase rate of absorbance relative to this was calculated and used as the proliferation rate of cells by each test piece.

[0071] The results are shown in Figure 6.

[0072] From FIG. 6, it can be seen that the smaller the zeta potential, the higher the cell proliferation rate. [Industrial Applicability]

[0073] According to the present invention, cell proliferation and regeneration can be achieved in a shorter period of time. [Explanation of symbols]

[0074] 100 Scaffolding 110 Molded body 120 Support 200 Scaffolding 210 Molded body 220 Support 230 Nerve cell axon

Claims

1. A molded body containing a polarized vinylidene fluoride (co)polymer; A scaffold for promoting cell proliferation or regeneration, comprising: a support for supporting the molded body; The support supports the molded body so that a surface to which a negative voltage is applied when the vinylidene fluoride (co)polymer is polarized comes into contact with a cell. A scaffolding material for promoting cell growth or regeneration.

2. The surface to which the negative voltage is applied has a contact angle with water of 50° or more and 85° or less. The scaffolding material according to claim 1 .

3. The surface to which the negative voltage is applied has a zeta potential of −15 mV or less. The scaffolding material according to claim 1.

4. Cell culture material, The scaffolding material according to claim 1.

5. A cell regenerating material or tissue regenerating material, The scaffolding material according to claim 1 .

6. A molded article comprising a polarized vinylidene fluoride (co)polymer, When polarized, the surface to which a negative voltage is applied has a contact angle with water of 50° or more and 85° or less, and a zeta potential of −15 mV or less. A molded article for promoting cell proliferation or regeneration.

Citation Information

Patent Citations

  • Stimulation of cell proliferation on the implant surface

    JP2008522769A

  • piezoelectric medical implant

    JP2016505325A