Porous membrane and manufacturing method thereof, and gas separation system

A hierarchical network structure in porous membranes, using bonded porous polymers and size exclusion polymers, addresses structural defects in mixed matrix membranes, enhancing both gas permeability and mechanical strength.

JP2024135023APending Publication Date: 2024-10-04KYOTO UNIV
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
JP2023045511
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional mixed matrix membranes suffer from structural defects due to aggregation of porous materials, leading to reduced mechanical strength and gas permeability, especially when the amount of porous material is increased for enhanced gas selectivity.

Method used

A porous membrane is constructed with a network structure formed by bonding porous polymers, such as metal-organic frameworks (MOFs), porous organic polymers (POPs), or metal-organic polyhedra (MOPs), using linker molecules, and size exclusion polymers to create a hierarchical network that maintains gas permeability and mechanical strength.

Benefits of technology

The new porous membrane achieves both excellent gas permeability and mechanical strength, outperforming conventional membranes in terms of permeability and selectivity, with a storage modulus at least twice that of membranes made of size exclusion polymers alone.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135023000001_ABST
    Figure 2024135023000001_ABST
Patent Text Reader

Abstract

To provide a new type of a porous membrane having both excellent gas permeability and mechanical strength.SOLUTION: A porous membrane according to the present invention includes a porous polymer having pores in a molecule, and a size exclusion polymer having molecular size that cannot occupy the pores. The porous polymer forms a plurality of particles, and the plurality of particles are bonded to each other by chemical bonding or physical cohesive force to form a network structure.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE The present disclosure relates to porous membranes and methods for making the same. The present disclosure also relates to gas separation systems including the porous membranes. [Background technology]

[0002] Traditionally, porous materials such as zeolites, activated carbon, and porous polymers have been widely studied. Examples of porous polymers include metal-organic frameworks (MOFs), porous organic polymers (POPs), and metal-organic polyhedra (MOPs) connected to each other by linker molecules. These porous materials are expected to be applied in fields such as gas adsorption and gas separation.

[0003] In order to apply porous materials, it is important to conduct research into controlling their morphology. In particular, if porous materials can be used as membranes, the range of their applications will expand dramatically.

[0004] From this perspective, research is being conducted on mixed matrix membranes (MMMs), which use crystalline porous materials as fillers and organic polymers as matrices (Non-Patent Document 1). Such mixed matrix membranes are expected to be hybrid materials that combine the porosity of the filler and the moldability of the matrix. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Dechnik, J.; Gascon, J.; Doonan, CJ; Janiak, C.; Sumby, CJ, Mixed-Matrix Membranes. Angew. Chem. Int. Ed. 2017, 56 (32), 9292-9310. Summary of the Invention [Problem to be solved by the invention]

[0006] However, the inventors have found that conventional mixed matrix membranes are prone to structural defects due to domain generation caused by the aggregation of porous materials. Such domains are vulnerable to stress concentration and can adversely affect the morphology of the membrane. This problem becomes more pronounced when the amount of porous material in the membrane is increased in order to increase the gas selectivity (i.e., permeability to a specific gas) of the membrane.

[0007] Therefore, an object of the present invention is to provide a new type of porous membrane that has both excellent gas permeability and mechanical strength. [Means for solving the problem]

[0008] For example, aspects of the present invention are as follows. [1] A porous membrane comprising: a porous polymer having voids in its molecule; and a size-exclusion polymer having a molecular size that is too large to occupy the voids, wherein the porous polymer forms a plurality of particles, and the plurality of particles are bonded to each other by chemical bonds or physical cohesive forces to form a network structure. [2] The porous membrane according to [1], wherein the porous polymer is at least one porous polymer selected from the group consisting of metal-organic frameworks (MOFs), porous organic polymers (POPs), and metal-organic polyhedra (MOPs) linked to each other by linker molecules. [3] The porous membrane according to [1] or [2], wherein the size-exclusion polymer is at least one polymer selected from the group consisting of thermoplastic resins, polymers of inherent microporosity (PIM), and silicones. [4] The porous membrane according to any one of [1] to [3], wherein the content of the porous polymer in the porous membrane is 10 mass% or more. [5] The porous membrane according to any one of [1] to [4], having a permeability to at least one type of gas molecule that is 1.2 times or more higher than the permeability in a membrane consisting of only the size exclusion polymer. [6] The porous membrane according to any one of [1] to [5], having a storage modulus at 1 rad / s that is at least twice as large as the storage modulus of a membrane consisting of only the size exclusion polymer. [7] The porous membrane according to any one of [1] to [6], which is prepared using a precursor gel containing the porous polymer. [8] A gas separation system comprising the porous membrane according to any one of [1] to [7]. [9] A method for producing a precursor gel containing a metal-organic framework (MOF) or a porous organic polymer (POP) having intramolecular pores, adding a solvent to the precursor gel to prepare a suspension, mixing the suspension with a size exclusion polymer, and removing the solvent; wherein the solvent has a molecular size large enough to occupy the pores, and the size exclusion polymer has a molecular size large enough not to occupy the pores.

[10] A method for producing a porous membrane, comprising the steps of: forming a precursor gel containing metal-organic polyhedra (MOPs) having intramolecular voids and connected to each other by linker molecules, a solvent, and a size-exclusion polymer; and removing the solvent, wherein the solvent has a molecular size large enough to occupy the voids, and the size-exclusion polymer has a molecular size large enough not to occupy the voids.

[11] The method according to

[10] , wherein the step of forming the precursor gel includes the steps of: preparing a first solution containing the metal-organic polyhedron, the solvent, and the size-exclusion polymer; preparing a second solution containing the linker molecule, the solvent, and the size-exclusion polymer; and mixing the first solution with the second solution.

[12] The method according to any one of [9] to

[11] , wherein the size-exclusion polymer is at least one polymer selected from the group consisting of thermoplastic resins, polymers of inherent microporosity (PIM), and silicones. Effect of the Invention

[0009] According to the present invention, a new type of porous membrane is provided which has both excellent gas permeability and mechanical strength. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 shows a schematic diagram of a method for measuring the permeability of gas molecules through a porous membrane. [Diagram 2] FIG. 2 is a conceptual diagram showing a method for producing a porous membrane according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a conceptual diagram showing a method for producing a porous membrane according to another embodiment of the present invention. [Figure 4] FIG. 4 shows the results of dynamic light scattering measurements showing the formation process of a precursor gel in a size-exclusion polymer. [Diagram 5] FIG. 5 shows SEM images of the surfaces of the films according to Comparative Example 1, Example 3, and Example 5. [Figure 6] FIG. 6 shows cross-sectional SEM images of the films according to Comparative Example 1, Example 3, and Example 5. [Figure 7] FIG. 7 shows surface SEM images of the samples according to Comparative Example 4 and Comparative Example 6. [Figure 8] FIG. 8 shows cross-sectional SEM images of the samples according to Comparative Example 4 and Comparative Example 6. [Figure 9]FIG. 9 shows optical microscope images of the samples of Example 5 and Comparative Example 6. [Figure 10] FIG. 10 shows an SEM image of the aerogel made from the porous membrane according to Example 5. [Figure 11] FIG. 11 shows the results of measuring the storage modulus of the film samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 and 4. [Figure 12] FIG. 12 shows the results of measuring the storage modulus of the membrane samples (MOP / PB) according to Examples 6 to 8 and Comparative Examples 7 to 10. [Figure 13] FIG. 13 shows the results of measuring the storage modulus of the membrane samples (MOP / PES) according to Examples 9 to 11 and Comparative Examples 11 to 14. [Figure 14] FIG. 14 shows the results of viscoelasticity measurement in the tensile mode of the membrane sample (MOP / AP) according to Example 12. [Figure 15] FIG. 15 shows the results of viscoelasticity measurement in a tensile mode of the film sample (AP) according to Comparative Example 15. [Figure 16] FIG. 16 shows the results of measuring the storage modulus of the membrane samples (MOF / PU) according to Examples 13 to 16 and Comparative Examples 1 and 16 to 18. [Figure 17] FIG. 17 shows the results of measuring the storage modulus of the membrane samples (MOF / PB) according to Examples 17 to 19 and Comparative Examples 7 and 19 to 21. [Figure 18] FIG. 18 shows the results of measuring the storage modulus of the membrane samples (MOF / PES) according to Examples 20 to 22 and Comparative Examples 11 and 22 to 24. [Figure 19] FIG. 19 shows the measurement results of the CO 2 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Figure 20] FIG. 20 shows the measurement results of N 2 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Figure 21]FIG. 21 shows the measurement results of CH4 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Figure 22] FIG. 22 shows the measurement results of H 2 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Diagram 23] FIG. 23 shows the measurement results of O 2 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Figure 24] FIG. 24 shows the measurement results of the CO2 / N2 permselectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Diagram 25] FIG. 25 shows the measurement results of the CO2 / H2 permselectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Figure 26] FIG. 26 shows the measurement results of the CO2 / CH4 permselectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Figure 27] FIG. 27 shows the measurement results of H2 / N2 permselectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Figure 28] FIG. 28 shows the measurement results of H2 / CH4 permselectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. [Figure 29] FIG. 29 shows the measurement results of O2 / N2 permselectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, a porous membrane according to one embodiment of the present invention and a method for producing the same will be described. In addition, a gas separation system including the above-mentioned porous membrane will also be described. In addition, when referring to drawings or chemical formulas, components that perform the same or similar functions are given the same reference symbols or symbols, and duplicated descriptions will be omitted. In addition, in the following, the new type of porous membrane according to the present invention is also referred to as a pore-networked membrane (PNM).

[0012] The porous membrane according to one embodiment of the present invention includes a porous polymer having a void in its molecule and a size-exclusion polymer having a molecular size that is large enough not to occupy the void. The porous polymer forms a plurality of particles, and the plurality of particles are bonded to each other by chemical bonds or physical cohesive forces to form a network structure. This network structure is typically a colloidal network structure. Here, the term "particle" refers to an aggregate composed of two or more molecules, and there is no restriction on its shape. Each of the plurality of particles may be, for example, a 0-dimensional shape such as a sphere, a 1-dimensional shape such as a rod or fiber, or a 2-dimensional shape such as a sheet. Each of the plurality of particles is typically a nanoparticle.

[0013] The porous membrane according to this embodiment has a hierarchical network structure. First, the molecular structure of the porous polymer itself can be regarded as a network in which a large number of pores are connected. This constitutes the first network in the porous membrane. Second, as described above, the particles of the porous polymer are bonded to each other by chemical bonds or physical cohesion to form a higher-order network structure. This constitutes the second network in the porous membrane. The presence of the first network ensures the gas permeability of the porous membrane. And the presence of the second network ensures the mechanical strength of the porous membrane. Therefore, the presence of these hierarchical network structures makes it possible to achieve both high gas permeability and mechanical strength. In addition, examples of the above-mentioned chemical bonds include coordinate bonds, covalent bonds, and ionic bonds.

[0014] As the porous polymer, any material can be used as long as it has pores in the molecule and can form the above-mentioned network structure. The porous polymer is, for example, at least one porous polymer selected from the group consisting of metal-organic frameworks (MOFs), porous organic polymers (POPs), and metal-organic polyhedra (MOPs) linked to each other by linker molecules. Hereinafter, MOPs linked to each other by linker molecules are also referred to as MOP supramolecular polymers. The porous polymer may be crystalline or amorphous.

[0015] The above-mentioned MOF may be, for example, one capable of forming a precursor gel, which will be described later. That is, the above-mentioned MOF may be one in which a plurality of MOF particles are bonded to each other by chemical bonds or physical cohesive forces to form a network structure. Such a precursor gel may be obtained, for example, by controlling the rate of nanoparticle formation and aggregation in a system containing MOF or its raw material and a solvent. Known MOF gels are summarized, for example, in the following literature. Literature: Jigwei Hou, Adam F. Sapnik and Thomas D. Bennett, Metal-Organic framework gels and monoliths, Chem. Sci. 2020, 11, 310

[0016] There is no limit to the type of MOF that can be used. By appropriately combining the type and coordination number of metal ions and the type and topology of multidentate ligands, MOFs having a desired structure can be produced. MOFs may contain two or more metal elements and may contain two or more multidentate ligands. MOFs are typically synthesized by reacting a metal ion donor with a multidentate ligand.

[0017] Examples of the metal element constituting the metal ion donor include any element belonging to alkali metals (Group 1), alkaline earth metals (Group 2), and transition metals (Groups 3 to 12). The metal element is typically selected from the group consisting of magnesium, calcium, iron, aluminum, zinc, copper, nickel, cobalt, zirconium, gallium, indium, and chromium. The metal ion donor may contain a plurality of metal elements. Alternatively, a plurality of metal ion donors containing different metal elements may be used in combination.

[0018] As the metal ion donor, typically, a metal salt is used. The metal ion donor may be an organic salt or an inorganic salt. The metal ion donor is typically selected from the group consisting of hydroxides, carbonates, acetates, sulfates, nitrates, and chlorides. A plurality of metal ion donors each containing the same metal element may be used in combination. The metal ion donor may be in the form of a so-called secondary building unit (SBU). As such a secondary building unit, any one used in the synthesis of known MOFs may be selected.

[0019] The polydentate ligand is typically an organic polydentate ligand, and is selected from the group consisting of, for example, a carboxylate anion, an amine compound, a sulfonate anion, a phosphate anion, and a heterocyclic compound. The carboxylate anion may be, for example, a dicarboxylate or tricarboxylate anion. Specific examples include anions of citric acid, malic acid, terephthalic acid, isophthalic acid, trimesic acid, and derivatives thereof. The heterocyclic compound may be, for example, bipyridine, imidazole, adenine, and derivatives thereof. A plurality of polydentate ligands may be used.

[0020] Examples of MOFs capable of forming precursor gels are given below in Table 1. These are merely examples and do not preclude the use of other MOFs. [Table 1-1] [Table 1-2] [Table 1-3]

[0021] The list of references cited in Table 1 is as follows: A1:Bart Bueken et al. Gel-based morphological design of zirconium metal-organic frameworks. Chem. Sci., 2017, 8, 3939-3948 A2:Tian Tian et al. Mechanically and chemically robust ZIF-8 monoliths with high volumetric adsorption capacity. J. Mater. Chem. A, 2015, 3, 2999-3005 A3:Abhijeet K. Chaudhari et al. Multifunctional Supramolecular Hybrid Materials Constructed from Hierarchical Self-Ordering of In Situ Generated Metal-Organic Framework (MOF) Nanoparticles. Advanced Materials, Volume 27, Issue 30, August 12, 2015, 4438-4446 A4:Li, L., Xiang, S., Cao, S. et al. A synthetic route to ultralight hierarchically micro / mesoporous Al(III)-carboxylate metal-organic aerogels. Nat Commun 4, 1774 (2013)

[0022] The POP may be, for example, one that can form a precursor gel, which will be described later. That is, the POP may be one in which a plurality of POP particles are bonded to each other by chemical bonds or physical cohesive forces to form a network structure. Such a precursor gel can be obtained, for example, by controlling the rate of nanoparticle formation and aggregation in a system containing the POP or its raw material and a solvent. The POP may be, for example, a covalent organic framework (COF).

[0023] There is no limit to the type of POP that can be used. By appropriately selecting the type and / or combination of highly symmetrical organic molecules, a POP having a desired structure can be produced. The POP may be obtained by polycondensation of one type of organic molecule, or may be obtained by polycondensation of two or more types of organic molecules.

[0024] The binding site of the POP may be any structure, such as a boroxine type (boroxine ring obtained by a dehydration condensation reaction of a boronic acid), a boronic acid ester type (boronic acid ester obtained by a condensation reaction of a boronic acid and a diol), an amide type (amide obtained by a dehydration condensation reaction of an amine and an acid halide), an imine type (amide obtained by a dehydration condensation reaction of an amine and an aldehyde or ketone), or a triazine type (1,3,5-triazine obtained by a trimerization reaction of a nitrile).

[0025] Examples of POPs that can form precursor gels are listed below in Table 2. These are merely examples and do not preclude the use of other POPs. [Table 2-1] [Table 2-2]

[0026] The list of references cited in Table 2 is as follows: B1: Y. Su, Z. Wang, A. Legrand, T. Aoyama, N. Ma, W. Wang, K. Otake, K. Urayama, S. Horike, S. Kitagawa, S. Furukawa, and C. Gu, J. Am. Chem. Soc. 2022, 144, 15, 6861-6870. B2:JA Martin-Illan, D. Rodriguez-San-Miguel, O. Castillo, G. Beobide, J. Perez-Carvajal, I. Imaz, D. Maspoch, F. Zamora, Angew. Chem. Int. Ed. 2021, 60, 13969. B3:Z. Liu, K. Zhang, G. Huang, B. Xu, Y.-l. Hong, X. Wu, Y. Nishiyama, S. Horike, G. Zhang, S. Kitagawa, Angew. Chem. Int. Ed. 2022, 61, e202110695. B4:Dongyang Zhu, Yifan Zhu, Qianqian Yan, Morgan Barnes, Fangxin Liu, Pingfeng Yu, Chia-Ping Tseng, Nicholas Tjahjono, Po-Chun Huang, Muhammad M. Rahman, Eilaf Egap, Pulickel M. Ajayan, and Rafael Verduzco, Chem. Mater. 2021, 33, 11, 4216-4224

[0027] The above-mentioned MOP may be, for example, one that can form a precursor gel described below by linking together with linker molecules. That is, the above-mentioned "MOP linked together with linker molecules" (i.e., a supramolecular polymer of MOP) may be, for example, one in which a plurality of these particles are linked together with chemical bonds such as coordinate bonds to form a network structure. Such a precursor gel can be obtained, for example, by controlling the rate of nanoparticle formation and aggregation in a system containing MOP or its raw material, linker molecules, and a solvent.

[0028] There is no limit to the type of MOP that can be used. By appropriately combining the type and coordination number of metal ions with the type and topology of polydentate ligands, MOPs having a desired structure can be produced. MOPs may contain two or more metal elements and may contain two or more polydentate ligands. MOPs are typically synthesized by reacting a metal ion donor with a polydentate ligand. The MOPs may be metal-organic cages (MOCs) or coordination cages.

[0029] Examples of the metal element constituting the metal ion donor include any element belonging to alkali metals (Group 1), alkaline earth metals (Group 2), and transition metals (Groups 3 to 12). The metal element is typically selected from the group consisting of rhodium, ruthenium, zirconium, vanadium, palladium, iron, magnesium, platinum, gallium, nickel, molybdenum, chromium, and copper. The metal ion donor may contain a plurality of metal elements. Alternatively, a plurality of metal ion donors containing different metal elements may be used in combination.

[0030] As the metal ion donor, typically, a metal salt is used. The metal ion donor may be an organic salt or an inorganic salt. The metal ion donor is typically selected from the group consisting of hydroxide salts, carbonate salts, acetate salts, sulfate salts, nitrate salts, and chloride salts. A plurality of metal ion donors each containing the same metal element may be used in combination.

[0031] The polydentate ligand is typically an organic polydentate ligand, and is selected from the group consisting of, for example, carboxylate anions, amine compounds, sulfonate anions, phosphate anions, and heterocyclic compounds. The carboxylate anions include, for example, dicarboxylate or tricarboxylate anions. Specific examples include anions of citric acid, malic acid, terephthalic acid, isophthalic acid, trimesic acid, and derivatives thereof. The heterocyclic compounds include, for example, bipyridine, imidazole, adenine, and derivatives thereof. The polydentate ligand may be a ligand based on a polymer or oligomer molecule such as PEG. A plurality of polydentate ligands may be used.

[0032] Typically, a bidentate ligand is used as a linker molecule for linking MOPs together, and examples of such linker molecules include bidentate linking groups such as bisimidazole and bispyridine.

[0033] Examples of MOPs that can form precursor gels are listed below in Table 3. These are merely examples and do not preclude the use of other MOPs. [Table 3-1] [Table 3-2] [Table 3-3] [Table 3-4]

[0034] The list of references cited in Table 3 is as follows: C1:Carne-Sanchez, A., Craig, GA, Larpent, P. et al. Self-assembly of metal-organic polyhedra into supramolecular polymers with intrinsic microporosity. Nat Commun 9, 2506 (2018). C2:A. Carne-Sanchez, GA Craig, P. Larpent, V. Guillerm, K. Urayama, D. Maspoch, S. Furukawa, Angew. Chem. Int. Ed. 2019, 58, 6347. C3:Z. Wang, GA Craig, A. Legrand, F. Haase, S. Minami, K. Urayama, S. Furukawa, Chem. Asian J. 2021, 16, 1092. C4:Zhukhovitskiy, A., Zhong, M., Keeler, E. et al. Highly branched and loop-rich gels via formation of metal-organic cages linked by polymers. Nature Chem 8, 33-41 (2016). C5:Gu, Y., Alt, E.A., Wang, H. et al. Photoswitching topology in polymer networks with metal-organic cages as crosslinks. Nature 560, 65-69 (2018). C6:Jonathan A. Foster, Richard M. Parker, Ana M. Belenguer, Norifumi Kishi, Sam Sutton, Chris Abell, and Jonathan R. Nitschke, Journal of the American Chemical Society 2015 137 (30), 9722-9729 C7:Li Shao, Bin Hua, Xiangquan Hu, David Stalla, Steven P. Kelley, and Jerry L. Atwood, Journal of the American Chemical Society 2020 142 (16), 7270-7275 C8:Chenjie Lu, Mingming Zhang, Danting Tang, Xuzhou Yan, ZeYuan Zhang, Zhixuan Zhou, Bo Song, Heng Wang, Xiaopeng Li, Shouchun Yin, Hajar Sepehrpour, and Peter J. Stang, Journal of the American Chemical Society 2018 140 (24), 7674-7680 C9:Sudhakar Ganta and Dillip K. Chand, Inorganic Chemistry 2018 57 (7), 3634-3645 C10:Sutar, P., Suresh, VM, Jayaramulu, K. et al. Binder driven self-assembly of metal-organic cubes towards functional hydrogels. Nat Commun 9, 3587 (2018). C11:Wei, S.-C., Pan, M., Fan, Y.-Z., Liu, H., Zhang, J. and Su, J.-Y. (2015), Creating Coordination-Based Cavities in a Multiresponsive Supramolecular Gel. Chem. Eur. J., 21: 7418-7427. C12:Wei Zheng, Li-Jun Chen, Guang Yang, Bin Sun, Xu Wang, Bo Jiang, Guang-Qiang Yin, Li Zhang, Xiaopeng Li, Minghua Liu, Guosong Chen, and Hai-Bo Yang, Journal of the American Chemical Society 2016 138 (14), 4927-4937 C13:J. Uchida, M. Yoshio, S. Sato, H. Yokoyama, M. Fujita, T. Kato, Angew. Chem. Int. Ed. 2017, 56, 14085. C14:Yu Qin, Lin-Lin Chen, Wei Pu, Peng Liu, Shi-Xi Liu, Yuan Li, Xiao-Lan Liu, Zhi-Xiang Lu, Li-Yan Zheng, and Qiu-E Cao, Chem. Commun., 2019,55, 2206-2209 C15:Ru-Jin Li, Cristian Pezzato, Cesare Berton, and Kay Severin, Chem. Sci., 2021,12, 4981-4984

[0035] As described above, the porous polymer constituting the porous membrane according to this embodiment has pores in the molecule. Due to the presence of these pores, the porous membrane according to this embodiment is typically configured to be permeable to at least one type of gas molecule. Here, "permeable to gas molecules" means that the permeability to the gas molecules is higher than the permeability of a membrane made using only a size exclusion polymer. The method for measuring the permeability to gas molecules will be described separately below.

[0036] Examples of gas molecules that can permeate the porous membrane include hydrogen; oxygen; nitrogen; carbon monoxide; carbon dioxide; nitrogen compounds such as nitrous oxide, nitric oxide, and ammonia; sulfur compounds such as hydrogen sulfide and sulfur dioxide; aliphatic hydrocarbons such as methane, ethane, and propane, and acetylene; noble gases such as argon and xenon; and halogen compounds such as chlorine and hydrogen bromide.

[0037] The gas molecules that can permeate the porous membrane may be vapors of molecules that are liquid at room temperature. Examples of such liquid molecules include aliphatic hydrocarbons such as n-hexane; aromatic hydrocarbons such as benzene, toluene, and dichlorobenzene; ethers such as diethyl ether, tetrahydrofuran (THF), and 1,4-dioxane; halogenated hydrocarbons such as chloroform and dichloromethane; esters such as ethyl acetate; ketones such as acetone; nitriles such as acetonitrile; amides such as N,N-dimethylformamide (DMF); sulfoxides such as dimethyl sulfoxide (DMSO); carboxylic acids such as formic acid and acetic acid; alcohols such as methanol, ethanol, n-propanol, i-propanol, and n-butanol; and water.

[0038] As described above, the porous polymer constituting the porous membrane according to this embodiment forms a plurality of particles, and these particles are bonded to each other by chemical bonds or physical cohesion to form a network structure. That is, this porous membrane has a higher-order structure such as a chemical gel that forms a colloidal network by covalent bonds, or a physical gel that forms a colloidal network by non-covalent bonds. The size exclusion polymer described below is included in the gaps of this network structure. Here, "covalently" means, for example, the formation of a network by covalent bonds, coordinate bonds, or ionic bonds. Here, "non-covalently" means, for example, the formation of a network by intermolecular interactions.

[0039] Each of the plurality of particles is typically a nanoparticle, for example, having a diameter of 1 nm to 100 nm, that is, the porous membrane is typically a nanoparticle membrane.

[0040] As described above, the size exclusion polymer constituting the porous membrane according to the present embodiment has a molecular size that is large enough not to occupy the pores of the porous polymer, and therefore the size exclusion polymer can effectively function as a matrix of the porous membrane without occupying the pores of the porous polymer as a filler.

[0041] As the size-exclusion polymer, for example, at least one polymer selected from the group consisting of thermoplastic resins, inherently microporous polymers (PIMs) and silicones can be used. As the thermoplastic resin, for example, polyurethane (PU), polyether block amide copolymers such as Pebax (registered trademark), polyethersulfone (PES), polyimides such as Matrimid (registered trademark) and 6-FDA-DAM, fluororesins such as PVDF, chlorine-based resins such as polyvinyl chloride, biodegradable plastics such as polylactic acid, or similar thermoplastics can be used. As the inherently microporous polymer (PIM), for example, AO-PIM-1 (amidoxime-functionalized inherently microporous polymer) or similar PIMs can be used. When a PIM is used as the size-exclusion polymer, a porous membrane can be provided in which both the pores of the porous polymer and the pores of the PIM can be used. As the silicone, for example, polydimethylsiloxane (PDMS) or similar silicones can be used.

[0042] In the porous membrane according to this embodiment, the content of the porous polymer in the membrane is, for example, 5% by mass or more, preferably 10% by mass or more, and more preferably 15% by mass or more. The content of the porous polymer in the membrane is, for example, 80% by mass or less, preferably 70% by mass or less. Any combination of these upper and lower limits is possible. If this content is too small, the gas permeability of the porous membrane may be insufficient. If this content is too large, it may be difficult to form the membrane. The porous membrane according to this embodiment may contain two or more types of porous polymers, and may contain two or more types of size exclusion polymers. In addition, when PIM is used as the size exclusion polymer, its content is not included in the content of the porous polymer. Furthermore, when MOPs linked to each other by linker molecules are used as the porous polymer, the content of the porous polymer is calculated as the content of MOPs used as raw materials.

[0043] As described above, the porous membrane according to this embodiment is preferably configured to allow at least one type of gas molecule to pass through. That is, the porous membrane according to this embodiment preferably has a higher permeability to at least one type of gas molecule than that of a membrane (hereinafter also referred to as a polymer membrane) made using only the corresponding size exclusion polymer. The permeability of the gas molecule through the porous membrane is more preferably 1.2 times or more, even more preferably 1.5 times or more, and particularly preferably 1.8 times or more, of the permeability of the gas molecule through the polymer membrane. For example, the permeability of carbon dioxide (CO2) can be used as a standard for evaluating the gas permeability.

[0044] The gas molecule permeability through the membrane is measured as follows. That is, the permeability is measured at room temperature using a constant volume variable pressure method. Gas recovery tests are carried out individually for all membranes, and the diffusion coefficient and dissolution coefficient of each sample are calculated using the time delay (θ) method. Three membranes are tested for each sample, and the permeability coefficient is calculated as the average value.

[0045] FIG. 1 shows a schematic diagram of a method for measuring the permeability of gas molecules through a porous membrane. As shown in FIG. 1, in this measurement method, a gas permeation cell having an effective area of ​​2 cm 2 and equipped with gas and vacuum lines is used as a gas permeation cell. 3 A stainless steel holder (Millipore XX 4502500) is used. The pressure and temperature changes are recorded by an absolute pressure sensor (Keller PAA33X). The gas permeability is then calculated using the formula shown in Figure 1.

[0046] In the formula shown in Figure 1, P i is the permeability for gas i, and j i is the flux of gas i, l is the thickness of the membrane, and Δp is the pressure difference between the supply side and the permeation side of the membrane. In the same formula, V is the permeation volume, A is the effective area of ​​the membrane, T is the measurement temperature, and dp / dt is the pressure difference rate during gas permeation in a steady state. Thus, the permeability P iThe gas selectivity can be calculated as the ratio of the above permeabilities. For example, the selectivity of the second gas (j) to the first gas (i) is calculated as P j / P i It can be evaluated by calculating:

[0047] The porous membrane according to this embodiment preferably has high selectivity for at least one combination of gas molecules. That is, the porous membrane according to this embodiment preferably has a selectivity for at least one combination of gas molecules higher than the selectivity of the corresponding polymer membrane. The selectivity of the porous membrane is more preferably 1.1 times or more than the selectivity of the corresponding polymer membrane, and even more preferably 1.2 times or more. For example, the selectivity of carbon dioxide to nitrogen (CO2 / N2) can be used as a standard for evaluating gas selectivity.

[0048] As described above, the porous membrane according to this embodiment can exhibit excellent mechanical strength. This mechanical strength can be evaluated, for example, by measuring the storage modulus at 1 rad / s in a viscoelastic measurement in a tensile mode. This evaluation is performed using a stress-controlled AR-G2 rheometer (manufactured by TA Instruments). In addition, dynamic mechanical analysis (DMA) measurement of the membrane is performed by frequency sweep in a tensile mode with a strain amplitude of 0.5%, which is well inside the linear region (initial strain fixed at 0.3%).

[0049] The storage modulus of the porous membrane according to this embodiment is preferably higher than that of the corresponding polymer membrane. The storage modulus of the porous membrane according to this embodiment is preferably at least twice, more preferably at least 5 times, and even more preferably at least 10 times that of the corresponding polymer membrane. In addition, the storage modulus of the porous membrane according to this embodiment is typically higher than that of the corresponding mixed matrix membrane.

[0050] Such an increase in mechanical strength is believed to be due to the presence of a network structure in the porous membrane according to this embodiment. That is, in the porous membrane according to this embodiment, the particles of the porous polymer are bonded to each other by chemical bonds or physical cohesive forces to form a network structure. In this case, the porous polymer can be distributed relatively uniformly in the membrane, so that domain generation due to aggregation of the porous material is unlikely to occur. Therefore, in the porous membrane according to this embodiment, stress concentration in the domain is unlikely to occur, and the mechanical strength is unlikely to decrease.

[0051] The presence of the network structure in the porous membrane can be confirmed, for example, by observation using SEM measurement and / or optical microscope measurement. These measurements can also be performed after removing the size exclusion polymer from the porous membrane and forming the sample into an aerogel. Specific examples of such morphological observation will be described in the examples below.

[0052] The porous membrane having the above-mentioned network structure is prepared, for example, by using a precursor gel containing a porous polymer. In this case, the network structure existing in the gel containing the porous polymer is maintained in the porous membrane, thereby obtaining a porous membrane having a hierarchical network structure.

[0053] In this way, the porous membrane can be produced, for example, by using a gel containing a porous polymer as a precursor. In the following, particularly suitable production methods will be described for the case where MOF or POP is used as the porous polymer, and the case where MOPs linked to each other by linker molecules are used as the porous polymer. The above-mentioned porous membrane may also be produced by other methods.

[0054] First, a manufacturing method particularly suitable for using MOF or POP as the porous polymer will be described. In this manufacturing method, a precursor gel containing MOF or POP is first formed. Next, a solvent is added to this precursor gel to prepare a suspension of MOF or POP. Next, this suspension is mixed with a size exclusion polymer. Thereafter, the solvent is removed to obtain a porous membrane.

[0055] Fig. 2 is a conceptual diagram showing a method for producing a porous membrane according to one embodiment of the present invention. In the example shown in Fig. 2, first, MOF / POP raw materials (not shown) react to form a plurality of MOF or POP particles. Next, these particles are bonded to each other by chemical bonds or physical cohesion to form a network structure, thereby forming a precursor gel. After that, a suspension is prepared (not shown), a size exclusion polymer is added, and the solvent is removed to form the porous membrane according to this embodiment.

[0056] As the precursor gel, for example, the known MOF or POP gel described above can be used. In this precursor gel, a plurality of MOF or POP particles are bonded to each other by chemical bonds or physical cohesive forces to form a network structure, and the synthesis solvent is encapsulated in the network structure. In addition, in this precursor gel, the pores of the MOF or POP are typically occupied by the synthesis solvent or gas molecules that were present in the system during the synthesis.

[0057] The synthesis solvent may be, for example, a solvent used in the preparation of the precursor gel. Examples of the synthesis solvent include amides such as N,N-dimethylformamide (DMF), sulfoxides such as dimethylsulfoxide (DMSO), ketones such as acetone, alcohols such as methanol, ethanol, n-propanol, i-propanol, and n-butanol, or water. A mixture of multiple solvents may also be used as the synthesis solvent.

[0058] The dispersion solvent used to prepare the suspension from the precursor gel may be the same as the synthesis solvent described above, or may be different from the synthesis solvent described above. In the latter case, the boiling point of the dispersion solvent is preferably lower than that of the synthesis solvent. The dispersion solvent can be appropriately selected from the viewpoints of the boiling point, miscibility with the size exclusion polymer, and the like. A mixture of multiple solvents may be used as the dispersion solvent.

[0059] The size-exclusion polymer added to the suspension is, for example, in the form of a solution. In this case, the solvent for dissolving or dispersing the size-exclusion polymer is typically the same as the synthesis solvent or dispersion solvent described above. A mixture of multiple solvents may be used as the solvent constituting the size-exclusion polymer solution.

[0060] The removal of the solvent from the mixed solution or suspension obtained as described above is carried out, for example, by heating. Specifically, the mixed solution or suspension obtained is first applied onto a substrate or a dish. Next, the mixture is heated to remove the solvent. Thereafter, the membrane is peeled off from the substrate or dish, if necessary. This results in a porous membrane containing MOF or POP as a porous polymer and a size exclusion polymer. This solvent removal step may also serve as an activation step for removing gas or liquid molecules present in the pores of the porous polymer. This makes it possible to make the pores of the porous polymer unoccupied, and to make the porous membrane more suitable for the permeation of gas molecules.

[0061] Next, a manufacturing method particularly suitable for using MOPs linked to each other by linker molecules as the porous polymer will be described. In this manufacturing method, a precursor gel is first formed, which contains MOPs linked to each other by linker molecules, a solvent, and a size exclusion polymer. The solvent is then removed to obtain a porous membrane. The formation of the precursor gel and the formation of the membrane by removing the solvent are typically performed by a one-pot process. However, the precursor gel is typically formed before the solvent is completely removed. This point can be confirmed, for example, by analysis using a dynamic light scattering (DLS) method, as will be further described in the examples described later.

[0062] Fig. 3 is a conceptual diagram showing a method for producing a porous membrane according to another embodiment of the present invention. In the example shown in Fig. 3, multiple particles of MOP supramolecular polymer are formed by the reaction of MOP with linker molecules. At the same time, in the presence of a solvent and a size exclusion polymer, these multiple particles are bonded to each other by coordinate bonds to form a network structure, thereby forming a precursor gel. The solvent is then removed to form the porous membrane according to this embodiment.

[0063] As the precursor gel, for example, a gel in which a size exclusion polymer is added to the known MOP gel described above can be used. The precursor gel formation process may include, for example, a process of preparing a first solution containing MOP, a solvent, and a size exclusion polymer, a process of preparing a second solution containing a linker molecule, a solvent, and a size exclusion polymer, and a process of mixing the first solution and the second solution. In this case, the solvents constituting the first and second solutions may be the same or different from each other. Examples of these solvents include those described above as examples of synthetic solvents.

[0064] The removal of the solvent from the precursor gel can be carried out, for example, in the same manner as described above for removing the solvent from the mixed solution or suspension. In this case, the mixed solution or suspension may be coated on a substrate or a dish before it is completely gelled. In this case, the film formation process can be more easily controlled.

[0065] In the porous membrane thus obtained, the particles of the porous polymer are bonded to each other by chemical bonds or physical cohesion to form a network structure. The presence of such a network structure allows the membrane to achieve higher mechanical strength than conventional mixed matrix membranes (MMMs) that do not have such a higher-order structure. In addition, since the pores of the porous polymer are maintained, the porous membrane thus obtained can exhibit excellent gas permeability and / or gas selectivity.

[0066] As described above, the porous membrane according to the present embodiment is a new type of porous membrane having both excellent gas permeability and mechanical strength. Therefore, such a membrane can be applied in fields such as gas separation. For example, by using the porous membrane according to the present embodiment as a gas separation membrane in an existing gas separation system, it is possible to provide a new gas separation system. EXAMPLES

[0067] The above porous membranes will now be further described with reference to examples.

[0068] In the following examples, rhodium acetate, 1-dodecyl-1H-imidazole (diz), and 1,4-bis(imidazol-1-ylmethyl)benzene (bix) were synthesized according to the above reference C2. Pebax2533 was purchased in pellet form from Arkema. Polyethersulfone (PES) was purchased from Goodfellow and poly(tetramethylene glycol) (PTMG; Mw=2000) was purchased from Sigma-Aldrich and vacuum dried overnight at 80°C to remove residual moisture before use. Octanediol chain extender and dibutyltin dilaurate (DBTDL) as catalyst were purchased from Sigma-Aldrich and dried over 4 Å molecular sieves before use. Isophorone diisocyanate (IPDI), ZrCl4, and ZrOCl2·8H2O were purchased from Wako Pure Chemical Industries and used as received. 1,3,5-Benzenetricarboxylic acid and hydroxylamine were purchased from Sigma-Aldrich. 5,5',6,6'-Tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spirobicindane (TTSBI), 2-aminoterephthalic acid, 1,4-dicyanotetrafluorobenzene (DCTB), and Al(NO3)3·9H2O were provided by Nacalai Tesque. Solvents were purchased from Wako Pure Chemical Industries, Ltd., except for HPLC grade, which was purchased from Fisher Chemical Co.

[0069] 1. Synthesis of raw materials The raw materials used in the membrane preparation described below were synthesized as follows.

[0070] (1) HRhMOP(diz) 12 The HRhMOP shown in Table 3-1 was synthesized according to literature C2. 200 mg of HRhMOP was dispersed in 40 mL of DCM (dichloromethane), and then 132.5 mg of diz (18 molar equivalents) was added. After 5 min of sonication, the solution was centrifuged to remove the precipitate. The upper purple solution was collected and evaporated in vacuum. The resulting purple solid HRhMOP (diz) 12The mixture was washed twice with EtOH to remove the remaining diz. In this way, HRhMOP(diz) 12 obtained.

[0071] (2) Polyurethane (PU) The PU was synthesized by a two-stage bulk polymerization method. First, PTMG was reacted with excess IPDI (PTMG:IPDI=1:3 molar ratio) under nitrogen atmosphere at 75 °C, followed by the addition of 0.1 mL of DBTDL to obtain a macrodiisocyanate prepolymer. After 2 h, a precise amount of octanediol chain extender was added for equimolar adjustment of the NCO:OH ratio. The synthesized polyurethane was washed and precipitated with methanol:water (50:50 wt%) to remove unreacted monomers or low molecular weight polymers. The samples were dried under vacuum at 70 °C before use. The molar ratio of PTMG:IPDI:chain extender was 1:3:2.

[0072] (3) Amidoxime-functionalized intrinsically microporous polymer (AO-PIM-1) AO-PIM-1 (hereafter also referred to as AP) was synthesized by a two-step protocol. First, a flask was charged with 3.0 g (15 mmol) of DCTB, 5.1 g (15 mmol) of TTSBI, 6.2 g (45 mmol) of K2CO3, and 25 mL of DMAc (N,N-dimethylacetamide). The mixture was vigorously stirred at 155 °C under Ar atmosphere for 6 min. Then, 20 mL of toluene and 0.2 mL of water were added sequentially with stirring to maintain the solubility of the monomer salt. After precipitation from a methanol / chloroform mixture and drying at 120 °C under vacuum for 12 h, a bright yellow powder (PIM-1) was recovered. The obtained PIM-1 was then dissolved in 40 mL of THF at 65 °C under N2, and refluxed at 69 °C for 20 h with dropwise addition of 6.0 mL of hydroxylamine. The polymer was precipitated by adding ethanol, then filtered and thoroughly washed with ethanol. The product was then dried at 110 °C for 3 h to give an off-white powder as AO-PIM-1.

[0073] 2. Membrane Preparation The membranes according to the examples and comparative examples were prepared as follows.

[0074] (Examples 1 to 5) We investigated the case where MOPs linked together by linker molecules were used as porous polymers. Specifically, HRhMOP(diz) was used as MOP. 12 A porous membrane (PNM) containing bix as a linker molecule and PU as a size-exclusion polymer was prepared by the solution casting method as follows. 12 The pore size is 0.65 nm.

[0075] First, the HRhMOP(diz) obtained as above 12 After drying in vacuum at room temperature, it was dissolved in a DMF solution of PU (3 wt%). 12 A PU / DMF solution of was obtained.

[0076] Next, bix (12 molar equivalents relative to MOP) was dissolved in a DMF solution of PU (3 wt%) to obtain a PU / DMF solution of bix.

[0077] Then, HRhMOP(diz) 12 The PU / DMF solution of bix was added to the PU / DMF solution of bix under vigorous stirring. The resulting clear purple solution was transferred to a Teflon Petri dish and heated at 80° C. overnight. After evaporating the DMF solvent by heating, the resulting membrane was removed from the Petri dish and dried under vacuum at 80° C. overnight. In this way, a porous membrane was obtained.

[0078] In the above process, HRhMOP(diz) 12 By appropriately adjusting the mass ratio of bix and PU, several samples with different porous polymer contents in the membrane were prepared. Example 1: 1% by weight (PNM-1) Example 2: 5% by weight (PNM-5) Example 3: 10% by mass (PNM-10) Example 4: 20% by mass (PNM-20) Example 5: 30% by mass (PNM-30) Five kinds of porous membranes were prepared.

[0079] Comparative Example 1 A filler-free PU membrane was prepared using a pure PU / DMF solution.

[0080] (Comparative Examples 2 to 4) HRhMOP(diz) as filler 12 A mixed matrix (MMM) containing PU as the matrix was prepared by solution casting method as follows.

[0081] Specifically, first, HRhMOP(diz) 12 The PU / DMF solution was added to the PU / DMF solution not containing bix with vigorous stirring. Using the obtained transparent pink solution, a membrane was formed in the same manner as in Examples 1 to 5.

[0082] In the above process, HRhMOP(diz) 12 By appropriately adjusting the mass ratio of the filler to the PU, several samples with different filler contents in the film were produced. Comparative example 2: 1% by mass (MMM-1) Comparative example 3: 5% by mass (MMM-5) Comparative example 4: 10% by mass (MMM-10) Three types of membranes were prepared. In this example, MMMs with a filler content of 20% by mass or more were extremely fragile and could not be molded into membranes. More specifically, such MMMs could not be non-destructively peeled off from the Petri dish. In the following, non-membrane samples with a filler content of 20% by mass were also used for evaluation as necessary. In the following, these non-membrane samples may also be referred to as MMM-20 or MMM-30 for convenience. Comparative example 5: 20% by mass (MMM-20) Comparative example 6: 30% by mass (MMM-30)

[0083] (Examples 6 to 8) We investigated the case where MOPs linked together by linker molecules were used as porous polymers. Specifically, HRhMOP(diz) was used as MOP. 12 A porous membrane (PNM) containing bix as a linker molecule and Pebax2533 (PB) as a size-exclusion polymer was prepared by solution casting as follows.

[0084] First, the HRhMOP(diz) obtained as above 12 After drying under vacuum at room temperature, it was dissolved in a DMF solution of PB (3 wt%) at 40°C. In this way, HRhMOP(diz) 12 A PB / DMF solution of was obtained.

[0085] Next, bix (12 molar equivalents relative to MOP) was dissolved in a PB / DMF solution (3 wt%) at 40° C. In this manner, a PB / DMF solution of bix was obtained.

[0086] Then, HRhMOP(diz) 12 The PB / DMF solution of was added to the PB / DMF solution of bix with vigorous stirring. The resulting clear purple solution was transferred to a Teflon Petri dish and heated at 80° C. overnight. After evaporating the DMF solvent by heating, the resulting membrane was removed from the Petri dish and dried under vacuum at 80° C. overnight. In this way, a porous membrane was obtained.

[0087] In the above process, HRhMOP(diz) 12 By appropriately adjusting the mass ratio of bix and PB, several samples with different porous polymer contents in the membrane were prepared. Example 6: 11.4% by weight Example 7: 22.8% by weight Example 8: 34.2% by weight Three types of porous membranes were prepared.

[0088] Comparative Example 7 Filler-free PB films were prepared using a pure PB / DMF solution.

[0089] (Comparative Examples 8 to 10) HRhMOP(diz) as filler 12 A mixed matrix (MMM) containing PB as the matrix was prepared by solution casting as follows.

[0090] Specifically, first, HRhMOP(diz) 12 The PB / DMF solution was added to the PB / DMF solution not containing bix with vigorous stirring. Using the obtained transparent pink solution, a membrane was formed in the same manner as in Examples 6 to 8.

[0091] In the above process, HRhMOP(diz) 12 By appropriately adjusting the mass ratio of PB to PB, several samples with different filler contents in the film were prepared. Comparative example 8: 11.4% by mass Comparative example 9: 22.8% by mass Comparative example 10: 34.2% by mass Three types of membranes were prepared:

[0092] (Examples 9 to 11) We investigated the case where MOPs linked together by linker molecules were used as porous polymers. Specifically, HRhMOP(diz) was used as MOP. 12 A porous membrane (PNM) containing bix as a linker molecule and PES as a size-exclusion polymer was prepared by solution casting as follows.

[0093] First, the HRhMOP(diz) obtained as above 12 After drying in vacuum at room temperature, it was dissolved in a DMF solution of PES (3 wt%). 12 A PES / DMF solution of

[0094] Next, bix (12 molar equivalents relative to MOP) was dissolved in a PES solution (3 wt%) in DMF to obtain a PES / DMF solution of bix.

[0095] Then, HRhMOP(diz) 12 The PES / DMF solution of bix was added to the PES / DMF solution of bix under vigorous stirring. The resulting clear purple solution was transferred to a glass Petri dish and heated at 80° C. overnight. After evaporating the DMF solvent by heating, the resulting membrane was removed from the Petri dish and dried under vacuum at 80° C. overnight. In this way, a porous membrane was obtained.

[0096] In the above process, HRhMOP(diz) 12 By appropriately adjusting the mass ratio of bix and PES, several samples with different porous polymer contents in the membrane were prepared. Example 9: 5% by weight Example 10: 10% by weight Example 11: 20% by weight Three types of porous membranes were prepared.

[0097] Comparative Example 11 Filler-free PES membranes were prepared using a pure PES / DMF solution.

[0098] (Comparative Examples 12 to 14) HRhMOP(diz) as filler 12 A mixed matrix (MMM) containing PES as the matrix was prepared by solution casting as follows.

[0099] Specifically, first, HRhMOP(diz) 12 The PES / DMF solution was added to a PES / DMF solution not containing bix with vigorous stirring. Using the obtained transparent pink solution, a membrane was formed in the same manner as in Examples 9 to 11.

[0100] In the above process, HRhMOP(diz) 12By appropriately adjusting the mass ratio of and PES, several samples with different filler contents in the membrane were prepared. Comparative example 12: 5% by mass Comparative example 13: 10% by mass Comparative example 14: 20% by mass Three types of membranes were prepared:

[0101] Example 12 We investigated the case where MOPs linked together by linker molecules were used as porous polymers. Specifically, HRhMOP(diz) was used as MOP. 12 A porous membrane (PNM) containing bix as a linker molecule and AP as a size-exclusion polymer was prepared by solution casting as follows.

[0102] First, the HRhMOP(diz) obtained as above 12 After drying under vacuum at room temperature, it was dissolved in a DMF solution (3 wt%) of AP. 12 AP / DMF solution was obtained.

[0103] Next, bix (12 molar equivalents relative to MOP) was dissolved in a DMF solution of AP (3 wt%) to obtain an AP / DMF solution of bix.

[0104] Then, HRhMOP(diz) 12 The AP / DMF solution of bix was added to the AP / DMF solution of bix under vigorous stirring. The resulting clear purple solution was transferred to a glass Petri dish and heated at 80° C. overnight. After evaporating the DMF solvent by heating, the resulting membrane was removed from the Petri dish and dried under vacuum at 80° C. overnight. In this way, a porous membrane was obtained.

[0105] The content of the porous polymer in the obtained membrane was adjusted as follows. Example 12: 5% by weight

[0106] Comparative Example 15 A pure AP / DMF solution was used to prepare filler-free AP membranes.

[0107] (Examples 13 to 16) We investigated the case where MOF was used as a porous polymer. Specifically, a porous membrane (PNM) containing UiO66-NH2 as MOF and PU as a size exclusion polymer was prepared by solution casting as follows. The pore size of UiO66-NH2 is 1.2 nm.

[0108] First, a precursor gel containing MOF was prepared as follows: 0.88 g (4.8 mmol) of 2-aminoterephthalic acid and 1.07 g (3.3 mmol) of ZrOCl2·8H2O were dissolved in 20 mL of DMF, followed by the addition of 0.5 mL of 37 wt% HCl and 0.67 mL of glacial acetic acid. After ultrasonication for 5 min, the resulting solution was placed in an oven and heated at 100 °C for 2 h to obtain MOF (UiO66-NH2) in a gel state.

[0109] Next, a suspension containing MOFs was prepared as follows: first, the obtained MOF gel was washed three times with DMF and three times with ethanol. Fresh solvent was added at each washing step so that the total mixed volume expanded to twice that of the as-synthesized gel. The gel was homogenized with fresh solvent using a vertex mixer and sonicator to obtain a suspension of MOFs. The expanded suspension was then heated overnight at 120 °C for the DMF washing process and at 60 °C for the ethanol washing process. The obtained ethanol suspension of MOFs was then centrifuged and the supernatant was decanted. For membrane synthesis, following the last washing step, the volume of the UiO66-NH2 suspension was adjusted again by adding fresh solvent to control the MOF concentration. In this way, an ethanol suspension of MOFs (UiO66-NH2) was obtained.

[0110] Then, the suspension of MOF (UiO66-NH2) was added to the ethanol solution of PU (6 wt%) in a certain volume ratio and homogenized using a Vertex mixer and a sonicator. The resulting solution was transferred to a Teflon Petri dish and heated at 60°C overnight. After evaporating the ethanol solvent by heating, the resulting membrane was removed from the Petri dish and dried under vacuum at 80°C overnight. In this way, a porous membrane was obtained.

[0111] In the above process, the mass ratio of UiO66-NH2 and PU was appropriately adjusted to produce several samples with different porous polymer contents in the membrane. Example 13: 16.5% by weight Example 14: 33% by weight Example 15: 49.5% by weight Example 16: 66% by weight Four types of porous membranes were prepared.

[0112] (Comparative Examples 16 to 18) A mixed matrix (MMM) containing UiO66-NH2 nanoparticles as filler and PU as matrix was prepared by solution casting method as follows.

[0113] First, MOF nanoparticles were prepared as follows: 447.1 g (2.47 mmol) of 2-aminoterephthalic acid and 417.1 g (1.79 mmol) of ZrCl4 were dissolved in a mixture of 50 mL of DMF and 3.3 mL of HCl. After sonication for mixing, the resulting solution was placed in an oven and heated at 120 °C for 24 h to obtain MOFs. The resulting MOF nanoparticles were washed three times with DMF and three times with ethanol. Using a vertex mixer and sonicator, the MOF nanoparticles were homogenized with fresh solvent to obtain a suspension of MOFs. The nanoparticles were then separated from the suspension by centrifugation and the supernatant solution was decanted. For membrane synthesis, following the final washing step, the volume of the MOF suspension was adjusted again by adding fresh solvent to control the MOF concentration. In this way, an ethanol suspension of MOF (UiO66-NH2) particles was obtained.

[0114] The suspension of MOF (UiO66-NH2) particles was then added to a PU ethanol solution (6 wt%) in a certain volume ratio and homogenized using a Vertex mixer and sonicator. The resulting solution was transferred to a Teflon Petri dish and heated at 60°C overnight. After evaporating the ethanol solvent by heating, the resulting film was removed from the Petri dish and dried under vacuum at 80°C overnight. In this way, the MMM was fabricated.

[0115] In the above process, the mass ratio of UiO66-NH2 and PU was appropriately adjusted to produce several samples with different filler contents in the film. Comparative example 16: 16.5% by mass Comparative example 17:33% by mass Comparative example 18: 49.5% by mass Three types of films were prepared. In this example, MMMs with a content of 66% by mass or more were extremely fragile and could not be molded into films. More specifically, for such MMMs, films could not be nondestructively peeled off from the Petri dish.

[0116] (Examples 17 to 19) An example of using MOF as a porous polymer was examined. Specifically, a porous membrane (PNM) containing UiO66-NH2 as MOF and PB as a size exclusion polymer was prepared by a solution casting method as follows. Specifically, the porous membrane was prepared in the same manner as in Examples 13 to 16, except that PB was used instead of PU.

[0117] In the above process, the mass ratio of UiO66-NH2 and PB was appropriately adjusted to produce several samples with different porous polymer contents in the membrane. Example 17: 16.5% by weight Example 18: 33% by weight Example 19: 49.5% by weight Three types of porous membranes were prepared.

[0118] (Comparative Examples 19 to 21) A mixed matrix (MMM) containing UiO66-NH2 nanoparticles as a filler and PB as a matrix was prepared by a solution casting method as follows. Specifically, a porous membrane was prepared in the same manner as in Comparative Examples 16 to 18, except that PB was used instead of PU.

[0119] In the above process, the mass ratio of UiO66-NH2 and PB was appropriately adjusted to produce several samples with different filler contents in the film. Comparative example 19: 16.5% by mass Comparative example 20:33% by mass Comparative example 21: 49.5% by mass Three types of membranes were prepared:

[0120] (Examples 20 to 22) An example of using MOF as a porous polymer was examined. Specifically, a porous membrane (PNM) containing UiO66-NH2 as MOF and PES as a size exclusion polymer was prepared by a solution casting method as follows. Specifically, the porous membrane was prepared in the same manner as in Examples 13 to 16, except that PES was used instead of PU.

[0121] In the above process, the mass ratio of UiO66-NH2 and PES was appropriately adjusted to produce several samples with different porous polymer contents in the membrane. Example 20: 16.5% by weight Example 21: 33% by weight Example 22: 49.5% by weight Three types of porous membranes were prepared.

[0122] (Comparative Examples 22 to 24) A mixed matrix (MMM) containing UiO66-NH2 nanoparticles as a filler and PES as a matrix was prepared by a solution casting method as follows: Specifically, a porous membrane was prepared in the same manner as in Comparative Examples 16 to 18, except that PES was used instead of PU.

[0123] In the above process, the mass ratio of UiO66-NH2 and PES was appropriately adjusted to produce several samples with different filler contents in the membrane. Comparative example 22: 16.5% by mass Comparative example 23: 33% by mass Comparative example 24: 49.5% by mass Three types of membranes were prepared:

[0124] Evaluation of the gelation process by dynamic light scattering (DLS) method In the above-mentioned solution casting method for forming a porous membrane using MOP, the following DLS measurement was carried out to confirm that a precursor gel was formed before the solvent was completely removed.

[0125] This study used HRhMOP(diz) as MOP. 12 The DLS was performed on a system containing bix as a linker molecule and PB as a size exclusion polymer. Specifically, the test is performed by heating sealed solutions of MOP and linker molecules in the presence and absence of PB in DMF solution without evaporating the solvent. DLS is the time-averaged scattered light intensity. T The change in the gel point is shown as a function of heating time. T It is calculated as the time when the value of starts to change.

[0126] FIG. 4 shows the results of dynamic light scattering measurements showing the formation process of a precursor gel in a size exclusion polymer. FIG. 4 shows the results of a time-resolved DLS experiment of a DMF solution of MOP under conditions of 80° C. and 0.35 mM (11 wt% MOP relative to PB) in the presence / absence of PB. As can be seen from the data shown at the bottom of FIG. 4, in the system in which PB is present, gelation occurred in about 10 minutes. In contrast, as shown in the above Examples 6 to 8, evaporation of the solvent during membrane formation typically takes about one night. From these observation results, it was confirmed that in membrane formation using a solution casting method in a porous membrane using MOP, a precursor gel is formed before the solvent is completely removed.

[0127] Formation of network structure In order to confirm that the porous polymer particles in the above-mentioned porous membrane are bound to each other by chemical bonds or physical cohesive forces to form a network structure, the following evaluation was carried out.

[0128] First, the surfaces of the samples of Comparative Example 1 (PU only), Example 3 (PNM-10), and Example 5 (PNM-30) were subjected to SEM measurement using an FESEM (Hitachi S-4800).

[0129] Fig. 5 shows surface SEM images of the films according to Comparative Example 1, Example 3, and Example 5. In Fig. 5, (a) to (c) are samples of Comparative Example 1, (d) to (f) are samples of Example 3, and (h) to (j) are samples of Example 5.

[0130] As shown in Fig. 5, the porous membranes according to Examples 3 and 5 had a homogeneous surface, similar to the membrane according to Comparative Example 1. Furthermore, in the porous membranes according to Examples 3 and 5, no domain generation due to the aggregation of the porous polymer was observed. Furthermore, in the porous membranes according to Examples 3 and 5, the formation of a colloid network structure inside the membrane surface was suggested.

[0131] To further investigate this point, cross-sectional SEM measurements were performed on the same samples using a JEOL Model JSM-7001F4 system.

[0132] Fig. 6 shows cross-sectional SEM images of the films according to Comparative Example 1, Example 3, and Example 5. In Fig. 6, (a) to (c) are samples of Comparative Example 1, (d) to (f) are samples of Example 3, and (h) to (j) are samples of Example 5.

[0133] 6, the presence of a colloidal network structure was observed in the porous membranes of Examples 3 and 5. In particular, the presence of colloidal particles was clearly observed in the porous membrane of Example 5.

[0134] Next, the same measurements were carried out on the samples according to Comparative Example 4 (MMM-10) and Comparative Example 6 (MMM-30).

[0135] 7 shows surface SEM images of samples according to Comparative Example 4 and Comparative Example 6. In FIG. 7, (a) to (c) are the sample of Comparative Example 4, and (d) to (f) are the sample of Comparative Example 6.

[0136] 8 shows cross-sectional SEM images of samples according to Comparative Example 4 and Comparative Example 6. In FIG. 8, (a) to (c) are samples according to Comparative Example 4, and (d) to (f) are samples according to Comparative Example 6.

[0137] As shown in Figures 7 and 8, clear phase separation occurred in these samples, and many spherical non-network type aggregates were observed, and the presence of such aggregates became more prominent with increasing amounts of MOP in the samples.

[0138] For further comparison, observations were also made using an optical microscope.

[0139] 9 shows optical microscope images of the samples of Example 5 and Comparative Example 6. In FIG. 9, (a) is the porous membrane according to Example 5, and (b) is the sample according to Comparative Example 6.

[0140] 9, no phase separation was observed in the porous membrane of Example 5, and a hierarchical hybrid system including a colloidal network structure was formed. In contrast, in the sample of Comparative Example 6, the generation of domains was observed due to the presence of discrete aggregates.

[0141] In addition, to confirm the presence of a colloidal network structure in the above-mentioned porous membrane, an aerogel was prepared from the porous membrane and observed by SEM. Specifically, the porous membrane according to Example 5 was first washed with DMF to remove PU. Then, a solvent exchange from DMF to acetone was performed. Then, the corresponding aerogel was prepared by applying a supercritical CO2 drying process. The drying process was carried out by a SCLEAD-2BD autoclave (KISCO) using supercritical CO2 at 14 MPa and 50°C.

[0142] Fig. 10 shows SEM images of the aerogel produced from the porous membrane of Example 5. In Fig. 10, (a) shows a schematic diagram of the aerogel production process, and (b) and (c) show SEM images of the obtained aerogel.

[0143] A characteristic colloidal network structure was confirmed in the aerogel obtained in this manner, as shown in Figure 10. This observation result strongly suggests that a similar colloidal network structure was also formed in the porous membrane.

[0144] Mechanical strength evaluation The mechanical strength of the membranes according to the examples and comparative examples obtained as described above was evaluated as follows. That is, the rheology measurements of the membrane samples were performed using a stress-controlled AR-G2 rheometer (manufactured by TA Instruments). Dynamic mechanical analysis (DMA) measurements of the membranes were performed by frequency sweep in tensile mode with a strain amplitude of 0.5%, well inside the linear region (initial strain fixed at 0.3%). Note that the storage modulus in the following refers to a value measured at 1 rad / s, unless otherwise specified.

[0145] Fig. 11 shows the results of measuring the storage modulus of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 and 4. As shown in Fig. 11, it was found that the porous membranes according to the Examples have superior mechanical strength compared to the polymer membranes or mixed matrix membranes according to the Comparative Examples.

[0146] Fig. 12 shows the results of measuring the storage modulus of the membrane samples (MOP / PB) according to Examples 6 to 8 and Comparative Examples 7 to 10. As shown in Fig. 12, it was found that the porous membranes according to the Examples have superior mechanical strength compared to the polymer membranes or mixed matrix membranes according to the Comparative Examples.

[0147] Fig. 13 shows the results of measuring the storage modulus of the membrane samples (MOP / PES) according to Examples 9 to 11 and Comparative Examples 11 to 14. As shown in Fig. 13, it was found that the porous membranes according to the Examples have superior mechanical strength compared to the polymer membranes or mixed matrix membranes according to the Comparative Examples.

[0148] Fig. 14 shows the results of viscoelasticity measurement in a tensile mode of the membrane sample (MOP / AP) according to Example 12. Fig. 15 shows the results of viscoelasticity measurement in a tensile mode of the membrane sample (AP) according to Comparative Example 15. In the viscoelasticity measurement data shown in Figs. 14 and 15, the filled data points indicate the storage modulus E', and the open data points indicate the loss modulus E''.

[0149] As shown in FIGS. 14 and 15, it was found that the porous membrane of Example 12 had superior mechanical strength compared to the polymer membrane of Comparative Example 15.

[0150] Fig. 16 shows the results of measuring the storage modulus of the membrane samples (MOF / PU) according to Examples 13 to 16 and Comparative Examples 1 and 16 to 18. As shown in Fig. 16, it was found that the porous membranes according to the Examples have superior mechanical strength compared to the polymer membranes or mixed matrix membranes according to the Comparative Examples.

[0151] Fig. 17 shows the results of measuring the storage modulus of the membrane samples (MOF / PB) according to Examples 17 to 19 and Comparative Examples 7 and 19 to 21. As shown in Fig. 17, it was found that the porous membranes according to the Examples have superior mechanical strength compared to the polymer membranes or mixed matrix membranes according to the Comparative Examples.

[0152] Fig. 18 shows the results of measuring the storage modulus of the membrane samples (MOF / PES) according to Examples 20 to 22 and Comparative Examples 11 and 22 to 24. As shown in Fig. 18, it was found that the porous membranes according to the Examples have superior mechanical strength compared to the polymer membranes according to the Comparative Examples. It was also found that the porous membranes according to the Examples have the same or higher mechanical strength compared to the mixed matrix membranes according to the Comparative Examples.

[0153] Gas Permeability and Gas Selectivity The gas permeability and gas selectivity of the membranes according to the examples and comparative examples obtained as described above were evaluated. The evaluation was performed by the method previously described with reference to Figure 1. The measurements were performed under the conditions of 2 bar / 25°C.

[0154] FIG. 19 shows the measurement results of CO2 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 20 shows the measurement results of N2 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 21 shows the measurement results of CH4 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 22 shows the measurement results of H2 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 23 shows the measurement results of O2 permeability of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. As can be seen from these results, the porous membranes according to the examples have superior gas permeability compared to the polymer membranes or mixed matrix membranes according to the comparative examples.

[0155] FIG. 24 shows the measurement results of the CO2 / N2 permeation selectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 25 shows the measurement results of the CO2 / H2 permeation selectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 26 shows the measurement results of the CO2 / CH4 permeation selectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 27 shows the measurement results of the H2 / N2 permeation selectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 28 shows the measurement results of the H2 / CH4 permeation selectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. FIG. 29 shows the measurement results of the O2 / N2 permeation selectivity of the membrane samples (MOP / PU) according to Examples 1 to 5 and Comparative Examples 1 to 4. As can be seen from these results, the porous membranes according to the examples have superior gas selectivity compared to the polymer membranes or mixed matrix membranes according to the comparative examples.

[0156] Table 4 shows the measurement results of gas permeability and gas selectivity of the membrane sample (MOP / AP) according to Example 12 and the membrane sample (AP) according to Comparative Example 15. As shown in Table 4, the porous membrane according to Example 12 had higher permeability to CO2 and N2 and lower permeability to CH4 than the polymer membrane according to Comparative Example 15. That is, it was found that the porous membrane according to Example 12 exhibited superior CO2 / CH4 selectivity compared to the polymer membrane according to Comparative Example 15.

[0157] [Table 4]

[0158] As described above, it has been found that the porous membrane according to the present invention can achieve both excellent gas permeability and mechanical strength due to the presence of a network structure. Therefore, the porous membrane according to the present invention can be used as a gas permeable membrane or gas separation membrane with excellent mechanical strength. This porous membrane can also be used as a part of a gas separation system.

Claims

1. A porous polymer having pores in its molecule; a size exclusion polymer having a molecular size that is too large to occupy the pores; Including, The porous polymer forms a plurality of particles, and the plurality of particles are bonded to each other by chemical bonds or physical cohesive forces to form a network structure. Porous membrane.

2. 2. The porous membrane according to claim 1, wherein the porous polymer is at least one porous polymer selected from the group consisting of metal-organic frameworks (MOFs), porous organic polymers (POPs), and metal-organic polyhedra (MOPs) linked together by linker molecules.

3. 3. The porous membrane of claim 1 or 2, wherein the size-exclusion polymer is at least one polymer selected from the group consisting of thermoplastics, inherently microporous polymers (PIMs), and silicones.

4. The porous membrane according to claim 1 or 2, wherein the content of the porous polymer in the porous membrane is 10 mass % or more.

5. 3. The porous membrane according to claim 1, wherein the permeability to at least one type of gas molecule is at least 1.2 times the permeability to a membrane consisting of only the size exclusion polymer.

6. 3. The porous membrane according to claim 1, wherein the storage modulus at 1 rad / s is at least twice as large as the storage modulus in a membrane consisting of only the size exclusion polymer.

7. The porous membrane according to claim 1 or 2, which is prepared using a precursor gel containing the porous polymer.

8. A gas separation system comprising the porous membrane of claim 1 or 2.

9. forming a precursor gel containing a metal-organic framework (MOF) or a porous organic polymer (POP) having intramolecular pores; adding a solvent to the precursor gel to prepare a suspension; mixing the suspension with a size exclusion polymer; removing the solvent; Including, the solvent has a molecular size large enough to occupy the pores, The size-exclusion polymer has a molecular size that is too large to occupy the pores. A method for producing a porous membrane.

10. forming a precursor gel including metal-organic polyhedra (MOPs) having intramolecular voids and interconnected by linker molecules, a solvent, and a size-exclusion polymer; removing the solvent; Including, the solvent has a molecular size large enough to occupy the pores, The size-exclusion polymer has a molecular size that is too large to occupy the pores. A method for producing a porous membrane.

11. The step of forming a precursor gel includes: providing a first solution comprising the metal-organic polyhedron, the solvent, and the size exclusion polymer; providing a second solution comprising the linker molecule, the solvent and the size exclusion polymer; mixing the first solution with the second solution; The method of claim 10, comprising:

12. 12. The method of any one of claims 9 to 11, wherein the size-exclusion polymer is at least one polymer selected from the group consisting of thermoplastics, inherently microporous polymers (PIMs), and silicones.

Citation Information

Cited By

  • Preparation method of defective MOF (Metal Organic Framework)-based intrinsic microporous polymer mixed matrix membrane for efficient separation of propylene and propane

    CN119819139A

  • Preparation method of defective MOF-based self-microporous polymer mixed matrix membrane for efficient separation of propylene and propane

    CN119819139B

  • CO gas separation sheet, CO gas separation solid membrane element, CO gas separation unit, and CO gas concentration system

    JP7906157B1

  • Co gas separation sheet, co gas separation solid membrane element, co gas separation unit, and co gas concentration system

    WO2026120836A1