Lithium sulfur battery
By optimizing the cell configuration of lithium-sulfur batteries with a DP value of 0.5 to 2.5 and separator porosity of 20% to 50%, the battery's cycle performance and voltage characteristics are enhanced, addressing the polysulfide loss issue and making it suitable for electric vehicles and energy storage.
Patent Information
- Application Number
- JP2023045959
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Lithium polysulfides have high solubility in electrolytic solutions, leading to a gradual loss of sulfur from the electrode during charging and discharging, which reduces the capacity of lithium-sulfur batteries, and existing solutions have not adequately addressed this issue for practical use.
The lithium-sulfur battery design focuses on the cell configuration by specifying the interelectrode distance divided by separator porosity (DP value) to be between 0.5 and 2.5, along with separator porosity of 20% to 50% and electrode distance of 25 to 100 microns, to improve cycle performance without degrading voltage characteristics.
This configuration results in a highly practical lithium-sulfur battery with high cycle performance and maintained voltage characteristics, suitable for applications like electric vehicles and energy storage.
Smart Images

Figure 2024135332000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to lithium-sulfur batteries. [Background technology]
[0002] As the application area of secondary batteries expands to electric vehicles (EVs) and energy storage systems (ESSs), there is a demand for batteries with high energy density, but existing lithium-ion secondary batteries (see, for example, Patent Document 1) have limitations, and the development of next-generation secondary battery technology is urgently needed. Among them, lithium-sulfur batteries have a large capacity per unit weight of sulfur and are positioned as a battery with high expectations for practical use.
[0003] Lithium-sulfur batteries use sulfur-based materials with S-S bonds (Sulfur-Sulfur Bonds) as the positive electrode active material and lithium metal as the negative electrode active material. Sulfur is inexpensive and abundant, with a Clarke number of 15, and elemental sulfur has low toxicity, making it a suitable material for next-generation batteries.
[0004] In lithium-sulfur batteries, when discharging, the negative electrode active material lithium releases electrons, and the positive electrode active material sulfur accepts electrons and is reduced. Here, the oxidation reaction of lithium is the process in which lithium metal releases electrons to become lithium ions. The reduction reaction of sulfur is the process in which the S-S bond accepts two electrons to become S. 2- The lithium ions produced by the oxidation reaction of lithium are transferred to the positive electrode through the electrolyte and combine with the sulfide ions produced by the reduction reaction of sulfur. Specifically, sulfur before discharge has a ring-shaped S8 structure, which is converted into lithium polysulfide (LiSx) through a reduction reaction. When lithium polysulfide is reduced, it goes through multiple reactions to finally become lithium sulfide (Li2S). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 4780960 Summary of the Invention [Problem to be solved by the invention]
[0006] However, this lithium polysulfide is highly soluble in electrolyte, and the sulfur used as an active material gradually disappears from the electrode during charging and discharging, causing a major problem of capacity reduction. This problem has long been well known among battery researchers and engineers, and measures have been developed to prevent dissolution of polysulfide into electrolyte by confining it in carbon materials, or by developing electrolytes with low polysulfide solubility. The above measures are gradually solving the problem of polysulfide dissolution, but the current situation is that they have not yet reached a level where practical use is possible.
[0007] Thus, while approaches to solving problems from the perspective of electrodes and electrolytes have been taken mainly by universities and research institutes, there have been almost no approaches to solving problems by devising the cell configuration of lithium-sulfur batteries. When attempting to put lithium-sulfur batteries into practical use, it is battery manufacturers, not universities or research institutes, that actually make the products, and the fact that there are still few manufacturers trying to commercialize them is cited as a reason for the lack of consideration of cell configuration. For this reason, when making lithium-sulfur batteries, the current situation is that the configuration of existing lithium-ion batteries (see Patent Document 1) is applied as is to lithium-sulfur batteries, but since the electrochemical principles themselves are different between lithium-ion batteries and lithium-sulfur batteries, it is necessary to consider a cell configuration suitable for lithium-sulfur batteries. [Means for solving the problem]
[0008] In order to solve the above problems, we focused on the cell configuration of lithium-sulfur batteries. As a result of extensive research, we found that by specifying the value obtained by dividing the distance between electrodes by the porosity of the separator (hereinafter referred to as the DP value) to be 0.5 to 2.5, the effects specific to the above combination are generated, and it is possible to improve the cycle performance without degrading the voltage characteristics of the lithium-sulfur battery, leading to the completion of the present invention.
[0009] In order to solve the above-mentioned problems and achieve the object, the lithium-sulfur battery of the present invention uses an electrode in which elemental sulfur and / or a sulfur compound is used as an electrode active material for a positive electrode, an electrode in which metallic lithium and / or an alloy thereof is used as an electrode active material for a negative electrode, and further has a structure in which the positive and negative electrodes are separated by a separator, and is characterized in that the value (DP value) obtained by dividing the distance between the positive and negative electrodes (microns) by the separator porosity (%) is 0.5 to 2.5.
[0010] In addition, in a second aspect, the lithium-sulfur battery according to the present invention is characterized in that in the first aspect, the DP value is 1.0 or more and 1.5 or less.
[0011] In addition, as a third aspect, the lithium-sulfur battery according to the present invention is characterized in that, in the above-mentioned first aspect, the separator porosity is 20% or more and 50% or less.
[0012] In addition, as a fourth aspect, the lithium-sulfur battery according to the present invention is characterized in that, in the above-mentioned first aspect, the distance between the positive and negative electrodes is 25 microns or more and 100 microns or less.
[0013] In addition, as a fifth aspect, the lithium-sulfur battery according to the present invention is characterized in that, in the above-mentioned first aspect, the distance between the positive and negative electrodes is 32 microns or more and 100 microns or less.
[0014] In addition, as a sixth aspect, the lithium-sulfur battery according to the present invention is characterized in that, in the above-mentioned first aspect, the lithium salt is lithium bistrifluorosulfonylamide (LiTFSA) and / or lithium bisfluorosulfonylamide (LiFSA), the solvent is at least one selected from triethylene glycol dimethyl ether (G3), tetraethylene glycol dimethyl ether (G4), and sulfolane, and further contains a fluorinated ether. Effect of the Invention
[0015] According to the present invention, it is possible to provide a highly practical lithium-sulfur battery that has high cycle performance without deteriorating voltage characteristics. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic cross-sectional view of a coin-type battery shown as an example of the lithium-sulfur battery according to the first embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a laminated battery shown as an example of a lithium-sulfur battery according to embodiment 2 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The following examples of forms and configurations of the present invention are given, but the present invention is not limited to these. All of the following are included in the present invention as long as they are in line with the intent of the claims, the means for solving the problems, the effects of the invention, and the like.
[0018] The present invention relates to a lithium-sulfur battery and has the following three features.
[0019] The first point is that the DP value is specified to be 0.5 or more and 2.5 or less. This value is generally less than 0.5 in lithium ion batteries, and is different from conventional cell configurations. The reason why the setting of the DP value is important is that the present battery system is not as simple as simply specifying the electrode distance and porosity. The balance between these two parameters is important, and only when this range is 0.5 or more and 2.5 or less, a practical lithium-sulfur battery with a good balance between voltage characteristics and cycle characteristics is obtained, and the present inventor has discovered this point ahead of others. For example, even if the cycle characteristics are improved, if the voltage characteristics are reduced, there is no practical or commercial value, and it goes without saying how useful the present invention is. When the DP value is 0.5 or more and 2.5 or less, qualitatively, the electrode distance is wider and the porosity of the separator is smaller than that of a lithium ion battery. More preferably, the DP value is 1.0 or more and 1.5 or less. If it is more than 2.5, the interelectrode distance is too large relative to the separator porosity, and the electrolyte resistance increases too much, causing a voltage drop. The DP value can be controlled by adjusting the thickness of the separator or by increasing the number of separators. The DP value is measured by disassembling the battery and taking the maximum value of the total thickness of all separators between positive and negative electrode plates. The present invention is applicable to both wound and stacked types. When measuring the DP value of a wound type lithium ion battery, the measurement is performed using the part of the electrode that is not bent and is flat.
[0020] The second point is that the porosity of the separator is set to 20% or more and 50% or less. In lithium ion batteries, it is common knowledge that the higher the porosity, the better, as long as the strength is not affected. In Patent Document 1, the separator porosity is set to 35% or more and 60% or less, which is a value larger than that of the present invention. In the case of lithium-sulfur batteries in the present invention, the tendency is the opposite to that of lithium-ion batteries, which was also discovered by the present inventors before others. In lithium-sulfur batteries, the redox shuttle phenomenon caused by polysulfide eluted at the positive electrode moving to the negative electrode becomes a problem, but the lower the separator porosity, the higher the shielding property, making it physically difficult for polysulfide to reach the negative electrode. However, if the porosity is too low, the interelectrode resistance becomes too large, which has a large effect on the voltage drop. In the present invention, in combination with the first point, the porosity of the separator is set to 20% or more and 50% or less, thereby obtaining the effect of improving cycle characteristics.
[0021] The third point is that the distance between the positive and negative electrodes is 25 microns or more and 100 microns or less. In lithium ion batteries, it is common knowledge that the shorter the distance between the positive and negative electrodes, the better. In Patent Document 1, the separator thickness (= the distance between the positive and negative electrodes) is less than 25 microns at most, which is a smaller value than in the present invention. In this respect, the lithium-sulfur battery in the present invention has a tendency opposite to that in the lithium ion battery, and this point was discovered by the inventor before others. In lithium sulfur batteries, the redox shuttle phenomenon caused by polysulfide dissolved at the positive electrode moving to the negative electrode becomes a problem, but the longer the distance between the positive and negative electrodes, the more the polysulfide dissolved at the positive electrode ends discharging before reaching the negative electrode, and as a result, it is possible to improve the cycle characteristics by suppressing the redox shuttle. However, if the distance between the positive and negative electrodes becomes too long, the amount of electrolyte contained between the electrodes becomes too large, which increases the amount of polysulfide dissolved, leading to a decrease in cycle characteristics.
[0022] [Lithium-sulfur battery] The lithium-sulfur battery of the present invention can be composed of, for example, a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, terminals, and an exterior body, all of which are described below.
[0023] <Positive electrode> The positive electrode is composed of, for example, a positive electrode active material mixture electrode layer (hereinafter, may be referred to as a "mixture layer") and a current collector.
[0024] (Positive electrode active material mixture electrode layer) The positive electrode active material mixture electrode layer can be composed of, for example, a positive electrode active material, a conductive material, a binder, and a solvent. Examples of the positive electrode active material include elemental sulfur or a sulfur compound. Elemental sulfur has allotropes such as α-type and γ-type, all of which act as electrode active materials. Examples of sulfur compounds include metal sulfides and sulfur-based polymer compounds, and all of these compounds that act as electrode active materials are included in the present invention.
[0025] In addition, the conductive material is not particularly limited in the present invention, and for example, known or commercially available conductive materials such as carbon black such as Ketjen black, open mesopore carbon materials, acetylene black, carbon nanotubes, carbon fibers, activated carbon, and graphite can be used. However, in the present invention, the conductive material can be used in a method of use that is characterized by grinding it together with the above-mentioned positive electrode active material in a mortar or the like to form a composite. Compared with the positive electrode active material used in lithium ion batteries, sulfur and sulfur compounds used as positive electrode active materials have very low electronic conductivity, and act as insulators by themselves, so they cannot be used as electrode active materials. For this reason, by forming a composite, the contact surface area with the carbon material is increased, and sulfur is used as an electrode active material.
[0026] There is no particular limitation on the binder, and known or commercially available binders can be used. For example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinylpyrrolidone (PVP), polyvinyl chloride (PVC), polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), acrylic resin, etc. can be used.
[0027] The solvent is not particularly limited in the present invention, and various solvents can be selected depending on the positive electrode active material or binder used. Specifically, when PVDF or PTFE is used as the binder, it is preferable to use N-methyl-2-pyrrolidone as the solvent, and when a rubber-based binder such as styrene butadiene rubber (SBR) is used, water is suitable as the solvent.
[0028] (current collector) The current collector is not particularly limited in the present invention, but aluminum foil is generally used as a current collector for the positive electrode of a lithium ion battery, and a porous aluminum current collector is also used depending on the application.
[0029] The positive electrode can be produced, for example, by the following method. First, a positive electrode active material and a conductive assistant are mixed in a mortar to produce a composite, and the composite and a binder, etc. are dispersed in a solvent to prepare a slurry. Next, the positive electrode slurry is applied to one or both surfaces of a positive electrode current collector, and then dried to form a positive electrode active material mixture electrode layer. A positive electrode can be produced by these steps.
[0030] <Negative electrode> The negative electrode is composed of a negative electrode active material and a current collector.
[0031] (Negative electrode active material) In the present invention, the negative electrode active material is limited to metallic lithium and its alloy. The form is used in the form of metal foil, and in the present invention, a thickness of approximately 100 microns or less is preferable. More precisely, the amount of metal foil that corresponds to the unit capacity of the positive electrode side is sufficient, and even 10 microns can be used. Lithium has the largest theoretical capacity of 3851 mAh / g among elements that can be used as an electrode active material for batteries, and has the characteristic of expressing a large capacity even in a small amount.
[0032] (current collector) The current collector is not particularly limited in the present invention, but from the viewpoint of electronic conductivity, copper foil is most suitable, but stainless steel foil, aluminum foil, etc. can also be used.
[0033] The negative electrode can be prepared, for example, by the following method. First, a rolled foil of metallic lithium is prepared, and then it is laminated on a current collector and pressed to prepare the negative electrode. Alternatively, metallic lithium can be provided on the current collector foil by a method such as vacuum deposition.
[0034] <Separator> As the separator interposed between the positive electrode and the negative electrode, a nonwoven fabric or a porous sheet made of a synthetic resin such as a polyolefin resin such as PE (polyethylene) or PP (polypropylene), or PTFE (polytetrafluoroethylene), which are commonly used, or a glass separator, can be used. The nonwoven fabric or the porous sheet may have a single layer or a multilayer structure. Both dry separators and wet separators can be used in the present invention, and the air permeability, lamination state, specific gravity, tensile strength, water absorption rate, etc. can be selected arbitrarily.
[0035] In the present invention, there is no limitation on the material of the separator, but there is a limitation on the porosity, and the second feature described above is effective only when the porosity is 20% or more and 50% or less. The porosity can be adjusted by the stretching rate when the separator is produced.
[0036] Furthermore, in the present invention, since there is a limit to the distance between the positive and negative electrodes, this distance between the positive and negative electrodes is adjusted by the thickness of the separator. Either the distance between the positive and negative electrodes may be set to a specified distance using one separator, or multiple separators may be stacked. The distance between the positive and negative electrodes may also be measured by an X-ray CT scanner, for example, a TOSCANER-32252μhd (manufactured by Toshiba Corporation) that penetrates the inside of the battery and can be measured.
[0037] <Non-aqueous electrolyte> The non-aqueous electrolyte is composed of an electrolyte and an electrolyte solvent, and may also use a diluent in some cases. The types of non-aqueous electrolytes in the present invention are diverse, including those composed of an electrolyte and a solvent like conventional lithium ion batteries, room temperature molten salt electrolytes, and those that generate clusters through the interaction between the electrolyte and the solvent (solvated ionic liquid, concentrated electrolyte system), and any electrolyte can be used.
[0038] The electrolyte is not particularly limited, and lithium salts containing lithium ions generally used in lithium ion secondary batteries can be used in the present invention. For example, lithium salts such as lithium bistrifluorosulfonylamide (LiTFSA), lithium bisfluorosulfonylamide (LiFSA), and LiPF6 can be used. These electrolytes may be used alone or in combination of two or more. The concentration of the lithium salt is not particularly limited, but in the case of an electrolyte solution for a lithium ion battery, it is preferably 0.1 mol / L or more and 2.0 mol / L or less relative to the electrolyte solvent, and in the case of an electrolyte solution that generates clusters, it is generally 2.0 mol / L or more and 5.0 mol / L or less.
[0039] More specifically, in the case of conventional electrolytes such as those for lithium ion batteries, examples of such electrolytes include those containing LiTFSA and / or LiFSA at 0.1 M (mol / L) or more and 2.0 M or less as an electrolyte, and using an ether such as dioxolane or dimethoxyethane as a solvent.
[0040] Examples of the cluster-forming electrolyte include solvated ionic liquids that contain LiTFSA and / or LiFSA at 2.0 mol / L or more and 5.0 mol / L or less and use a medium-chain ether such as triethylene glycol dimethyl ether (G3) and / or tetraethylene glycol dimethyl ether (G4) as a solvent, and examples of the concentrated electrolyte include electrolytes that use sulfolane as a solvent. The lithium-sulfur battery preferably contains at least one of these. It is more preferable that the battery further contains a fluorinated ether.
[0041] Furthermore, in the case of a cluster-forming electrolyte, a diluent may be used. Cluster-forming electrolytes generally have a high viscosity due to their high electrolyte concentration, and there are cases where they cannot penetrate the pores of the separator as is. The reason they are called diluents rather than solvents is that they can reduce the viscosity without destroying the clusters that are formed. Specifically, hydrofluoroethers are used as fluorinated ethers, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether is preferred in the present invention.
[0042] <Terminal> Metal is generally used for the terminals. There is no limitation on the material and shape, but in the present invention, for example, aluminum and copper are preferable as the material, and the shape is preferable so as not to be deformed by wiring or the like.
[0043] <Exterior body> The exterior body may be made of, for example, a can material or a laminate material. There are no restrictions on the material or shape, but for example, stainless steel is suitable for the can material, and aluminum foil coated with a plastic film is suitable for the laminate material. The shape can be changed according to the cell capacity, and generally the larger the cell capacity, the larger the shape.
[0044] The shape of the lithium-sulfur battery of the present invention is not particularly limited, but examples thereof include coin type, button type, sheet type, laminated type, cylindrical type, square type, flat type, and the like.
[0045] (Embodiment 1) Hereinafter, the structure of the lithium-sulfur battery according to the first embodiment of the present invention will be described with reference to the drawings, taking a coin-type lithium-sulfur battery as an example. Fig. 1 is a schematic cross-sectional view of a coin-type battery shown as an example of the lithium-sulfur battery according to the first embodiment of the present invention.
[0046] The coin-type lithium-sulfur battery 1 includes a positive electrode 2, a negative electrode 3, and a separator 4 disposed between the positive electrode 2 and the negative electrode 3. The positive electrode 2, the negative electrode 3, and the separator 4 are housed between a first external terminal 5 located at the lower side of the figure and a second external terminal 6 located at the upper side of the figure. The connection portion between the first external terminal 5 and the second external terminal 6 is insulated by a gasket 7.
[0047] The positive electrode 2 is composed of a positive electrode current collector 21 located on the inner surface of the first external terminal 5 and connected thereto, and a positive electrode layer 22 provided on the surface of the positive electrode current collector 21 facing the separator 4.
[0048] The negative electrode 3 is composed of a negative electrode current collector 31 located on the inner surface of the second external terminal 6 and connected to it, and a negative electrode layer 32 made of metallic lithium provided on the surface of the negative electrode current collector 31 facing the separator 4.
[0049] The separator 4 is impregnated with, for example, a non-aqueous electrolyte.
[0050] The second external terminal 6 is inserted into the first external terminal 5 with its lower end and both side surfaces wrapped in a gasket 7, and the opening end of the first external terminal 5 on the lower side is bent toward the gasket 7 to crimp and fix the second external terminal 6 to the first external terminal 5, and the connection portion of the first external terminal 5 and the second external terminal 6 is insulated by the gasket 7.
[0051] In the first embodiment, by satisfying at least the first condition among the first to third conditions described above, a highly practical lithium-sulfur battery having high cycle performance without degrading voltage characteristics can be obtained.
[0052] (Embodiment 2) Next, a stacked battery as an example of the lithium-sulfur battery according to the second embodiment of the present invention will be described with reference to Fig. 2. Fig. 2 is a schematic cross-sectional view of a stacked battery shown as an example of the lithium-sulfur battery according to the second embodiment of the present invention.
[0053] The laminated lithium-sulfur battery 100 includes a bag-shaped exterior body 200 made of a laminate film. An electrode group 300 having a laminated structure is housed inside the exterior body 200. The laminate film has a structure in which, for example, a plurality of (for example, two) plastic films are laminated with a metal foil such as aluminum foil sandwiched between the films. Of the two plastic films, a heat-sealable resin film is used for one of the plastic films. The exterior body 200 includes two laminate films stacked such that the heat-sealable resin films face each other, houses the electrode group 300 between these laminate films, and seals the two laminate film portions around the electrode group 300 by heat-sealing each other, thereby hermetically housing the electrode group 300.
[0054] The electrode group 300 includes a positive electrode 400, a negative electrode 500, and a separator 600 interposed between the positive electrode 400 and the negative electrode 500. The lithium-sulfur battery 100 has a structure in which a plurality of electrode groups 300 are stacked such that the negative electrode 500 is located in the outermost layer and the separator 600 is located between the negative electrode 500 and the inner surface of the exterior body 200.
[0055] The positive electrode 400 is composed of a positive electrode current collector 410 and a positive electrode layer 420 formed on both sides of the positive electrode current collector 410. The negative electrode 500 is composed of a negative electrode current collector 510 and a negative electrode layer 520 made of metallic lithium formed on both sides of the negative electrode current collector 510.
[0056] The positive electrode 400 has a positive electrode lead 700 in which the positive electrode current collector 410 extends from, for example, the left side surface of the positive electrode layer 420. The positive electrode leads 700 are bundled at the tip side and joined to each other inside the exterior body 200. One end of the positive electrode tab 800 is joined to the joint of the positive electrode lead 700, and the other end extends to the outside through the sealing portion of the exterior body 200.
[0057] The negative electrode 500 has a negative electrode lead 900 in which the negative electrode current collector 510 extends from, for example, the right side surface of the negative electrode layer 520. The negative electrode leads 900 are bundled at their tip sides within the exterior body 200 and joined to each other. One end of the negative electrode tab 1000 is joined to the joint of the negative electrode lead 900, and the other end extends to the outside through the sealing part of the exterior body 200. The nonaqueous electrolyte is injected into the exterior body 200. The injection part of the exterior body 200 is sealed after the injection of the nonaqueous electrolyte.
[0058] In the second embodiment, by satisfying at least the first condition among the above-mentioned first to third points, a highly practical lithium-sulfur battery having high cycle performance without degrading the voltage characteristics can be obtained. EXAMPLES
[0059] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The various properties (Properties 1 and 2) of the polyolefin microporous membrane of the present invention were evaluated by the following test methods. 1. Film thickness (μm) Measure using a micrometer at an ambient temperature of 23±2°C. 2.Porosity (%) A rectangular sample of X cm × Y cm was cut out and calculated using the following formula (1). Porosity={1-(10000×M / ρ) / (X×Y×T)}×100 (1) In the above formula (1), T is the sample thickness (μm), M is the sample weight (g), and ρ is the density of the resin.
[0060] <Example 1> (1) Preparation of electrolyte 4.0 g of LiTFSA and 3.3 g of sulfolane were mixed and stirred overnight. The salt concentration at this time was 3.0 mol / L. Then, 12.0 g of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether was added as a diluent to prepare an electrolyte solution.
[0061] (2) Preparation of sulfur complex 10 g each of cyclic elemental sulfur (S8) and mesoporous carbon material (CNovel (registered trademark) MH00 manufactured by Toyo Tanso Co., Ltd.) were put into a grinder and mixed overnight. The mixture was then transferred to a heat-resistant container and heated in an oven at 165°C for 10 hours to obtain a sulfur composite (cathode composite).
[0062] (3) Preparation of sulfur electrode The sulfur composite, conductive material, and binder prepared above were mixed in a ball mill using water as a solvent to prepare a sulfur electrode slurry. At this time, the conductive material was Denka Black (registered trademark, manufactured by Denka) and the binder was a mixture of SBR (manufactured by JSR) and CMC (Sunrose, Nippon Paper Industries Co., Ltd.), with the mixing ratio of sulfur composite:conductive material:binder being 90:10:10 by weight. The prepared sulfur electrode slurry was applied to an aluminum current collector and then dried to prepare a sulfur electrode.
[0063] (4) Preparation of metallic lithium electrode A 50-micron-thick layer of metallic lithium was attached to a 10-micron-thick copper foil serving as a negative electrode current collector, and pressed to produce a metallic lithium electrode.
[0064] (5) Fabrication of lithium-sulfur battery (coin cell type) In an atmosphere with a dew point of -50°C or less, a sulfur electrode, a metallic lithium electrode, two polyethylene separators (total thickness 50 microns, porosity 40%, DP value 1.3), and a nonaqueous electrolyte were placed inside the coin cell exterior body, and the top lid was then placed on the battery. The battery was then crimped around the periphery using a crimping machine to produce a coin-shaped lithium-sulfur battery (2032 type), which was designated as Example 1.
[0065] (6) Charge / discharge test A charge / discharge test was performed using a charge / discharge tester (TOSCAT-3000) manufactured by Toyo Systems Co., Ltd. The discharge capacity was measured by discharging the lithium-sulfur battery of Example 1 at a constant current of 0.1C to 1.0V, and the discharge capacity was calculated to be 1195mAh / g from the time to reach 1.0V, the current value, and the weight of sulfur in the sulfur electrode. In addition, the cycle test was performed by taking a 15-minute break after the above discharge, followed by a constant current / constant voltage charge at 0.1C and 3.0V, and then taking another 15-minute break, which was defined as one cycle. The discharge capacity retention rate after 50 cycles was 80%, and the average discharge voltage at the 50th cycle was 1.82V. The discharge capacity retention rate and the average discharge voltage were calculated using the following formulas.
[0066] The physical properties and test results of Example 1 are shown in Table 1. [Table 1]
[0067] <Example 2> A lithium-sulfur battery was prepared in the same manner as in Example 1, except that three polyethylene separators (total thickness 75 microns, porosity 40%, DP value 1.9) were used, and designated as Example 2. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1182 mAh / g, the discharge capacity retention rate was 83%, and the average discharge voltage was 1.77 V. The physical properties and test results in Example 2 are shown in Table 1.
[0068] <Example 3> A lithium-sulfur battery was prepared as Example 3 in the same manner as in Example 1, except that four polyethylene separators (total thickness 100 microns, porosity 40%, DP value 2.5) were used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1177 mAh / g, the discharge capacity retention rate was 87%, and the average discharge voltage was 1.70 V. The physical properties and test results in Example 3 are shown in Table 1.
[0069] <Example 4> A lithium-sulfur battery was prepared as Example 4 in the same manner as in Example 1, except that one polyethylene separator (total thickness 25 microns, porosity 40%, DP value 0.6) was used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1250 mAh / g, the discharge capacity retention rate was 72%, and the average discharge voltage was 1.88 V. The physical properties and test results in Example 4 are shown in Table 1.
[0070] <Example 5> A lithium-sulfur battery was prepared as Example 5 in the same manner as in Example 1, except that two polyethylene separators (total thickness 50 microns, porosity 50%, DP value 1.0) were used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1202 mAh / g, the discharge capacity retention rate was 73%, and the average discharge voltage was 1.79 V. The physical properties and test results of Example 5 are shown in Table 1.
[0071] <Example 6> A lithium-sulfur battery was prepared as Example 6 in the same manner as in Example 1, except that three polyethylene separators (total thickness 75 microns, porosity 50%, DP value 1.5) were used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1190 mAh / g, the discharge capacity retention rate was 75%, and the average discharge voltage was 1.75 V. The physical properties and test results of Example 6 are shown in Table 1.
[0072] <Example 7> A lithium-sulfur battery was prepared as Example 7 in the same manner as in Example 1, except that four polyethylene separators (total thickness 100 microns, porosity 50%, DP value 2.0) were used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1188 mAh / g, the discharge capacity retention rate was 78%, and the average discharge voltage was 1.70 V. The physical properties and test results of Example 7 are shown in Table 1.
[0073] <Example 8> A lithium-sulfur battery was prepared in the same manner as in Example 1, except that one polyethylene separator (total thickness 25 microns, porosity 50%, DP value 0.5) was used, and designated as Example 8. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1154 mAh / g, the discharge capacity retention rate was 70%, and the average discharge voltage was 1.88 V. The physical properties and test results of Example 8 are shown in Table 1.
[0074] <Example 9> A lithium-sulfur battery was prepared as Example 9 in the same manner as in Example 1, except that one polyethylene separator (total thickness 25 microns, porosity 20%, DP value 1.3) was used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1178 mAh / g, the discharge capacity retention rate was 81%, and the average discharge voltage was 1.73 V. The physical properties and test results of Example 9 are shown in Table 1.
[0075] <Example 10> A lithium-sulfur battery was prepared as Example 10 in the same manner as in Example 1, except that two polyethylene separators (total thickness 32 microns, porosity 50%, DP value 0.6) were used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1158 mAh / g, the discharge capacity retention rate was 76%, and the average discharge voltage was 1.87 V. The physical properties and test results of Example 10 are shown in Table 1.
[0076] <Example 11> A lithium-sulfur battery was prepared as Example 11 in the same manner as in Example 1, except that one polyethylene separator (total thickness 20 microns, porosity 10%, DP value 2.0) was used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1058 mAh / g, the discharge capacity retention rate was 85%, and the average discharge voltage was 1.70 V. The physical properties and test results of Example 11 are shown in Table 1.
[0077] <Example 12> A lithium-sulfur battery was prepared in the same manner as in Example 1, except that two polyethylene separators (total thickness 50 microns, porosity 60%, DP value 0.8) were used, and designated as Example 12. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1255 mAh / g, the discharge capacity retention rate was 70%, and the average discharge voltage was 1.86 V. The physical properties and test results of Example 12 are shown in Table 1.
[0078] <Example 13> A lithium-sulfur battery was prepared in the same manner as in Example 1, except that five polyethylene separators (total thickness 125 microns, porosity 60%, DP value 2.1) were used, and designated as Example 13. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1176 mAh / g, the discharge capacity retention rate was 72%, and the average discharge voltage was 1.71 V. The physical properties and test results of Example 13 are shown in Table 1.
[0079] <Example 14> A lithium-sulfur battery was prepared in the same manner as in Example 1, except that one polyethylene separator (total thickness 16 microns, porosity 10%, DP value 1.6) was used, and designated as Example 14. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1105 mAh / g, the discharge capacity retention rate was 83%, and the average discharge voltage was 1.73 V. The physical properties and test results of Example 14 are shown in Table 1.
[0080] <Example 15> A lithium-sulfur battery was prepared in the same manner as in Example 1, except that 1.0 M LiTFSA and dioxolane / dimethoxyethane (1:1 volume ratio) with 0.1 wt% lithium nitrate added was used as the electrolyte, and this was designated Example 15. A charge / discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1304 mAh / g, the discharge capacity retention rate was 73%, and the average discharge voltage was 1.93 V. The physical properties and test results of Example 15 are shown in Table 1.
[0081] <Conventional example> A lithium-sulfur battery was fabricated as a conventional example in the same manner as in Example 1, except that one polyethylene separator (total thickness 16 microns, porosity 50%, DP value 0.3) was used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1350 mAh / g, the discharge capacity retention rate was 48%, and the average discharge voltage was 1.86 V. The physical properties and test results of the conventional example are shown in Table 1.
[0082] <Comparative Example 1> A lithium-sulfur battery was prepared in the same manner as in Example 1, except that five polyethylene separators (total thickness 125 microns, porosity 40%, DP value 3.1) were used, and this battery was designated Comparative Example 1. A charge-discharge test was carried out in the same manner as in Example 1, and the battery had a discharge capacity of 1200 mAh / g, a discharge capacity retention rate of 80%, and an average discharge voltage of 1.60 V. The physical properties and test results of Comparative Example 1 are shown in Table 1.
[0083] <Comparative Example 2> A lithium-sulfur battery was prepared as Comparative Example 2 in the same manner as in Example 1, except that two polyethylene separators (total thickness 50 microns, porosity 10%, DP value 5.0) were used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1089 mAh / g, the discharge capacity retention rate was 90%, and the average discharge voltage was 1.51 V. The physical properties and test results in Comparative Example 2 are shown in Table 1.
[0084] <Comparative Example 3> A lithium-sulfur battery was prepared as Comparative Example 3 in the same manner as in Example 1, except that one polyethylene separator (total thickness 25 microns, porosity 60%, DP value 0.4) was used. A charge-discharge test was carried out in the same manner as in Example 1, and the discharge capacity was 1322 mAh / g, the discharge capacity retention rate was 65%, and the average discharge voltage was 1.90 V. The physical properties and test results of Comparative Example 3 are shown in Table 1.
[0085] As shown in Table 1, the initial discharge capacity was 1000-1400mAh / g at all levels, so there was no problem in preparing the test cells, and it is believed that the difference in capacity retention rate and average discharge voltage after 50 cycles depends on the DP value. In Examples 1-14, the capacity retention rate was 70-90%, and the average discharge voltage was 1.70V or more. The present invention aims to provide a highly practical lithium-sulfur battery that improves cycle characteristics without lowering voltage characteristics, and this has been proven. When the DP value is less than 0.5, the capacity retention rate is low, and it is believed that the redox shuttle phenomenon occurred. When the DP value is greater than 2.5, the average voltage is low, and it is believed that the electrolyte resistance is too high, causing a voltage drop.
[0086] In particular, when the initial discharge capacity was considered to be better if it was 1178 (mAh / g) or higher, the retention rate was considered to be better if it was 73% or higher, and the average voltage was considered to be better if it was 1.73V or higher, it was shown that all values were good when the DP value was between 1.0 and 1.5.
[0087] The conventional example is an example where the general structure of a lithium-ion battery is applied to a lithium-sulfur battery. In recent years, lithium-ion batteries have been increasingly required to have high output for in-vehicle applications, and the trend has been to make the separator thinner in order to reduce electrolyte resistance. However, lithium-sulfur batteries have an element not found in lithium-ion batteries, namely the elution of polysulfides from the positive electrode, which is thought to be the direct cause of the decrease in capacity retention. In the conventional example, a separator with a porosity of 50% was used, but even if it were 40%, a significant decrease in capacity retention would have been unavoidable, and this result shows how important it is to set the DP value.
[0088] Comparative Example 1 is an example in which five separators were inserted. Since the initial discharge capacity was 1200mAh / g and the capacity retention rate after 50 cycles was 80%, it is considered that the effect of the distance between the positive and negative electrodes on these performances is small at a low discharge rate such as 0.1C. However, the average discharge voltage after 50 cycles was 1.60V, which was extremely lower than other levels, and the result was not a highly practical lithium-sulfur battery. Although the effect of polysulfide was suppressed to a small level by inserting five separators, on the contrary, the interelectrode resistance became too large, resulting in a battery that had capacity but did not produce the essential voltage. In this respect, too, it can be said that the result shows how important it is to set the DP value.
[0089] From the above, it has been found that by specifying the value obtained by dividing the distance between the positive and negative electrodes by the porosity of the separator (hereinafter referred to as the DP value) in lithium-sulfur batteries as 0.5 to 2.5, it is possible to improve cycle performance without sacrificing voltage characteristics. This makes it possible to expect use of the battery in a wide range of fields, including mobility applications such as electric vehicles and drones, as well as natural energy storage applications. [Explanation of symbols]
[0090] REFERENCE SIGNS LIST 1 Lithium-sulfur battery, 2 Positive electrode, 3 Negative electrode, 4 Separator, 5 First external terminal, 6 Second external terminal, 7 Gasket, 21 Positive electrode current collector, 22 Positive electrode layer, 31 Negative electrode current collector, 32 Negative electrode layer, 100 Laminated lithium-sulfur battery, 200 Exterior body, 300 Electrode group, 400 Positive electrode, 500 Negative electrode, 600 Separator, 410 Positive electrode current collector, 420 Positive electrode layer, 510 Negative electrode current collector, 520 Negative electrode layer, 700 Positive electrode lead, 800 Positive electrode tab, 900···Negative lead, 1000···Negative tab
Claims
1. A lithium-sulfur battery having a structure in which an electrode using elemental sulfur and / or a sulfur compound as an electrode active material is used as a positive electrode, and an electrode using metallic lithium and / or an alloy thereof as an electrode active material is used as a negative electrode, and further in which the positive and negative electrodes are separated by a separator, wherein the DP value, obtained by dividing the distance (microns) between the positive and negative electrodes by the porosity (%) of the separator, is 0.5 or more and 2.5 or less.
2. 2. The lithium-sulfur battery according to claim 1, wherein the DP value is 1.0 or more and 1.5 or less.
3. 2. The lithium-sulfur battery according to claim 1, wherein the separator has a porosity of 20% or more and 50% or less.
4. 2. The lithium-sulfur battery according to claim 1, wherein the distance between the positive and negative electrodes is 25 microns or more and 100 microns or less.
5. 2. The lithium-sulfur battery according to claim 1, wherein the distance between the positive and negative electrodes is 32 microns or more and 100 microns or less.
6. The lithium-sulfur battery according to claim 1, characterized in that it contains lithium bistrifluorosulfonylamide (LiTFSA) and / or lithium bisfluorosulfonylamide (LiFSA) as a lithium salt, at least one selected from triethylene glycol dimethyl ether (G3), tetraethylene glycol dimethyl ether (G4) and sulfolane as a solvent, and further contains a fluorinated ether.
Citation Information
Patent Citations
Lithium-sulfur battery
JP2014523083A
lithium-sulphur battery
JP2017526109A
Separator containing laser-induced graphene carbonized layer and lithium-sulfur battery containing the separator
JP2019515478A
Electrolyte for lithium sulfur battery
JP2022155874A
Microporous membranes made of polyolefin and methods for evaluating them
JP4780960B2