Primer composition, functional member and method for producing functional member

A primer composition with alkoxysilanes and (meth)acryloyl groups enhances the durability of functional layers on resin or painted surfaces by improving adhesion, addressing the lack of durability in existing technologies.

JP2024135046APending Publication Date: 2024-10-04LIXIL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023045542
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

The functional layer in existing technologies lacks durability against chemical and physical influences such as abrasion and chemical substances.

Method used

A primer composition containing specific alkoxysilanes, aminoalkylalkoxysilanes, and (meth)acryloyl groups, along with an organic solvent, is used to form a primer layer that enhances the adhesion and durability of a functional layer on resin or painted surfaces.

Benefits of technology

The primer composition improves the durability of the functional layer, maintaining its functionality under chemical and physical stress, such as abrasion and weathering, by promoting strong adhesion and resistance to peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135046000017
    Figure 2024135046000017
  • Figure 2024135046000001
    Figure 2024135046000001
  • Figure 2024135046000002
    Figure 2024135046000002
Patent Text Reader

Abstract

To provide a primer composition that can impart durability to a functional layer of a functional member; to provide a functional member; and to provide a method for producing a functional member.SOLUTION: A primer composition contains alkoxysilane with a specific structure (A), aminoalkyl alkoxysilane with a specific structure (B), alkoxysilane with at least one group selected from the group consisting of (meth)acryloyl groups and epoxy groups (C), and organic solvent (D).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a primer composition, a functional member, and a method for producing a functional member. [Background technology]

[0002] Surface modification treatments are carried out to impart various functionalities such as hydrophilicity, antibacterial properties, and antiviral properties to resin products and painted surfaces of building materials. One method of such surface modification treatments is a treatment of providing a functional layer that imparts functionality to the surface. A silane coupling agent having functional groups with various functionalities introduced therein is used as a raw material for the functional layer. In the treatment of providing the functional layer, a treatment of providing a primer layer between the resin product, the painted surface, and the functional layer may be carried out in order to increase the adhesion between the resin product, the painted surface, and the functional layer. The primer layer is formed from a primer composition.

[0003] For example, Patent Document 1 proposes a hydrophilic member having, in this order, a substrate, an undercoat layer (primer layer) formed from a primer composition containing an alkoxysilane having a specific structure, and an overcoat layer (functional layer) formed from a hydrophilic silane coupling agent. In the hydrophilic member of Patent Document 1, the adhesion between the substrate and the functional layer is enhanced by providing a primer layer on the surface of the substrate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-064474 A Summary of the Invention [Problem to be solved by the invention]

[0005] The functional layer of Patent Document 1 does not have sufficient durability against chemical influences such as chemical substances and physical influences such as abrasion.

[0006] The present disclosure has been made in consideration of such problems, and aims to provide a primer composition, a functional member, and a method for manufacturing a functional member that can impart durability to a functional layer. [Means for solving the problem]

[0007] One aspect of the present disclosure is a primer composition containing one or more alkoxysilanes (A) selected from compounds represented by the following general formula (I-1) and compounds represented by the following general formula (I-2), one or more aminoalkylalkoxysilanes (B) selected from compounds represented by the following general formula (II-1) and compounds represented by the following general formula (II-2), an alkoxysilane (C) having one or more groups selected from the group consisting of a (meth)acryloyl group and an epoxy group, and an organic solvent (D). In this specification, the term "(meth)acryloyl group" refers to at least one of an acryloyl group and a methacryloyl group.

[0008] [ka]

[0009] In formula (I-1), R 1 Each independently represents an alkyl group having 1 to 4 carbon atoms. 2 each independently represents an alkyl group having 1 to 4 carbon atoms.

[0010] [ka]

[0011] In formula (II-1), R 3 each independently represents an alkyl group having 1 or 2 carbon atoms, x is an integer of 1 to 6, y is an integer of 1 to 10, and n is an integer of 0 to 10. In formula (II-2), R 4 each independently represents an alkyl group having 1 or 2 carbon atoms, z is an integer of 1 to 10, and w is an integer of 1 to 10. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a cross-sectional view illustrating an example of a functional member according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In this specification, a numerical range expressed using "~" includes the numerical values ​​on both ends of the "~". In this specification, for preferred numerical ranges (for example, ranges of content, etc.), lower limit values ​​and upper limit values ​​described stepwise can be combined independently. Hereinafter, one embodiment of the present disclosure will be described with reference to Fig. 1. The functional member 100 shown in Fig. 1 includes a resin substrate / coated substrate 10, a primer layer 20, and a functional layer 30, in this order.

[0014] Thickness T of the functional member 100 100 is not particularly limited. 100 is, for example, preferably 0.001 mm or more and 500 mm or less, more preferably 0.001 mm or more and 300 mm or less, and even more preferably 0.001 mm or more and 200 mm or less. 100 When the thickness T is equal to or greater than the lower limit, the strength of the functional member 100 is easily increased. 100 When the thickness T of the functional member 100 is equal to or less than the upper limit, the functional member 100 can be made lighter and easier to handle. 100 can be measured, for example, using a vernier caliper.

[0015] The resin substrate / coated substrate 10 may be made of general-purpose plastic materials, engineering plastic materials, or materials obtained by coating these plastic materials or metals. General-purpose plastic materials include, for example, polyolefin resins such as acrylic resin, polyethylene resin, and polypropylene resin, acrylonitrile-butadiene-styrene (ABS) resin, polyvinyl chloride resin, polystyrene (PS), polyethylene terephthalate (PET), and unsaturated polyester (UP) resin. Engineering plastic materials include polycarbonate (PC), nylon resin, and polyphenylene ether (PPE). Coating resins include acrylic urethane and acrylic melamine coating. The resin substrate 10 may be made of a resin containing fillers such as glass fiber, calcium carbonate, aluminum hydroxide, aluminum oxide, and silica.

[0016] Thickness T of the resin substrate 10 10 is not particularly limited. 10 is, for example, preferably 0.001 mm or more and 500 mm or less, more preferably 0.001 mm or more and 300 mm or less, and even more preferably 0.001 mm or more and 200 mm or less. 10 When the thickness T is equal to or greater than the lower limit, the strength of the functional member 100 is easily increased. 10 When the thickness T of the resin substrate 10 is equal to or less than the upper limit, the weight of the functional member 100 can be reduced, and the functional member 100 is easy to handle. 10 can be measured, for example, using a vernier caliper.

[0017] The primer layer 20 is a primer composition according to the present disclosure or a cured product thereof. In this specification, the cured product refers to one or more selected from hydrolyzable alkoxysilanes and their hydrolyzed condensation polymers that have been condensed or crosslinked by heat, a catalyst, or the like to become insoluble and infusible. The primer composition according to the present disclosure contains an alkoxysilane (A), an aminoalkylalkoxysilane (B), an alkoxysilane (C) having one or more groups selected from the group consisting of a (meth)acryloyl group and an epoxy group, and an organic solvent (D).

[0018] The alkoxysilane (A) is at least one selected from the group consisting of compounds represented by the following general formula (I-1) and compounds represented by the following general formula (I-2).

[0019] [ka]

[0020] In formula (I-1), R 1 Each independently represents an alkyl group having 1 to 4 carbon atoms. 2 each independently represents an alkyl group having 1 to 4 carbon atoms.

[0021] Examples of the compound represented by formula (I-1) include tetraalkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane. Among the compounds represented by formula (I-1), tetramethoxysilane and tetraethoxysilane are preferred from the viewpoint of ease of dehydration condensation.

[0022] The compound represented by formula (I-2) is, for example, 2 Compounds with methyl group and m between 0 and 1000, R 2 Compounds with ethyl groups and m between 0 and 1000, R 2 is a butyl group and m is 0 to 1000.

[0023] The compound represented by formula (I-2) has a degree of polymerization m of 0 to 1000, preferably 10 to 80, and more preferably 30 to 50. When the degree of polymerization m is equal to or greater than the lower limit, more silanol groups are easily formed on the surface of the primer layer 20. When the degree of polymerization m is equal to or less than the upper limit, the compound is easily dissolved in the organic solvent (D). The compound represented by formula (I-2) is a polymer in which two or more molecules of tetraalkoxysilane are dehydrated and condensed intermolecularly. When the degree of polymerization m is 0, the compound represented by formula (I-2) is a dimer of tetraalkoxysilane in which two molecules of tetraalkoxysilane are dehydrated and condensed. The degree of polymerization m can be controlled by the concentration of tetraalkoxysilane, the temperature during dehydration and condensation, and the like.

[0024] The compound represented by formula (I-2) may be polymerized by dehydration condensation of tetraalkoxysilane represented by formula (I-1), or a commercially available product may be used. Examples of commercially available products of the compound represented by formula (I-2) include methyl silicate oligomer MS51 and MS56 manufactured by Mitsubishi Chemical Corporation.

[0025] The content of alkoxysilane (A) is preferably 0.01% by mass or more and 2.0% by mass or less, more preferably 0.02% by mass or more and 1.5% by mass or less, and even more preferably 0.03% by mass or more and 1.0% by mass or less, based on the total mass of the primer composition. When the content of alkoxysilane (A) is equal to or more than the lower limit, it is easy to introduce various types of functionality-imparting compounds into the functional layer 30, and the functional layer 30 is excellent in abrasion resistance, light resistance, and the like. When the content of alkoxysilane (A) is equal to or less than the upper limit, it is easy to suppress the change in appearance when the primer composition is applied to the resin substrate 10. The alkoxysilane (A) may be used alone or in combination of two or more types.

[0026] The alkoxysilane (C) having one or more groups selected from the group consisting of an acryloyl group and an epoxy group preferably contains one or more compounds selected from the group consisting of a compound (C1) represented by the following general formula (III-1), a compound (C2) represented by the following general formula (III-2), and a compound (C3) containing a structural unit represented by the following general formula (III-3) or the following general formula (III-4).

[0027] [ka]

[0028] [ka]

[0029] [ka]

[0030] In formula (III-1), R 5 each independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent, and at least one of these has a (meth)acryloyl group or an epoxy group as a substituent. 6 each independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent, at least one of which has a (meth)acryloyl group or an epoxy group as a substituent. s is an integer of 0 to 1000. In formula (III-3), R 7 R each independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent, and at least one of these has a (meth)acryloyl group or an epoxy group as a substituent. 8 Each of R independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent. Each of Y independently represents a divalent linking group. n is an integer of 1 to 1000. In formula (III-4), R 7 , R 8 and Y is R in formula (III-3). 7 , R 8and Y. R 9 each independently represents a hydrogen atom, a hydroxyl group, or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. p, q, and r each independently represent 0 to 1000, and when p is 0, q and r each independently represent 1 to 1000, with the proviso that when p is 1 or more, q and r each independently represent 0 to 1000.

[0031] Examples of the compound (C1) represented by formula (III-1) include alkoxysilanes having (meth)acryloyloxy, such as (meth)acryloyloxypropyltrimethoxysilane, (meth)acryloyloxypropyltriethoxysilane, (meth)acryloyloxypropyltripropoxysilane, (meth)acryloyloxypropyltributoxysilane, 3-(meth)acryloyloxypropylmethyldimethoxysilane, and 3-(meth)acryloyloxypropylmethyldiethoxysilane; and alkoxysilanes having an epoxy group, such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyltripropoxysilane, and 3-glycidoxypropyltributoxysilane. Among the compounds (C1) represented by formula (III-1), from the viewpoint of ease of dehydration condensation, alkoxysilanes having an alkoxy group having 1 to 4 carbon atoms and having a (meth)acryloyloxy group as a substituent, alkoxysilanes having an alkoxy group having 1 to 4 carbon atoms and having an epoxy group as a substituent, and the like are listed, with 3-(meth)acryloyloxypropyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane being preferred.

[0032] The compound (C2) represented by formula (III-2) is, for example, R 6 Compounds with methyl group and s between 0 and 1000, R 6 Compounds with ethyl group and s between 0 and 1000, R 6 Examples of compounds include those in which is a butyl group and s is 0 to 1000.

[0033] In the compound (C2) represented by formula (III-2), s represents the degree of polymerization, and is 0 to 1000, preferably 10 to 80, and more preferably 30 to 50. When the degree of polymerization s is equal to or greater than the lower limit, more silanol groups are easily formed on the surface of the primer layer 20. When the degree of polymerization s is equal to or less than the upper limit, the compound is easily dissolved in the organic solvent (D). The compound (C2) represented by formula (III-2) is a polymer in which two or more molecules of tetraalkoxysilane having a (meth)acryloyl group or an epoxy group as a substituent are dehydrated and condensed intermolecularly. When the degree of polymerization s is 0, the compound (C2) represented by formula (III-2) is a dimer of tetraalkoxysilane in which two molecules of tetraalkoxysilane having a (meth)acryloyl group or an epoxy group as a substituent are dehydrated and condensed. The degree of polymerization s can be controlled by the concentration of the tetraalkoxysilane, the temperature during dehydration and condensation, and the like.

[0034] The compound (C1) represented by formula (III-1) may be commercially available. Examples of the commercially available compound (C1) represented by formula (III-1) include KBM403 and KBM503 manufactured by Shin-Etsu Chemical Co., Ltd.

[0035] The compound (C2) represented by formula (III-2) may be commercially available. Examples of the commercially available compound (C2) represented by formula (III-2) include KR516 manufactured by Shin-Etsu Chemical Co., Ltd.

[0036] In the compound (C3) represented by formula (III-3) or formula (III-4), Y is a divalent linking group. Examples of the divalent linking group include a divalent hydrocarbon group having 1 to 10 carbon atoms, an ether bond (-O-), and combinations thereof. In the compound (C3) having one or more groups selected from the group consisting of (meth)acryloyl groups and epoxy groups and a trialkoxysilyl group, the alkoxy group is preferably an alkoxy group having 1 to 4 carbon atoms, more preferably a methoxy group or an ethoxy group. As the compound (C3), a compound having one or more groups selected from the group consisting of (meth)acryloyl groups and epoxy groups and one or more groups selected from the group consisting of trimethoxysilyl groups and triethoxysilyl groups is preferred, and a compound having one or more groups selected from the group consisting of acryloyl groups and epoxy groups and one or more groups selected from the group consisting of trimethoxysilyl groups and triethoxysilyl groups is more preferred. As the compound (C3), a commercially available product may be used. Examples of commercially available products of the compound (C3) include X-12-984S, X-12-1048, and X-12-1050 manufactured by Shin-Etsu Chemical Co., Ltd.

[0037] The content of alkoxysilane (C) is preferably 0.01% by mass or more and 3.0% by mass or less, more preferably 0.02% by mass or more and 2.0% by mass or less, and even more preferably 0.03% by mass or more and 1.5% by mass or less, based on the total mass of the primer composition. When the content of alkoxysilane (C) is equal to or more than the lower limit, it is easy to introduce various types of functionality-imparting compounds into the functional layer 30. When the content of alkoxysilane (C) is equal to or less than the upper limit, it is easy to suppress changes in appearance when the primer composition is applied to the resin substrate 10.

[0038] The sum of the content of alkoxysilane (A) and the content of alkoxysilane (C) (hereinafter also referred to as the A+C amount) is preferably 0.01% by mass or more and 5% by mass or less, more preferably 0.02% by mass or more and 3% by mass or less, and even more preferably 0.04% by mass or more and 2.0% by mass or less, based on the total mass of the primer composition. When the A+C amount is equal to or more than the lower limit, it is easy to introduce various types of functionality-imparting compounds into the functional layer 30. When the A+C amount is equal to or less than the upper limit, it is easy to suppress changes in appearance when the primer composition is applied to the resin substrate 10.

[0039] The aminoalkylalkoxysilane (B) is at least one selected from the group consisting of compounds represented by the following general formula (II-1) and compounds represented by the following general formula (II-2).

[0040] [ka]

[0041] In formula (II-1), R 3 each independently represents an alkyl group having 1 or 2 carbon atoms, x is an integer of 1 to 6, y is an integer of 1 to 10, and n is an integer of 0 to 10. In formula (II-2), R 4 each independently represents an alkyl group having 1 or 2 carbon atoms, z is an integer of 1 to 10, and w is an integer of 1 to 10.

[0042] In formula (II-1), x is an integer of 1 to 6, preferably 2 to 6. When x is within the above range, it is easy to promote the hydrolysis of alkoxysilane (A) and the condensation polymerization reaction following the hydrolysis. In formula (II-1), y is an integer of 1 to 10, preferably 2 to 3. When y is within the above range, it is easy to promote the dehydration condensation reaction of alkoxysilane (A). In formula (II-1), n ​​is an integer of 0 to 10, preferably 1 to 2. When n is within the above range, it is easy to promote the dehydration condensation reaction of alkoxysilane (A).

[0043] Examples of the compound represented by formula (II-1) include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, 3-(6-aminohexyl)aminopropyltrimethoxysilane, 3-(6-aminohexyl)aminopropyltriethoxysilane, trimethoxysilylpropyldiethylenetriamine, etc. As the compound represented by formula (II-1), 3-(2-aminoethyl)aminopropyltrimethoxysilane and 3-(6-aminohexyl)aminopropyltrimethoxysilane are preferred from the viewpoint of being more easily able to exhibit adhesion to the silane coupling agent.

[0044] In formula (II-2), z is an integer of 1 to 10, preferably 2 to 4. When z is within the above numerical range, the dehydration condensation reaction of the alkoxysilane (A) is easily promoted. In formula (II-2), w is an integer of 1 to 10, preferably 2 to 4. When w is within the above numerical range, the dehydration condensation reaction of the alkoxysilane (A) is easily promoted.

[0045] Examples of the compound represented by formula (II-2) include bis(3-(triethoxysilyl)propyl)amine, bis(3-(trimethoxysilyl)propyl)amine, etc. As the compound represented by formula (II-2), bis(3-(trimethoxysilyl)propyl)amine is preferred from the viewpoint of ease of hydrolysis.

[0046] The content of aminoalkylalkoxysilane (B) is added in an amount of 10% to the same amount as the content of alkoxysilane (A) and the content of alkoxysilane (C), and is preferably 0.001% by mass to 1.5% by mass, more preferably 0.005% by mass to 1.0% by mass, and even more preferably 0.01% by mass to 0.8% by mass, based on the total mass of the primer composition. When the content of aminoalkylalkoxysilane (B) is equal to or greater than the lower limit, it is easy to introduce various types of functionality-imparting compounds into the functional layer 30. When the content of aminoalkylalkoxysilane (B) is equal to or less than the upper limit, it is easy to suppress changes in appearance when the primer composition is applied to the resin substrate 10.

[0047] The ratio of the content of aminoalkylalkoxysilane (B) in the primer composition to the sum of the content of alkoxysilane (A) and the content of alkoxysilane (C) (hereinafter also referred to as the B / (A+C) ratio) is preferably 0.005 to 1, more preferably 0.015 to 0.7, and even more preferably 0.05 to 0.5. When the B / (A+C) ratio is equal to or greater than the lower limit, it is easy to introduce various types of functionality-imparting compounds into the functional layer 30. When the B / (A+C) ratio is equal to or less than the upper limit, it is easy to suppress changes in appearance when the primer composition is applied to the resin substrate 10.

[0048] The total content of alkoxysilane (A) and the content of aminoalkylalkoxysilane (B) and alkoxysilane (C) (hereinafter also referred to as A+B+C amount) is preferably 0.01% by mass or more and 5% by mass or less, more preferably 0.03% by mass or more and 3.5% by mass or less, and even more preferably 0.05% by mass or more and 2.5% by mass or less, based on the total mass of the primer composition. When the A+B+C amount is equal to or more than the lower limit, it is easy to introduce various types of functionality-imparting compounds into the functional layer 30. When the A+B+C amount is equal to or less than the upper limit, it is easy to suppress changes in appearance when the primer composition is applied to the resin substrate 10.

[0049] The organic solvent (D) is not particularly limited as long as it dissolves or disperses the alkoxysilane (A), the aminoalkylalkoxysilane (B), and the alkoxysilane (C) having one or more groups selected from the group consisting of an acryloyl group and an epoxy group to form a primer composition. Examples of the organic solvent (D) include alcohol-based solvents such as methanol, ethanol, 1-propanol, 2-propanol (IPA), 1-butanol, 2-butanol, and 2-methyl-2-propanol, ketone-based solvents such as acetone, methyl ethyl ketone, and diethyl ketone, chlorine-based solvents such as dichloromethane and trichloromethane, aromatic solvents such as toluene and xylene, ester-based solvents such as ethyl acetate, butyl acetate, and isopropyl acetate, ether-based solvents such as diethyl ether, tetrahydrofuran, and dioxane, and glycol ether-based solvents such as ethylene glycol monomethyl ether and ethylene glycol dimethyl ether. Among these organic solvents, alcohol-based solvents and ketone-based solvents that easily dissolve the alkoxysilane (A) and aminoalkylalkoxysilane (B) are preferred, alcohol-based solvents are more preferred, and ethanol, 2-propanol, and 1-butanol are even more preferred. The organic solvent (D) may be used alone or in combination of two or more kinds.

[0050] The content of the organic solvent (D) is preferably 95% by mass or more and 99.99.9% by mass or less, more preferably 96% by mass or more and 99.9% by mass or less, and even more preferably 97% by mass or more and 99.9% by mass or less, based on the total mass of the primer composition. When the content of the organic solvent (D) is equal to or more than the above lower limit, it is easy to suppress a change in appearance when the primer composition is applied to the resin substrate 10. When the content of the organic solvent (D) is equal to or less than the above upper limit, it is easy to introduce various types of functionality-imparting compounds into the functional layer 30.

[0051] The primer composition according to the present disclosure may contain optional components other than the alkoxysilane (A), the aminoalkylalkoxysilane (B), the alkoxysilane (C), and the organic solvent (D) as necessary. Examples of the optional components include a surface conditioner and water. When the primer composition according to the present disclosure contains the optional components, the content of the optional components is preferably 0.00001 to 1 mass% based on the total mass of the primer composition.

[0052] Thickness T of primer layer 20 20 is not particularly limited. 20 is, for example, preferably 0.001 μm or more and 2 μm or less, more preferably 0.002 μm or more and 0.6 μm or less, and further preferably 0.005 μm or more and 0.2 μm or less. 20 When the thickness T is equal to or greater than the lower limit, the functional layer 30 can be easily formed uniformly on the surface of the primer layer 20. 20 When the thickness T of the primer layer 20 is equal to or less than the upper limit, the adhesion between the one surface of the resin substrate 10 and the primer layer 20 is easily improved. 20 can be measured using an X-ray electron spectrometer or the like.

[0053] The functional layer 30 is a layer that can impart various functionalities to the resin substrate 10. Examples of the functional layer 30 include a hydrophilic layer having hydrophilic properties, a water-repellent layer having water repellency, and an antibacterial / antiviral layer having either antibacterial properties or antiviral properties.

[0054] The functional layer 30 may contain a silane coupling agent. In this specification, a silane coupling agent refers to a compound composed of an organic substance and silicon, and has two or more different reactive groups in the molecule. One of the reactive groups is a reactive group that chemically bonds with an inorganic material, and the other is a reactive group that chemically bonds with an organic material. By using a silane coupling agent, it is possible to bond an organic material and an inorganic material that are usually very difficult to bond with each other.

[0055] Examples of the silane coupling agent include vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldichlorosilane, vinylmethyldimethoxysilane, vinylmethyldiethoxysilane, 5-hexenyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryl ... Examples of the silane include dipropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, 4-vinylphenyltrimethoxysilane, 3-(4-vinylphenyl)propyltrimethoxysilane, 4-vinylphenylmethyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, and partial hydrolysates thereof. As silane coupling agents that impart functionality, compounds that impart water repellency include perfluoroalkyl group-containing silane coupling agents such as trifluoropropyltrimethoxysilane (KBM-7103, manufactured by Shin-Etsu Chemical Co., Ltd.), fluororesins (FG-5084F130-0.1, manufactured by Fluoro Technology Co., Ltd.), etc. Compounds that impart antibacterial and antiviral properties include quaternary ammonium salt-containing silane coupling agents such as dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride (KBM-9418-40, manufactured by Shin-Etsu Chemical Co., Ltd., AEM-5700, manufactured by AEGIS ENVIRONMENTS). As the silane coupling agent, methoxysilane or ethoxysilane is preferred from the viewpoint of operability and ease of distilling off by-products. These silane coupling agents may be used alone or in combination of two or more.

[0056] The functional layer 30 may contain a compound other than a silane coupling agent that can impart various functionalities to the resin substrate / coated substrate 10 (hereinafter also referred to as a "functionality imparting compound"). The functionality imparting compound is preferably one having a reactive group that can react with the alkoxysilane (A), aminoalkylalkoxysilane (B), alkoxysilane (C) in the primer layer, or the silane coupling agent added to the functional layer to form a chemical bond. Examples of the reactive group include groups having radical polymerizable unsaturated bonds such as alkoxysilyl groups, hydroxyl groups, carboxy groups, amino groups, sulfone groups, epoxy groups, and (meth)acryloyl groups. Examples of the functionality imparting compound include compounds that can impart hydrophilicity (hereinafter also referred to as a "hydrophilicity imparting compound"), compounds that can impart water repellency (hereinafter also referred to as a "water repellency imparting compound"), and compounds that can impart antibacterial and antiviral properties (hereinafter also referred to as an "antibacterial and antiviral properties imparting compound"). Examples of the hydrophilicity-imparting compound include the hydrophilic compounds described in JP 2016-020461 A. Examples of the hydrophilic compound include 2-acrylamido-2-methylpropanesulfonic acid and its salts, sodium Nt-butylacrylamidosulfonate, sodium vinylsulfonate, 2-sodium sulfoethyl methacrylate, sodium allylsulfonate, sodium p-styrenesulfonate, and sodium 3-mercapto-1-propanesulfonate. This functional layer 30 may be formed by applying different components in two or more separate applications.

[0057] Thickness T of the functional layer 30 30 is not particularly limited. 30 is, for example, preferably 0.0004 μm or more and 1 μm or less, more preferably 0.0008 μm or more and 0.5 μm or less, and further preferably 0.001 μm or more and 0.3 μm or less. 30 When the thickness T is equal to or greater than the lower limit, the resin substrate 10 can be easily provided with sufficient functionality. 30 When the thickness T of the functional layer 30 is equal to or less than the upper limit, the adhesion to the primer layer 20 is easily improved. 30 can be measured using an X-ray electron spectrometer or the like.

[0058] The amount of the silane coupling agent introduced is proportional to the amount of silanol groups in the primer layer 20. The amount of silanol groups in the primer layer 20 can be confirmed by the peak of siloxane bonds in infrared spectroscopy. The larger the peak of the siloxane bonds, the greater the amount of silanol groups in the primer layer 20. The peak of the siloxane bonds in infrared spectroscopy is at 1050 cm -1 The amount of silanol groups in the primer layer 20 can also be confirmed by the methylene group peak in infrared spectroscopy. The smaller the methylene group peak, the fewer the alkoxy groups remaining in the primer layer 20, and the more silanol groups there are. The methylene group peak in infrared spectroscopy is located around 2950 cm -1 Can be seen nearby.

[0059] The functional member 100 is preferably a hydrophilic member having hydrophilicity from the viewpoint of use in a wet space having equipment using water. When the functional member 100 is a hydrophilic member, an index for evaluating the hydrophilicity of the functional member 100 is a method of dropping a water drop on the surface of the functional member 100 and measuring the contact angle of water. For example, a contact angle meter (manufactured by Kyowa Interface Science Co., Ltd.) is used as a device for measuring the contact angle of water. The dropped liquid is distilled water, the amount of drop is 1.0 μL, and the contact angle can be calculated by the θ / 2 method (A half-angle method). The contact angle of water is defined as 0° to 180°, and the smaller the angle, the more hydrophilic the material is. When the functional member 100 is a hydrophilic member, the contact angle of water is preferably 0° to 60°, more preferably 0° to 40°, and even more preferably 0° to 30°. When the contact angle of water is equal to or less than the upper limit, the functional member 100 has excellent hydrophilicity. The lower limit of the contact angle of water is preferably smaller. The lower limit of the water contact angle is substantially about 5°.

[0060] Examples of applications in which the hydrophilic member can be used include housing equipment, toilets, bathtubs, wash basins, kitchen utensils, windows, doors, floors, desks, vehicle bodies, solar panels, walls, displays, signs, and touch panels.

[0061] When the functional member 100 is a water-repellent member, an index for evaluating the water repellency of the functional member 100 can be a method for measuring the contact angle of water, similar to the index for evaluating the hydrophilicity of the functional member 100. When the functional member 100 is a water-repellent member, the contact angle of water is preferably 60° or more and 180° or less, more preferably 70° or more and 180° or less, and even more preferably 80° or more and 180° or less. When the contact angle of water is equal to or more than the lower limit, the functional member 100 has excellent water repellency. The larger the upper limit of the contact angle of water, the more preferable. The upper limit of the contact angle of water is substantially about 150°.

[0062] Examples of applications in which the water-repellent member can be used include housing equipment, toilets, bathtubs, wash basins, kitchen utensils, windows, doors, floors, desks, vehicle bodies, solar panels, walls, displays, signs, and touch panels.

[0063] When the functional member 100 is an antibacterial / antiviral member, the antibacterial properties of the functional member 100 are evaluated in accordance with the antibacterial test method described in JIS Z2801. The antibacterial properties of the functional member 100 are judged based on the antibacterial activity value specified in JIS Z2801. When the antibacterial activity value is 2.0 or more, the functional member 100 has excellent antibacterial properties. The antiviral properties of the functional member 100 are evaluated in accordance with the antiviral test method specified in ISO 21702. The antiviral properties of the functional member 100 are judged based on the antiviral activity value specified in ISO 21702. When the antiviral activity value is 2.0 or more, the functional member 100 has excellent antiviral properties.

[0064] Applications in which antibacterial and antiviral materials can be used include, for example, housing facilities, toilets, bathtubs, wash basins, kitchen utensils, windows, doors, floors, desks, walls, handles, touch panels, toys, and medical equipment.

[0065] The shape of the functional member 100 is not particularly limited, and may be, for example, rectangular in plan view or elliptical in plan view.

[0066] The method for producing a functional member according to the present disclosure includes a step of forming a primer layer and a step of forming a functional layer. The method for producing a functional member according to the present disclosure provides a functional member having a primer layer located on one side of a substrate and a functional layer located on the surface of the primer layer. The step of forming the primer layer is a step of applying a primer composition according to the present disclosure to one side of a resin substrate and curing the primer composition.

[0067] The primer composition according to the present disclosure is obtained by dissolving an alkoxysilane (A), an aminoalkylalkoxysilane (B), an alkoxysilane (C), and, if necessary, a surface conditioner (optional component) in an organic solvent (D), and then stirring the mixture. The method of stirring the primer composition is not particularly limited, and stirring can be performed by a conventional method. The method of applying the primer composition to one side of the resin substrate 10 is not particularly limited, and for example, a spray coating method, a dip coating method, a flow coating method, a spin coating method, a roll coating method, a film applicator method, a screen printing method, a bar coater method, a brush coating method, a sponge coating method, and the like can be applied. The amount of application of the primer composition is not particularly limited, and for example, 1 to 50 g is preferable, and 5 to 20 g is more preferable, for a resin substrate 10 having a size of 100 cm x 100 cm. When the amount of application of the primer composition is within the above numerical range, the thickness T of the primer layer 20 is 100 g. 20 It is easy to make the size 0.001 to 2 μm.

[0068] Before applying the primer composition, it is preferable to degrease one surface of the resin substrate / coated substrate 10 in advance. By degreasing one surface of the resin substrate / coated substrate 10 in advance, it is possible to further increase the adhesion between the resin substrate / coated substrate 10 and the primer layer 20. For degreasing, an organic solvent such as acetone, ethanol, or 2-propanol can be used.

[0069] The method of curing the primer composition is not particularly limited, and includes a method of curing by heating at an arbitrary temperature. The temperature at which the primer composition is cured can be appropriately determined taking into consideration the composition of the primer composition, the amount applied, and the curing time. The temperature at which the primer composition is cured is, for example, preferably 10°C or higher and 120°C or lower, more preferably 20°C or higher and 100°C or lower. If the temperature at which the primer composition is cured is equal to or higher than the above lower limit, the dehydration condensation reaction of the alkoxysilane (A), the aminoalkylalkoxysilane (B), and the alkoxysilane (C) is likely to proceed. If the temperature at which the primer composition is cured is equal to or lower than the above upper limit, the deterioration of the resin substrate and the coating surface 10 is likely to be suppressed.

[0070] The step of forming the functional layer is a step of applying a functional composition containing a functionality-imparting compound to the surface of the primer layer and curing the functional composition. The method of applying the functional composition to the surface of the primer layer 20 is not particularly limited, and the same method as the method of applying the primer composition to one side of the resin substrate 10 can be applied. The amount of the functional composition applied is, for example, preferably 0.5 to 50 g, more preferably 1 to 20 g, per 100 cm × 100 cm area of ​​the primer layer 20. When the amount of the functional composition applied is within the above numerical range, the thickness T of the functional layer 30 can be increased by 100 g. 30 It is easy to make the size of the particle size 0.0004 to 1 μm.

[0071] The method of curing the functional composition is not particularly limited, and includes a method of curing by heating at an arbitrary temperature. The temperature at which the functional composition is cured can be appropriately determined taking into consideration the composition of the functional composition, the amount of application, and the curing time. The temperature at which the functional composition is cured is, for example, preferably 10°C or more and 120°C or less, more preferably 20°C or more and 100°C or less. If the temperature at which the functional composition is cured is equal to or more than the lower limit, the dehydration condensation reaction of the silane coupling agent is likely to proceed. If the temperature at which the functional composition is cured is equal to or less than the upper limit, the deterioration of the resin substrate 10 is likely to be suppressed. In addition, when the functional composition has a polymerizable unsaturated bond, it can also be cured by electron beams, ultraviolet rays, LEDs, etc.

[0072] By the step of forming a primer layer, a primer layer 20 is formed on one surface of the resin substrate 10. By the step of forming a functional layer, a functional member 100 in which a functional layer 30 is formed on the surface of the primer layer 20 is obtained.

[0073] The embodiments of the present disclosure have been described above in detail with reference to the drawings. However, the present disclosure is not limited to the above embodiments, and can be modified as appropriate without departing from the spirit of the present disclosure. The components in the above embodiments can be replaced with well-known components as appropriate.

[0074] In the above-described embodiment, the primer layer 20 is provided on one surface of the resin substrate 10. However, the present disclosure is not limited to this, and the primer layer 20 may be provided on both surfaces of the resin substrate 10.

[0075] In the above-described embodiment, the functional layer 30 is provided on one surface of the resin substrate 10. However, the present disclosure is not limited to this, and the functional layer 30 may be provided on both surfaces of the resin substrate 10. EXAMPLES

[0076] The present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to these examples.

[0077] The base material, alkoxysilane (A), aminoalkylalkoxysilane (B) and alkoxysilane (C) used in this example are as shown in [Raw Materials Used] below.

[0078] [Raw materials used] ≪Base material≫ Substrate with a urethane coating formed on acrylic resin: Sanyu Paint Co., Ltd. (Cerawood) coating.

[0079] Base material made of acrylic resin: Mitsubishi Chemical Corporation (Acrylite). Base material made of polypropylene resin: Purchased from AS ONE Co., Ltd.

[0080] <Alkoxysilane (A)> MS56: Methyl silicate oligomer MS56, R in formula (I-2) 2 is a methyl group, m is 0-98, manufactured by Mitsubishi Chemical Corporation.

[0081] <Aminoalkylalkoxysilane (B)> KBM603: 3-(2-aminoethyl)aminopropyltrimethoxysilane, R in formula (II-1) 3 is a methyl group, x is 2, y is 3, n is 1, manufactured by Shin-Etsu Chemical Co., Ltd.

[0082] <Alkoxysilane (C)> X-12-981S: a compound having an epoxy group and a triethoxysilyl group, number of epoxy groups / number of triethoxysilyl groups=3, manufactured by Shin-Etsu Chemical Co., Ltd.

[0083] KBM403: R in formula (III-1) 5 is a methyl group or a 3-glycoxypropyl group, manufactured by Shin-Etsu Chemical Co., Ltd.

[0084] KR516: R in formula (III-2) 6 is a methyl group or an ethyl group, s is 1 to 1000, manufactured by Shin-Etsu Chemical Co., Ltd.

[0085] KBM5103: R in formula (III-1) 5 is a methyl group or a 3-acryloyloxypropyl group, manufactured by Shin-Etsu Chemical Co., Ltd.

[0086] KBM503: R in formula (III-1) 5 is a methyl group or a 3-methacryloyloxypropyl group, manufactured by Shin-Etsu Chemical Co., Ltd.

[0087] <Antibacterial and antiviral ingredients> KBM-9418-40: dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, manufactured by Shin-Etsu Chemical Co., Ltd.

[0088] ≪Hydrophilic component≫ 2-Acrylamide-2-methylpropanesulfonic acid: Fujifilm Wako Pure Chemical Industries, Ltd.

[0089] <Water-repellent ingredients> FG-5084F130-0.1: A 0.1% by mass solution of a fluororesin obtained by incorporating a synthetic resin obtained by polymerizing fluorine-containing olefin into an inert organic solvent, manufactured by Fluorotechnology Co., Ltd.

[0090] <Other ingredients> D-20: Titanium-based curing catalyst, manufactured by Shin-Etsu Chemical Co., Ltd.

[0091] [Example 1] <Preparation of primer composition> 0.36 g of MS56 as alkoxysilane (A), 0.14 g of KBM603 as aminoalkylalkoxysilane (B), and 0.54 g of X-12-981S as alkoxysilane (C) were mixed with 1-butanol and dissolved by stirring for 5 minutes to obtain a primer composition containing 99.5% by mass of 1-butanol. In Tables 1 to 4, "-" indicates that the corresponding component was not added or that an evaluation test was not performed. "%" indicates "% by mass".

[0092] <Preparation of antibacterial and antiviral composition (F1)> An antibacterial and antiviral composition (F1) was prepared by mixing 4.0 g of KBM-9418-40 as an antibacterial and antiviral component, 0.04 g of D-20 as a curing catalyst, 34.92 g of 1-butanol, and 55.04 g of 2-propanol.

[0093] <Formation of primer layer and functional layer> A substrate (S1) having a urethane coating formed on an acrylic resin measuring 5 cm x 5 cm was used as the resin substrate, and 2 mL of the primer composition was applied to the surface of the substrate (S1) by soaking kitchen paper (Lion Corporation, "Lead Cooking Paper") and curing at room temperature for 1 hour to form a primer layer. Thereafter, 2 mL of the antibacterial and antiviral composition (F1) was soaked into lead cooking paper as a functional layer composition and applied onto the primer layer, and cured at room temperature for 2 hours to produce a functional coating member having antibacterial and antiviral properties. The surface free energy and antibacterial activity value of the obtained functional coating member were measured by the following method.

[0094] <Measurement of surface free energy> (1) Measurement of initial surface free energy The value calculated from the contact angle using the Kitazaki-Hata formula was taken as the surface free energy. Using a contact angle meter (Kyowa Interface Science Co., Ltd.), distilled water, diiodomethane, and hexadecane were dropped onto the surface of the functional coating member obtained by the above method, and the contact angle of each was measured. The amount of drops was 2.0 μL, and the contact angle was calculated using the θ / 2 method. The value calculated from this contact angle using the Kitazaki-Hata formula was taken as the initial surface free energy.

[0095] (2) Measurement of surface free energy after wiping with ethanol The surface of the functional coated member obtained by the above method was rubbed 50 times with a paper wiper wetted with ethanol under a load of 1 kg, and then the surface free energy was determined by the same method as above, and the obtained value was used as the surface free energy after wiping with ethanol.

[0096] <Measurement of antibacterial activity value> (1) Measurement of initial antibacterial activity The antibacterial properties were evaluated by measuring the antibacterial activity value according to the antibacterial test method described in JIS Z2801, except that only Escherichia coli was used as the test bacterial species, and the obtained value was taken as the initial antibacterial activity value.

[0097] (2) Measurement of antibacterial activity after 300 hours of exposure to a sunshine weather meter The surface of the functional coating material obtained by the above method was subjected to a weather resistance test of 78.5 W / m according to the weather resistance test method described in JIS B7753. 2 The antibacterial activity value was measured in the same manner as above, and the obtained value was taken as the antibacterial activity value after 300 hours of exposure using a sunshine weather meter.

[0098] [Examples 2 to 7, Reference Example 1, Comparative Example 1] A functional coating member was prepared and the surface free energy was measured in the same manner as in Example 1, except that the primer composition shown in Table 1 was used. In Reference Example 1, neither the primer composition nor the antibacterial and antiviral composition was used.

[0099] [Examples 8 to 11, Reference Example 2, Comparative Example 2] A functional coating member was prepared and the surface free energy was measured in the same manner as in Example 1, except that the substrate, primer composition, and antibacterial and antiviral composition shown in Table 2 were used. In Reference Example 2, the primer composition and antibacterial and antiviral composition were not used.

[0100] [Example 12] <Preparation of primer composition> 0.07 g of MS56 as the alkoxysilane (A), 0.05 g of KBM603 as the aminoalkylalkoxysilane (B), and 0.07 g of X-12-981S as the alkoxysilane (C) were mixed in 1-butanol and dissolved by stirring for 5 minutes to obtain a primer composition containing 99.81 mass% of 1-butanol.

[0101] <Preparation of hydrophilic composition (F2)> Solution(1) 0.13 g of KBM5103 was dissolved in 9.7 g of distilled water, and 0.2 g of a 4% aqueous hydrogen chloride solution was mixed therewith to prepare a hydrophilic composition (F2-1). Solution(2) 1.74g of sodium hydroxide was dissolved in 17.43g of distilled water, and 69.74g of 2-butoxyethanol was added. 9.03g of 2-acrylamido-2-methylpropanesulfonic acid and 1.57g of urea were added and dissolved therein. Then, 0.48g of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone was added and mixed to obtain a hydrophilic composition (F2-2).

[0102] <Formation of primer layer and functional layer> A substrate (S1) having a urethane coating formed on an acrylic resin measuring 5 cm x 5 cm was used as the resin substrate, and 2 mL of the primer composition was applied to the surface of the substrate (S1) by soaking it into lead cooking paper, and cured at room temperature for 1 hour to form a primer layer. Thereafter, as a composition for the functional layer, 2 mL of a hydrophilic composition (F2-1) was soaked into lead cooking paper and applied onto the primer layer, and after curing at room temperature for 5 minutes, 2 mL of a hydrophilic composition (F2-2) was soaked into lead cooking paper and applied onto the hydrophilic composition (F2-1), and the hydrophilic composition was measured by a metal halide lamp at a 1 cm angle. 2 After irradiating the substrate with ultraviolet light at an intensity of 30 mW per unit area for 10 seconds, the substrate was washed with water to prepare a functional coating member having hydrophilicity. Using the obtained functional coating member, the surface free energy was measured in the same manner as in Example 1, and the hydrophilicity was measured by the following method.

[0103] <Measurement of hydrophilicity> (1) Measurement of initial water contact angle A water droplet was dropped onto the surface of the functional coating member obtained by the above method using a contact angle meter (manufactured by Kyowa Interface Science Co., Ltd.), and the contact angle was measured. The drop liquid was distilled water, the drop amount was 2.0 μL, and the contact angle was calculated by the θ / 2 method. The obtained value was the initial water contact angle.

[0104] (2) Measurement of water contact angle after 2000 abrasions Using an abrasion tester manufactured by Shinto Scientific, the surface of the functional coating member obtained by the above method was rubbed 2000 times with a cotton cloth moistened with distilled water under a load of 1 kg, and then the water contact angle was measured using the same method as above, and the obtained value was taken as the water contact angle after 2000 abrasions.

[0105] (3) Measurement of water contact angle after 4,000 abrasions Using an abrasion tester manufactured by Shinto Scientific, the surface of the functional coating member obtained by the above method was rubbed 4,000 times with a cotton cloth moistened with distilled water under a load of 1 kg, and then the water contact angle was measured using the same method as above, and the obtained value was taken as the water contact angle after 4,000 abrasions.

[0106] [Examples 14 to 20, Reference Examples 3 to 5, Comparative Examples 3 and 5 to 6] A functional coating member was prepared and the surface free energy and hydrophilicity were measured in the same manner as in Example 12, except that the substrate and primer composition shown in Tables 3 and 4 were used. In Reference Examples 3 to 5, no primer composition or hydrophilic composition was used.

[0107] [Example 13] <Formation of primer layer and functional layer> Except for using FG-5084F130-0.1 as the water-repellent composition (F3) instead of the antibacterial and antiviral composition (F1), a functional coating member having water repellency was produced in the same manner as in Example 1. Using the obtained functional coating member, the surface free energy was measured in the same manner as in Example 1, and the water repellency was measured by the following method.

[0108] <Water repellency measurement> In the same manner as in the measurement of hydrophilicity, a water droplet was dropped on the surface of the functional coating member obtained by the above method, and the contact angle was measured using a contact angle meter (manufactured by Kyowa Interface Science Co., Ltd.) The dropped liquid was distilled water, the amount of drop was 2.0 μL, and the contact angle was calculated by the θ / 2 method.

[0109] [Reference Examples 3 to 5, Comparative Example 4] A functional coating member was prepared and the surface free energy and water repellency were measured in the same manner as in Example 13, except that the substrate and primer composition shown in Tables 3 and 4 were used. In Reference Examples 3 to 5, no primer composition or water repellent composition was used.

[0110] [Table 1]

[0111] [Table 2]

[0112] [Table 3]

[0113] [Table 4]

[0114] As shown in Tables 1 to 4, in Examples 1 to 20 to which the present disclosure is applied, the difference in surface free energy before and after wiping with ethanol is small, and therefore it is found that the functional layer on the primer layer is not easily peeled off and durability against chemical influences can be imparted. In Example 1, the difference in antibacterial activity value before and after 300 hours of irradiation with a sunshine weather meter is small, and therefore it is found that the function of the functional layer on the primer layer is easily maintained and durability against physical influences can be imparted. Examples 12 and 14 to 20 are examples in which a hydrophilic functional layer is formed, and the difference in water contact angle before and after abrasion is small, and therefore it is found that the function of the functional layer on the primer layer is easily maintained and durability against physical influences can be imparted. Example 13 is an example in which a water-repellent functional layer is formed, and the difference in water contact angle before and after abrasion is small, and therefore it is found that the function of the functional layer on the primer layer is easily maintained and durability against physical influences can be imparted.

[0115] On the other hand, in Comparative Examples 1 and 2 not containing alkoxysilane (C), the difference in surface free energy before and after wiping with ethanol was larger than in Examples 1 to 11 containing alkoxysilane (C), so it was found that the functional layer on the primer layer was easily peeled off and durability against chemical influences was not imparted. In Comparative Example 1, the difference in antibacterial activity value before and after 300 hours of irradiation with a sunshine weather meter was larger than in Example 1 containing alkoxysilane (C), so it was found that the function of the functional layer on the primer layer was difficult to maintain and durability against physical influences was not imparted.

[0116] Comparative Examples 3 and 5 to 6 are examples in which a hydrophilic functional layer was formed, and since the difference in surface free energy before and after wiping with ethanol was large compared to Examples 12 and 14 to 20 containing alkoxysilane (C), it was found that the functional layer on the primer layer was easily peeled off and durability against physical effects was not imparted. Comparative Example 3 is an example in which a hydrophilic functional layer was formed, and since the difference in water contact angle before and after abrasion was large compared to Examples 12 and 14 to 20, it was found that the function of the functional layer on the primer layer was difficult to maintain and durability against physical effects was not imparted.

[0117] Comparative Example 4 is an example in which a water-repellent functional layer was formed, and since the difference in surface free energy before and after wiping with ethanol was large compared to Example 13 containing alkoxysilane (C), it was found that the functional layer on the primer layer was easily peeled off and durability against physical influences was not imparted. Comparative Example 4 is an example in which a water-repellent functional layer was formed, and since the difference in water contact angle before and after abrasion was large compared to Example 13, it was found that the function of the functional layer on the primer layer was difficult to maintain and durability against physical influences was not imparted. [Explanation of symbols]

[0118] 10...resin substrate, 20...primer layer, 30...functional layer, 100...functional member

Claims

1. One or more alkoxysilanes (A) selected from the group consisting of compounds represented by the following general formula (I-1) and compounds represented by the following general formula (I-2), One or more aminoalkylalkoxysilanes (B) selected from the group consisting of compounds represented by the following general formula (II-1) and compounds represented by the following general formula (II-2), an alkoxysilane (C) having one or more groups selected from the group consisting of a (meth)acryloyl group and an epoxy group; and an organic solvent (D). [Case 1] (In formula (I-1), R 1 Each independently represents an alkyl group having 1 to 4 carbon atoms. 2 each independently represents an alkyl group having 1 to 4 carbon atoms; and m is 0 or more and 1,000 or less. [Case 2] (In formula (II-1), R 3 each independently represents an alkyl group having 1 or 2 carbon atoms, x is an integer from 1 to 6, y is an integer from 1 to 10, and n is an integer from 0 to 10. In formula (II-2), R 4 each independently represents an alkyl group having 1 or 2 carbon atoms; z is an integer from 1 to 10, and w is an integer from 1 to 10.

2. The alkoxysilane (C) is a compound (C1) represented by the following general formula (III-1), a compound (C2) represented by the following general formula (III-2), and a compound (C3) containing a structural unit represented by the following general formula (III-3) or the following general formula (III-4). The primer composition according to claim 1, comprising at least one compound selected from the group consisting of: [C3] [C4] [C5] (In formula (III-1), R 5each independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent, at least one of which has a (meth)acryloyl group or an epoxy group as a substituent. 6 each independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent, at least one of which has a (meth)acryloyl group or an epoxy group as a substituent. s is an integer of 0 to 1000. In formula (III-3), R 7 R each independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent, and at least one of these has a (meth)acryloyl group or an epoxy group as a substituent. 8 Each of R independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent. Each of Y independently represents a divalent linking group. n is an integer of 1 to 1000. In formula (III-4), R 7 R each independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent, at least one of which has a (meth)acryloyl group or an epoxy group as a substituent. 8 Each of R1, R2, and R3 independently represents an alkyl group having 1 to 4 carbon atoms which may have a substituent. Each of Y's independently represents a divalent linking group. 9 each independently represents a hydrogen atom, a hydroxyl group, or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent; p, q, and r each independently represent a number from 0 to 1000, provided that when p is 0, q and r each independently represent a number from 1 to 1000, and when p is 1 or more, q and r each independently represent a number from 0 to 1000.

3. A functional member comprising a resin substrate, a primer layer located on one surface of the resin substrate, and a functional layer located on a surface of the primer layer, The primer layer is a cured product of the primer composition according to claim 1 .

4. The functional member according to claim 3 , wherein the functional layer is a hydrophilic layer having hydrophilic properties, a water-repellent layer having water repellency, or an antibacterial and antiviral layer having either antibacterial properties or antiviral properties.

5. A method for producing a functional member, comprising applying the primer composition according to claim 1 to one surface of a resin substrate and curing the composition.

Citation Information

Patent Citations

  • Primer composition and adhesion method

    JP2001323210A

  • Primer composition and bonding method

    JP2002080783A

  • Resin laminate

    JP2007245709A

  • Coating method using curing composition, and coated object

    JP2009040874A

  • Transparent resin laminate, method for producing the same, and primer liquid for forming primer layer having thermal ray-shielding function

    JP2014094493A