Battery, battery pack, vehicle, and stationary power source
The battery design with a Ti-containing oxide and water-containing binder in the negative electrode, adhering to a specific ratio, addresses electrolyte depletion and water electrolysis issues, improving charge/discharge cycle performance and longevity.
Patent Information
- Application Number
- JP2023045835
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Aqueous lithium secondary batteries face issues with electrolyte depletion and electron conduction path disruption due to volume changes in the titanium composite oxide during charging and discharging, leading to decreased charge/discharge characteristics, and lowering electrode density to prevent electrolyte depletion results in water electrolysis.
A battery design that includes a negative electrode with a Ti-containing oxide and a water-containing binder, adhering to the ratio 0.2≦Wbind/WH2O≦15, where Wbind is the water-containing binder content in the negative electrode active material-containing layer and WH2O is the electrolyte water content by weight, ensuring the binder does not dissolve in the electrolyte and maintains adhesion to the current collector.
This design improves charge/discharge cycle performance by preventing electrolyte depletion and suppressing water electrolysis, enhancing the battery's longevity and efficiency.
Smart Images

Figure 2024135243000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE Embodiments of the present invention relate to batteries, battery packs, vehicles, and stationary power sources. [Background technology]
[0002] In aqueous lithium secondary batteries equipped with a negative electrode containing a titanium composite oxide, the titanium composite oxide undergoes volume changes during charging and discharging, which may lead to depletion of the electrolyte and disconnection of the electron conduction path. In order to prevent the electrolyte from depleting, it has been proposed to reduce the electrode density. However, in aqueous batteries such as aqueous lithium secondary batteries, if the electrode density is reduced too much, water electrolysis is more likely to occur, which reduces the charge and discharge characteristics. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-156895 A [Patent Document 2] JP 2018-163893 A [Non-patent literature]
[0004] [Non-Patent Document 1] Jijian Xu et al., Aqueous electrolyte design for super-stable 2.5V LiMn2O4 / Li4Ti5O12 pouch cells, Nature Energy volume 7, pages186-193 (2022) Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved is to provide a battery, a battery pack, a vehicle, and a stationary power source that have excellent life performance. [Means for solving the problem]
[0006] According to an embodiment, a battery is provided that includes a positive electrode, a negative electrode, and an electrolyte containing water. The negative electrode includes a negative electrode active material layer that includes a Ti-containing oxide and a water-containing binder. The battery satisfies the following formula (1).
[0007] 0.2≦W bind / W H2O <= 15 (1) However, W bind is the content (wt%) of the hydrous binder in the negative electrode active material-containing layer, and W H2O is the water content in the electrolyte (wt%).
[0008] According to the embodiment, a battery pack including the battery of the embodiment is provided.
[0009] According to the embodiment, a vehicle including the battery pack of the embodiment is provided.
[0010] According to the embodiment, there is also provided a stationary power source including the battery pack of the embodiment. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Diagram 2] 2 is a schematic cross-sectional view taken along line II-II of the secondary battery shown in FIG. 1. [Diagram 3] FIG. 4 is a partially cutaway perspective view illustrating a secondary battery according to another embodiment of the present invention. [Figure 4] FIG. 4 is an enlarged cross-sectional view of a portion E of the secondary battery shown in FIG. [Diagram 5] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 6] FIG. 13 is an exploded perspective view illustrating a battery pack according to another embodiment of the present invention. [Figure 7] 7 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. 6. [Figure 8] 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 9] FIG. 1 is a block diagram showing an example of a system including a stationary power supply according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (First embodiment) According to the first embodiment, a battery is provided that includes a positive electrode, a negative electrode, and an electrolyte containing water. The negative electrode includes a negative electrode active material layer that includes a Ti-containing oxide and a water-containing binder. The battery satisfies the following formula (1).
[0013] 0.2≦W bind / W H2O <= 15 (1) However, W bind is the content (wt%) of the hydrous binder in the negative electrode active material-containing layer, and W H2O is the water content in the electrolyte (wt%).
[0014] In a battery having an electrolyte containing water, a binder soluble in an organic solvent, such as polyvinylidene fluoride (PVdF), is used to prevent the binder from dissolving in the electrolyte. As a result of intensive research, the present inventors have found for the first time that when the content of the water-containing binder in the negative electrode active material-containing layer and the content of water in the electrolyte satisfy the relationship of formula (1), the generation of hydrogen gas due to electrolysis of water can be suppressed, and the water-containing binder is retained in the electrolyte without dissolving in the electrolyte, thereby improving the adhesion between the active material-containing layer and the current collector and the retention of the aqueous electrolyte in the active material-containing layer. Therefore, the battery of the embodiment can improve the charge-discharge cycle performance.
[0015] Ratio W bind / W H2O The reason why the value of is specified within the range of the above formula (1) will be explained. bind / W H2O By making the value of W 0.2 or more, the weight of water relative to the weight of the hydrous binder can be appropriately reduced, so that the hydrous binder is less likely to dissolve in the electrolyte and the binding strength between the active material-containing layer and the current collector can be maintained, thereby suppressing the deterioration of cycle performance. bind / W H2O When the value of W is 15 or less, the electrolyte can be easily impregnated into the water-containing binder. bind / W H2O The preferred range of the value is 1 or more and 8 or less.
[0016] The negative electrode, positive electrode, and electrolyte will be described in detail below. <Negative electrode> The negative electrode includes a negative electrode current collector and a negative electrode active material-containing layer formed or laminated on one or both sides of the negative electrode current collector. The negative electrode active material-containing layer includes a negative electrode active material and a water-containing binder.
[0017] The negative electrode current collector may be formed of a material that is electrochemically stable at a potential at which lithium (Li) is inserted and removed from the active material. Examples of the negative electrode current collector include a conductive sheet containing a conductive material and a polymeric material, a conductive sheet containing at least one metal element selected from the group consisting of Pb, Bi, Zn, Sb, and Sn, a metal foil such as copper, nickel, stainless steel, or aluminum, and an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. Examples of the polymeric material of the conductive sheet include polyethylene, polypropylene, polyethylene terephthalate, polyacrylonitrile, polymethyl methacrylate, and polyvinylidene fluoride. The conductive material is preferably a conductive filler such as a carbonaceous material. Examples of the carbonaceous material include carbon black, ketjen black, graphite, fibrous carbon, and carbon nanotubes. The conductive material and the polymeric material may each be one or more types.
[0018] The thickness of the negative electrode current collector is preferably 5 μm or more and 50 μm or less. A current collector having such a thickness can achieve a good balance between the strength and weight reduction of the electrode.
[0019] The negative electrode current collector may include a portion on the surface of which no active material-containing layer is formed, and this portion may function as a current collecting tab or a current collecting lead.
[0020] The negative electrode active material contains a Ti-containing oxide. This Ti-containing oxide is, for example, a lithium ion (Li + A Ti-containing oxide that can be changed into a Ti-containing oxide containing Li by an absorption / release reaction of lithium ions (Li) or a charge / discharge reaction. Therefore, this Ti-containing oxide can be a Ti-containing oxide that does not contain Li. This Li-containing oxide is a Ti-containing oxide that is changed into a Ti-containing oxide containing Li by an absorption / release reaction of lithium ions (Li) or a charge / discharge reaction. + Before the absorption / release reaction of lithium ions occurs or before the charge / discharge reaction occurs, the Ti-containing oxide does not contain Li. Due to the lithium ion absorption / release reaction or the irreversible reaction that occurs during the charge / discharge reaction, Li may remain in the Ti-containing oxide. Therefore, the Ti-containing oxide that does not contain Li includes the one that does not substantially contain Li.
[0021] Examples of Ti-containing oxides include niobium titanium-containing oxides and titanium oxides. Each oxide does not contain Li when the oxide is synthesized, before the lithium ion absorption / release reaction occurs, or before the charge / discharge reaction occurs, but it can be changed to a Ti-containing oxide containing Li by the lithium ion absorption / release reaction or the charge / discharge reaction. The lithium ion insertion / release reaction of the niobium titanium-containing oxide is a solid solution reaction, so the operating potential of the negative electrode containing the niobium titanium-containing oxide has a range. For example, the operating potential of the negative electrode containing the niobium titanium-containing oxide containing the crystalline phase represented by TiNb2O7 has a range from about 1.7V to about 0.7V. Therefore, the negative electrode containing the niobium titanium-containing oxide can set the negative electrode potential to a potential at which film formation is likely to occur, and therefore can promote the formation of a film of a nitrogen-containing compound on the negative electrode active material. On the other hand, Li4Ti5O 12 Such spinel-type lithium titanate has a composition containing Li during synthesis, in other words, before the lithium ion absorption / release reaction occurs. The operating potential of a negative electrode containing spinel-type lithium titanate is constant at 1.55 V. Therefore, it is difficult to set the potential of a negative electrode containing spinel-type lithium titanate to a potential favorable for the formation of a coating film such as a nitrogen-containing compound, and there is a risk that a coating film will not be formed uniformly on the negative electrode active material.
[0022] In addition, when at least one of a niobium titanium-containing oxide and a titanium oxide is used as a negative electrode active material, a high electromotive force can be obtained by combining it with, for example, a lithium manganese composite oxide or a lithium nickel cobalt manganese composite oxide as a positive electrode active material.
[0023] Examples of niobium titanium-containing oxides include TiNb2O7, Ti2Nb2O9, Ti2Nb 10 O 29 , TiNb 14 O 37 and TiNb 24 O 62 The niobium titanium-containing oxide may be a substituted niobium titanium composite oxide in which at least a part of Nb and / or Ti is substituted with a different element. Examples of the substituted element include Na, K, Ca, Co, Ni, Si, P, V, Cr, Mo, Ta, Zr, Mn, Fe, Mg, B, Pb, and Al. The substituted niobium titanium composite oxide may contain one type of substituted element, or may contain two or more types of substituted elements. The active material particles may contain one type of niobium titanium-containing oxide, or may contain multiple types of niobium titanium-containing oxide. The niobium titanium-containing oxide preferably contains Nb2TiO7 having a monoclinic structure. In this case, an electrode having excellent capacity and rate performance can be obtained.
[0024] Examples of monoclinic niobium titanium oxides include Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0025] Other examples of monoclinic niobium titanium oxides include Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0026] Another example of a monoclinic niobium titanium oxide is Li a TiM b Nb 2±β O 7±σ (0≦a≦5, 0≦b≦0.3, 0≦β≦0.3, 0≦σ≦0.3, M is at least one element selected from the group consisting of Fe, V, Mo and Ta).
[0027] Titanium oxide includes, for example, titanium oxide with a monoclinic structure, titanium oxide with a rutile structure, and titanium oxide with anatase structure. Titanium oxide with each crystal structure has a composition of TiO2 before charging and a composition of LiO2 after charging. x It can be expressed as TiO2 (x is 0≦x≦1). The structure of titanium oxide with a monoclinic crystal structure before charging can be expressed as TiO2(B).
[0028] The negative electrode active material may be of one type or two or more types.
[0029] The negative electrode active material is contained in the negative electrode active material-containing layer in the form of particles, for example. The negative electrode active material particles may be primary particles, secondary particles which are aggregates of primary particles, or a mixture of a single primary particle and a secondary particle. The shape of the particles is not particularly limited, and may be, for example, spherical, elliptical, flat, or fibrous.
[0030] The average particle size (diameter) of the primary particles of the negative electrode active material is preferably 3 μm or less, more preferably 0.01 μm or more and 1 μm or less, and the average particle size (diameter) of the secondary particles of the negative electrode active material is preferably 30 μm or less, more preferably 5 μm or more and 20 μm or less.
[0031] The hydrous binder may contain water, and may or may not actually contain water. Examples of the hydrous binder include water-soluble binders and hydrophilic binders. Examples of the hydrous binder include carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), polyvinylpyrrolidone (PVP), and salts of CMC (e.g., sodium salt of CMC, potassium salt of CMC). The type of hydrous binder used may be one or more. CMC and salts of CMC can each increase the viscosity of the negative electrode slurry. On the other hand, SBR acts to reduce the viscosity when it contains water. By using at least one of CMC or salts of CMC and SBR, it becomes easy to adjust the viscosity of the negative electrode slurry to the desired range.
[0032] W bind The content of the water-containing binder can be set to 0.8% by weight or more and 6% by weight or less. This makes it easier for the water-containing binder to be retained in the electrolyte without being dissolved in the electrolyte, thereby further improving the charge-discharge cycle performance. bind A more preferable range is from 2% by weight to 6% by weight.
[0033] The negative electrode active material-containing layer may contain, in addition to the negative electrode active material and the binder, a conductive agent, etc. The conductive agent is mixed as necessary in order to improve current collecting performance and reduce contact resistance between the active material and the current collector.
[0034] Examples of the conductive agent include carbonaceous materials such as acetylene black, ketjen black, graphite, and coke. The conductive agent may be used alone or in combination of two or more kinds.
[0035] The mixing ratio of the negative electrode active material and the conductive agent in the negative electrode active material-containing layer can be appropriately changed. For example, the content of the negative electrode active material in the negative electrode active material-containing layer can be 68% by weight or more and 96% by weight or less. On the other hand, the content of the conductive agent in the negative electrode active material-containing layer can be 2% by weight or more and 30% by weight or less. By making the amount of the conductive agent 2% by weight or more, the current collection performance of the negative electrode active material-containing layer can be improved. In addition, it is preferable to make the content of the conductive agent 30% by weight or less in order to achieve high capacity.
[0036] A nitrogen-containing compound may be present on at least a part of the surface of the negative electrode active material-containing layer. The nitrogen-containing compound is a compound containing a nitrogen atom (N). The nitrogen-containing compound can contribute to suppressing the electrolysis of water. The surface part where the nitrogen-containing compound is present is not particularly limited, but may be a part of the surface of the negative electrode active material-containing layer that is not in contact with the negative electrode current collector and faces the positive electrode via a separator. One example of this part is the main surface of the negative electrode active material-containing layer that constitutes the surface of the negative electrode. Examples of the nitrogen-containing compound include compounds having a functional group containing a nitrogen atom (N). Examples of the functional group containing a nitrogen atom (N) include an amide bond. Therefore, a compound containing an amide bond may be present on at least a part of the surface of the negative electrode active material-containing layer. Examples of the compound containing an amide bond include urea, N-methylurea, N,N'-dimethylpropyleneurea, acetamide, and thioacetamide. The type of compound containing an amide bond may be one type or two or more types.
[0037] The negative electrode can be produced, for example, by the following method. First, a negative electrode active material, a conductive agent, and a water-containing binder are suspended in an aqueous solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. Then, the laminate is pressed. In this manner, a negative electrode is produced.
[0038] <Positive electrode> The positive electrode includes a positive electrode current collector and a positive electrode active material-containing layer formed or laminated on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer includes a positive electrode active material. The positive electrode active material-containing layer may further include a conductive agent and a binder (positive electrode binder). The conductive agent is mixed as necessary to improve current collection performance and reduce contact resistance between the active material and the current collector. The binder has the function of binding the active material, the conductive agent, and the current collector.
[0039] The positive electrode current collector may be formed of a material that is electrochemically stable at a potential at which lithium (Li) is inserted and removed from the active material. Examples of the positive electrode current collector include a conductive sheet containing a conductive material and a polymeric material, a conductive sheet containing at least one metal element selected from the group consisting of Pb, Bi, Zn, Sb, and Sn, a metal foil such as nickel, stainless steel, or aluminum, and an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The polymeric material and conductive material of the conductive sheet may be the same as those described for the negative electrode current collector.
[0040] The thickness of the positive electrode current collector is preferably 5 μm or more and 50 μm or less. A current collector having such a thickness can achieve a good balance between the strength and weight reduction of the electrode.
[0041] The positive electrode current collector may include a portion on the surface of which no active material-containing layer is formed, and this portion may function as a current collecting tab or a current collecting lead.
[0042] The positive electrode active material has a lithium ion absorption and release potential of 3V (vs. Li / Li) based on metallic lithium. + ) or more and 5.5V or less (vs.Li / Li + The positive electrode may contain one type of positive electrode active material, or may contain two or more types of positive electrode active materials.
[0043] Examples of the positive electrode active material include lithium manganese composite oxides, lithium nickel composite oxides, lithium cobalt aluminum composite oxides, lithium nickel cobalt manganese composite oxides, spinel-type lithium manganese nickel composite oxides, lithium manganese cobalt composite oxides, lithium iron oxides, lithium fluorinated iron sulfate, phosphate compounds having an olivine crystal structure (e.g., Li x FePO4(0 < x ≦ 1), Li x MnPO4(0 < x ≦ 1)), etc. Phosphate compounds having an olivine crystal structure are excellent in thermal stability.
[0044] Examples of the positive electrode active material capable of obtaining a high positive electrode potential include lithium nickel cobalt manganese composite oxides (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≦ 1, 0 < y < 1, 0 < z < 1, y + z < 1), for example, lithium manganese composite oxides such as spinel-structured Li x Mn2O4(0 < x ≦ 1), Li x MnO2(0 < x ≦ 1)), lithium nickel aluminum composite oxides such as Li x Ni 1-y Al y O2(0 < x ≦ 1, 0 < y < 1)), lithium cobalt composite oxides such as Li x CoO2(0 < x ≦ 1)), lithium nickel cobalt composite oxides such as Li x Ni 1-y―z Co y Mn z O2(0 < x ≦ 1, 0 < y < 1, 0 ≦ z < 1)), lithium manganese cobalt composite oxides such as Li x Mn y Co 1-y O2(0 < x ≦ 1, 0 < y < 1)), spinel-type lithium manganese nickel composite oxides such as Li x Mn 1-y Ni y O4(0 < x ≦ 1, 0 < y < 2, 0 < 1 - y < 1)), for example, Li x FePO4(0 < x ≦ 1), Li x Fe 1-y Mn yPO4 (0 < x ≤ 1, 0 ≤ y ≤ 1), Li x Lithium phosphate oxides having an olivine structure such as CoPO4 (0 < x ≤ 1), iron fluorosulfate (e.g., Li x FeSO4F (0 < x ≤ 1)) can be mentioned.
[0045] The positive electrode active material is contained in the positive electrode in the form of particles, for example. The positive electrode active material particles can be single primary particles, secondary particles that are aggregates of primary particles, or a mixture of primary particles and secondary particles. The shape of the particles is not particularly limited and can be, for example, spherical, elliptical, flat, or fibrous.
[0046] The average particle diameter (diameter) of the primary particles of the positive electrode active material is preferably 10 μm or less, more preferably 0.1 μm or more and 5 μm or less. The average particle diameter (diameter) of the secondary particles of the positive electrode active material is preferably 100 μm or less, more preferably 10 μm or more and 50 μm or less.
[0047] The binder is blended to fill the gaps between the dispersed positive electrode active materials and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these can be used as the binder, or two or more can be combined and used as the binder.
[0048] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0049] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in proportions of 80% by weight to 98% by weight and 2% by weight to 20% by weight, respectively.
[0050] By making the amount of binder 2% by weight or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by weight or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0051] When a conductive agent is added, the positive electrode active material, binder, and conductive agent are preferably mixed in proportions of 77% by weight to 95% by weight, 2% by weight to 20% by weight, and 3% by weight to 15% by weight, respectively.
[0052] By setting the amount of the conductive agent to 3% by weight or more, the above-mentioned effects can be achieved. Also, by setting the amount of the conductive agent to 15% by weight or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.
[0053] For example, the positive electrode is prepared by suspending a positive electrode active material, a conductive agent, and a binder in a solvent to prepare a slurry. The slurry is then applied to one or both sides of a current collector. The applied slurry is then dried to obtain a laminate of an active material-containing layer and a current collector. Then, the laminate is pressed. In this manner, the positive electrode is produced. Alternatively, the positive electrode may be produced by the following method. First, the active material, the conductive agent, and the binder are mixed to obtain a mixture. Then, the mixture is formed into pellets. Then, the pellets are placed on the current collector to obtain a positive electrode. <Aqueous electrolyte> The electrolyte contains water. Hereinafter, an electrolyte containing water may be referred to as an aqueous electrolyte.
[0054] The aqueous electrolyte includes an aqueous solvent and an electrolyte salt dissolved in the aqueous solvent. The aqueous electrolyte may be liquid or gel. The liquid aqueous electrolyte is, for example, an aqueous solution prepared by dissolving an electrolyte salt as a solute in an aqueous solvent. The gel aqueous electrolyte is, for example, prepared by mixing a liquid aqueous electrolyte with a polymer compound to form a composite. Examples of the polymer compound include polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), and polyethylene oxide (PEO). When the aqueous electrolyte is held in both the negative electrode active material-containing layer and the positive electrode active material-containing layer, the types of the aqueous electrolytes may be the same or different.
[0055] As the aqueous solvent, a solution containing water can be used. The aqueous solution may be pure water or a mixed solvent of water and an organic solvent. The aqueous solvent contains water at a ratio of, for example, 50% by volume or more.
[0056] W H2O The amount of W can be 10% by weight or less. This can suppress the electrolysis of water, thereby further improving the charge-discharge cycle performance. H2O The lower limit of W can be 0.3% by weight. H2O can be 0.3% by weight or more and 10% by weight or less.
[0057] The electrolyte salt may be, for example, a lithium salt, a sodium salt, or a mixture thereof. One or more kinds of electrolyte salts may be used.
[0058] The content of the electrolyte salt in the aqueous electrolyte can be in the range of 45% by weight or more and 65% by weight or less, more preferably in the range of 50% by weight or more and 60% by weight or less.
[0059] Examples of the lithium salt that can be used include lithium chloride (LiCl), lithium bromide (LiBr), lithium hydroxide (LiOH), lithium sulfate (Li2SO4), lithium nitrate (LiNO3), lithium acetate (CH3COOLi), lithium oxalate (Li2C2O4), lithium carbonate (Li2CO3), lithium difluorooxalatoborate (LiDFOB, C2BF2LiO4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI; LiN(CF3SO2)2), lithium bis(fluorosulfonyl)imide (LiFSI; LiN(FSO2)2), lithium bis(pentafluoroethanesulfonyl)imide (LiBETI; LiN(SO2C2F5)2), and lithium bisoxalatoborate (LiBOB: LiB[(OCO)2]2).
[0060] The lithium salt preferably contains at least one selected from the group consisting of LiN(FSO2)2, LiN(CF3SO2)2, and LiN(SO2C2F5)2. Each lithium salt is solid at room temperature, but can be changed to a liquid state by a eutectic reaction with a compound containing an amide bond. Therefore, the water content W in the aqueous electrolyte is H2O Lithium salts including LiTFSI (LiN(CF3SO2)2) are preferred.
[0061] As the sodium salt, sodium chloride (NaCl), sodium sulfate (Na2SO4), sodium hydroxide (NaOH), sodium nitrate (NaNO3), sodium trifluoromethanesulfonylamide (NaTFSA), and the like can be used.
[0062] Aqueous electrolytes contain chloride ions (Cl - ), hydroxide ion (OH - ), sulfate ion (SO4 2- ), nitrate ion (NO3 - ) may contain at least one selected from the following.
[0063] The aqueous electrolyte may contain a compound containing an amide bond. This allows the water-containing binder to cover the surface of the negative electrode active material particles while containing the aqueous electrolyte without dissolving in the aqueous electrolyte. As a result, even if the volume of the negative electrode changes due to charging and discharging, the aqueous electrolyte can be prevented from being depleted, thereby improving the charge and discharge characteristics. The compound containing an amide bond can form a liquid mixture by a eutectic reaction with at least one lithium salt selected from the group consisting of LiTFSI, LiFSI, and LiBETI. Therefore, an aqueous electrolyte containing a compound containing an amide bond and at least one lithium salt selected from the group consisting of LiTFSI, LiFSI, and LiBETI can have a desired lithium ion concentration even with a small amount of aqueous solvent. Therefore, it is possible to suppress the electrolysis of water without impairing the ionic conductivity of the aqueous electrolyte.
[0064] Examples of the compound containing an amide bond include urea, N-methylurea, N,N'-dimethylpropyleneurea, acetamide, and thioacetamide. The type of compound containing an amide bond may be one or more.
[0065] The content of the compound containing an amide bond in the aqueous electrolyte can be 30% by weight or more and 55% by weight or less, preferably 30% by weight or more and 45% by weight or less. If the content of the compound containing an amide bond in the aqueous electrolyte is low, a coating may not be formed on the surface of the negative electrode active material particles. In addition, a part of the lithium salt may precipitate in the solvent as a solid. On the other hand, if the content of the compound containing an amide bond in the aqueous electrolyte is high, the coating formed on the surface of the negative electrode active material particles may be excessive, which may increase the resistance of the negative electrode.
[0066] The aqueous electrolyte may contain potassium hydroxide (KOH). Potassium hydroxide can function as a catalyst for a reaction that forms a coating on the surface of the negative electrode active material particles. Therefore, when the aqueous electrolyte contains a compound containing an amide bond and potassium hydroxide, the formation of a coating on the surface of the negative electrode active material particles can be promoted.
[0067] The pH of the aqueous electrolyte is preferably 3 or more and 14 or less, and more preferably 4 or more and 13 or less. When separate electrolytes are used for the negative electrode side electrolyte and the positive electrode side electrolyte, the pH of the negative electrode side electrolyte is preferably in the range of 3 or more and 14 or less, and the pH of the positive electrode side electrolyte is preferably in the range of 1 or more and 8 or less.
[0068] When the pH of the negative electrode electrolyte is within the above range, the hydrogen generation potential at the negative electrode is reduced, and hydrogen generation at the negative electrode is suppressed. This improves the storage performance and cycle life performance of the battery. When the pH of the positive electrode electrolyte is within the above range, the oxygen generation potential at the positive electrode is increased, and oxygen generation at the positive electrode is reduced. This improves the storage performance and cycle life performance of the battery. It is more preferable that the pH of the positive electrode electrolyte is within the range of 3 to 7.5.
[0069] The aqueous electrolyte may contain a surfactant. Examples of the surfactant include nonionic surfactants such as polyoxyalkylene alkyl ether, polyethylene glycol, polyvinyl alcohol, thiourea, disodium 3,3'-dithiobis(1-propanephosphoric acid), dimercaptothiadiazole, boric acid, oxalic acid, malonic acid, saccharin, sodium naphthalenesulfonate, gelatin, potassium nitrate, aromatic aldehyde, and heterocyclic aldehyde. The surfactant may be used alone or in combination of two or more.
[0070] The battery of the embodiment may further include at least one of a separator or an exterior member.
[0071] <separator> The separator is disposed, for example, between the positive electrode and the negative electrode. The separator may include a separator that covers only one of the positive electrode or the negative electrode.
[0072] The separator can have a porous structure. Examples of the porous separator include nonwoven fabric, film, and paper. Examples of the constituent materials of the porous separator that constitutes the nonwoven fabric, film, and paper include polyolefins such as polyethylene and polypropylene, and cellulose. Examples of preferred porous separators include nonwoven fabrics containing cellulose fibers and porous films containing polyolefin fibers.
[0073] The porosity of the porous separator is preferably 60% or more. The fiber diameter is preferably 10 μm or less. By making the fiber diameter 10 μm or less, the affinity of the porous separator to the electrolyte is improved, so that the battery resistance can be reduced. The fiber diameter is more preferably in the range of 3 μm or less. A cellulose fiber-containing nonwoven fabric with a porosity of 60% or more has good electrolyte impregnation and can provide high output performance from low to high temperatures. The porosity is more preferably in the range of 62% to 80%.
[0074] The porous separator has a thickness of 20 μm to 100 μm and a density of 0.2 g / cm 3 More than 0.9g / cm 3 Within this range, a balance between mechanical strength and reduced battery resistance can be achieved, and a secondary battery with high output and suppressed internal short circuit can be provided. In addition, the separator undergoes little thermal shrinkage in a high-temperature environment, and good high-temperature storage performance can be achieved.
[0075] The separator may be a composite separator including a porous separator and a layer containing inorganic particles formed on one or both sides of the porous separator. Examples of inorganic particles include aluminum oxide and silicon oxide.
[0076] A solid electrolyte layer may be used as the separator. The solid electrolyte layer may include solid electrolyte particles and a polymer component. The solid electrolyte layer may be composed of only solid electrolyte particles. The solid electrolyte layer may include one type of solid electrolyte particles, or may include multiple types of solid electrolyte particles. The solid electrolyte layer may include at least one selected from the group consisting of a plasticizer and an electrolyte salt. When the solid electrolyte layer includes an electrolyte salt, for example, the alkali metal ion conductivity of the solid electrolyte layer can be further increased. The form of the polymer material may be, for example, granular or fibrous.
[0077] The solid electrolyte layer is preferably in a sheet shape and has few or no pores such as pinholes. The thickness of the solid electrolyte layer is not particularly limited, but is, for example, 150 μm or less, and preferably in the range of 20 μm to 50 μm.
[0078] The polymer component used in the solid electrolyte layer is preferably a polymer component insoluble in an aqueous solvent. Examples of polymer components that satisfy this condition include polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), and fluorine-containing polymer components. By using a fluorine-containing polymer component, water repellency can be imparted to the separator. In addition, inorganic solid electrolytes have high stability against water and excellent lithium ion conductivity. By forming a composite of a lithium ion conductive inorganic solid electrolyte and a fluorine-containing polymer component, a flexible solid electrolyte layer with alkali metal ion conductivity can be realized. A separator made of this solid electrolyte layer can reduce resistance, thereby improving the large current performance of a secondary battery.
[0079] Examples of the fluorine-containing polymer component include polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), ethylene-tetrafluoroethylene copolymer, polyvinylidene fluoride (PVdF), etc. The type of the fluorine-containing polymer component can be one or more types.
[0080] When the solid electrolyte layer contains a polymer component, the content of the polymer component in the solid electrolyte layer is preferably 1% by weight or more and 20% by weight or less. In this range, when the thickness of the solid electrolyte layer is set in the range of 10 to 100 μm, high mechanical strength can be obtained and resistance can be reduced. Furthermore, there is little risk that the solid electrolyte will become a factor that inhibits lithium ion conductivity. A more preferable range of this content is 3% by weight or more and 10% by weight or less.
[0081] As the solid electrolyte, it is preferable to use an inorganic solid electrolyte. The inorganic solid electrolyte is a solid substance having Li-ion conductivity. Here, having Li-ion conductivity is 1×10 -6 It means that the inorganic solid electrolyte has a lithium ion conductivity of 1.0 S / cm or more. Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes. Specific examples of the inorganic solid electrolyte are as follows.
[0082] As the oxide-based solid electrolyte, it is preferable to use a lithium phosphate solid electrolyte having a NASICON (Sodium (Na) Super Ionic Conductor) type structure and represented by the general formula Li 1+x Mα2(PO4)3. In the above general formula, Mα is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is in the range of 0 ≦ x ≦ 2.
[0083] Specific examples of the lithium phosphate solid electrolyte having a NASICON type structure include LATP compounds represented by Li 1+x Al x Ti 2-x (PO4)3 with 0.1 ≦ x ≦ 0.5; compounds represented by Li 1+x Al y Mβ 2-y (PO4)3 where Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca and 0 ≦ x ≦ 1 and 0 ≦ y ≦ 1; compounds represented by Li 1+x Al x Ge 2-x (PO4)3 with 0 ≦ x ≦ 2; and compounds represented by Li 1+x Al x Zr 2-x (PO4)3 with 0 ≦ x ≦ 2; compounds represented by Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 where Mγ is one or more selected from the group consisting of Ti and Ge and 0 < x ≦ 2, 0 ≦ y < 3; compounds represented by Li 1+2x Zr 1-x Ca x (PO4)3 with 0 ≦ x < 1 can be mentioned.
[0084] In addition, as the oxide-based solid electrolyte, in addition to the above lithium phosphate solid electrolyte, Li x PO y N zand 2.6≦x≦3.5, 1.9≦y≦3.8, and 0.1≦z≦1.3. 2.9 PO 3.3 N 0.46 ); Garnet-type structure La 5+x A x La 3-x MδO 12 A is 1 or more selected from the group consisting of Ca, Sr, and Ba, Mδ is 1 or more selected from the group consisting of Nb and Ta, and 0≦x≦0.5; Li3Mδ 2-x L2O 12 wherein Mδ is at least one selected from the group consisting of Nb and Ta, and L may contain Zr, and 0≦x≦0.5; Li 7-3x Al x La3Zr3O 12 and 0≦x≦0.5; Li 5+x La3Mδ 2-x Zr x O 12 where Mδ is at least one selected from the group consisting of Nb and Ta, and 0≦x≦2. LLZ compounds (e.g., Li7La3Zr2O 12 ); and La 2 / 3-x Li x Examples of such compounds include those represented by TiO3, where x is 0.3≦x≦0.7.
[0085] One or more of the above compounds can be used as the solid electrolyte. Two or more of the above solid electrolytes can also be used.
[0086] <Exterior materials> The exterior member contains at least a positive electrode, a negative electrode, a separator, and an aqueous electrolyte. For example, a metal container, a laminated film container, or a resin container can be used as the exterior member. For the metal container, a metal can made of nickel, iron, stainless steel, or the like, having a rectangular or cylindrical shape can be used. For the resin container, a container made of polyethylene, polypropylene, or the like can be used.
[0087] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0088] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0089] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0090] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by weight or less.
[0091] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.
[0092] The secondary battery according to the embodiment can be used in various forms such as a square, cylindrical, flat, thin, coin type, etc. The secondary battery may be a secondary battery having a bipolar structure. For example, the electrode group may have a bipolar structure in which a positive electrode active material-containing layer is provided on one side of a single current collector and a negative electrode active material-containing layer is provided on the other side. In this case, there is an advantage that a plurality of cells connected in series can be produced from a single cell.
[0093] The methods for checking the positive electrode active material, negative electrode active material, negative electrode binder, and aqueous electrolyte are described below.
[0094] If the battery contains positive and negative electrodes, disassemble the battery, remove the positive or negative electrode, and clean it with dimethyl carbonate (DMC). The cleaning method is explained below. Immerse the electrode (positive or negative) in DMC for 5 minutes and remove the electrode. Repeat this three times, dry the electrode, and then subject it to measurement. When repeating the immersion, use new DMC solution each time.
[0095] When extracting the aqueous electrolyte from a battery, the battery is disassembled, and if the aqueous electrolyte is present outside the electrodes, the aqueous electrolyte that is not impregnated in the electrodes is extracted. If the aqueous electrolyte cannot be extracted from outside the electrodes, the electrode group is placed in a centrifuge and the aqueous electrolyte is extracted by centrifugation. <Cathode active material> The crystal structure and elemental composition of the positive electrode active material can be confirmed by powder X-ray diffraction (XRD) measurement and inductively coupled plasma (ICP) emission spectroscopy. <Negative electrode active material> The crystal structure and elemental composition of the negative electrode active material can be confirmed by powder X-ray diffraction (XRD) measurement and inductively coupled plasma (ICP) emission spectroscopy. <Negative electrode binder> The composition of the binder contained in the negative electrode can be confirmed by GC-MS (Gas Chromatography-Mass Spectrometry) measurement.
[0096] W bindThe measurement is performed by the following method. Disassemble the battery and collect the negative electrode. Next, cut out a part of this negative electrode to obtain a test piece. The size of the test piece is, for example, a square plate with a side length of 2 cm. The test piece is washed in advance with, for example, dimethyl carbonate (DMC) and then vacuum dried at 80 °C. After drying, the active material-containing layer is collected from the current collector of the test piece, and thermal gravimetric analysis (TG) is performed. The weight loss up to 600 °C is regarded as the binder weight. Calculate the ratio (weight %) of the binder weight to the weight of the active material-containing layer contained in the test piece from the obtained binder weight and the weight of the active material-containing layer of the test piece to obtain W bind to obtain. <XPS analysis> Whether or not a nitrogen-containing compound is present on the surface of the negative electrode can be confirmed by XPS analysis under the conditions described below.
[0097] As the XPS apparatus, Quantera SXM manufactured by ULVAC-PHI, Inc., or an apparatus having equivalent functions can be used. As the excitation X-ray source, a single crystal spectroscopic Al-Kα line (1486.6 eV) is used. The X-ray output is 4 kW (13 kV × 310 mA), the photoelectron detection angle is 45°, and the analysis area is about 4 mm × 0.2 mm. The scan is performed at 0.10 eV / step. <Aqueous electrolyte> That water is contained in the aqueous electrolyte can be confirmed by GC-MS (Gas Chromatography-Mass Spectrometry) measurement. Also, the water content W H2O in the aqueous electrolyte can be measured, for example, by evaporating the water in the aqueous electrolyte and measuring the weight ratio of the aqueous electrolyte to the residue. Weigh a specified amount of the aqueous electrolyte and evaporate the aqueous electrolyte in an inert atmosphere. The water content W H2O can be calculated from the weight ratio to the residue.
[0098] The presence of a compound having an amide bond in the aqueous electrolyte can be confirmed as follows. First, whether the aqueous electrolyte contains a compound containing nitrogen is confirmed by using inductively coupled plasma emission spectrometry (ICP (Inductively Coupled Plasma) emission spectrometry). Then, for example, infrared spectrometry is performed on the electrolyte to confirm that the compound has a nitrogen-containing compound. -1 When the electrolyte has a peak at 100%, it can be confirmed that the electrolyte contains a compound having an amide bond because the electrolyte contains a compound containing nitrogen.
[0099] An example in which the battery of the embodiment is applied to a secondary battery will be described with reference to FIGS.
[0100] The secondary battery 1 includes an electrode group 2 and an exterior member 20 in which the electrode group 2 is housed. The electrode group 2 is housed in the exterior member 20, which is a rectangular cylindrical metal container. The electrode group 2 includes a negative electrode 3, a separator 4, and a positive electrode 5. The electrode group 2 has a structure in which the separator 4 is interposed between the positive electrode 5 and the negative electrode 3 and wound in a spiral shape to form a flat shape. An aqueous electrolyte (not shown) is held in the electrode group 2. As shown in FIG. 2, a strip-shaped negative electrode lead 16 is electrically connected to each of a plurality of points on the end of the negative electrode 3 located on the end face of the electrode group 2. In addition, a strip-shaped positive electrode lead 17 is electrically connected to each of a plurality of points on the end of the positive electrode 5 located on this end face. The plurality of negative electrode leads 16 are connected to the negative electrode terminal 6 in a bundled state as shown in FIG. 2. In addition, although not shown, the positive electrode lead 17 is also electrically connected to the positive electrode terminal 7 in a bundled state.
[0101] The metal sealing plate 21 is fixed to an opening of the metal exterior member 20 by welding or the like. The negative electrode terminal 6 and the positive electrode terminal 7 are each drawn out to the outside through an extraction hole provided in the sealing plate 21. A negative electrode gasket 8 and a positive electrode gasket 9 are disposed on the inner circumferential surface of each extraction hole of the sealing plate 21 to prevent a short circuit due to contact with the negative electrode terminal 6 and the positive electrode terminal 7, respectively. By disposing the negative electrode gasket 8 and the positive electrode gasket 9, the airtightness of the secondary battery 100 can be maintained.
[0102] A control valve 22 (safety valve) is disposed on the sealing plate 21. When the internal pressure of the battery cell increases due to gas generated in the exterior member 20, the generated gas can be released to the outside from the control valve 22. The control valve 22 may be of a reset type that operates when the internal pressure exceeds a set value and functions as a sealing plug when the internal pressure decreases. Alternatively, a non-reset type control valve that does not recover its function as a sealing plug once it is activated may be used. In FIG. 1, the control valve 22 is disposed in the center of the sealing plate 21, but the control valve 22 may be located at the end of the sealing plate 21. The control valve 22 may be omitted.
[0103] Further, the sealing plate 21 is provided with a liquid inlet 23. The electrolyte can be injected through this liquid inlet 23. After the electrolyte is injected, the liquid inlet 23 can be closed by a sealing plug 24. The liquid inlet 23 and the sealing plug 24 may be omitted.
[0104] Another example of the secondary battery will be described with reference to Figures 3 and 4. Figures 3 and 4 show an example of a secondary battery 1 that uses an exterior member made of a laminate film as a container.
[0105] The secondary battery 1 shown in Figures 3 and 4 includes an electrode group 2 shown in Figures 3 and 4, an exterior member 20 shown in Figure 3, and an electrolyte (not shown). The electrode group 2 and the electrolyte are housed in the exterior member 20. The electrolyte is held in the electrode group 2.
[0106] The exterior member 20 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0107] The electrode group 2 is a laminated type electrode group, as shown in Fig. 4. The laminated type electrode group 2 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.
[0108] The electrode group 2 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 2 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0109] The negative electrode current collector 3a of each negative electrode 3 includes a portion 3c on one side of which the negative electrode active material-containing layer 3b is not supported on any surface. This portion 3c serves as a negative electrode current collector tab. As shown in FIG. 4, the portion 3c serving as the negative electrode current collector tab does not overlap with the positive electrode 5. The multiple negative electrode current collector tabs (portions 3c) are electrically connected to a strip-shaped negative electrode terminal 6. The tip of the strip-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 20.
[0110] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is located on the opposite side of the electrode group 2 to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side to the negative electrode terminal 6, and is drawn out to the outside of the exterior member 20.
[0111] The battery according to the embodiment described above includes a positive electrode, a negative electrode, and an electrolyte containing water. The negative electrode includes a negative electrode active material layer containing a Ti-containing oxide and a water-containing binder. The battery satisfies formula (1).
[0112] 0.2≦W bind / W H2O <= 15 (1) However, W bind is the content (wt%) of the hydrous binder in the negative electrode active material-containing layer, and W H2O is the water content in the electrolyte (wt%).
[0113] According to the battery, it is possible to suppress electrolysis of water, and to improve the adhesion between the active material-containing layer and the current collector and the ability of the active material-containing layer to retain the aqueous electrolyte, thereby improving the charge-discharge cycle performance of the battery of the embodiment.
[0114] Second embodiment According to a second embodiment, there is provided a battery pack including a plurality of secondary batteries according to the embodiment.
[0115] In the battery pack according to this embodiment, the individual cells may be electrically connected in series or in parallel, or may be connected in a combination of series and parallel.
[0116] Next, an example of a battery pack will be described with reference to the drawings.
[0117] 5 includes five cells 100a to 100e, four bus bars 201, a positive electrode lead 207, and a negative electrode lead 206. Each of the five cells 100a to 100e is a secondary battery according to the embodiment.
[0118] The bus bar 201 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 201. That is, the battery pack 200 in FIG. 5 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, thereby electrically connecting the plurality of cells.
[0119] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 207 for external connection. In addition, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 206 for external connection.
[0120] The battery pack according to the embodiment includes the batteries according to the embodiment, and therefore the battery pack can have excellent life performance.
[0121] [Third embodiment] According to a third embodiment, a battery pack including the battery according to the embodiment is provided. The battery pack may include the battery assembly according to the embodiment. The battery pack may include a single battery instead of the battery assembly according to the embodiment.
[0122] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0123] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0124] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0125] The battery pack 300 shown in Figs. 6 and 7 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0126] 6 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0127] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 207, a negative electrode lead 206, and an adhesive tape .
[0128] At least one of the plurality of unit cells 100 is a secondary battery according to the embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 7. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0129] The adhesive tape 36 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 36. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0130] One end of the positive electrode lead 207 is connected to the battery pack 200. One end of the positive electrode lead 207 is electrically connected to the positive electrode of one or more of the cells 100. One end of the negative electrode lead 206 is connected to the battery pack 200. One end of the negative electrode lead 206 is electrically connected to the negative electrode of one or more of the cells 100.
[0131] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0132] The other end 207a of the positive electrode lead 207 is electrically connected to the positive electrode connector 342. The other end 206a of the negative electrode lead 206 is electrically connected to the negative electrode connector 343.
[0133] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to a protection circuit 346.
[0134] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0135] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0136] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0137] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0138] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0139] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0140] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0141] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 207 and the negative electrode lead 206 may be used as the positive and negative terminals of the external terminals for current supply, respectively.
[0142] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0143] The battery pack according to the third embodiment includes the battery according to the embodiment or the battery assembly according to the embodiment, and therefore has excellent life performance.
[0144] [Fourth embodiment] According to a fourth embodiment, a vehicle including a battery pack according to an embodiment is provided.
[0145] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0146] Examples of vehicles according to the embodiment include two-wheeled to four-wheeled hybrid electric vehicles, two-wheeled to four-wheeled electric vehicles, power-assisted bicycles, and rail vehicles.
[0147] The mounting position of the battery pack in the vehicle according to the embodiment is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0148] The vehicle according to the embodiment may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections.
[0149] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0150] A vehicle 400 shown in Fig. 8 includes a vehicle body 40 and a battery pack 300 according to the embodiment. In the example shown in Fig. 8, the vehicle 400 is a four-wheeled automobile.
[0151] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0152] 8 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0153] The vehicle according to the fourth embodiment is equipped with the battery pack according to the embodiment, and therefore the vehicle can exhibit high performance and is highly reliable.
[0154] [Fifth embodiment] According to a fifth embodiment, there is provided a stationary power source including a battery pack according to an embodiment.
[0155] Such a stationary power source may be equipped with a battery pack according to an embodiment or a battery according to an embodiment instead of the battery pack according to an embodiment. Such a stationary power source can exhibit a long life.
[0156] FIG. 9 is a diagram showing an application example to stationary power sources 112 and 123 as an example of use of the battery packs 300A and 300B according to the embodiment. In the example shown in FIG. 9, a system 110 in which the stationary power sources 112 and 123 are used is shown. The system 110 includes a power plant 111, a stationary power source 112, a consumer-side power system 113, and an energy management system (EMS) 115. A power grid 116 and a communication network 117 are also formed in the system 110, and the power plant 111, the stationary power source 112, the consumer-side power system 113, and the EMS 115 are connected via the power grid 116 and the communication network 117. The EMS 115 utilizes the power grid 116 and the communication network 117 to perform control to stabilize the entire system 110.
[0157] The power plant 111 generates a large amount of power using fuel sources such as thermal power and atomic power. Power is supplied from the power plant 111 through a power grid 116 or the like. A battery pack 300A is mounted on the stationary power source 112. The battery pack 300A can store the power supplied from the power plant 111. The stationary power source 112 can supply the power stored in the battery pack 300A through the power grid 116 or the like. The system 110 is provided with a power conversion device 118. The power conversion device 118 includes a converter, an inverter, a transformer, and the like. Thus, the power conversion device 118 can perform conversion between direct current and alternating current, conversion between alternating currents having different frequencies, and voltage transformation (boosting and bucking), and the like. Thus, the power conversion device 118 can convert the power from the power plant 111 into power that can be stored in the battery pack 300A.
[0158] The consumer-side power system 113 includes a power system for a factory, a power system for a building, a power system for a home, etc. The consumer-side power system 113 includes a consumer-side EMS 121, a power conversion device 122, and a stationary power source 123. The stationary power source 123 is equipped with a battery pack 300B. The consumer-side EMS 121 performs control to stabilize the consumer-side power system 113.
[0159] The consumer-side power system 113 is supplied with power from the power plant 111 and power from the battery pack 300A through the power grid 116. The battery pack 300B can store the power supplied to the consumer-side power system 113. Similarly to the power conversion device 118, the power conversion device 122 includes a converter, an inverter, a transformer, and the like. Therefore, the power conversion device 122 can perform conversion between DC and AC, conversion between ACs with different frequencies, and voltage transformation (boost and step-down), etc. Therefore, the power conversion device 122 can convert the power supplied to the consumer-side power system 113 into power that can be stored in the battery pack 300B.
[0160] The power stored in the battery pack 300B can be used, for example, to charge a vehicle such as an electric car. The system 110 may also be provided with a natural energy source. In this case, the natural energy source generates power using natural energy such as wind power and solar power. Power is supplied from the natural energy source in addition to the power plant 111 through the power grid 116. EXAMPLES
[0161] The above embodiment will be specifically described below using examples, but the present invention is not limited to the following examples as long as they do not deviate from the gist of the present invention.
[0162] Example 1 A secondary battery was fabricated according to the following procedure.
[0163] <Preparation of negative electrode> As the negative electrode active material, particles of a monoclinic niobium titanium-containing oxide having a composition represented by the formula TiNb2O7 were prepared. This monoclinic niobium titanium-containing oxide has a high affinity for Li in a battery. a It has a composition represented by TiNb2O7 (0≦a≦5). In addition, acetylene black as a conductive agent, and carboxymethylcellulose (CMC) and styrene butadiene rubber (SBR) as water-containing binders were prepared. These were mixed in pure water so that the weight ratio (weight %) of negative electrode active material: acetylene black: carboxymethylcellulose: styrene butadiene rubber was 95: 4.2: 0.4: 0.4 to obtain a slurry. This slurry was applied to a current collector made of aluminum foil with a thickness of 15 μm, and the coating was dried. Thus, a composite including a current collector and a negative electrode active material-containing layer formed on the current collector was obtained. The obtained composite was then subjected to roll pressing. Next, this composite was further subjected to vacuum drying to obtain a negative electrode.
[0164] <Preparation of positive electrode> The positive electrode active material is LiNi 0.33 Mn 0.33 Co 0.33Particles of lithium nickel cobalt manganese composite oxide represented by O2 (referred to as NMC111) were prepared. In addition, acetylene black as a conductive agent and polyvinylidene fluoride (PVdF) as a binder were prepared. These were mixed so that the weight ratio (weight %) of the positive electrode active material: conductive agent: binder was 90:5:5 to obtain a mixture. Next, the obtained mixture was dispersed in n-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry. This slurry was applied onto a current collector made of aluminum foil with a thickness of 15 μm, and the coating was dried. Thus, a composite including a current collector and a positive electrode active material-containing layer formed on both sides of the current collector was obtained. Next, the obtained composite was subjected to roll pressing. Next, this composite was further subjected to vacuum drying to obtain a positive electrode.
[0165] The positive and negative electrodes were each cut out so that the area where the active material-containing layer was formed was 3 cm wide and 5 cm high. One negative electrode and one positive electrode were attached to each other via a 30 μm thick cellulose separator to produce an electrode laminate as an electrode group. In addition, aluminum tabs with a thickness of 0.2 mm were attached to the negative and positive electrodes to collect current. The produced electrode laminate was housed in an exterior member made of a laminate film, and after pouring in a liquid aqueous electrolyte (aqueous electrolyte solution), it was sealed to obtain a secondary battery.
[0166] The liquid aqueous electrolyte had a composition of 56.0 wt% LiN(CF3SO2)2 (LiTFSI), 39.8 wt% urea, 0.2 wt% KOH, and 4 wt% H2O.
[0167] Example 2 A negative electrode was produced in the same manner as in Example 1, except that the weight ratio (wt %) of the negative electrode active material: acetylene black: CMC: SBR was 92.5:4.0:1.5:2.0.
[0168] In addition, the composition of the liquid aqueous electrolyte was changed to 56.0 wt% LiN(CF3SO2)2 (LiTFSI), 40.4 wt% urea, 0.1 wt% KOH, and 3.5 wt% H2O.
[0169] Other than these, the secondary battery was fabricated in the same manner as in Example 1.
[0170] Example 3 A negative electrode was produced in the same manner as in Example 1, except that the weight ratio (wt %) of the negative electrode active material: acetylene black: CMC: SBR was 91.5:4.0:2.0:2.5.
[0171] In addition, the composition of the liquid aqueous electrolyte was changed to 58.2 wt% LiN(CF3SO2)2 (LiTFSI), 41.3 wt% urea, 0.2 wt% KOH, and 0.3 wt% H2O.
[0172] Other than these, the secondary battery was fabricated in the same manner as in Example 1.
[0173] (Examples 4-7) A negative electrode was prepared in the same manner as in Example 2, except that the composition of the negative electrode active material was changed to the composition shown in Table 1. A secondary battery was prepared in the same manner as in Example 2, except that this negative electrode was used. a Ti2Nb 10 O 29 The negative electrode active material of Example 5 has a composition represented by the formula: (0≦a≦22). a The negative electrode active materials of Examples 6 and 7 have a composition represented by Ti2Nb2O9 (0≦a≦6). x It has a composition represented by TiO2 (x is 0≦x≦1).
[0174] Example 8 The composition of the liquid aqueous electrolyte was changed to 55.9% by weight of LiN(CF3SO2)2(LiTFSI), 40.5% by weight of acetamide, 0.1% by weight of KOH, and 3.5% by weight of H2O. A secondary battery was fabricated in the same manner as in Example 2, except for using this liquid aqueous electrolyte.
[0175] Example 9 Polyvinylpyrrolidone (PVP) and styrene butadiene rubber (SBR) were prepared as hydrous binders. A negative electrode was produced in the same manner as in Example 1, except that these were mixed so that the weight ratio (weight %) of the negative electrode active material: acetylene black: PVP: SBR was 92.5: 4.0: 1.8: 1.7.
[0176] The composition of the liquid aqueous electrolyte was changed to 51.3 wt% LiN(CF3SO2)2(LiTFSI), 45.0 wt% N-methylurea, 0.2 wt% KOH, and 3.5 wt% H2O. A secondary battery was fabricated in the same manner as in Example 1, except that the above negative electrode and liquid aqueous electrolyte were used.
[0177] Example 10 LiNi as the positive electrode active material 0.8 Mn 0.1 Co 0.1 A positive electrode was prepared in the same manner as in Example 1, except that particles of a lithium nickel cobalt manganese composite oxide represented by O2 (referred to as NMC811) were used.
[0178] In addition, the composition of the liquid aqueous electrolyte was changed to 54.0% by weight of LiN(CF3SO2)2 (LiTFSI), 2.0% by weight of lithium difluorooxalatoborate (LiDFOB), 40.4% by weight of urea, 0.1% by weight of KOH, and 3.5% by weight of H2O. A secondary battery was fabricated in the same manner as in Example 2, except that the above positive electrode and liquid aqueous electrolyte were used.
[0179] Example 11 Spinel-structured Li as a positive electrode active material 1.05 Al 0.05 Except for using particles of lithium manganese composite oxide represented by Mn2O4 (referred to as LMO), a positive electrode was produced in the same manner as in Example 1. Except for using this positive electrode, a secondary battery was produced in the same manner as in Example 2.
[0180] Example 12 Spinel-structured Li as a positive electrode active material 1.05 Al 0.05A positive electrode was prepared in the same manner as in Example 1, except that particles of a lithium manganese composite oxide represented by Mn2O4 (referred to as LMO) were used.
[0181] The composition of the liquid aqueous electrolyte was changed to 57.7 wt% LiN(CF3SO2)2 (LiTFSI), 41.1 wt% urea, 0.2 wt% KOH, and 1.0 wt% H2O.
[0182] A secondary battery was fabricated in the same manner as in Example 2, except that the above positive electrode and liquid aqueous electrolyte were used.
[0183] Example 13 Spinel-structured Li as a positive electrode active material 1.05 Al 0.05 A positive electrode was prepared in the same manner as in Example 1, except that particles of a lithium manganese composite oxide represented by Mn2O4 (referred to as LMO) were used.
[0184] A negative electrode was produced in the same manner as in Example 1, except that the weight ratio (wt %) of the negative electrode active material: acetylene black: CMC: SBR was 92:4.0:2.0:2.0.
[0185] In addition, the composition of the liquid aqueous electrolyte was changed to 53.7 wt% LiN(CF3SO2)2 (LiTFSI), 38.1 wt% urea, 0.2 wt% KOH, and 8.0 wt% H2O.
[0186] A secondary battery was fabricated in the same manner as in Example 1, except that the above positive electrode, negative electrode, and liquid aqueous electrolyte were used.
[0187] Comparative Example 1 The composition of the liquid aqueous electrolyte was changed to 53.7% by weight of LiN(CF3SO2)2(LiTFSI), 38.1% by weight of urea, 0.2% by weight of KOH, and 8.0% by weight of H2O. A secondary battery was fabricated in the same manner as in Example 1, except for using this liquid aqueous electrolyte.
[0188] Comparative Example 2 A negative electrode was produced in the same manner as in Example 1, except that the weight ratio (wt %) of the negative electrode active material: acetylene black: CMC: SBR was 90:4.0:2.0:4.0.
[0189] In addition, the composition of the liquid aqueous electrolyte was changed to 58.2 wt% LiN(CF3SO2)2 (LiTFSI), 41.3 wt% urea, 0.2 wt% KOH, and 0.3 wt% H2O.
[0190] A secondary battery was fabricated in the same manner as in Example 1, except that the above negative electrode and liquid aqueous electrolyte were used.
[0191] Comparative Example 3 As the negative electrode active material, particles of niobium titanium-containing oxide having a monoclinic structure and the same composition as in Example 1 were prepared. In addition, acetylene black as a conductive agent and polyvinylidene fluoride (PVdF) as a binder were prepared. These were mixed in n-methylpyrrolidone (NMP) so that the weight ratio (weight %) of negative electrode active material: acetylene black: PVdF was 94: 4.0: 2.0 to obtain a slurry. This slurry was applied to a current collector made of aluminum foil with a thickness of 15 μm, and the coating was dried. Thus, a composite including a current collector and a negative electrode active material-containing layer formed on the current collector was obtained. Next, the obtained composite was subjected to roll pressing. Next, this composite was further subjected to vacuum drying to obtain a negative electrode.
[0192] A secondary battery was produced in the same manner as in Example 2, except that the above negative electrode was used. <Evaluation> The secondary batteries obtained in the above examples and comparative examples were subjected to an initial charge and discharge, and then the charge and discharge cycle life was measured at 25° C. At 25° C., the battery was charged to 2.6 V at 0.2 C, and then discharged to 1.5 V at 0.2 C. This charge and discharge cycle was repeated 50 times, and the retention rate (%) of the discharge capacity at the 50th cycle relative to the discharge capacity at the 1st cycle was calculated and shown in Table 3 as the capacity retention rate during the charge and discharge cycles.
[0193] Table 1 shows the composition of the negative electrode active material, the composition of the positive electrode active material, and the content W of the water-containing binder in the negative electrode active material-containing layer. bind (wt%), water content in the electrolyte W H2O (wt%), W bind / W H2O The value of the ratio is expressed as W bind (wt%) and W H2O The method for measuring (wt %) is as described above. Table 2 shows the type of binder for the negative electrode and the composition of the aqueous electrolyte.
[0194] [Table 1]
[0195] [Table 2]
[0196] [Table 3]
[0197] As is clear from Tables 1 to 3, 0.2≦W bind / W H2O The secondary batteries of Examples 1 to 13, which satisfy the condition of ≦15, have a charge-discharge cycle life superior to that of Comparative Examples 1 to 3. Comparative Examples 1 and 2 use a water-containing binder, but W bind / W H2O The ratio value represented by does not satisfy the above range. On the other hand, in Comparative Example 3, since PVdF was used as a binder, PVdF was decomposed by water in the electrolyte, and the negative electrode active material-containing layer peeled off from the current collector. Therefore, the charge-discharge cycle life of the battery in Comparative Example 3 was shorter than those in Examples 1 to 13.
[0198] By comparing Example 2 with Examples 4 to 7, Li a TiM b Nb 2±β O 7±σIt can be seen that the charge / discharge cycle life of the battery of Example 2 containing the monoclinic niobium titanium-containing oxide represented by the formula (0≦a≦5, 0≦b≦0.3, 0≦β≦0.3, 0≦σ≦0.3, M is at least one element selected from the group consisting of Fe, V, Mo, and Ta) as the negative electrode active material is superior to that of Examples 4 to 7.
[0199] A comparison of Example 2 with Examples 8 to 9 shows that the charge-discharge cycle life of the battery of Example 2, which contains urea as the compound containing an amide bond, is superior to those of Examples 8 to 9.
[0200] According to the battery of at least one of these embodiments or examples, since formula (1) is satisfied, the electrolysis of water can be suppressed and the life performance can be improved.
[0201] 0.2≦W bind / W H2O <= 15 (1) However, W bind is the content (wt%) of the hydrous binder in the negative electrode active material-containing layer, and W H2O is the water content in the electrolyte (wt%).
[0202] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims.
[0203] The following describes the embodiments of the invention. <1> A positive electrode and a negative electrode including a negative electrode active material-containing layer including a Ti-containing oxide and a water-containing binder; and an electrolyte comprising water, A battery that satisfies the following formula (1).
[0204] 0.2≦W bind / W H2O <= 15 (1) However, W bind is the content (wt%) of the water-containing binder in the negative electrode active material-containing layer, and W H2O is the water content (wt%) in the electrolyte. <2> The above W H2O is 10% by weight or less, bind is 0.8% by weight or more and 6% by weight or less; <1> 2. The battery according to claim 1 . <3> The above W H2O is 0.3% by weight or more; <1> or <2> 2. The battery according to claim 1 . <4> The hydrous binder includes at least one selected from the group consisting of carboxymethyl cellulose and its salts, styrene-butadiene rubber, and polyvinylpyrrolidone. <1> from <3> 13. The battery according to any one of claims 1 to 12. <5> The electrolyte further contains a compound containing an amide bond and at least one lithium salt selected from the group consisting of LiN(FSO2)2, LiN(CF3SO2)2, and LiN(SO2C2F5)2. <1> from <4> 13. The battery according to any one of claims 1 to 12. <6> The Ti-containing oxide includes at least one of a niobium titanium-containing oxide or a titanium oxide. <1> from <5> 13. The battery according to any one of claims 1 to 12. <7> The Ti-containing oxides are TiNb2O7, Ti2Nb2O9, Ti2Nb 10 O 29 , TiNb 14 O 37 and TiNb 24 O 62 At least one selected from the group consisting of a niobium titanium-containing oxide having at least one crystal phase selected from the group consisting of a titanium oxide having a monoclinic structure, a titanium oxide having a rutile structure, and a titanium oxide having an anatase structure. <1> from <5> 13. The battery according to any one of claims 1 to 12. <8> The Ti-containing oxide includes at least one selected from the group consisting of a niobium titanium-containing oxide having a monoclinic structure, a titanium oxide having a monoclinic structure, a titanium oxide having a rutile structure, and a titanium oxide having an anatase structure. <1> from <5> 13. The battery according to any one of claims 1 to 12. <9> <1> from <8> A battery pack comprising the battery according to any one of claims 1 to 5. <10> Further including an external terminal for current supply and a protection circuit. <9> The battery pack according to claim 1 . <11> The battery includes a plurality of the batteries, the batteries being electrically connected in series, in parallel, or in a combination of series and parallel. <9> or <10> The battery pack according to claim 1 . <12> <9> from <11> A vehicle equipped with the battery pack according to any one of claims 1 to 5. <13> A mechanism for converting the kinetic energy of the vehicle into regenerative energy. <12> A vehicle as described in. <14> <9> from <11> A stationary power source comprising the battery pack according to any one of claims 1 to 5. [Explanation of symbols]
[0205] 1...battery, 2...electrode group, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode composite layer (negative electrode active material-containing layer), 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode composite layer (positive electrode active material-containing layer), 6...negative electrode terminal, 7...positive electrode terminal, 8...negative electrode gasket, 9...positive electrode gasket, 16...negative electrode lead, 17...positive electrode lead, 20...exterior member, 21...sealing plate, 22...control valve, 23...filling port, 24...sealing plug, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 36...adhesive tape, 40...vehicle body, 100...secondary battery, 110...system, 111...power plant, 112...stationary power source, 113...consumer side Power system, 115...energy management system, 116...power grid, 117...communication network, 118...power conversion device, 121...demand side EMS, 122...power conversion device, 123...stationary power source, 200...battery pack, 201...bus bar, 206...negative side lead, 207...positive side lead, 300...battery pack, 300A...battery pack, 300B...battery pack, 342...positive side connector, 342a...wiring, 343...negative side connector, 343a...wiring, 345...thermistor, 346...protection circuit, 348a...positive side wiring, 348b...negative side wiring, 350...external terminal for energization, 352...positive side terminal, 353...negative side terminal, 400...vehicle.
Claims
1. A positive electrode and a negative electrode including a negative electrode active material-containing layer including a Ti-containing oxide and a water-containing binder; and an electrolyte comprising water, A battery that satisfies the following formula (1). 0.2≦W bind / W H2O ≦15 (1) However, W bind is the content (wt%) of the water-containing binder in the negative electrode active material-containing layer, W H2O is the water content (wt%) in the electrolyte.
2. The W H2O is 10% by weight or less, bind The battery of claim 1 , wherein the weight percent of the electrolyte is greater than or equal to 0.8% and less than or equal to 6%.
3. The W H2O The battery of claim 2 , wherein the weight percent of the cations in the battery is 0.3 weight percent or more.
4. 2. The battery according to claim 1, wherein the hydrous binder comprises at least one selected from the group consisting of carboxymethyl cellulose and its salts, styrene-butadiene rubber, and polyvinylpyrrolidone.
5. The electrolyte is a compound containing an amide bond and LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) 2 and LiN(SO 2 C 2 F 5 ) 2 and at least one lithium salt selected from the group consisting of:
6. 2. The battery of claim 1, wherein the Ti-containing oxide comprises at least one of a niobium titanium-containing oxide or a titanium oxide.
7. The Ti-containing oxide is TiNb 2 O 7 , Ti 2 Nb 2 O 9 , Ti 2 Nb 10 O 29 , TiNb 14 O 37 and TiNb 24 O 62 2. The battery according to claim 1, comprising at least one selected from the group consisting of a niobium titanium-containing oxide having at least one crystal phase selected from the group consisting of a titanium oxide having a monoclinic structure, a titanium oxide having a rutile structure, and a titanium oxide having an anatase structure.
8. 2. The battery according to claim 1, wherein the Ti-containing oxide comprises at least one selected from the group consisting of a niobium titanium-containing oxide having a monoclinic structure, a titanium oxide having a monoclinic structure, a titanium oxide having a rutile structure, and a titanium oxide having an anatase structure.
9. A battery pack comprising the battery according to any one of claims 1 to 8.
10. 10. The battery pack according to claim 9, further comprising an external terminal for current flow and a protection circuit.
11. The battery pack according to claim 10 , comprising a plurality of the batteries, the batteries being electrically connected in series, in parallel, or in a combination of series and parallel.
12. A vehicle comprising the battery pack according to claim 9.
13. The vehicle of claim 12 including a mechanism for converting kinetic energy of the vehicle into regenerative energy.
14. A stationary power source comprising the battery pack according to claim 9.
Citation Information
Patent Citations
Aqueous lithium titanate battery and preparation method thereof
CN111211255A
Secondary battery, battery pack, and vehicle
JP2017174810A
Aqueous electrolyte solution for power storage device, and power storage device including the same
JP2020155277A
Secondary battery, battery pack and vehicle
JP2018156895A
Secondary battery, battery pack and vehicle
JP2018163893A
Cited By
Post-treatment method for flame synthesis of titanium niobium oxide powder and application
CN119841349A