Laminate and packaging body
By controlling the hydrogen bond term difference in a laminate with a water-based flexographic ink and solvent-free adhesive, the issues of ink layer swelling and poor appearance during high-speed coating are resolved, resulting in a laminate with enhanced darkening resistance and adhesive strength.
Patent Information
- Application Number
- JP2023045774
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing laminates using water-based inks and solvent-free adhesives face issues such as ink layer swelling due to adhesive penetration, leading to darkening and poor laminate appearance during high-speed coating, particularly when using metal vapor deposited films or foils.
A laminate structure with a water-based flexographic ink layer and a solvent-free adhesive layer, where the hydrogen bond term difference (Δδh) between the ink and adhesive layers is controlled within specific ranges (4.0-8.0 MPa1/2) to prevent adhesive penetration and enhance leveling properties.
The laminate achieves excellent darkening resistance and appearance even at low temperatures and high speeds, with improved adhesive strength and suppression of defects.
Smart Images

Figure 2024135207000001 
Figure 2024135207000002 
Figure 2024135207000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate applicable to packaging materials for food, medical products, cosmetics, etc., and a package using the laminate. The present invention further relates to a laminate that has an ink layer made of a water-based flexographic ink and an adhesive layer made of a solvent-free adhesive, and is capable of achieving both excellent darkening resistance, laminate appearance during high-speed coating, and adhesive performance, and a package using the laminate. [Background technology]
[0002] A laminate in which an ink layer and an adhesive layer are disposed between two substrates is suitably used as a packaging material for packaging food, medical products, cosmetics, etc. In recent years, from the viewpoint of reducing the environmental load, it has been considered to form the ink layer and the adhesive layer using a water-based ink and a solvent-free adhesive that do not contain organic solvents or that contain very little organic solvent.
[0003] In the above situation, for example, Patent Document 1 discloses a laminate having excellent hot tack properties and laminate appearance, which is provided in order with an ink layer formed from a water-based ink and an adhesive layer formed from a solvent-free adhesive containing a polyol component containing castor oil and a polyisocyanate component. Furthermore, for example, Patent Document 2 discloses a laminated film including an aqueous ink layer formed from a specific aqueous ink, and an adhesive layer formed using a solventless urethane adhesive containing a polyester polyol and a polyisocyanate component containing XDI and HDI. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-116009 A [Patent Document 2] Patent Publication No. 2021-66031 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the laminate described in Patent Document 1 has a problem that the components in the adhesive permeate the ink layer during the aging period, causing the ink layer to swell and the hiding power to decrease. When the hiding power decreases, a problem of darkening occurs, in which the metal deposition layer or metal foil is visible when the laminate is viewed from the outside, particularly in a laminate laminated with a metal deposition film or metal foil. It is believed that the above-mentioned darkening is due to the fact that the number-average molecular weight of the polyisocyanate composition contained in the adhesive used in the laminate of Patent Document 1 is low, at around 1,000, and further contains a large amount of castor oil, which gives it high affinity with the water-based ink layer.
[0006] In addition, the laminated film described in Patent Document 2 uses a solvent-free adhesive containing XDI and HDI as polyisocyanate components, and therefore has low affinity with the water-based ink layer and poor leveling properties. As a result, when the temperature of the coating roll is lowered to perform high-speed coating in order to improve processability, air bubbles are likely to form in the laminate, and there is a problem that the laminate appearance is poor, especially in a configuration having a deposition layer.
[0007] In other words, there is a trade-off between the issue of darkening and the issue of laminate appearance when applied at low temperature and high speed, and it has been difficult to solve both issues at the same time. Therefore, an object of the present invention is to provide a laminate which has a configuration including an adhesive layer using a solvent-free adhesive in contact with an ink layer using a water-based flexographic ink, yet which simultaneously suppresses penetration into the ink layer and has excellent leveling properties, does not cause darkening, and has excellent appearance and adhesive strength even when applied at low temperature and high speed, as well as a packaging product using said laminate. [Means for solving the problem]
[0008] As a result of intensive research into solving the above problems, the inventors have found that in a laminate comprising, in this order, a first substrate layer, an aqueous flexographic ink layer, an adhesive layer made of a solventless adhesive containing polyol and polyisocyanate, and a second substrate layer, the value of the hydrogen bond term in the Hansen solubility parameters between the solventless adhesive and the aqueous resin in the aqueous flexographic ink satisfies certain conditions, thereby completing the present invention.
[0009] <1> That is, the present invention relates to a laminate comprising a first base layer, an ink layer, an adhesive layer, and a second base layer in this order, which satisfies the following (1) to (4). (1) The ink layer is a layer formed using a water-based flexographic ink (F) containing a colorant and a water-based resin (P). (2) The adhesive layer is a layer formed using a solvent-free adhesive (S) containing a polyol (A) and a polyisocyanate (B). (3) The hydrogen bond term (δh ink ) and the hydrogen bond term (δh adh ) The value of Δδh calculated by the following formula (1) is 4.0 MPa 1 / 2 That's all. Equation (1): Δδh=δh ink -δh adh (4) The hydrogen bond term (δh adh ) is 8.0MPa 1 / 2 That's all.
[0010] <2> The present invention relates to a polyol (A) comprising at least one polyol selected from the group consisting of polyester polyols (a1) and polyether polyols (a2). <1> The present invention relates to a laminate according to the above item 1.
[0011] <3> The present invention relates to a polyether polyol (a2) comprising a triol which is a polypropylene glycol ether of glycerin. <2> The present invention relates to a laminate according to the above item 1.
[0012] <4> The present invention relates to a polyisocyanate (B) having a urethane bond, which is a reaction product of a polyisocyanate and a polyol. <1> ~ <3> The present invention relates to a laminate according to any one of claims 1 to 5.
[0013] <5> The present invention relates to a polyisocyanate having a urethane bond, the polyisocyanate including at least one selected from the group consisting of 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and tolylene diisocyanate. <4> The present invention relates to a laminate according to the above item 1.
[0014] <6> The present invention relates to <1> ~ <5> The present invention relates to a packaging material using the laminate according to any one of claims 1 to 4. Effect of the Invention
[0015] The present invention can provide a laminate having a configuration including an adhesive layer using a solvent-free adhesive in contact with an ink layer using a water-based flexographic ink, which simultaneously suppresses penetration into the ink layer and has excellent leveling properties, does not cause darkening, and has excellent appearance and adhesive strength even when applied at low temperature and high speed, as well as a package using said laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The laminate of the present invention is a laminate comprising a first base layer, an ink layer, an adhesive layer, and a second base layer in this order, and is characterized by satisfying the following (1) to (4). (1) The ink layer is a layer formed using a water-based flexographic ink (F) containing a colorant and a water-based resin (P). (2) The adhesive layer is a layer formed using a solvent-free adhesive (S) containing a polyol (A) and a polyisocyanate (B). (3) The hydrogen bond term (δh ink) and the hydrogen bond term (δh adh ) The value of Δδh calculated by the following formula (1) is 4.0 MPa 1 / 2 That's all. Equation (1): Δδh=δh ink -δh adh (4) The hydrogen bond term (δh adh ) is 8.0MPa 1 / 2 That's all.
[0017] Hydrogen bond term of solvent-free adhesive (δh adh ) value is 8.0MPa 1 / 2 This means that the hydrogen bond term in the Hansen solubility parameters (δh ink ) on water-based flexographic inks, which tend to have a relatively high viscosity, resulting in excellent laminate appearance when applied at low temperatures and high speeds. It also improves adhesion to the water-based flexographic ink layer, resulting in high adhesive performance. In addition, the hydrogen bond term (δh ink ) is (δh adh ) value is 4.0MPa 1 / 2 By satisfying the condition that the thickness of the ink layer is greater than or equal to the thickness of the ink layer, in a configuration in which the water-based ink layer and the adhesive layer are in contact with each other, penetration of the adhesive resin into the ink layer can be suppressed, and the occurrence of darkening defects can be suppressed. The present invention will be described in detail below.
[0018] <<Adhesive layer>> The adhesive layer in the present invention is a layer formed using a solvent-free adhesive (S) containing a polyol (A) and a polyisocyanate (B).
[0019] <Polyol (A)> The polyol (A) may be any compound having two or more hydroxyl groups, and may be selected from known polyols, such as polyester polyols, polycarbonate polyols, polycaprolactone polyols, polyether polyols, polyolefin polyols, acrylic polyols, silicone polyols, castor oil-based polyols, and fluorine-based polyols.
[0020] The polyol (A) may be a polyurethane polyol, which is a reaction product of a polyol and a polyisocyanate. It is preferable to include a polyurethane polyol having a urethane bond, since the cohesive force of the adhesive layer is improved and the adhesive strength is improved. As the polyisocyanate, the compounds described in the section <Polyisocyanate (B)> described later can be used.
[0021] The polyol (A) may be one in which a carboxyl group is introduced by reacting an acid anhydride with a part of the hydroxyl group. Examples of the acid anhydride include pyromellitic anhydride, mellitic anhydride, trimellitic anhydride, and trimellitic ester anhydride. Examples of the trimellitic ester anhydride include ester compounds obtained by esterifying an alkylene glycol or alkanetriol having 2 to 30 carbon atoms with trimellitic anhydride, and ethylene glycol bis-anhydrotrimellitate, propylene glycol bis-anhydrotrimellitate, etc. can be used. These polyols (A) may be used alone or in combination of two or more.
[0022] As the polyol (A), one containing at least one polyol selected from the group consisting of polyester polyols (a1) and polyether polyols (a2) is preferably used.
[0023] The polyester polyol (a1) may be a reaction product of a polybasic acid and a polyhydric alcohol, the polybasic acid preferably containing 90% by mass or more, more preferably 100% by mass of an aliphatic polybasic acid, and the polyhydric alcohol preferably containing 90% by mass or more, more preferably 100% by mass of an aliphatic polyhydric alcohol. In this specification, a polyester polyol that is a reaction product of a polybasic acid containing 90% by mass or more of an aliphatic polybasic acid and a polyhydric alcohol containing 90% by mass or more of an aliphatic polyhydric alcohol is referred to as an aliphatic polyester polyol. When the polyester polyol contains an aliphatic polyester polyol, the flexibility of the adhesive layer is improved and the conformability to the substrate is improved, which is preferable.
[0024] The polyester polyol (a1) has a number average molecular weight in the range of preferably 100 to 5,000, more preferably 500 to 4,000. The above range is preferable because fluidity is generated at room temperature or by heating. The polyester polyol (a1) has an acid value in the range of preferably 0 to 5.0 mgKOH / g, more preferably 0 to 3.0 mgKOH / g. The above range is preferable because rapid increase in viscosity after mixing of the two liquids can be suppressed. The polyester polyol (a1) has a hydroxyl value in the range of preferably 10 to 300 mgKOH / g, more preferably 30 to 200 mgKOH / g. The above range is preferable because adjustment to a viscosity / number average molecular weight range suitable for a solventless adhesive is easy.
[0025] The polyether polyol (a2) may be a compound having two or more hydroxyl groups and two or more ether bonds in the molecule, and may contain a reaction product (polyether urethane polyisocyanate) between a polyol containing a polyether polyol and a polyisocyanate, in addition to a bifunctional or trifunctional or higher polyether polyol. When the polyol for forming the reaction product contains both a polyether polyol and a polyester polyol, the resulting reaction product is treated as the polyether polyol (a2). The polyether polyol (a2) has a hydroxyl value in the range of preferably 10 to 300 mgKOH / g, more preferably 30 to 200 mgKOH / g. This range is preferable because it is easy to adjust the viscosity and number average molecular weight to be suitable for the solventless adhesive.
[0026] From the viewpoint of improving the adhesive strength on the water-based flexographic ink, the polyether polyol (a2) preferably contains a reaction product between a polyol component containing a triol (hereinafter also referred to as tris(polyoxypropylene)glyceryl ether) which is a propylene glycol ether of glycerin, and a polyisocyanate component. The polyether polyol (a2) preferably contains a triol which is a propylene glycol ether of glycerin. The number average molecular weight of the above triol is preferably in the range of 100 to 1,000.
[0027] <Polyisocyanate (B)> Examples of the polyisocyanate include aromatic polyisocyanates, araliphatic polyisocyanates, aliphatic polyisocyanates, alicyclic polyisocyanates, and modified products thereof. These polyisocyanates may be used alone or in combination of two or more.
[0028] (Aromatic polyisocyanate) Examples of the aromatic polyisocyanate include aromatic diisocyanates such as diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, phenylene diisocyanate, tolylene diisocyanate, and naphthalene diisocyanate; and aromatic polyisocyanates such as polymeric diphenylmethane diisocyanate.
[0029] (Aromatic aliphatic polyisocyanate) Examples of the araliphatic polyisocyanate include araliphatic diisocyanates such as 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or a mixture thereof.
[0030] (Aliphatic polyisocyanate) Examples of the aliphatic polyisocyanate include aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, 2,6-diisocyanate methyl caproate, lysine diisocyanate, and dimer acid diisocyanate.
[0031] (alicyclic polyisocyanate) Examples of alicyclic polyisocyanates include alicyclic diisocyanates such as 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, isophorone diisocyanate, 4,4'-methylene bis(cyclohexyl isocyanate), methyl 2,4-cyclohexane diisocyanate, methyl 2,6-cyclohexane diisocyanate, 1,4-bis(isocyanate methyl)cyclohexane, 1,3-bis(isocyanate methyl)cyclohexane, and norbornene diisocyanate.
[0032] Examples of modified polyisocyanates include allophanate-type modified products, isocyanurate-type modified products, biuret-type modified products, and adduct-type modified products. In addition, as the modified polyisocyanate, a polyisocyanate having a urethane bond, which is a reaction product of the above polyisocyanate and a polyol, may be used.
[0033] From the viewpoint of adhesive strength, it is preferable that the polyisocyanate (B) contains the above-mentioned polyisocyanate having a urethane bond (polyurethane polyisocyanate). By containing a polyisocyanate having a urethane bond, the cohesive force of the adhesive layer is improved, and the adhesive strength is improved.
[0034] The polyol that forms the polyisocyanate having a urethane bond is not particularly limited, and those described in the above section <Polyol (A)> can be used. Examples thereof include polyester polyols, polyether polyols, polycarbonate polyols, polycaprolactone polyols, polyolefin polyols, acrylic polyols, silicone polyols, castor oil-based polyols, and fluorine-based polyols. From the viewpoint of increasing the cohesive force of the adhesive layer and improving the adhesive strength, the polyol preferably contains castor oil.
[0035] The polyisocyanate forming the modified product of the polyisocyanate preferably contains an aromatic polyisocyanate. That is, when the polyisocyanate (B) contains a polyisocyanate having a urethane bond, the polyisocyanate having a urethane bond preferably contains a structural unit derived from an aromatic polyisocyanate. When the structural unit derived from an aromatic polyisocyanate is contained, the cohesive force of the adhesive layer increases, and the shear stress increases rapidly. This results in excellent appearance. In addition, the adhesive layer can be stored for a short period of time, and is excellent in terms of the next lamination step and packaging bag processing. As the aromatic polyisocyanate, at least one selected from the group consisting of 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and tolylene diisocyanate is preferably used.
[0036] When obtaining the polyurethane polyisocyanate, the ratio of the number of isocyanate groups in the polyisocyanate to the number of hydroxyl groups in the polyol (NCO moles / OH moles) is preferably 3 to 5. When the ratio is 3 or more, the concentration of urethane bonds in the adhesive layer increases, and the adhesive strength is improved, which is preferable. When the ratio is 5 or less, the amount of residual isocyanate monomer is reduced, and the flexibility of the adhesive layer is improved, and the adhesive strength is improved, which is preferable.
[0037] The isocyanate group content of the polyisocyanate (B) is preferably in the range of 5% by mass to 25% by mass, more preferably 8% by mass to 20% by mass, and even more preferably 12% by mass to 20% by mass. When the content is 5% by mass or more, the concentration of urethane bonds in the adhesive layer increases, and the adhesive strength is improved, which is preferable. When the content is 25% by mass or less, the amount of residual isocyanate monomer is reduced, and the flexibility of the adhesive layer is improved, and the conformability to the substrate is improved, which is preferable.
[0038] In the solventless adhesive (S), when polyol (A) and polyisocyanate (B) are mixed, the ratio of the number of isocyanate groups in polyisocyanate (B) to the number of hydroxyl groups in polyol (A) (NCO moles / OH moles) is preferably 1.0 to 3.0, more preferably 1.2 to 2.2. The above range is preferable because it provides an excellent balance of crosslink density and improves adhesive strength.
[0039] <Other ingredients> The solventless adhesive (S) may contain other components in addition to those described above in order to satisfy various physical properties required for the adhesive or packaging material. These other components may be blended with either the polyol (A) or the polyisocyanate (B), or may be added when blending the polyol (A) and the polyisocyanate (B). These other components may be used alone or in combination of two or more.
[0040] (Silane coupling agent) The solventless adhesive (S) may contain a silane coupling agent from the viewpoint of improving the adhesive strength to metal-based materials such as metal foil. Examples of the silane coupling agent include trialkoxysilanes having a vinyl group, such as vinyltriethoxysilane and vinyltriethoxysilane; trialkoxysilanes having an amino group, such as 3-aminopropyltriethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane; and trialkoxysilanes having a glycidyl group, such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane. The content of the silane coupling agent is preferably 0.1 to 5 mass %, more preferably 0.2 to 3 mass %, based on the total amount of the solventless adhesive. By setting it in the above range, it is possible to improve the adhesive strength to the metal foil, which is preferable.
[0041] (Phosphoric acid or phosphoric acid derivatives) The solvent-free adhesive (S) may contain phosphoric acid or a phosphoric acid derivative from the viewpoint of improving the adhesive strength to metallic materials such as metal foils. The phosphoric acid may be any phosphoric acid having at least one free oxygen acid, and examples of the phosphoric acid include phosphoric acids such as hypophosphorous acid, phosphorous acid, orthophosphoric acid, and hypophosphoric acid; and condensed phosphoric acids such as metaphosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, and ultraphosphoric acid. Examples of phosphoric acid derivatives include those obtained by partially esterifying the above phosphoric acid with alcohols while leaving at least one free oxygen acid. Examples of the alcohols include aliphatic alcohols such as methanol, ethanol, ethylene glycol, and glycerin; and aromatic alcohols such as phenol, xylenol, hydroquinone, catechol, and phloroglucinol. The content of phosphoric acid or a derivative thereof is preferably 0.01 to 10 mass %, more preferably 0.05 to 5 mass %, and particularly preferably 0.05 to 1 mass %, based on the total amount of the solventless adhesive.
[0042] (Leveling agent or defoamer) The solvent-free adhesive (S) may further contain a leveling agent and / or an antifoaming agent to improve the appearance of the laminate. Examples of the leveling agent include polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, aralkyl-modified polymethylalkylsiloxane, polyester-modified hydroxyl-containing polydimethylsiloxane, polyetherester-modified hydroxyl-containing polydimethylsiloxane, acrylic copolymer, methacrylic copolymer, polyether-modified polymethylalkylsiloxane, acrylic acid alkyl ester copolymer, methacrylic acid alkyl ester copolymer, and lecithin. Examples of the defoaming agent include silicone resin, silicone solution, and copolymers of alkyl vinyl ether, alkyl acrylate, and alkyl methacrylate.
[0043] (Reaction accelerator) The solvent-free adhesive (S) may further contain a reaction accelerator to accelerate the curing reaction. Examples of reaction accelerators include metal catalysts such as dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin dimaleate; tertiary amines such as 1,8-diaza-bicyclo(5,4,0)undecene-7, 1,5-diaza-bicyclo(4,3,0)nonene-5,6-dibutylamino-1,8-diaza-bicyclo(5,4,0)undecene-7; and reactive tertiary amines such as triethanolamine.
[0044] (Other additives) The solventless adhesive (S) may contain various additives within the range that does not impair the effects of the present invention. Examples of additives include inorganic fillers such as silica, alumina, mica, talc, aluminum flakes, and glass flakes, layered inorganic compounds, stabilizers (antioxidants, heat stabilizers, ultraviolet absorbers, hydrolysis inhibitors, etc.), rust inhibitors, thickeners, plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, crystal nucleating agents, and catalysts for adjusting the curing reaction.
[0045] <Formation of adhesive layer> The solventless adhesive (S) is cured by, for example, curing under conditions of 20 to 60° C. for about 24 hours to 1 week after a known lamination process such as roll coating, to form an adhesive layer. The thickness of the adhesive layer is preferably 1.0 μm to 5.0 μm, more preferably 1.5 μm to 4.5 μm, from the viewpoint of improving the appearance and physical properties of the laminate. When the thickness of the adhesive layer is 1.0 μm or more, the leveling property after the adhesive is applied is improved, and the unevenness of the printed surface is filled, thereby improving the appearance performance, which is preferable. In addition, when the laminate is folded, the elongation rate of the adhesive layer increases, thereby improving the conformability to the substrate, which is preferable. When the thickness of the adhesive layer is 5.0 μm or less, the cohesive force of the adhesive layer is increased, the movement of trapped fine air bubbles is suppressed, and the appearance performance is improved, which is preferable.
[0046] <Hydrogen bond term in Hansen solubility parameters> The laminate of the present invention has a hydrogen bond term (δh adh ) is 8.0MPa 1 / 2 It is important that this is the case. In addition, the hydrogen bond term (δh ink ) and the hydrogen bond term (δh adh ) The value of Δδh calculated by the following formula (1) is 4.0 MPa 1 / 2 It is important that this is the case. Equation (1): Δδh=δh ink -δh adh
[0047] The hydrogen bond term (δh) in the Hansen solubility parameters is a parameter that indicates the energy due to hydrogen bonds between molecules, and can be calculated by the following method based on the solubility in a solvent with a known hydrogen bond term. First, 16 sample tubes are prepared, and 1.75 mL of each of 16 types of evaluation reagents with known hydrogen bond parameters (see Table 1 below) is placed in each tube. Two drops of the evaluation sample are dropped into each sample tube using a Pasteur pipette, and the tubes are shaken well and left to stand for 24 hours in a 20°C environment. Thereafter, the solubility between the evaluation sample and the evaluation reagent is visually observed, and samples in which the evaluation sample has dissolved and samples in which the evaluation sample has not precipitated / separated are extracted, and the average δh value of the evaluation reagents is taken as the δh of the evaluation sample.
[0048] From the viewpoint of suppressing darkening defects, Δδh represented by the formula (1) is preferably 4.5 MPa. 1 / 2 More preferably, 5.5MPa 1 / 2 On the other hand, from the viewpoint of laminate appearance and adhesive performance during low-temperature and high-speed coating, it is preferably 7.0 MPa 1 / 2 Less than or equal to 6.0MPa, more preferably 1 / 2 The following is the result.
[0049] In addition, the hydrogen bond term (δh adh ) is preferably 10.0 MPa from the viewpoint of having a large number of options for water-based flexographic inks that satisfy the above Δδh condition. 1 / 2 Less than or equal to 9.0MPa, more preferably 1 / 2 The following is the result.
[0050] <<Ink layer>> The ink layer in the present invention is a layer formed using a water-based flexographic ink (F) and contains at least a colorant and a water-based resin (P).
[0051] <Coloring agent> As the colorant, pigments such as inorganic colorants and organic colorants can be suitably used. Examples of inorganic colorants include titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, aluminum hydroxide, chromium oxide, silica, carbon black, aluminum, and mica. In terms of coloring power, hiding power, chemical resistance, and weather resistance, titanium oxide is preferred as a white colorant, and titanium oxide having a basic pigment surface is more preferred. Aluminum is in the form of a powder or paste, but it is preferred to use it in the form of a paste in terms of handling and safety, and whether leafing or non-leafing is used is appropriately selected in terms of brightness and concentration. Examples of organic colorants include organic pigments and dyes used in general inks, paints, and recording materials. Examples of such organic colorants include azo, phthalocyanine, anthraquinone, perylene, perinone, quinacridone, thioindigo, dioxazine, isoindolinone, quinophthalone, azomethine azo, dictopyrrolopyrrole, and isoindoline pigments. Any compound listed in the Color Index can be used as the colorant, and it is preferable to use copper phthalocyanine for indigo ink and CI Pigment Yellow 83 for yellow ink in terms of cost and light resistance.
[0052] <Aqueous resin (P)> The aqueous resin (P) refers to a water-soluble or water-dispersible (emulsion) resin, and examples of the resin include urethane resin, acrylic resin, urethane acrylic resin, styrene-acrylic resin, styrene-acrylic resin, styrene-maleic anhydride resin, polyester resin, rosin-modified maleic acid resin, cellulose-based resin, and chlorinated polyolefin. The aqueous resin (P) may be used alone or in combination of two or more kinds. The content of the aqueous resin (P) is preferably in the range of 5 to 20 mass % based on the mass of the aqueous flexo ink (F).
[0053] [Water-based urethane resin] From the viewpoint of laminate properties, the aqueous resin (P) is preferably an aqueous urethane resin. The aqueous urethane resin preferably has an ionic group such as a carboxy group or a sulfone group in the resin, and can be obtained by, for example, reacting a polyol having an ionic group such as a polyol, a polyisocyanate, and a polyhydroxy acid, and then neutralizing the ionic group. The ionic group is preferably a carboxy group from the viewpoint of water resistance.
[0054] (Polyol) Examples of polyols that can be used in the synthesis of aqueous polyurethane resins include polyether polyols such as PEG (polyethylene glycol), PPG (polypropylene glycol) and PTMG (polyoxytetramethylene glycol); low molecular weight glycols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentadiol, methylpentanediol, hexadiol, octanediol, nonanediol, methylnonanediol, diethylene glycol, triethylene glycol and dipropylene glycol; and polyols such as adipic acid, phthalic acid, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, succinic acid, oxalic acid, malonic acid, and glycolic acid. Examples of the polyols include polyester polyols obtained by dehydration condensation of dibasic acids such as tartaric acid, pimelic acid, azelaic acid, sebacic acid, dimer acid, etc., or anhydrides thereof; polyols having a tertiary amino group, such as N-methyldiethanolamine, N-ethyldiethanolamine, N-butyldiethanolamine, Nt-butyldiethanolamine, dihydroxyisopropylethylamine, dihydroxyisopropyl n-butylamine, dihydroxyisopropyl t-butylamine, N,N-bis(2-hydroxypropyl)aniline, etc.; various known polyols such as polycarbonate diols, polybutadiene glycols, glycols obtained by adding ethylene oxide or propylene oxide to bisphenol A, and dimer diols.
[0055] These polyols may be used alone or in combination of two or more. From the viewpoint of resolubility of the water-based flexographic ink (F), the polyol preferably contains a polyether polyol, and more preferably contains PEG (polyethylene glycol).
[0056] The content of polyethylene glycol-derived structural units in the aqueous urethane resin (solid mass ratio of polyethylene glycol in the aqueous urethane resin, hereinafter abbreviated as PEG%) is preferably in the range of 5 to 50 mass%. When the PEG% is 5 mass% or more, the hydrophilicity of the resin is increased, improving the stability of the aqueous flexographic ink (F). When it is 50 mass% or less, the viscosity of the resin is low, satisfying the effective binder amount in the ink, and reducing the decrease in strength of the ink film can be suppressed.
[0057] To introduce an ionic group into the resin, it is preferable to use a polyol having an ionic group. The ionic group is preferably a carboxyl group. Examples of polyols having such an ionic group include dimethylol alkanoic acids such as dimethylol acetic acid, dimethylol propionic acid, dimethylol butanoic acid, 2,2-dimethylol butyric acid, and 2,2-dimethylol pentanoic acid, as well as dihydroxysuccinic acid, dihydroxypropionic acid, and dihydroxybenzoic acid. These may be used alone or in combination of two or more.
[0058] The polyols used in the synthesis of the aqueous polyurethane resin preferably have a number average molecular weight of 3,000 or less. The number average molecular weight is calculated from the hydroxyl value, which is a value calculated by esterifying or acetylating the hydroxyl groups in the resin and back titrating the remaining acid with an alkali, and converting the amount of hydroxyl groups in 1 g of the resin into mg of potassium hydroxide, and can be measured in accordance with JIS K 0070. By using a polyol with a number average molecular weight of 3,000 or less, the ionic groups incorporated for water solubility can be scattered in the aqueous polyurethane resin, improving resolubility. On the other hand, the larger the number average molecular weight of the polyol, the softer the polyurethane resin film becomes and the better the laminate strength tends to be, so the number average molecular weight is preferably 500 or more.
[0059] (Polyisocyanate) Examples of polyisocyanates that can be used in the synthesis of the aqueous polyurethane resin include various known aromatic, aliphatic, or alicyclic diisocyanates. Examples of aromatic diisocyanates include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, and m-tetramethylxylylene diisocyanate. Examples of the aliphatic diisocyanate include butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate. Examples of alicyclic diisocyanates include cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, and norbornane diisocyanate.
[0060] [Urea modified (water-based urethane urea resin)] The aqueous urethane resin may be an aqueous urethane urea resin obtained by reacting a polyol (including a polyol having an ionic group) with a polyisocyanate to form a polyurethane resin, and then introducing a urea bond using a chain extender and a reaction terminator. The aqueous urethane resin in the present invention is preferably an aqueous urethane urea resin, since the introduction of a urea bond tends to make the coating film stronger and improve the coating film physical properties.
[0061] (Chain extender) As the chain extender, known amines can be used, such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, ethylenediamine, propylenediamine, hexamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and dimer diamine obtained by converting the carboxyl group of dimer acid to an amino group. These amines may be used alone or in combination of two or more. The amines are preferably amines having a hydroxyl group, which are preferred because they have good resolubility.
[0062] (Reaction stopper) Examples of the reaction terminator include dialkylamines such as di-n-dibutylamine; amines having a hydroxyl group such as monoethanolamine, diethanolamine, 2-amino-2-methyl-1-propanol, tri(hydroxymethyl)aminomethane, 2-amino-2-ethyl-1,3-propanediol, N-di-2-hydroxyethylethylenediamine, N-di-2-hydroxyethylpropylenediamine, and N-di-2-hydroxypropylethylenediamine; and monoamine-type amino acids such as glycine, alanine, glutamic acid, taurine, aspartic acid, aminobutyric acid, valine, aminocaproic acid, aminobenzoic acid, aminoisophthalic acid, and sulfamic acid.
[0063] (neutralization) The aqueous urethane resin is preferably neutralized by neutralizing the ionic group in the urethane resin with a basic compound. Examples of the basic compound include inorganic basic compounds such as sodium hydroxide, potassium hydroxide, and ammonia; and organic basic compounds such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, ethanolamine, propanolamine, diethanolamine, N-methyldiethanolamine, dimethylamine, diethylamine, triethylamine, N,N-dimethylethanolamine, 2-dimethylamino-2-methyl-1-propanol, 2-amino-2-methyl-1-propanol, and morpholine; and these may be used alone or in combination of two or more. The basic compound is preferably ammonia or an organic basic compound in terms of the water resistance of the printed matter, residual odor, and the like.
[0064] From the viewpoints of solubility and blocking resistance, the aqueous urethane resin in the present invention preferably has an acid value of 15 to 65 mgKOH / g and a weight average molecular weight of 5,000 to 100,000.
[0065] <Other ingredients> (Acetylene glycol compounds) The water-based flexographic ink (F) may further contain an acetylene glycol compound, which may improve the leveling property of the ink layer. The acetylene glycol compound is a nonionic surfactant having an acetylene group at the center and a symmetrical structure. Commercially available acetylene glycol compounds include, for example, Olfin E1010, Olfin E1020, Surfynol 104, Surfynol 420, Surfynol 440, Surfynol 465, and Surfynol 485 manufactured by Nissin Chemical Industry Co., Ltd. When the acetylene glycol compound is contained, the content of the acetylene glycol compound is preferably 0.3 to 15 mass%, more preferably 0.6 to 9 mass%, and even more preferably 1.5 to 6 mass%, based on the solid mass of the aqueous flexo ink (F), from the viewpoint of laminate properties.
[0066] (Extender pigment) The water-based flexographic ink (F) may further contain an extender pigment. By containing an extender pigment, the blocking resistance of the ink layer may be improved. Examples of the extender pigment include barium sulfate, calcium carbonate, magnesium carbonate, kaolin clay, silica, etc., which are used alone or in combination of two or more. When the extender pigment is contained, from the viewpoint of laminate properties, the content of the extender pigment is preferably 1 to 45 mass %, more preferably 3 to 30 mass %, and further preferably 10 to 20 mass %, based on the solid content mass of the water-based flexo ink (F).
[0067] (Additives) The water-based flexographic ink (F) may contain additives as necessary, such as an adhesion promoter, a curing agent, an antifoaming agent, a wax, a silane coupling agent, a plasticizer, an infrared absorbing agent, an ultraviolet absorbing agent, an aromatic agent, and a flame retardant. The adhesive aid is preferably a compound containing a hydrazide group, such as adipic acid dihydrazide (ADH). By using a compound containing a hydrazide group, it interacts with the keto group in the resin or curing agent described below, improving the adhesion to plastic films and the strength of the ink film. The curing agent may be, for example, a resin microparticle dispersion containing a reactive group such as a carbodiimide group or a keto group. Commercially available resin microparticle dispersions include, for example, Carbodilite E-02, SV-02, V-02, V-02-L2, and V-04 manufactured by Nisshinbo Co., Ltd., Acronal YJ2716D, YJ2720D, YJ2727DN, YJ2741D, and YJ2746DS manufactured by BASF, and NEOCRYLA-1127, A-1125, A-1120, and A-1131 manufactured by DSM Neoresin Co., Ltd. The use of the above curing agent can further improve adhesion to the substrate and ink film strength. The content of the curing agent is preferably 1 to 45% by mass, more preferably 5 to 20% by mass, based on the solid content of the water-based flexo ink (F).
[0068] The aqueous flexographic ink (F) preferably contains water as a medium and further contains an alcohol. Examples of the alcohol include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, and iso-butanol. When the ink is applied to food packaging, it is preferable to use ethanol, 1-propanol, or 2-propanol as the alcohol from the viewpoints of safety and hygiene and residual odor. Furthermore, for the purpose of adjusting dryness, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol and mono- or diethers thereof may be used as required.
[0069] The ink layer may contain other resins besides the aqueous urethane resin, so long as the effects of the present invention are not impaired. Examples of such other resins include aqueous resins such as polyester resins, acrylic resins, styrene-acrylic resins, styrene-maleic anhydride resins, rosin-modified maleic acid resins, cellulose-based resins, and chlorinated polyolefins, and two or more of these may be used in combination.
[0070] <Production of Water-Based Flexographic Ink (F)> The method for producing the water-based flexographic ink (F) is not particularly limited, and the water-based flexographic ink (F) can be produced by dispersing and mixing the above-mentioned raw materials using a known dispersing machine such as a roller mill, a ball mill, a pebble mill, an attritor, a sand mill, etc. If air bubbles or unexpectedly large particles are contained in the water-based flexographic ink (F), they are preferably removed by filtration or the like, since they deteriorate the quality of the printed matter. Any conventionally known filter can be used.
[0071] (Minimum autocorrelation length of the ink layer surface Sal) The water-based flexographic ink (F) in the present invention preferably has a minimum autocorrelation length (Sal) of 10 μm or less on the surface of an ink layer formed using the water-based flexographic ink (F). The minimum autocorrelation length Sal of the ink layer surface is a value specified in accordance with ISO 25178, and is an evaluation index that expresses the fineness of the ink layer. Specifically, it is a numerical value that expresses the density of the unevenness of the ink layer surface in units of length, and it can be said that the smaller the minimum autocorrelation length Sal value, the finer the ink layer. Sal can be measured, for example, using a white light interference surface texture measuring instrument (TALYSURF CCIMP-HS, manufactured by AMETEK Corporation). The minimum autocorrelation length Sal of the ink layer surface is more preferably 1 to 10 μm, further preferably 2 to 8 μm, and particularly preferably 4 to 7 μm. When Sal is 1 μm or more, the surface area of the ink layer surface is reduced, and the penetration of the isocyanate component in the solvent-free adhesive (S) into the ink layer and the penetration of the low-molecular hydroxyl component in the ink layer into the adhesive layer are suppressed. This allows for good physical properties such as suppression of residual tack, adhesive strength, and heat seal strength to be obtained. When Sal is 10 μm or less, the surface of the ink layer becomes finer, and when the solvent-free adhesive (S) is applied, air bubbles are less likely to be trapped between the ink layer and the adhesive layer, improving the appearance after lamination.
[0072] <Ink layer formation> The ink layer can be formed by printing the above-mentioned water-based flexographic ink (F) on the substrate described below. As the printing method, a known flexographic printing method or gravure printing method is suitably used, and the ink is applied by the above-mentioned printing method, and then dried and fixed by using an oven or the like. The drying temperature is usually about 40 to 100°C. The thickness of the ink layer is preferably 0.1 to 5 μm, more preferably 0.1 to 2 μm.
[0073] As the printing method, flexographic printing is more preferably used. As the anilox used in flexographic printing, a ceramic anilox roll with cell engraving, a chrome-plated anilox roll, etc. can be used. In order to obtain a printed matter with excellent dot reproducibility, an anilox roll having a number of lines 5 or more times, preferably 6 or more times, the number of lines used in printing is preferred. For example, when the number of lines used is 75 lpi, an anilox roll of 375 lpi or more is preferred. The anilox capacity is preferably 1 to 8 cc / m from the viewpoint of drying property and blocking property of the water-based flexographic ink (F). 2 , more preferably 2 to 6 cc / m 2 It is.
[0074] Plates used in flexographic printing include photosensitive resin plates that utilize ultraviolet curing with a UV light source, and elastomer material plates that use a direct laser engraving method. Regardless of the method for forming the image part of the flexographic plate, it is preferable for the screening line count of the plate to be 75 lpi or more. Any sleeve or cushion tape can be used to attach the plate.
[0075] Flexographic printing machines include CI type multi-color flexographic printing machines and unit type multi-color flexographic printing machines, and ink supply methods include chamber methods and two-roll methods, and any suitable printing machine can be used.
[0076] <Production of Laminate> The laminate of the present invention comprises a first substrate layer, an ink layer, an adhesive layer, and a second substrate layer in this order, and is preferably produced by a production method having the following steps (1) and (2). Step (1): A step of flexographically printing a water-based flexographic ink (F) on a first substrate to form an ink layer. Step (2): A step of applying a solvent-free adhesive (S) onto the ink layer to form an adhesive layer.
[0077] [Base material] The first and second substrates are not particularly limited, and examples thereof include conventionally known plastic films, papers, metal foils, etc., and the two substrates may be the same or different. The plastic film may be a film of a thermoplastic resin or a thermosetting resin, and is preferably a film of a thermoplastic resin, such as polyolefin, polyester, polyamide, polystyrene, vinyl chloride resin, vinyl acetate resin, ABS resin, acrylic resin, acetal resin, polycarbonate resin, or cellulose-based plastic. The first and second substrates may each have a barrier layer formed of, for example, a vapor-deposited layer of a metal or metal oxide. Examples of the barrier layer include vapor-deposited layers of aluminum, silica, alumina, and the like.
[0078] The first substrate is preferably a plastic film. Examples of plastic films include those generally used for packaging materials, such as polyester resin films such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polylactic acid (PLA); polyolefin resin films such as polyethylene (PE) and polypropylene (PP); polystyrene resin films; polyamide resin films such as nylon 6 and poly-p-xylylene adipamide (MXD6 nylon); polycarbonate resin films; polyacrylonitrile resin films; polyimide resin films; laminates thereof (for example, nylon 6 / MXD6 / nylon 6, nylon 6 / ethylene-vinyl alcohol copolymer / nylon 6) and mixtures thereof. Among them, those having mechanical strength and dimensional stability are preferred.
[0079] When the second substrate is to be the outermost layer of the laminate, the second substrate is preferably a sealant substrate among plastic films. Examples of sealant base materials include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE), acid-modified polyethylene, polypropylene (PP), acid-modified polypropylene, copolymerized polypropylene, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid ester copolymer, ethylene-(meth)acrylic acid copolymer, and ionomer. Furthermore, by providing the sealant base material with unevenness having a height difference of about several μm, it is possible to impart slipperiness and tearability to the packaging bag.
[0080] The thickness of the first substrate can be selected arbitrarily, and is preferably 5 μm to 50 μm, more preferably 10 μm to 40 μm, from the viewpoints of moldability and transparency. When the thickness of the first substrate is 5 μm or more, the rigidity of the laminate increases, improving the strength of the laminate, and for example, it is preferable because it can suppress the occurrence of delamination and wrinkles that tend to occur when an impact is applied. When the thickness of the first substrate is 50 μm or less, the flexibility of the laminate increases, and for example, it is preferable because it can be easily processed when filling a packaging bag with contents.
[0081] The thickness of the second substrate can be selected arbitrarily, and is preferably 5 μm to 500 μm, more preferably 10 μm to 250 μm, and even more preferably 15 μm to 200 μm, from the viewpoint of strength as a packaging material. When the thickness of the second substrate is 5 μm or more, the heat seal strength is improved. This is preferable because it allows heavier contents to be filled, and the application as a packaging bag is expanded. In addition, when the thickness of the second substrate is 500 μm or less, this leads to cost reduction and increases the flexibility of the laminate, and for example, it is preferable because the processability of filling the above-mentioned contents is improved.
[0082] In order to improve adhesion to the ink layer or adhesive layer, the substrate may be subjected to surface treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas or nitrogen gas, physical treatments such as glow discharge treatment, chemical treatments such as oxidation treatment using chemicals, treatments for forming an adhesive layer, a primer coating layer, an undercoat layer, a vapor deposition anchor coating layer, etc., and other treatments before lamination or vapor deposition. Furthermore, an inorganic vapor deposition layer may be provided after the surface treatment, and a barrier coat layer may be provided on the inorganic vapor deposition layer.
[0083] The resin film used for the first substrate and the second substrate can be produced by using one or more resins selected from the above-mentioned group of resins and using a known film-forming method. Examples of such film-forming methods include extrusion, cast molding, T-die, cutting, inflation, and multi-layer co-extrusion. Furthermore, from the viewpoint of strength, dimensional stability, and heat resistance of the film, it can be stretched in uniaxial or biaxial directions using, for example, a tenter method or a tubular method.
[0084] If necessary, plastic compounding agents and additives such as lubricants, crosslinking agents, antioxidants, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, etc. can be added to the plastic film for the purpose of improving or modifying processability, heat resistance, weather resistance, mechanical properties, dimensional stability, oxidation resistance, slipperiness, release properties, flame retardancy, mold resistance, electrical properties, strength, etc., and the like. The amount of these additives can be freely selected depending on the purpose as long as it does not adversely affect other performance properties.
[0085] The laminate of the present invention can be produced, for example, by printing an aqueous flexographic ink (F) on a first substrate, drying the ink, applying a solvent-free adhesive (S), superimposing a second substrate, and curing the adhesive by an aging process. A plurality of ink layers and second substrates may be provided. For example, the ink layers may be configured as color ink layer / white ink layer, color ink layer / white ink layer / white ink layer, or color ink layer / color ink layer / white ink layer / white ink layer.
[0086] An example of the structure of the laminate of the present invention is shown below, but is not limited thereto. When the laminate has a plurality of adhesive layers, at least one of the adhesive layers in contact with the aqueous flexographic ink layer should be an adhesive layer formed from the solvent-free adhesive (S) of the present invention. In the following, transparent vapor deposition means a vapor-deposited layer of silica or alumina. Biaxially oriented polypropylene (OPP) / ink layer / adhesive layer / unoriented polypropylene (CPP), OPP / ink layer / adhesive layer / AL vapor deposition CPP, OPP / ink layer / adhesive layer / aluminum-deposited polyethylene terephthalate (aluminum-deposited PET), OPP / ink layer / adhesive layer / polyethylene (PE), OPP / ink layer / adhesive layer / AL vapor deposition polyethylene (AL vapor deposition PE), PET / ink layer / adhesive layer / CPP, PET / ink layer / adhesive layer / Al vapor deposition CPP, PET / ink layer / adhesive layer / AL-deposited PET, PET / ink layer / adhesive layer / PE, PET / ink layer / adhesive layer / AL vapor-deposited PE, PE / ink layer / adhesive layer / CPP, PE / ink layer / adhesive layer / Al vapor deposition CPP, PE / ink layer / adhesive layer / AL-deposited PET, PE / ink layer / adhesive layer / PE, PE / ink layer / adhesive layer / AL vapor-deposited PE, Nylon (NY) / ink layer / adhesive layer / CPP, NY / ink layer / adhesive layer / Al vapor deposition CPP, NY / ink layer / adhesive layer / AL vapor-deposited PET, NY / ink layer / adhesive layer / PE, NY / ink layer / adhesive layer / AL vapor-deposited PE PET / ink layer / adhesive layer / NY / adhesive layer / CPP, PET / ink layer / adhesive layer / NY / adhesive layer / PE, Transparent vapor deposition PET / ink layer / adhesive layer / NY / adhesive layer / CPP, Transparent vapor deposition PET / ink layer / adhesive layer / NY / adhesive layer / PE, PET / ink layer / adhesive layer / AL-deposited PET / adhesive layer / CPP, PET / ink layer / adhesive layer / AL-deposited PET / adhesive layer / PE, NY / ink layer / adhesive layer / AL-deposited PET / adhesive layer / CPP, NY / ink layer / adhesive layer / AL-deposited PET / adhesive layer / PE, PET / ink layer / adhesive layer / AL-deposited PET / adhesive layer / NY / adhesive layer / CPP, PET / ink layer / adhesive layer / AL-deposited PET / adhesive layer / NY / adhesive layer / PE, PET / ink layer / adhesive layer / AL / adhesive layer / CPP, PET / ink layer / adhesive layer / AL / adhesive layer / PE, PET / ink layer / adhesive layer / NY / adhesive layer / AL / adhesive layer / CPP, PET / ink layer / adhesive layer / NY / adhesive layer / AL / adhesive layer / PE, PET / ink layer / adhesive layer / AL / adhesive layer / NY / adhesive layer / CPP, PET / ink layer / adhesive layer / AL / adhesive layer / NY / adhesive layer / PE
[0087] <<Packaging>> The packaging body of the present invention may be any one that uses the laminate, and examples thereof include two-sided bags, three-sided bags, three-sided bags with zippers, palm-shaped bags, gusset bags, bottom gusset bags, stand bags, stand zipper bags, two-sided bags, four-column flat-bottom gusset bags, side seal bags, and bottom seal bags. The packaging body of the present invention can suppress the decrease in flexibility of the adhesive layer and the decrease in substrate followability caused by the reaction between the residual hydroxyl group components derived from the water-based flexo ink (F) and the isocyanate components derived from the solvent-free adhesive (S), and is therefore suitable for use in summer, when residual hydroxyl group components are likely to remain in the water-based flexo ink (F), and in high humidity environmental regions. In addition, the packaging body is particularly effective when the packaging bag is subjected to distortion for a long time in the processing process, filling process, distribution process, etc. EXAMPLES
[0088] The present invention will be specifically described below with reference to examples and comparative examples. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.
[0089] <Number average molecular weight (Mn)> The number average molecular weight was measured using a GPC (gel permeation chromatography) "Shodex GPC System-21" manufactured by Showa Denko Co., Ltd. GPC is a liquid chromatography that separates and quantifies substances dissolved in a solvent based on the difference in their molecular size. Tetrahydrofuran was used as the solvent, and the molecular weight was determined in terms of polystyrene.
[0090] <Calculation of hydrogen bond term (δh) in Hansen solubility parameters> Sixteen 2 mL sample tubes were prepared and 1.75 mL of the evaluation reagent with known δh listed in Table 1 was added to each tube. Two drops of the sample for which hydrogen bond parameters were to be determined were placed in each sample tube using a Pasteur pipette, and the tubes were shaken well and then left to stand for 24 hours in a 20°C environment. The state inside the sample tubes was then visually observed and scored according to the following criteria. 4 points: completely dissolved 3 points: Cloudy but uniformly dispersed, no precipitation 2 points: Cloudy but uniformly dispersed, and precipitation has occurred 1 point: Sample and reagent are separated The known δh values of the reagents that were given 3 or 4 points in the above evaluation were extracted, and the average value was determined as the δh of the sample. adh is the δh of polyol (A) and polyisocyanate (B) A and δh B Calculate each of these and multiply them by the compounding ratio (%) of (A) and (B) to obtain the δh of the solvent-free adhesive (S) after compounding. adh The calculated values are shown in Table 2.
[0091] [Table 1]
[0092] [Table 2]
[0093] <Production of Water-Based Flexographic Ink (F)> (Water-based flexographic ink (F-1)) 20.0 parts of phthalocyanine (LIONOL BLUE FG7400-G manufactured by Toyo Color Co., Ltd.), 5.0 parts of barium sulfate, 1.0 parts of silica, 20.0 parts of aqueous resin (P-1) solution, 10.0 parts of water, and 5.0 parts of n-propyl alcohol were stirred and mixed and ground in a sand mill, and then 20.0 parts of aqueous resin (P-1) solution, 14.0 parts of water, 2.0 parts of propylene glycol, 0.5 parts of an acetylene glycol compound (Surfynol 420 manufactured by Nissin Chemical Industry Co., Ltd.), 2.0 parts of polyethylene wax (Chemipearl W300 manufactured by Mitsui Chemicals, Inc.), 0.1 parts of an antifoaming agent (TEGO FOAMEX1488 manufactured by EVONIK Co., Ltd.), 0.2 parts of adipic acid dihydrazide, and 0.2 parts of 25% ammonia water were stirred and mixed to obtain an aqueous flexographic ink (F-1).
[0094] (Water-based flexographic ink (F-2)~(F-4)) Water-based flexographic inks (F-2) to (F-4) were obtained in the same manner as in (F-1) above, except that the water-based resin (P-1) solution was changed to solutions of water-based resins (P-2) to (P-4).
[0095] The aqueous resins (P-1) to (P-4) are shown below. Water-based resin (P-1) solution: urethane resin (acid value 35 mg KOH / g, hydroxyl value 10 mg KOH / g, solid content 24%) Water-based resin (P-2) solution: urethane resin (acid value 35 mg KOH / g, hydroxyl value 9 mg KOH / g, solid content 16%) Water-based resin (P-3) solution: urethane resin (acid value 40 mg KOH / g, hydroxyl value 5 mg KOH / g, solid content 20%) Water-based resin (P-4) solution: urethane urea resin (acid value 35 mg KOH / g, hydroxyl value 24 mg KOH / g, solid content 24%)
[0096] <Production of water-based inkjet inks> (Water-based resin (P-5)) In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen gas inlet tube, 93.4 parts of butanol were charged while introducing nitrogen gas, and the temperature was raised to 110°C, and then a mixture of 25 parts of styrene as a polymerizable monomer, 5 parts of methacrylic acid, 70 parts of methyl methacrylate and 6 parts of V-601 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator was dropped over 2 hours to carry out a polymerization reaction. After the dropwise addition, the mixture was further reacted at 110°C for 3 hours, and then 0.6 parts of V-601 was added and the reaction was continued for another 1 hour at 110°C. Then, the mixture was cooled to 30°C, 37.1 parts of dimethylaminoethanol was added to carry out a neutralization process, and 100 parts of distilled water was added to make it water-soluble. Then, the mixture was heated to 100°C or higher, and butanol was distilled off by azeotroping butanol with water, and the solid content was adjusted to 30%, to obtain a solution of aqueous resin (P-5). δh of water-based resin (P-5) ink is 7.1MPa 1 / 2 It was.
[0097] (Water-based inkjet ink (IJ-1)) 25 parts of aqueous resin (P-5) solution, 25 parts of a pigment dispersion with a solid content of 30% prepared by mixing titanium dioxide CR-90-21 (manufactured by Ishihara Industrial Co., Ltd.) and water, 20 parts of 1,2-propanediol, 1 part of Surfynol 465 (an acetylene diol-based surfactant manufactured by Air Products Co., Ltd.), 1 part of TEGO WET280 (a siloxane-based surfactant manufactured by Evonik Japan Co., Ltd.), and 27.95 parts of ion-exchanged water were stirred and mixed in a disper until homogenous, and the mixture was filtered using a membrane filter with a pore size of 1 μm to prepare an aqueous inkjet ink (IJ-1).
[0098] <Synthesis of polyol (A)> (Polyester polyol (a1)-1) In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel, and a nitrogen gas inlet tube, 208 parts of adipic acid and 192 parts of diethylene glycol were charged, and the mixture was heated to 240° C. with stirring under a nitrogen stream. After the reaction was continued until the acid value was 5 mgKOH / g or less, the pressure was gradually reduced and the reaction was continued at 1.3 mmHg or less to obtain a polyester polyol (a1)-1 having an acid value of 0.5 mgKOH / g, a hydroxyl value of 56.1 mgKOH / g, and a number average molecular weight of 2,000.
[0099] (Polyester polyols (a1)-2 to (a1)-3) Except for changing the composition as shown in Table 3, polyester polyols (a1)-2 to (a1)-3 were obtained in the same manner as (a1)-1.
[0100] [Table 3]
[0101] The abbreviations for each raw material compound in Table 3 are as follows. IPA: Isophthalic acid ADA: Adipic acid EG: Ethylene glycol DEG: Diethylene glycol NPG: Neopentyl glycol
[0102] (Polyether polyol (a2)-1) In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen gas inlet tube, 330 parts of polypropylene glycol having a number average molecular weight of about 400, 190 parts of polypropylene glycol having a number average molecular weight of about 2,000, 330 parts of a triol having a number average molecular weight of about 400, which is a polypropylene glycol ether of glycerin, and 130 parts of 4,4'-diphenylmethane diisocyanate were charged into the reaction vessel while introducing nitrogen gas, and the mixture was heated at 80°C to 90°C for 5 hours while stirring under a nitrogen gas flow to carry out a urethane reaction, and the disappearance of the isocyanate group was confirmed by IR to obtain a polyether polyol (a2)-1 having a number average molecular weight of 2,000. The above (a2)-1 contains a triol having a number average molecular weight of about 400, which is a polypropylene glycol ether of glycerin, which is unreacted.
[0103] (Polyether polyols (a2)-2 to (a2)-3) Except for changing the composition as shown in Table 4, polyether polyols (a2)-2 to (a2)-3 were obtained in the same manner as (a2)-1.
[0104] [Table 4]
[0105] The abbreviations for each raw material compound in Table 4 are as follows. PPG-400: Polypropylene glycol with a number average molecular weight of approximately 400 PPG-2000: Polypropylene glycol with a number average molecular weight of approximately 2,000 PPG-400-3 functional group: A triol having a number average molecular weight of about 400, which is a polypropylene glycol ether of glycerin (a tris(polyoxypropylene)glyceryl ether having a number average molecular weight of about 400) 4,4'-MDI: 4,4'-diphenylmethane diisocyanate Castor oil: Industrial No. 1 castor oil manufactured by Toyokuni Oil Co., Ltd.
[0106] <Production of polyol (A)> (Polyols (A-1) to (A-6)) The obtained polyester polyol (a1), polyether polyol (a2), and other polyol (a3) were mixed and stirred in the compounding ratios shown in Table 5 to obtain polyols (A-1) to (A-6).
[0107] [Table 5]
[0108] The abbreviations for each raw material compound in Table 5 are as follows. PPG-400: Polypropylene glycol with a number average molecular weight of approximately 400
[0109] <Production of Polyisocyanate (B)> (Polyisocyanate (B-1)) While introducing nitrogen gas into a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank and a nitrogen gas inlet tube, 200 parts of polypropylene glycol having a number average molecular weight of about 400 and 550 parts of a mixture of 2,4'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate (mass ratio 50:50) were charged, and the mixture was heated at 80°C to 90°C for 3 hours while stirring under a nitrogen gas flow to carry out a urethane reaction. After that, the mixture was cooled to 60°C, and 250 parts of crude MDI were added to obtain a polyisocyanate (B-1) having an NCO content of 21.5%. The ratio (NCO / OH) of the number of hydroxyl groups of the polyol and the number of isocyanate groups of the polyisocyanate in the urethane reaction was 4.5.
[0110] (Polyisocyanates (B-2), (B-3), (B-5)) Except for changing the composition to that shown in Table 6, polyisocyanates (B-2), (B-3) and (B-5) were obtained in the same manner as (B-1).
[0111] (Polyisocyanate (B-4)) In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, 250 parts of HDI beurette, 500 parts of HDI nurate, and 250 parts of IPDI nurate were charged while introducing nitrogen gas, and the mixture was heated at 80°C to 90°C for 3 hours while stirring under a nitrogen gas flow, dissolving the IPDI nurate and obtaining polyisocyanate (B-4).
[0112] [Table 6]
[0113] The abbreviations for each raw material compound in Table 6 are as follows. PPG-400: Polypropylene glycol with a number average molecular weight of approximately 400 PPG-2000: Polypropylene glycol with a number average molecular weight of approximately 2,000 Castor oil: Industrial No. 1 castor oil manufactured by Toyokuni Oil Co., Ltd. 4,4'-MDI: 4,4'-diphenylmethane diisocyanate 2,4'-MDI / 4,4'-MDI: A mixture of 2,4'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate (mass ratio 50:50) TDI: Tolylene diisocyanate Crude MDI: A mixture of polymeric diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate HDI billet: Hexamethylene diisocyanate billet HDI Nurate: Nurate form of hexamethylene diisocyanate IPDI Nurate: Nurate form of isophorone diisocyanate
[0114] <Manufacture of solvent-free adhesives (S)> (Solvent-free adhesives (S-1 to S-6)) Polyol (A) and polyisocyanate (B) were mixed according to the formulation in Table 7 to obtain solvent-free adhesives (S-1) to (S-6). The calculated Δh adh is shown in Table 7.
[0115] [Table 7]
[0116] <Creating printed matter> (PET / water-based flexographic ink) Water-based flexographic inks (F1) to (F4) were printed on a flexographic plate (photosensitive resin plate, KODAK FLEXCELNXH digital flexographic plate, plate thickness 1.14 mm, screen ruling 150 lpi) and an anilox roll (900 lpi 3 cc / m 2 Using a flexographic printing machine (MIRAFLEXCM) equipped with a 300-mm roll, printing was performed on a corona-treated polyester (PET) substrate (Toyobo Co., Ltd. "E5102", thickness 12 μm) at a speed of 200 m / min to obtain a PET print with an ink layer of 1.4 to 1.6 μm in thickness. The drying conditions for the ink layer were an intercolor dryer at 100°C and a tunnel dryer at 100°C.
[0117] (PET / water-based inkjet ink) An inkjet head was installed on top of a conveyor capable of transporting the printing substrate, and water-based inkjet ink (F5) was filled in. A PET substrate was fixed on the conveyor, which was driven at 50 m / min. The water-based inkjet ink was ejected as it passed the area where the inkjet head was installed, and printing was performed. The drop volume during printing was adjusted to the desired layer thickness within the range of 1.5 pL to 5 pL. The printed PET substrate was then placed in an air oven at 70°C and dried for 3 minutes to produce a PET / water-based inkjet ink print.
[0118] <Preparation of Laminate> [Example 1] (Printing (PET / Flexo ink layer)) Water-based flexographic ink (F-1) was applied to a flexographic plate (photosensitive resin plate, KODAK FLEXCELNXH digital flexographic plate, plate thickness 1.14 mm, screen ruling 150 lpi) and an anilox roll (900 lpi 3 cc / m 2Using a flexographic printing machine (MIRAFLEXCM) equipped with a 300-mm roll, printing was performed on a corona-treated polyester (PET) substrate (Toyobo Co., Ltd. "E5102", thickness 12 μm) at a speed of 200 m / min, resulting in a printed matter with an ink layer 1.4 to 1.6 μm thick. The drying conditions for the ink layer were an intercolor dryer at 100°C and a tunnel dryer at 100°C.
[0119] (Preparation of laminate (structure 1): PET / ink layer / adhesive layer / VM-CPP) Using a solvent-free adhesive laminator in a room temperature environment, the ink surface of the printed matter and the aluminum-vapor-deposited surface of a 25μm-thick aluminum-vapor-deposited unstretched polypropylene film ("2703" manufactured by Toray Industries, hereafter referred to as VM-CPP) were bonded together using a solvent-free adhesive (S-1) to obtain a 1000m-long laminate. The lamination conditions were doctor roll and application roll temperatures of 50°C, coating roll temperature of 60°C, lamination speed of 250 [m / min], and adhesive layer thickness of 1.9-2.1μm. The laminate was stored in an environment of 40°C and 65% RH, and taken out after 48 hours to obtain a laminate having a structure of "PET / ink layer / adhesive layer / VM-CPP" (structure 1).
[0120] (Preparation of laminate (structure 2): PET / ink layer / adhesive layer / VMPET) Using a solvent-free adhesive laminator in a room temperature environment, the ink surface of the printed matter and the aluminum-evaporated surface of a 12μm-thick aluminum-evaporated polyethylene terephthalate film (Reiko's "Dialastar H27", hereafter referred to as VM-PET) were bonded together using a solvent-free adhesive (S-1) to obtain a 1000m-long laminate. The lamination conditions were doctor roll and application roll temperatures of 50°C, coating roll temperature of 60°C, lamination speed of 200 [m / min], and adhesive layer thickness of 1.9-2.1μm. The laminate was stored in an environment of 40°C and 65% RH, and taken out after 48 hours to obtain a laminate having a structure of "PET / ink layer / adhesive layer / VM-PET" (structure 2).
[0121] [Examples 2 to 10, Comparative Examples 1 to 6] Laminates of Configuration 1 and Configuration 2 were obtained in the same manner as in Example 1, except that the water-based flexographic ink and solvent-free adhesive used were changed to those shown in Table 8.
[0122] [Comparative Example 7] (Printing (PET / IJ ink layer)) An inkjet head was installed on top of a conveyor capable of transporting the printing substrate, and water-based inkjet ink (IJ-1) was filled in. A PET substrate (Toyobo's "E5102", thickness 12 μm) was fixed on the conveyor and driven at 50 m / min. The water-based inkjet ink was ejected as it passed the area where the inkjet head was installed, and printing was performed. The drop volume during printing was adjusted to a range of 1.5 pL to 5 pL. The substrate was then placed in an air oven at 70°C and dried for 3 minutes to obtain a printed matter.
[0123] Laminates of structure 1 and structure 2 were obtained in the same manner as in Example 1, except that the IJ printed matter obtained above was used.
[0124] [Comparative Example 8] Laminates of configuration 1 and configuration 2 were obtained in the same manner as in Comparative Example 7, except that the solventless adhesive used was changed to (S-5).
[0125] <Evaluation of the laminate> The two resulting laminates were subjected to the following evaluations, and the results are shown in Table 8.
[0126] (Darkening rating) The obtained laminate (Structure 1) was unwound by 100 m, and the reflection density (L value) of the white printed part from the PET side was measured using X-Rite. The higher the value, the higher the whiteness, and the more the darkening phenomenon was suppressed. From the measured values, the state of darkening was judged according to the following criteria. A: L value is 70 or more (very good) B:L value is 65 or more and less than 70 (good) C:L value is 60 or more and less than 65 (usable) D:L value is less than 60 (bad)
[0127] (Evaluation of laminate appearance) The obtained laminate (Configuration 1) was rewound, and the appearance of the laminate at a point where 100 m had been rewound was visually observed and evaluated according to the following criteria. A: No bubbles of size less than 1 mm (good) B: There are very few bubbles of less than 1mm in size (usable). C: Numerous air bubble patterns of 1 mm or less in size are present, or air bubble patterns of 1 mm or more in size are present (unusable)
[0128] (Adhesive strength) The obtained laminate (Structure 2) was unwound by 100 m and cut into a test piece with a length of 300 mm and a width of 15 mm. Using an Instron tensile tester, the test piece was pulled at a peel rate of 300 mm / min in an environment of 25°C, and the T-type peel strength (N / 15 mm) between PET / VM-PET was measured. This test was performed five times, and the average value was calculated and evaluated according to the following criteria. A: 1.5 [N / 15mm] or more (very good) B: 1.0 [N / 15mm] or more, less than 1.5 [N / 15mm] (good) C: 0.5 [N / 15mm] or more, less than 1.0 [N / 15mm] (usable) D: Less than 0.5 [N / 15mm] (unusable)
[0129] [Table 8]
[0130] According to the evaluation results, Δδh and δh adh The laminates of the present invention (Examples 1 to 10) having a ΔΔh of 5.5 to 6.0 MPa achieved a balance between darkening resistance, laminate appearance during low-temperature and high-speed coating, and adhesive performance. 1 / 2 It is a combination of water-based resin and solvent-free adhesive, and δh adh is 9.0MPa 1 / 2When the following solvent-free adhesive was used, the best results were obtained in all performance areas (Example 3). On the other hand, Δδh and δh adh The laminates of Comparative Examples 1 to 8, in which the value did not satisfy the predetermined value, were unable to simultaneously achieve darkening resistance, laminate appearance during low-temperature / high-speed coating, and adhesive performance.
Claims
1. A laminate comprising a first substrate layer, an ink layer, an adhesive layer, and a second substrate layer in this order, the laminate satisfying the following (1) to (4). (1) The ink layer is a layer formed using a water-based flexographic ink (F) containing a colorant and a water-based resin (P). (2) The adhesive layer is a layer formed using a solvent-free adhesive (S) containing a polyol (A) and a polyisocyanate (B). (3) The hydrogen bond term (δh) in the Hansen solubility parameter of the aqueous resin (P) ink ) and the hydrogen bond term (δh adh The value of Δδh calculated by the following formula (1) based on the above is 4.0 MPa 1/2 That's all. Formula (1): Δδh=δh ink -dh adh (4) The hydrogen bond term (δh adh ) is 8.0 MPa 1/2 That's all.
2. The laminate according to claim 1, wherein the polyol (A) comprises at least one polyol selected from the group consisting of polyester polyols (a1) and polyether polyols (a2).
3. 3. The laminate of claim 2, wherein the polyether polyol (a2) comprises a triol which is a polypropylene glycol ether of glycerin.
4. The laminate according to any one of claims 1 to 3, wherein the polyisocyanate (B) comprises a polyisocyanate having a urethane bond which is a reaction product of a polyisocyanate and a polyol.
5. 5. The laminate according to claim 4, wherein the polyisocyanate forming the polyisocyanate having a urethane bond comprises at least one member selected from the group consisting of 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and tolylene diisocyanate.
6. A packaging material using the laminate according to any one of claims 1 to 3.
Citation Information
Patent Citations
Laminate
JP2019116009A
Laminate film, packaging bag, method for producing laminate film, and method for producing packaging bag
JP2021066031A
Cited By
Laminate and method for manufacturing the same
JP2026113787A
Laminate and manufacturing method thereof
JP7800642B1