Substrate for semiconductor device

By using Ni-P with controlled magnetic properties in the external electrode, the semiconductor device minimizes magnetic interference on sensitive elements, improving reliability and reducing costs through optimized magnetic flux and coercive force management.

JP2024135343APending Publication Date: 2024-10-04MAXELL LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023045972
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing semiconductor devices with non-magnetic Ni-P external electrodes may still suffer adverse magnetic effects on sensitive semiconductor elements, despite being categorized as non-magnetic, due to the inclusion of paramagnetic, diamagnetic, or antiferromagnetic materials.

Method used

The external electrode main body is formed with Ni-P having specific magnetic properties, including an amplitude relative magnetic permeability of 4.0 or less, maximum magnetic flux density of 7.0 mT or less, residual magnetic flux density of 0.10 mT or less, and coercive force of 23 A/m or less, to minimize magnetic influence on semiconductor elements.

Benefits of technology

This configuration effectively prevents the external electrode from becoming magnetized and reduces magnetic flux density, thereby protecting sensitive semiconductor elements from malfunction or accuracy deterioration, enhancing device reliability and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135343000001_ABST
    Figure 2024135343000001_ABST
Patent Text Reader

Abstract

To reduce the adverse effects of the magnetism of an external electrode main body on a semiconductor element even when the semiconductor element is highly sensitive in a substrate for a semiconductor device.SOLUTION: An external electrode 3 includes a third surface layer 7 formed on the surface of a substrate 16, an external electrode main body 9 formed on the surface of the third surface layer 7, and a fourth surface layer 13 formed on the surface of the external electrode main body 9. The external electrode main body 9 of the external electrode 3 is made of nonmagnetic Ni-P, and the amplitude specific permeability of the Ni-P is 4.0 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a substrate for a semiconductor device having external electrodes formed on the substrate. [Background technology]

[0002] In the substrate for a semiconductor device of the present invention, the external electrode main body of the external electrode is made of Ni-P, which is disclosed in Patent Document 1. The external electrode of the substrate for a semiconductor device in Patent Document 1 comprises a third surface layer formed on the substrate, an external electrode main body formed on the surface of the third surface layer, and a fourth surface layer formed on the surface of the external electrode main body, and the external electrode main body of the external electrode is made of non-magnetic Ni-P. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2021-145060 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the semiconductor device of Patent Document 1, since the external electrode main body of the external electrode is formed of nonmagnetic Ni-P, it is expected that even if the semiconductor element mounted on the board is easily sensitive to magnetism, the adverse magnetic effects on the semiconductor element can be minimized. However, in general, the term "nonmagnetic material" is a general term for materials that are not ferromagnetic, and includes paramagnetic materials, diamagnetic materials, antiferromagnetic materials, etc., so that even if the external electrode main body is formed of "nonmagnetic" material as described above, depending on the sensitivity of the semiconductor element mounted on the board, the magnetism may have a significant adverse effect on the semiconductor element.

[0005] The present invention has been made with the aim of solving the problems associated with conventional substrates for semiconductor devices as described above, and its object is to minimize the adverse effects that the magnetism of the external electrode main body portion has on a semiconductor element in a substrate for semiconductor device in which the external electrode main body portion of the external electrode is formed of Ni-P, even if the semiconductor element is highly sensitive. [Means for solving the problem]

[0006] The present invention is directed to a substrate for a semiconductor device, on the surface of which an external electrode 3 connected to a semiconductor element 1 is formed. The external electrode 3 comprises a third surface layer 7 formed on the surface of the substrate 16, an external electrode main body 9 formed on the surface of the third surface layer 7, and a fourth surface layer 13 formed on the surface of the external electrode main body 9. The external electrode main body 9 of the external electrode 3 is made of nonmagnetic Ni-P, and is characterized in that the amplitude specific permeability of the Ni-P is 4.0 or less.

[0007] The amplitude specific permeability of Ni-P is preferably 2.0 or more and 4.0 or less, and more preferably 2.3 or more and 3.1 or less.

[0008] The maximum magnetic flux density of Ni-P is 7.0 mT or less.

[0009] The maximum magnetic flux density of Ni-P is preferably 4.0 mT or more and 7.0 mT or less, and more preferably 4.7 mT or more and 6.2 mT or less.

[0010] The residual magnetic flux density of Ni-P is less than 0.10 mT.

[0011] The residual magnetic flux density of Ni-P is preferably 0.04 mT or more and 0.10 mT or less, and more preferably 0.048 mT or more and 0.066 mT or less.

[0012] The coercive force of Ni-P is less than 23 A / m.

[0013] The coercive force of Ni-P is preferably 10 A / m or more and 23 A / m or less, and more preferably 11 A / m or more and 21 A / m or less. Effect of the Invention

[0014] When the amplitude ratio magnetic permeability of Ni-P forming the external electrode main body 9 is 4.0 or less as in the present invention, the external electrode main body 9 can be prevented from being easily magnetized even when a magnetic field is applied to the external electrode main body 9 due to an external factor or the like. This can effectively prevent the semiconductor element 1 from being adversely affected by the magnetism emitted from the external electrode main body 9 that would otherwise be caused by the external electrode main body 9 being magnetized and reaching the semiconductor element 1. More specifically, it can effectively prevent the semiconductor element 1 from being adversely affected by the magnetism emitted from the external electrode main body 9, such as the semiconductor element 1 being malfunctioned due to high sensitivity, or the semiconductor element 1 being a magnetic sensor and having a deteriorated detection accuracy.

[0015] The amplitude specific magnetic permeability of Ni-P is preferably 2.0 or more and 4.0 or less. Also, the amplitude specific magnetic permeability of Ni-P is more preferably 2.3 or more and 3.1 or less. This makes it possible to prevent the external electrode main body 9 from being easily magnetized even when a magnetic field is applied to the external electrode main body 9.

[0016] If the maximum magnetic flux density of the Ni-P forming the external electrode main body 9 is 7.0 mT or less, even if the external electrode main body 9 is magnetized due to an external factor, etc., the magnetic flux density when the external electrode main body 9 is magnetically saturated can be made small. As a result, even if the magnetism generated by the external electrode main body 9 affects the semiconductor element 1, the adverse effect of this on the semiconductor element 1 can be kept as small as possible.

[0017] The maximum magnetic flux density of Ni-P is preferably 4.0 mT or more and 7.0 mT or less. Also, the maximum magnetic flux density of Ni-P is more preferably 4.7 mT or more and 6.2 mT or less. This makes it possible to reduce the magnetic flux density when the external electrode main body 9 is magnetically saturated, even if the external electrode main body 9 is magnetized.

[0018] It is preferable that the residual magnetic flux density of the Ni-P that forms the external electrode main body 9 is 0.10 mT or less, which makes it possible to reduce the magnetic force remaining in the magnetized external electrode main body 9, thereby minimizing the adverse effects of the magnetism originating from the external electrode main body 9 on the semiconductor element 1 as much as possible.

[0019] The residual magnetic flux density of Ni-P is preferably 0.04 mT or more and 0.10 mT or less. Also, the residual magnetic flux density of Ni-P is more preferably 0.048 mT or more and 0.066 mT or less. This allows the magnetic force remaining in the magnetized external electrode main body 9 to be reduced.

[0020] It is preferable that the coercive force of the Ni-P forming the external electrode main body 9 is 23 A / m or less, which allows the magnetic force remaining in the magnetized external electrode main body 9 to be eliminated by a small magnetic field, thereby minimizing the adverse effects of the magnetism originating from the external electrode main body 9 on the semiconductor element 1 as much as possible.

[0021] The coercive force of Ni-P is preferably 10 A / m or more and 23 A / m or less. Also, the coercive force of Ni-P is more preferably 11 A / m or more and 21 A / m or less. This allows the magnetic force remaining in the magnetized external electrode main body 9 to be eliminated with a smaller magnetic field. [Brief description of the drawings]

[0022] [Figure 1] 1 is a vertical sectional front view of a semiconductor device in which a semiconductor element is mounted on a substrate for a semiconductor device according to an embodiment of the present invention. [Diagram 2] 2 is a perspective view of the semiconductor device as viewed from the bottom side; FIG. [Diagram 3] 1(a) to 1(f) are explanatory views showing a manufacturing process of a substrate for a semiconductor device according to an embodiment of the present invention. [Figure 4] 1A to 1D are explanatory views showing a manufacturing process of a semiconductor device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] 1 to 4 show a semiconductor device substrate according to an embodiment of the present invention, a manufacturing process thereof, and a semiconductor device having a semiconductor element 1 mounted on the semiconductor device substrate. As shown in FIG. 1, the semiconductor device is configured by sealing a semiconductor element 1 that is sensitive to magnetism (easily affected by magnetic fields), a mounting pad 2 and six external electrodes 3 exposed on a mounting surface S of the semiconductor device, and a wire 4 that electrically connects the semiconductor element 1 and the external electrodes 3 inside an insulating resin (sealing material) 5, and is used as a unit electronic component (semiconductor device) for surface mounting. The mounting pad 2 is disposed at the center of the mounting surface S of the semiconductor device, and the external electrodes 3 are disposed in a linear row of three electrodes each, with the mounting pad 2 sandwiched between them. The semiconductor device is formed in a flat rectangular parallelepiped shape.

[0024] As shown in FIG. 1, the mounting pad 2 and the external electrode 3 each include a first surface layer 6 and a third surface layer 7 exposed on the mounting surface S of the semiconductor device, a mounting pad main body 8 continuous with the first surface layer 6, an external electrode main body 9 continuous with the third surface layer 7, and a second surface layer 12 and a fourth surface layer 13 covering the surfaces of both main bodies 8 and 9. The mounting pad main body 8 and the external electrode main body 9 are each formed of nonmagnetic Ni-P, and each of the surface layers 6, 7, 12, and 13 is composed of a single layer made of one type of nonmagnetic metal (precious metal) such as gold, silver, palladium, and tin, or a layer in which two or more types of metal (precious metal) are laminated. In this embodiment, the first surface layer 6 and the third surface layer 7 exposed on the mounting surface S are made of gold, and the second surface layer 12 and the fourth surface layer 13 covering the surfaces of both main bodies 8 and 9 are made of silver.

[0025] The semiconductor device is formed through a process of forming a substrate for a semiconductor device and a process of mounting a semiconductor element 1 on the substrate for a semiconductor device. The substrate for a semiconductor device is formed through a resist patterning process of forming a pattern resist 21 on the surface of a substrate 16, a first metal layer forming process of forming a first surface layer 6 and a third surface layer 7 on the surface of the substrate 16 using the pattern resist 21 formed in the resist patterning process, a body forming process of forming a mounting pad main body 8 and an external electrode main body 9 on the surfaces of the first surface layer 6 and the third surface layer 7, and a second metal layer forming process of forming a second surface layer 12 and a fourth surface layer 13 on the surfaces of the mounting pad main body 8 and the external electrode main body 9. After this, the semiconductor device is completed through a mounting process of a semiconductor element 1, a bonding process using a wire 4, a resin sealing process, a substrate peeling process, and a dicing process. The manufacturing process of the substrate for a semiconductor device and the semiconductor device will be outlined below.

[0026] As shown in Fig. 3(a), in the resist patterning process, a photosensitive film resist is laminated on the surface of a substrate 16 formed of a conductive metal plate to form a resist layer 17, a pattern film 18 is attached to the surface of the resist layer 17, and ultraviolet light is irradiated from an ultraviolet lamp 19 to expose the resist layer 17. At this time, the ultraviolet light is irradiated to the resist layer 17 facing the light transmitting hole 20 formed in the pattern film 18, and the exposed resist layer 17 is hardened. The unexposed parts of the resist layer 17 shielded by the pattern film 18 are dissolved and removed by development, and only the exposed parts remain on the substrate 16 as shown in Fig. 3(b), forming a pattern resist 21 having through holes for forming the mounting pads 2 and the external electrodes 3 between the exposed parts.

[0027] As shown in FIG. 3(c), in the first metal layer forming step, the substrate 16 that has been subjected to pre-plating treatment (degreasing, acid immersion, oxide film removal, activation, chemical etching, electrolytic treatment, strike plating, etc.) is immersed in an electroforming tank, and gold is electroformed (plated) on the substrate 16 exposed to the pattern resist 21 to form the first surface layer 6 and the third surface layer 7. At this time, the thickness of the first surface layer 6 and the third surface layer 7 is preferably 0.04 μm or more and 1.0 μm or less, and in this embodiment, the electroforming (plating) time was adjusted so that the thickness is 0.1 μm. If the thickness of the first surface layer 6 and the third surface layer 7 is less than 0.04 μm, the solder wettability during mounting of the semiconductor device is poor. In addition, the adhesion between the Ni-P layer (mounting pad main body 8 and external electrode main body 9) and the substrate 16 becomes too strong, which may make it difficult to peel and remove the substrate 16. Furthermore, if the thickness of the first surface layer 6 and the third surface layer 7 exceeds 1.0 μm, the solder joint strength of the mounted semiconductor device may deteriorate.

[0028] In the next main body forming step, as shown in FIG. 3(d), the substrate 16 is again immersed in the electroforming tank, and the surface sides of the surface layers 6 and 7 are electroplated with Ni-P to form the mounting pad main body 8 and the external electrode main body 9. At this time, by adjusting the electroforming (plating) processing time, overhangs 10 and 11 can be formed on the upper parts of the mounting pad main body 8 (mounting pad 2) and the external electrode main body 9 (external electrode 3). The overhangs 10 and 11 are formed by electroforming (plating) each of the main bodies 8 and 9 beyond the thickness of the resist layer 17 in the main body forming step, and the peripheral parts (tip parts) of the overhangs 10 and 11 are formed to protrude toward the previously hardened resist layer 17. Note that if the Ni-P layer is directly formed on the surface of the substrate 16 without forming the first surface layer 6 or the third surface layer 7, the Ni-P layer and the substrate 16 will adhere strongly to each other, making it difficult to peel off and remove the substrate 16.

[0029] The surface roughness (arithmetic mean roughness Ra) of the mounting pad body 8 of the mounting pad 2 and the external electrode body 9 of the external electrode 3, which are formed of a Ni-P layer, is 0.2 to 0.3 μm, and by forming the second surface layer 12 and the fourth surface layer 13 formed on the surface of each body 8 and 9 to be thin, the surface state of each surface layer 12 and 13 appears in accordance with the surface of each body 8 and 9. Incidentally, as the surface roughness of the second surface layer 12 and the fourth surface layer 13 decreases (becomes smoother), the mountability of the semiconductor element 1 on the mounting pad 2 improves, but the adhesion to the resin 5 deteriorates. Conversely, as the surface roughness increases (becomes rougher), the adhesion to the resin 5 improves, but the bonding ability when electrically connecting the electrode of the semiconductor element 1 and the external electrode 3 deteriorates. In addition, when the mounting pad main body and the external electrode main body are formed of Ni, the surface roughness (arithmetic mean roughness Ra) of each surface layer is 0.3 to 0.5 μm, and the surfaces of the mounting pad 2 and the external electrode 3 formed of a Ni-P layer are slightly smoother.

[0030] In the next second metal layer forming step, as shown in FIG. 3(e), the surface of each of the main body parts 8 and 9 is electroformed (plated) with silver to form the second surface layer 12 and the fourth surface layer 13. At this time, the thickness of each of the surface layers 12 and 13 is preferably 1.5 μm or more and 6.0 μm or less, and in this embodiment, the electroforming (plating) time is adjusted so that the thickness is 2 μm. If the thickness of each of the surface layers 12 and 13 is less than 1.5 μm, the bondability is deteriorated, and if the thickness of each of the surface layers 12 and 13 exceeds 6.0 μm, there is a disadvantage in that the cost increases. Note that, if it is difficult to form the surface layers 12 and 13 in close contact with the surfaces of the main body parts 8 and 9, it is preferable to perform a plating pretreatment on the surfaces of each of the main body parts 8 and 9 before electroforming (plating) the surface layers 12 and 13 to improve the adhesion of each of the surface layers 12 and 13 to each of the main body parts 8 and 9. The mounting pad main body 8 and the external electrode main body 9 are preferably formed so that the total thickness T1 of the mounting pad 2 and the external electrode 3 is within a range of 20 to 100 μm, and in this embodiment, they are formed so that the total thickness T1 of the mounting pad 2 and the external electrode 3 is 40 μm. If the second surface layer 12 and the fourth surface layer 13 are thin, the effect on the magnetic sensor (semiconductor element 1) is small. However, the degree of the effect on the magnetic sensor (semiconductor element 1) may vary depending on the characteristics of the semiconductor element 1 and the thickness and area of ​​each of the surface layers 12 and 13.

[0031] By removing the resist layer 17 remaining on the blank of the semiconductor device substrate obtained through the second metal layer forming process, a semiconductor device substrate having the mounting pad 2 and the external electrode 3 formed on the substrate 16 can be obtained as shown in FIG. 3(f). When the hardness of each of the main body parts 8 and 9 of the semiconductor device substrate was measured, the Vickers hardness of the mounting pad main body part 8 and the external electrode main body part 9 was 400 to 600 HV. In addition, a shear strength test of the mounting pad 2 and the external electrode 3 was performed on the semiconductor device substrate from which the resist layer 17 was removed to confirm the degree of adhesion between the mounting pad 2 and the external electrode 3 and the substrate 16. In the shear strength test, after the substrate 16 is fixed, a shear tool is applied to the peripheral side surfaces of the mounting pad 2 and the external electrode 3, and a force parallel to the substrate 16 is applied to the shear tool to measure the load when the mounting pad 2 and the external electrode 3 fall off the substrate 16. The target value of the shear strength of the semiconductor device substrate of this embodiment is 100 to 500 g, and the average load of the measurement result was 297 g. The shear strength of a conventional semiconductor device substrate in which the mounting pad main body and the external electrode main body are made of Ni is 324g in average load, and therefore it is possible to exhibit approximately the same shear strength. If the adhesive strength between the mounting pad 2 and the external electrode 3 and the substrate 16 is small, the mounting pad 2 and the external electrode 3 may fall off the substrate 16 when mounting the semiconductor element 1, when performing bonding processing, when performing resin sealing processing, etc. Also, if the adhesive strength between the mounting pad 2 and the external electrode 3 and the substrate 16 is too large, it becomes difficult to peel off and remove the substrate 16.

[0032] In the mounting process of the semiconductor element 1 on the semiconductor device substrate obtained as described above, as shown in FIG. 4(a), the semiconductor element 1 is fixed on the mounting pad 2 with a bonding material (solder, paste, tape, die attach film, etc.) interposed therebetween, and as shown in FIG. 4(b), the electrodes on the upper surface of the semiconductor element 1 and the external electrodes 3 are connected with wires 4 made of thin wires such as gold or copper. After the bonding process is completed by electrically connecting the semiconductor element 1 and the external electrodes 3, the process proceeds to the resin sealing process. In the resin sealing process, the front side of the substrate 16 is attached to a molding die that serves as the upper die, the substrate 16 serves as the lower die, and a thermosetting epoxy resin is injected into the molding die and heated to harden. At this time, as shown in FIG. 4(c), a large number of combinations of the mounting pad 2 and a plurality of external electrodes 3 that form one semiconductor device are uniformly sealed in an aligned state on the substrate 16, and a large number of semiconductor devices are connected.

[0033] Next, as shown in FIG. 4(d), the substrate 16 is removed, so that the back side of the mounting pad 2 (first surface layer 6) and the external electrode 3 (third surface layer 7) are exposed at the bottom (mounting surface S) of each semiconductor device. The substrate 16 is removed, for example, by physically peeling the substrate 16 off from the semiconductor device. By using a stainless steel material with excellent strength and peelability as the substrate 16, the substrate 16 can be quickly peeled off and removed by peeling it off from the semiconductor device. In addition, when the substrate 16 is made of another metal material, for example, a copper material, the substrate 16 can be removed by immersing the substrate 16 in an etching solution to dissolve it. Then, a dicing process (cutting process) is performed to obtain the semiconductor device.

[0034] As described above, in the semiconductor device of the above embodiment, the mounting pad main body 8 of the mounting pad 2 and the external electrode main body 9 of the external electrode 3 are each formed of nonmagnetic Ni-P, so that the structures of the mounting pad main body 8 and the external electrode main body 9 can be simplified compared to a conventional semiconductor device in which a nonmagnetic Ni-P layer is formed on the surface layer by electroless plating, a Cu layer with an overhang is formed on the Ni-P layer, and a thin Au layer is further formed on the Cu layer. Furthermore, since the mounting pad main body 8 and the external electrode main body 9 are entirely formed of nonmagnetic Ni-P, it is possible to eliminate (demagnetize) the magnetic sensitivity of both (the mounting pad main body 8 and the external electrode main body 9), so that even if a semiconductor device including a magnetically sensitive semiconductor element 1, such as a magnetic sensor, is configured, it is possible to prevent magnetic influence, which contributes to improving the reliability of the semiconductor device.

[0035] Since the mounting pad body 8 of the mounting pad 2 and the external electrode body 9 of the external electrode 3 are each formed from an electrolytic plating layer of Ni-P, it is possible to reduce the number of plating steps for forming the mounting pad 2 and the external electrode 3 compared to conventional semiconductor devices, and accordingly the semiconductor device can be provided at even lower cost.

[0036] The Vickers hardness of the mounting pad main body 8 of the mounting pad 2 and the external electrode main body 9 of the external electrode 3 is preferably 400 to 600 HV. By forming the mounting pad main body 8 and the external electrode main body 9 to have a Vickers hardness in the range of 400 to 600 HV, the strength (rigidity) of the mounting pad 2 and the external electrode 3 can be ensured, and even if the mounting pad 2 and the external electrode 3 are formed thinner than conventional products, the mounting pad 2 and the external electrode 3 can be prevented from falling off. The total thickness T1 of each of the mounting pad 2 and the external electrode 3 is preferably 20 to 100 μm. If the total thickness T1 of the mounting pads 2 and the external electrodes 3 is less than 20 μm, the contact area with the resin 5 will be small, and there is a risk that the mounting pads 2 and the external electrodes 3 will fall off when the substrate 16 is physically peeled off or in the completed semiconductor device. If the total thickness T1 of the mounting pads 2 and the external electrodes 3 exceeds 100 μm, it will take time to form the mounting pads 2 and the external electrodes 3, resulting in poor productivity (cost).

[0037] (Magnetic analysis) The magnetic properties of the external electrode main body 9 of the external electrode 3 according to the above embodiment were measured. The measurement device, measurement conditions, etc. were as follows. Equipment: BH-Analyzer Model number: SY-8219 (manufactured by Iwasaki Electric Co., Ltd.) Measurement conditions: Empty toroidal core SY-513 Ni-P powder and Ni powder as a comparison example were analyzed (filling ratio 17-19%). Number of turns: Primary turns (excitation) 100 turns Number of secondary turns (detection): 100 turns Maximum magnetic field: 1630A / m (applied magnetic field) Measurement frequency: 50Hz (0.05kHz) Waveform: Sine wave (AC power wavelength)

[0038] Under the above conditions, the maximum magnetic flux density, residual magnetic flux density, coercive force, and amplitude specific permeability of Ni-P were measured. Specifically, measurements were performed on three types of Ni-P: two types of Ni-P (referred to as "Ni-P(A)" and "Ni-P(B)") and Ni-P(A) heated at 150°C (referred to as "Ni-P(A2)"). Similar measurements were also performed on Ni as a comparative example. The results are shown in Table 1.

[0039] [Table 1]

[0040] From a comparison of the magnetic property measurement results for the three Ni-P samples and the magnetic property measurement results for Ni, it can be seen that the amplitude specific permeability of the Ni-P of the external electrode body 9 of the external electrode 3 is preferably 4.0 or less. It can be seen that the maximum magnetic flux density of Ni-P is preferably 7.0 mT or less. It can be seen that the residual magnetic flux density of Ni-P is preferably 0.10 mT or less. It can be seen that the coercive force of Ni-P is preferably 23 A / m or less. When the electrical resistance value of each of the above Ni-P samples and the electrical resistance value of Ni were measured, the electrical resistance value of each Ni-P was higher than that of Ni (Ni-P>Ni).

[0041] The amplitude ratio permeability of Ni-P is preferably 2.0 or more and 4.0 or less, more preferably 2.3 or more and 3.1 or less. The maximum magnetic flux density of Ni-P is preferably 4.0 mT or more and 7.0 mT or less, more preferably 4.7 mT or more and 6.2 mT or less. The residual magnetic flux density of Ni-P is preferably 0.04 mT or more and 0.10 mT or less, more preferably 0.048 mT or more and 0.066 mT or less. The coercive force of Ni-P is preferably 10 A / m or more and 23 A / m or less, more preferably 11 A / m or more and 21 A / m or less.

[0042] In addition to the above-mentioned embodiment, the mounting pad 2 can be formed in a state where another metal layer consisting of one or more layers is interposed between the mounting pad main body 8 and the first surface layer 6 and / or between the mounting pad main body 8 and the second surface layer 12. Similarly, the external electrode 3 can be formed in a state where another metal layer consisting of one or more layers is interposed between the external electrode main body 9 and the third surface layer 7 and / or between the external electrode main body 9 and the fourth surface layer 13. In addition, the mounting pad 2 and the external electrode 3 may be formed in a form where one or both of the surface layers 6 and 7 exposed on the mounting surface S of the semiconductor device and the surface layers 12 and 13 covering the surfaces of the main bodies 8 and 9 are omitted. Each of the surface layers 6, 7, 12 and 13 can be formed of a layer made of an alloy mainly containing gold, silver, palladium, tin, etc. The substrate for semiconductor device according to the present invention can also be applied to a semiconductor device in a form where the mounting pad 2 is not provided. In this case, the semiconductor element is mounted on the substrate (wire bonding connection) or on the external electrodes 3 (flip chip connection).

[0043] The substrate for semiconductor device according to the present invention can contribute to Goal 9 (Build resilient infrastructure, promote inclusive and sustainable industrialization, and innovate innovative technologies) and Goal 12 (Responsible consumption and production) of the Sustainable Development Goals (SDGs) advocated by the United Nations. [Explanation of symbols]

[0044] 3 External electrode 7 Third surface layer 9 External electrode body 13 4th surface layer 16 Substrate

Claims

1. A substrate for a semiconductor device, in which an external electrode (3) connected to a semiconductor element (1) is formed on the surface of the substrate (16), The external electrode (3) comprises a third surface layer (7) formed on the surface of the substrate (16), an external electrode main body (9) formed on the surface of the third surface layer (7), and a fourth surface layer (13) formed on the surface of the external electrode main body (9); The external electrode body (9) of the external electrode (3) is made of non-magnetic Ni—P, A substrate for a semiconductor device, characterized in that the amplitude ratio permeability of Ni--P is 4.0 or less.

2. 2. The substrate for a semiconductor device according to claim 1, wherein the amplitude ratio permeability of Ni--P is 2.0 or more and 4.0 or less.

3. 2. The substrate for a semiconductor device according to claim 1, wherein the maximum magnetic flux density of Ni--P is 7.0 mT or less.

4. 4. The substrate for a semiconductor device according to claim 3, wherein the maximum magnetic flux density of Ni--P is 4.0 mT or more and 7.0 mT or less.

5. 4. The substrate for a semiconductor device according to claim 3, wherein the residual magnetic flux density of Ni--P is 0.10 mT or less.

6. 6. The substrate for a semiconductor device according to claim 5, wherein the residual magnetic flux density of Ni--P is 0.04 mT or more and 0.10 mT or less.

7. 6. The substrate for a semiconductor device according to claim 5, wherein the coercive force of Ni--P is 23 A / m or less.

8. 8. The substrate for a semiconductor device according to claim 7, wherein the coercive force of Ni--P is 10 A / m or more and 23 A / m or less.

Citation Information

Patent Citations

  • Substrate for semiconductor device, method for manufacturing substrate for semiconductor device, and semiconductor device