Wavelength conversion material

By recovering and treating phosphor particles with dilute hydrochloric acid to remove carbonates and using a metal carbonate coating, the recycling method enhances the efficiency and reduces the amount of wavelength conversion materials required, addressing the challenges of recycling and maintaining brightness in display devices.

JP2024135345APending Publication Date: 2024-10-04TOPPAN HOLDINGS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023045974
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing technologies face challenges in efficiently recycling wavelength conversion materials used in display devices, particularly due to the formation of carbonates on phosphor particles during development, which affect luminescence efficiency and require excessive amounts to achieve the same brightness as new materials.

Method used

A method for recycling wavelength conversion materials involves recovering phosphor particles from used developers, treating them with dilute hydrochloric acid to partially remove surface carbonates, and using a coating layer made of metal carbonates to maintain refractive index differences, ensuring efficient light scattering and luminescence.

Benefits of technology

The recycled wavelength conversion materials achieve similar brightness and luminescence efficiency to new materials while reducing the amount needed, thus lowering manufacturing costs and maintaining optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135345000002
    Figure 2024135345000002
  • Figure 2024135345000003
    Figure 2024135345000003
  • Figure 2024135345000004
    Figure 2024135345000004
Patent Text Reader

Abstract

To provide a technique which is useful for recycling a wavelength conversion material.SOLUTION: A method for manufacturing a wavelength conversion material recycled product includes: containing phosphor particles and a photosensitive resin, exposing a photosensitive layer containing one or more selected from a group consisting of strontium, calcium and barium with the phosphor particles, and spray developing the photosensitive layer; supplying a developer used in the spray development to filtration, and recovering the phosphor particles contained in the developer; and treating the recovered phosphor particles with a diluted hydrochloric acid, and partially removing a carbonate produced on the surface of the phosphor particles by the spray development.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wavelength converting material. [Background technology]

[0002] Phosphors such as inorganic phosphors emit light at a wavelength different from the wavelength of the excitation light when irradiated with the excitation light, and are therefore used, for example, as wavelength conversion materials in display devices. Patent documents 1 and 2 describe the manufacture of a full-color light-emitting diode display panel by forming a photosensitive resin layer containing a phosphor, and then sequentially subjecting this photosensitive resin layer to pattern exposure and development to form a fluorescent layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-28380 A [Patent Document 2] JP 2019-140361 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a technique useful for recycling wavelength converting materials. [Means for solving the problem]

[0005] According to one aspect of the present invention, there is provided a wavelength conversion material comprising phosphor particles and a coating layer covering the phosphor particles, the coating layer being made of a metal carbonate containing one or more selected from the group consisting of strontium, calcium and barium, and the proportion of carbon dioxide in the total of the phosphor particles and the carbonate being within the range of 1 to 4 mass %.

[0006] According to another aspect of the present invention, there is provided a wavelength converting material according to the above aspect, which is a recycled product obtained by recycling particles recovered from a used developer after exposure and development of a photosensitive layer containing phosphor particles and a photosensitive resin.

[0007] According to yet another aspect of the present invention, there is provided the wavelength converting material according to any of the above aspects, wherein the refractive index of the coating layer is smaller than the refractive index of the phosphor particles.

[0008] According to yet another aspect of the invention, the phosphor particles have the general formula MAlSiN3:Eu 2+ (M is Sr or a combination of Sr and one or more selected from Mg, Ca and Ba; Eu 2+ represents a luminescent center), and a red phosphor particle containing a crystal represented by the general formula (Ba, Sr, Ca, Mg) 10 There is provided a wavelength converting material according to any of the above aspects, which includes one of blue phosphor particles including crystals represented by (PO4)6Cl2:Eu.

[0009] According to still another aspect of the present invention, the particle size distribution measured by the laser diffraction / scattering method has a median diameter D in the range of 3.5 to 4.5 μm in a volume-based cumulative distribution. 50 and has a 90% diameter D in the range of 7.0 to 8.4 μm. 90 There is provided a wavelength converting material according to any of the above aspects, comprising:

[0010] According to yet another aspect of the present invention, there is provided a method for manufacturing a display device, the method including sequentially exposing and developing a photosensitive layer containing a wavelength converting material according to any of the above aspects and a photosensitive resin.

[0011] According to yet another aspect of the present invention, there is provided a display device including the wavelength converting material according to the above aspect.

[0012] According to yet another aspect of the present invention, there is provided a display device according to the above aspect, comprising a plurality of wavelength conversion layers, at least one of the plurality of wavelength conversion layers containing the wavelength conversion material, the phosphor particles contained therein being red or blue phosphor particles, and at least one other of the plurality of wavelength conversion layers containing a wavelength conversion material comprising green phosphor particles and a coating layer made of an oxide or phosphate coating the green phosphor particles.

[0013] According to yet another aspect of the present invention, there is provided a method for producing a recycled wavelength conversion material, the method including: exposing the phosphor particles to a photosensitive layer containing phosphor particles and a photosensitive resin, the phosphor particles containing one or more selected from the group consisting of strontium, calcium and barium, spray-developing the photosensitive layer, filtering the developer used in the spray development to recover the phosphor particles contained therein, and treating the recovered phosphor particles with dilute hydrochloric acid to partially remove carbonates formed on the surfaces of the phosphor particles by reaction with components contained in the developer.

[0014] According to yet another aspect of the present invention, there is provided a method for producing a regenerated wavelength converting material according to the above aspect, comprising partially removing the carbonate so that the proportion of carbon dioxide in the total of the phosphor particles and the carbonate is within the range of 1 to 4 mass %.

[0015] According to yet another aspect of the present invention, there is provided a regeneration system including a spray developing device which contains phosphor particles and a photosensitive resin and spray-develops an exposed photosensitive layer, a filtration device which filters the developer used in the spray development to recover the phosphor particles contained therein, and a regeneration device which treats the recovered phosphor particles with dilute hydrochloric acid to partially remove carbonates formed on the surfaces of the phosphor particles by reaction with components contained in the developer.

[0016] According to yet another aspect of the present invention, there is provided a regeneration system according to the above aspect, further comprising a controller that controls the operation of the regeneration device so that the proportion of carbon dioxide in the total of the phosphor particles and the carbonate is within the range of 1 to 4 mass % by partially removing the carbonate. Effect of the Invention

[0017] According to the present invention, a technique useful for recycling wavelength converting materials is provided. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of an article including a wavelength converting material. [Diagram 2] FIG. 2 is a schematic diagram showing a reproducing system according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a cleaning device that can be included in the regeneration system of FIG. [Figure 4] FIG. 4 is a schematic diagram showing an example of a recovery device that can be included in the recycling system of FIG. [Diagram 5] FIG. 5 is a cross-sectional view illustrating a wavelength converting material according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.

[0020] The embodiments described below are merely examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of ​​the present invention within the technical scope defined by the claims.

[0021] In addition, elements having the same or similar functions are given the same reference numerals in the drawings referred to below, and duplicated explanations are omitted. In addition, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual ones.

[0022] <1> Examples of wavelength conversion materials FIG. 1 is a cross-sectional view illustrating an example of an article including a wavelength converting material.

[0023] 1 illustrates a display device 1 as an example of an article containing a wavelength conversion material. The display device 1 is a micro LED display capable of color display using an active matrix driving method, in which each subpixel contains a light emitting diode (LED).

[0024] 1, the X direction and the Y direction are parallel to the display surface of the display device 1 and intersect with each other. According to one example, the X direction and the Y direction are perpendicular to each other. The Z direction is perpendicular to the X direction and the Y direction. That is, the Z direction is the thickness direction of the display device 1.

[0025] The display device 1 shown in FIG. 1 includes a light control device 2, a black matrix substrate 3, and an adhesive layer 4.

[0026] The light control device 2 is a device that emits light toward the black matrix substrate 3 and is capable of adjusting at least one of the intensity of the light and the time for emitting the light for each pixel or each subpixel. The light control device 2 includes a substrate 21, a multilayer wiring layer 22, and a light emitting diode 23.

[0027] The substrate 21 includes an insulating substrate such as a glass substrate. The substrate 21 may further include an undercoat layer provided on a main surface of the insulating substrate facing the black matrix substrate 3. The undercoat layer is, for example, a laminate of a silicon nitride layer and a silicon oxide layer sequentially laminated on the insulating substrate. The substrate 21 may be a semiconductor substrate such as a silicon substrate. The substrate 21 may be either rigid or flexible.

[0028] The multilayer wiring layer 22 is provided on a main surface of the substrate 21 facing the black matrix substrate 3. The multilayer wiring layer 22 includes video signal lines, first power supply lines, second power supply lines, scanning signal lines, pixel circuits, and an interlayer insulating film.

[0029] The video signal lines each extend in the Y direction and are arranged in the X direction. The scanning signal lines each extend in the X direction and are arranged in the Y direction. The first and second power lines each extend in the Y direction and are arranged in the X direction in correspondence with the video signal lines. The first and second power lines may each extend in the X direction and be arranged in the Y direction in correspondence with the scanning signal lines. Alternatively, one of the first and second power lines may each extend in the Y direction and be arranged in the X direction in correspondence with the video signal lines, and the other of them may each extend in the X direction and be arranged in the Y direction in correspondence with the scanning signal lines.

[0030] The pixel circuits are arranged in the X-direction and the Y-direction on the main surface of the substrate 21. Each pixel circuit includes a drive control element, a switch, and a capacitor. The drive control element is, for example, a p-channel field effect transistor having a source connected to the first power supply line. The switch is, for example, an n-channel field effect transistor having a gate connected to a scanning signal line, a source connected to a video signal line, and a drain connected to the gate of the drive control element. The capacitor is, for example, a thin film capacitor having one electrode connected to the gate of the drive control element and the other electrode connected to the first power supply line. The pixel circuits may have other configurations.

[0031] The light emitting diode 23 has a multi-layer structure. Here, the stacking direction of the layers included in the light emitting diode 23 is the Z direction. This stacking direction may be perpendicular to the Z direction.

[0032] The light emitting diodes 23 have the same emission spectrum. The light emitting diodes 23 emit short wavelength light such as blue light and ultraviolet light. Here, as an example, the light emitting diodes 23 are blue light emitting diodes that emit blue light.

[0033] The light emitting diodes 23 are arranged corresponding to the pixel circuits on the multi-layer wiring layer 22. Each of the light emitting diodes 23 has an anode connected to the drain of the drive control element and a cathode connected to the second power supply line.

[0034] The black matrix substrate 3 faces the light control device 2. Specifically, the black matrix substrate 3 faces the substrate 21 with the light emitting diodes 23 and the like sandwiched therebetween.

[0035] The black matrix substrate 3 includes a transparent substrate 31, a black matrix 32, a partition layer 34, a color filter including a first colored layer 33R and a second colored layer 33G, a base layer 33B, a first wavelength conversion layer 36R, a second wavelength conversion layer 36G, and a filling layer 36B.

[0036] The transparent substrate 31 has visible light transmissibility. The transparent substrate 31 is, for example, a colorless substrate. The transparent substrate 31 may have a single-layer structure or a multi-layer structure. The transparent substrate 31 is made of, for example, glass, a transparent resin, or a combination thereof. The transparent substrate 31 may be hard or flexible. The transparent substrate 31 has a first main surface facing the light control device 2 and a second main surface that is the rear surface of the first main surface.

[0037] The black matrix 32 is provided on the first main surface of the transparent substrate 31. The black matrix 32 is a black layer that blocks visible light. The black matrix 32 is made of, for example, a mixture containing a binder resin and a colorant. The colorant is, for example, a black pigment, or a mixture of pigments that exhibit black color by subtractive color mixing, for example, a mixture containing a blue pigment, a green pigment, and a red pigment.

[0038] The black matrix 32 has first through holes at the positions of the light emitting diodes 23. The opening of each first through hole on the transparent substrate 31 side has a larger dimension in the direction perpendicular to the Z direction than the light emitting diodes 23.

[0039] The first colored layer 33R, the second colored layer 33G, and the underlayer 33B form a stripe arrangement on the transparent substrate 31 provided with the black matrix 32. These form a plurality of pixels, each of which is made up of the first colored layer 33R, the second colored layer 33G, and the underlayer 33B, and these pixels are arranged in the X direction and the Y direction.

[0040] As described above, here, the first colored layer 33R is a red colored layer, and the second colored layer 33G is a green colored layer. Also, here, the base layer 33B is a colorless light-transmitting layer or a blue colored layer. Each of the first colored layers 33R fills one of the first through holes. Each of the second colored layers 33G fills another one of the first through holes. Each of the base layers 33B fills yet another one of the first through holes.

[0041] The partition layer 34 is provided on a composite film including the first colored layer 33R, the second colored layer 33G, and the undercoat layer 33B. According to one example, the partition layer 34 is transparent. In this case, the partition layer 34 may be colored or colorless. The partition layer 34 may have a light scattering property.

[0042] The partition layer 34 has second through holes at the positions of the first through holes. Here, the second through holes are provided such that the outline of the orthogonal projection of the opening on the transparent substrate 31 side onto the first main surface (hereinafter referred to as the second outline) surrounds the outline of the orthogonal projection of the first through hole onto the first main surface (hereinafter referred to as the first outline). The second outline does not have to surround the first outline. In a structure in which the second outline surrounds the first outline, the effect of stray light on the display is smaller than in a structure in which the second outline does not surround the first outline.

[0043] A portion of the partition layer 34 that is sandwiched between adjacent second through holes has a rectangular cross-sectional shape. This portion may have a forward tapered cross-sectional shape, a reverse tapered cross-sectional shape, or another cross-sectional shape.

[0044] The partition layer 34 may have a multi-layer structure. For example, the partition layer 34 may include a resin layer and a reflective layer that at least partially covers the surface of the resin layer.

[0045] The reflective layer may have a single-layer structure or a multi-layer structure. The layers contained in the reflective layer are, for example, a metal, an alloy, or a transparent dielectric. The reflective layer made of a metal or an alloy is, for example, made of aluminum or an aluminum alloy.

[0046] The first wavelength conversion layer 36R is provided on the first colored layer 33R. The first wavelength conversion layer 36R is a layer containing a phosphor such as an inorganic phosphor and a transparent resin. Here, the first wavelength conversion layer 36R converts the blue light emitted by the light emitting diode 23 into red light.

[0047] The second wavelength conversion layer 36G is provided on the second colored layer 33G. The second wavelength conversion layer 36G is a layer containing a phosphor such as an inorganic phosphor and a transparent resin. Here, the second wavelength conversion layer 36G converts the blue light emitted by the light emitting diode 23 into green light.

[0048] The filling layer 36B is provided on the base layer 33B. As described above, the filling layer 36B is a colorless and transparent layer. In this case, the filling layer 36B is made of, for example, a transparent resin.

[0049] When the light emitting diode 23 is an ultraviolet light emitting diode, the filling layer 36B is a third wavelength conversion layer. The third wavelength conversion layer is a layer containing a phosphor such as an inorganic phosphor and a transparent resin. The third wavelength conversion layer converts, for example, ultraviolet light emitted by the ultraviolet light emitting diode into blue light. In this case, the first wavelength conversion layer 36R and the second wavelength conversion layer 36G convert the ultraviolet light emitted by the ultraviolet light emitting diode into red light and green light, respectively. The wavelength-converting layer preferably does not contain scattering particles.

[0050] The adhesive layer 4 is interposed between the light control device 2 and the black matrix substrate 3, and bonds them to each other. The adhesive layer 4 transmits light emitted by the light emitting diodes 23. The adhesive layer 4 is, for example, a colorless and transparent layer. The adhesive layer 4 is made of an adhesive or a pressure sensitive adhesive.

[0051] The display device 1 described above contains a phosphor such as an inorganic phosphor as a wavelength converting material. The wavelength converting material can also be used in other display devices. For example, the wavelength converting material may be used in an organic electroluminescence display device. Alternatively, the wavelength converting material may be used in a liquid crystal display device, for example, in the backlight of a liquid crystal display device.

[0052] Wavelength converting materials may be used in devices other than displays, for example, they may be used in lighting devices.

[0053] <2> Playback System FIG. 2 is a schematic diagram showing a reproducing system according to an embodiment of the present invention.

[0054] In the manufacture of the display device 1 described above, each of the first wavelength conversion layer 36R and the second wavelength conversion layer 36G can be obtained by a process including forming a coating film made of a photosensitive resin composition containing phosphor particles as wavelength conversion materials and a photosensitive resin, and sequentially performing pattern exposure and development on this coating film. In addition, when the filling layer 36B is the third wavelength conversion layer, this can also be obtained by a process including forming a coating film made of a photosensitive resin composition containing phosphor particles as wavelength conversion materials and a photosensitive resin, and sequentially performing pattern exposure and development on this coating film. The regeneration system 100 shown in FIG. 2 can be used, for example, in these developments. The regeneration system 100 shown in FIG. 2 includes a spray developing device 200, a developer storage tank 300, a circulation pump 400, a filtering device 500, a cleaning device 600, a regeneration device 700, a controller 800, and a drying device 900.

[0055] The spray developer apparatus 200 includes a developer container 210 , a spray nozzle assembly 220 , and a transport apparatus 230 .

[0056] The developing container 210 contains a plurality of spray nozzle assemblies 220 and a conveying device 230. A drain port for discharging used developing solution is provided at the bottom of the developing container 210. One end of a pipe L1 is connected to this drain port.

[0057] Each of the spray nozzle assemblies 220 includes a header 221 and a nozzle tip 222. The header 221 is a hollow body having a shape extending in one direction. The spray nozzle assemblies 220 are arranged such that the length directions of the headers 221 are parallel to each other and the headers 221 are arranged in the width direction.

[0058] Each of the headers 221 has an inlet in its wall. Each of the headers 221 also has a number of through holes in its lower wall arranged in the length direction. In each of the spray nozzle assemblies 220, a nozzle tip 222 is attached to the header 221 at the position of the through holes. The nozzle tip 222 may be, for example, one that sprays the developer in a fan or cone shape.

[0059] Each of the spray nozzle assemblies 220 sprays the developer supplied into the header 221 via an inlet downward through a nozzle provided in the nozzle tip 222. The spray nozzle assembly 220 may be one that sprays the developer in one fluid or two fluids.

[0060] The transport device 230 includes a plurality of transport rollers 231 arranged below the spray nozzle assembly 220, and a motor for driving the transport rollers 231. The transport device 230 rotates the transport rollers 231 counterclockwise in the figure to transport the workpiece W to the left in the figure. The workpiece W is, for example, a transparent substrate 31 or the like on which a coating film made of the photosensitive resin composition is formed, and the coating film is then pattern-exposed.

[0061] The developer storage tank 300 contains a developer DL1. The developer used in the spray developing device 200 is supplied to the developer storage tank 300 via a pipeline L1. Therefore, the developer DL1 contained in the developer storage tank 300 contains substances removed from the workpiece W by development in the spray developing device 200, such as phosphor particles and resin, as impurities.

[0062] At least a part of the impurities settles to the bottom of the developer storage tank 300. The bottom of the developer storage tank 300 has a discharge port for discharging the precipitate generated in the developer DL1. One end of a pipe line L4 is connected to this discharge port.

[0063] The side wall of the developer storage tank 300 has a discharge port for discharging the supernatant of the developer DL1. One end of a pipe L2 is connected to the discharge port. The circulation pump 400 is attached to the pipe L2.

[0064] The filtering device 500 has an inlet and first and second outlets. The other end of the pipe L2 is connected to the inlet of the filtering device 500. The developer DL1 supplied through the pipe L2 may contain impurities. The filtering device 500 removes at least a part of the impurities from the developer DL1 supplied through the inlet by filtration.

[0065] The filtering device 500 discharges the filtrate from a first outlet. One end of a pipe L3 is connected to the first outlet. The other end of the pipe L3 is connected to an inlet of the header 221.

[0066] Furthermore, the filtering device 500 discharges the residue from a second outlet. One end of a pipe L5 is connected to the second outlet.

[0067] The cleaning device 600 has first and second inlets and an outlet. The first and second inlets of the cleaning device 600 are connected to the other end of the pipe L4 and the other end of the pipe L5, respectively. The cleaning device 600 cleans the precipitate supplied from the developer storage tank 300 via the pipe L4 and the residue discharged from the second outlet of the filtration device 500. For example, the cleaning device 600 sequentially performs cleaning with pure water and cleaning with an organic solvent.

[0068] The cleaning device 600 discharges the precipitate and residue after cleaning, i.e., the recovered matter, from a discharge port. One end of a pipe L6 is connected to this discharge port.

[0069] The regenerating device 700 has an inlet and an outlet. The other end of the pipe L6 is connected to the inlet of the regenerating device 700. The regenerating device 700 subjects the recovered phosphor particles to a treatment with dilute hydrochloric acid to partially remove carbonates formed on the surfaces of the phosphor particles by reaction with the components contained in the developer DL1. One end of the pipe L11 is connected to the outlet of the regenerating device 700.

[0070] The controller 800 is connected to the reproducing device 700. The controller 800 includes a processing unit and a memory unit. The processing unit includes a central processing unit. The central processing unit is a large-scale integrated circuit and includes an arithmetic unit and a control unit. The memory unit includes a main memory unit and an auxiliary memory unit. The main memory unit is a large-scale integrated circuit and includes a volatile memory such as a random access memory. The auxiliary memory unit is a non-volatile memory device such as a hard disk drive and a solid state drive. The controller 800 controls the operation of the reproducing device 700 so that an appropriate amount of carbonate remains on the surface of the phosphor particles.

[0071] The other end of the pipe L1 is connected to the drying device 900. The drying device 900 dries the regenerated product supplied from the regenerator 700. For example, the drying device 900 heats and dries the regenerated product, dries it under reduced pressure, or dries it under reduced pressure while heating it.

[0072] FIG. 3 is a schematic diagram showing an example of a cleaning device that can be included in the regeneration system of FIG. The cleaning device 600 shown in FIG. 3 includes a filtering device 600A, a first cleaning device 600B, and a second cleaning device 600C.

[0073] In the above-described regeneration system 100, a developer solution containing a high concentration of solids is supplied to the cleaning device 600 via the lines L4 and L5. The filtering device 600A further increases the solids concentration of this solution.

[0074] The filtering device 600A includes a container 610A and a filter 620A. The filter 620A divides the internal space of the container 610A into an upper space and a lower space.

[0075] A liquid DL2 containing high concentrations of phosphor particles and resin is supplied to the upper space in the container 610A via a pipe L4 or L5. A first outlet is provided at the bottom of the container 610A. One end of a pipe L8A is connected to the first outlet. The developer DL3 from which impurities have been removed by passing through the filter 620A is discharged to the outside of the filtration device 600A via the first outlet and the pipe L8A.

[0076] The side wall of the container 610A has a second outlet above the filter 620A. One end of a pipe L7A is connected to the second outlet.

[0077] A valve 630B and a pump 640B are attached to the pipe L7A. ​​The liquid DL2, whose solid content concentration has been further increased by filtration in the filtration device 600A, is discharged to the outside of the container 610A via the second outlet and the pipe L7A by opening the valve 630B and driving the pump 640B.

[0078] The first cleaning device 600B performs a cycle including supplying pure water as the first cleaning liquid and filtering the pure water at least once, thereby removing water-soluble impurities, such as inorganic impurities, from the liquid containing the solid contents.

[0079] The first cleaning device 600B includes a container 610B and a filter 620B. The filter 620B divides the internal space of the container 610B into an upper space and a lower space.

[0080] A liquid DL2 having an increased solid content concentration is supplied to the upper space in the container 610B via a pipe L7A, and pure water as a first cleaning liquid is supplied via a pipe L9B. The bottom of the container 610B has a first outlet. One end of a pipe L8B is connected to the first outlet. The liquid WL2B that has permeated the filter 620B is discharged to the outside of the first cleaning device 600B via the first outlet and the pipe L8B.

[0081] The side wall of the container 610B has a second outlet above the filter 620B. One end of a pipe L10 is connected to the second outlet.

[0082] A valve 630C and a pump 640C are attached to the pipe L10. The liquid WL1B from which water-soluble impurities have been removed by cleaning in the first cleaning device 600B is discharged to the outside of the container 610B via the second outlet and the pipe L10 by opening the valve 630C and driving the pump 640C.

[0083] The second cleaning device 600C performs a cycle including supplying an organic solvent as the second cleaning liquid and filtering the liquid one or more times. As a result, the second cleaning device 600C removes impurities soluble in the organic solvent, such as organic impurities, from the liquid from which the water-soluble impurities have been removed. The second cleaning liquid is, for example, an amphipathic organic solvent such as acetone and ethanol.

[0084] The second cleaning device 600C includes a container 610C and a filter 620C. The filter 620C divides the internal space of the container 610C into an upper space and a lower space.

[0085] A liquid WL1B from which water-soluble impurities have been removed is supplied to the upper space in the container 610C via a pipe L10, and an organic solvent as a second cleaning liquid is supplied via a pipe L9C. A first outlet is provided at the bottom of the container 610C. One end of a pipe L8C is connected to the first outlet. The liquid WL2C that has permeated the filter 620C is discharged to the outside of the second cleaning device 600C via the first outlet and the pipe L8C.

[0086] The side wall of the container 610C has a second outlet above the filter 620C. One end of a pipe L6 is connected to the second outlet.

[0087] A valve and a pump (not shown) are attached to the pipe L6. The liquid WL1C from which impurities soluble in an organic solvent have been removed by the cleaning in the second cleaning device 600C is discharged to the outside of the container 610C through the second outlet and the pipe L6 by opening the valve and driving the pump.

[0088] 3, the phosphor particles are transferred from container 610A to container 610B and from container 610B to container 610C in the form of a slurry containing the phosphor particles at a high concentration. The phosphor particles may be transferred from container 610A to container 610B and from container 610B to container 610C in the form of a filter cake.

[0089] 3 uses three containers for cleaning. Cleaning may be performed using, for example, one container. For example, after filtration in the filtration device 600A, the cleaning described above for the first cleaning device 600B and the cleaning described above for the second cleaning device 600C may be performed in this order in the filtration device 600A.

[0090] FIG. 4 is a schematic diagram showing an example of a playback device that can be included in the playback system of FIG. The regeneration apparatus 700 shown in FIG. 4 includes an acid treatment apparatus 700A, a first cleaning apparatus 700B, and a second cleaning apparatus 700C.

[0091] In the regeneration system 100, the regeneration device 700 is supplied with a liquid containing a high concentration of phosphor particles after cleaning by the cleaning device 600 via a pipe L6. The liquid discharged from the cleaning device 600 via the pipe L6 is an alkaline aqueous solution with phosphor particles dispersed therein. Prior to supplying the liquid to the regeneration device 700, it is possible to adjust the pH of the liquid with an acid or increase the concentration of phosphor particles in the liquid.

[0092] The solution contains carbonates on the surfaces of the phosphor particles due to retention in the developer reservoir 300. The acid treatment device 700A partially removes the carbonates from the phosphor particles.

[0093] The acid treatment device 700A includes a container 710A and a filter 720A. The filter 720A divides the internal space of the container 710A into an upper space and a lower space.

[0094] A liquid containing phosphor particles and dilute hydrochloric acid are supplied to the upper space in the container 710A via the pipes L6 and L14, respectively. The bottom of the container 710A has a first outlet. One end of the pipe L18A is connected to the first outlet. The liquid DHC2 from which the phosphor particles have been removed by passing through the filter 720A is discharged to the outside of the acid treatment device 700A via the first outlet and the pipe L18A.

[0095] The side wall of the container 710A has a second outlet above the filter 720A. One end of a pipe L17A is connected to the second outlet.

[0096] A valve 730B and a pump 740B are attached to the pipe L17A. The liquid DHC1 containing the phosphor particles after the acid treatment is discharged to the outside of the container 710A through the second outlet and the pipe L17A by opening the valve 730B and driving the pump 740B.

[0097] The first cleaning device 700B performs a cycle including supplying and filtering pure water as a first cleaning liquid one or more times, thereby removing hydrochloric acid from the phosphor particles.

[0098] The first cleaning device 700B includes a container 710B and a filter 720B. The filter 720B divides the internal space of the container 710B into an upper space and a lower space.

[0099] A liquid DHC1 containing phosphor particles after acid treatment is supplied to the upper space in the container 710B via a pipe L17A, and pure water as a first cleaning liquid is supplied via a pipe L19B. The bottom of the container 710B has a first outlet. One end of a pipe L18B is connected to the first outlet. The liquid WL4B that has passed through the filter 720B is discharged to the outside of the first cleaning device 700B via the first outlet and the pipe L18B.

[0100] The side wall of the container 710B has a second outlet above the filter 720B. One end of a pipe L20 is connected to the second outlet.

[0101] A valve 730C and a pump 740C are attached to the pipe L20. The liquid WL3B from which hydrochloric acid has been removed by cleaning in the first cleaning device 700B is discharged to the outside of the container 710B via the second outlet and the pipe L20 by opening the valve 730C and driving the pump 740C.

[0102] The second cleaning device 700C performs a cycle including supplying an organic solvent as the second cleaning liquid and filtering the organic solvent one or more times, thereby removing moisture from the phosphor particles.

[0103] The second cleaning device 700C includes a container 710C and a filter 720C. The filter 720C divides the internal space of the container 710C into an upper space and a lower space.

[0104] A liquid WL3B, which is an aqueous dispersion of phosphor particles from which hydrochloric acid has been removed, is supplied to the upper space in the container 710C via a pipe L20, and an organic solvent as a second cleaning liquid is supplied via a pipe L19C. The bottom of the container 710C has a first outlet. One end of a pipe L18C is connected to the first outlet. The liquid WL4C that has permeated the filter 720C is discharged to the outside of the second cleaning device 700C via the first outlet and the pipe L18C.

[0105] The side wall of the container 710C has a second outlet above the filter 720C. One end of a pipe L11 is connected to the second outlet.

[0106] A valve and a pump (not shown) are attached to the pipe L11. The liquid WL3C, which is an organic solvent dispersion of phosphor particles from which moisture has been removed by cleaning in the second cleaning device 700C, is discharged to the outside of the container 710C through the second outlet and the pipe L11 by opening the valve and driving the pump.

[0107] The organic solvent used as the second cleaning liquid is preferably a low boiling point solvent such as acetone, that is, an organic solvent having a boiling point of less than 100° C. When a low boiling point solvent is used as the second cleaning liquid, drying by the drying device 900 can be performed, for example, at a low temperature.

[0108] 4, the phosphor particles are transferred from vessel 710A to vessel 710B and from vessel 710B to vessel 710C in the form of a slurry containing the phosphor particles at a high concentration. The phosphor particles may be transferred from vessel 710A to vessel 710B and from vessel 710B to vessel 710C in the form of a filter cake.

[0109] 4 uses three containers for the acid treatment and cleaning. The acid treatment and cleaning may be performed, for example, using one container. For example, after the acid treatment in the acid treatment device 700A, the cleaning described above for the first cleaning device 700B and the cleaning described above for the second cleaning device 700C may be performed in this order in the acid treatment device 700A.

[0110] 2 to 4, the regeneration system 100 is configured to transfer the phosphor particles from the cleaning device 600 to the regeneration device 700 in the form of a slurry. The regeneration system 100 may also be configured to transfer the phosphor particles from the cleaning device 600 to the regeneration device 700 in the form of a filter cake. Alternatively, the regeneration system 100 may further include a drying device for drying the phosphor particles after cleaning by the cleaning device 600, and the dried phosphor particles may be supplied to the regeneration device.

[0111] <3> Manufacturing method for recycled wavelength conversion material / manufacturing method for display device The above-described reproducing system 100 can be used, for example, in the manufacture of a display device including a wavelength converting material. As an example, a method for manufacturing a display device 1 using the reproducing system 100 will be described below.

[0112] First, a structure including a transparent substrate 31, a black matrix 32, a first colored layer 33R, a second colored layer 33G, a base layer 33B, and a partition layer 34 is prepared. Next, a first wavelength conversion layer 36R, a second wavelength conversion layer 36G, and a filling layer 36B are formed. The first wavelength conversion layer 36R, the second wavelength conversion layer 36G, and the filling layer 36B may be formed in any order.

[0113] Each of the first wavelength conversion layer 36R and the second wavelength conversion layer 36G is formed, for example, by the following method.

[0114] First, a photosensitive resin composition containing a wavelength converting material and a photosensitive resin is prepared. The photosensitive resin may be either a negative type or a positive type. The composition of the photosensitive resin composition will be described in detail later.

[0115] Next, a photosensitive resin composition is applied to the structure to form a photosensitive layer. The photosensitive layer is then partially exposed to light. If the photosensitive resin is a negative type, the region of the photosensitive layer corresponding to the wavelength conversion layer to be formed is exposed to light. If the photosensitive resin is a positive type, the region of the photosensitive layer other than the region corresponding to the wavelength conversion layer to be formed is exposed to light.

[0116] The exposed photosensitive layer is then spray developed. In general, inorganic alkali such as sodium carbonate, sodium bicarbonate, and sodium hydroxide, or aqueous solutions such as tetramethylammonium hydroxide (TMAH) are used as the developer for the pattern-exposed photosensitive layer. Here, a developer containing carbonate ions is used. For this spray development, for example, a spray development device 200 shown in FIG. 2 is used.

[0117] In the spray developing apparatus 200, the above-mentioned structure including the exposed photosensitive layer is used as the processing target W. In the spray developing apparatus 200, the circulation pump 400 is driven to circulate the developer DL1 in a circulation path including the developer storage tank 300, the pipe L2, the circulation pump 400, the filtration apparatus 500, the pipe L3, and the spray developing apparatus 200. When the developer DL1 is circulated, the spray nozzle assembly 220 sprays the developer DL1 downward. In this state, the conveying apparatus 230 conveys the above-mentioned structure placed on the conveying roller 231 to the left in the figure so that the photosensitive layer faces upward. When the photosensitive resin is a negative type, this removes the unexposed portion of the photosensitive layer.

[0118] Dip development is also widely used for developing a pattern-exposed photosensitive layer. There are two types of dip development: one that does not use a jet of developer, and one that does. In either dip development method, the part of the photosensitive layer that is removed by development is transferred into the developer as a relatively large peeled piece.

[0119] These peeled pieces are a mixture of the photosensitive resin and the wavelength converting material, and therefore, even if one tries to recover the wavelength converting material from the developer used in the dip development, it is difficult to remove impurities from the wavelength converting material by filtration.

[0120] When spray development is used to develop the pattern-exposed photosensitive layer, the portion of the photosensitive layer that is to be removed by development can be finely crushed, and therefore impurities can be removed from the wavelength converting material by filtration.

[0121] The spray development is preferably carried out at a spray pressure in the range of 0.03 to 0.3 MPa so as to eject droplets having an average particle size in the range of 10 to 100 μm as measured by a laser Doppler method. When the spray development is carried out under such conditions, an impact force that moves the particles of the wavelength conversion material can be applied to the part of the photosensitive layer that is to be removed by development. When such an impact force is applied to the particles of the wavelength conversion material, the crushing of the part of the photosensitive layer that is to be removed by development is promoted, enabling further miniaturization.

[0122] Each of the above spray developments may be followed by a two-fluid wash, which allows for the break-up and removal of resin residues.

[0123] The photosensitive layer is then heated to harden it, thus forming the first wavelength conversion layer 36R and the second wavelength conversion layer 36G.

[0124] The filling layer 36B can be formed in the same manner as the first wavelength conversion layer 36R and the second wavelength conversion layer 36G, except that, for example, a photosensitive resin composition that does not contain the wavelength conversion material is used and the wavelength conversion material is not recovered. When the filling layer 36B is the above-mentioned third wavelength conversion layer, it can be formed in the same manner as the first wavelength conversion layer 36R and the second wavelength conversion layer 36G.

[0125] In this manner, the black matrix substrate 3 is obtained. The black matrix substrate 3 and the separately prepared light control device 2 are bonded together via the adhesive layer 4. In this manner, the display device 1 shown in FIG. 1 is obtained.

[0126] While the developer DL1 is circulated in the above-mentioned spray development, the precipitate formed at the bottom of the developer storage tank 300 is sent to the cleaning device 600 via a pipe L4, and the residue separated from the filtrate in the filtration device 500 is sent to the cleaning device 600 via a pipe L5. The sending of the precipitate from the developer storage tank 300 to the cleaning device 600 and the sending of the residue from the filtration device 500 to the cleaning device 600 may each be performed continuously or intermittently.

[0127] The above-mentioned cleaning is performed in the cleaning device 600. As a result, most of the components other than the wavelength converting material are removed from the collected solid matter.

[0128] In the used developer, some of the wavelength converting material is bonded to each other via the photosensitive resin, and therefore the wavelength converting material contained in the used developer has a larger maximum particle size than that of the unused wavelength converting material.

[0129] On the other hand, impurities contained in the used developer, such as photosensitive resins, siloxane resins, photopolymerization initiators, or polymerizable compounds, that are not involved in the aggregation of the wavelength converting material, have small particle sizes because they are pulverized by spray development. According to one example, most of the impurity particles contained in the used developer have a particle size of less than 1 μm.

[0130] In this case, for example, if a filter that does not transmit particles with a particle diameter of more than 1 μm but transmits particles with a particle diameter of 1 μm or less is used, most of the impurities can be separated from the wavelength converting material by filtration. Note that, although the maximum particle diameter of particles that the filter transmits is set to 1 μm here, the maximum particle diameter of particles that the filter transmits can be appropriately selected depending on the minimum particle diameter of the wavelength converting material.

[0131] In addition, in the cleaning device 600, inorganic impurities are removed in the first cleaning device 600B, and organic impurities are removed in the second cleaning device 600C. Some siloxane resins form compounds that are poorly soluble in organic solvents due to reactions such as siloxane polymerization and saponification when they come into contact with an aqueous developer. Since the first cleaning device 600B uses pure water for cleaning, such compounds can be removed together with the inorganic components contained in the developer. And since the second cleaning device 600C uses an organic solvent for cleaning, other impurities can also be removed.

[0132] In this way, impurities involved in the aggregation of the wavelength converting material are also removed. Therefore, the wavelength converting material after cleaning by the second cleaning device 600C has a maximum particle size that is almost the same as that of an unused wavelength converting material. Note that the wavelength converting material after cleaning by the second cleaning device 600C has been filtered multiple times, so that the minimum particle size is almost the same as or larger than that of an unused wavelength converting material.

[0133] Thereafter, the cleaning device 600 sends out a slurry containing phosphor particles, which are a wavelength conversion material, and an organic solvent to the regenerating device 700 via the pipeline L6. As described above, the supply of the phosphor particles from the cleaning device 600 to the regenerating device 700 may be in the form of a filter cake or after drying.

[0134] In the regeneration apparatus 700, first, the above-mentioned acid treatment is carried out in the acid treatment unit 700A.

[0135] As described above, the developer DL1 contains carbonate ions, so that the phosphor particles may have carbonates on their surfaces that are generated by the reaction of the developer components while suspended in the developer reservoir 300.

[0136] This carbonate does not contribute to light emission. Therefore, when a complex of phosphor particles and carbonate is used as a wavelength conversion material, the photoluminescence quantum yield per mass decreases as the proportion of carbonate in the complex increases. That is, when the above complex is used as a wavelength conversion material to form a wavelength conversion layer, a larger amount of wavelength conversion material is required to achieve the same brightness as when new phosphor particles are used as the wavelength conversion material to form the wavelength conversion layer. Therefore, from the viewpoint of making the formation conditions of the wavelength conversion layer almost the same when a new wavelength conversion material is used and when a recycled wavelength conversion material is used, it is preferable that the proportion of carbonate in the above complex is small.

[0137] It has been found that the proportion P of carbon dioxide derived from the carbonate generated by the above reaction in the composite of the carbonate and phosphor particles is about 6 mass %. In order to achieve substantially the same brightness as when a new product is used when a wavelength conversion layer is formed under the same conditions as when a new product is used, except that a recycled product is used, the carbonate is preferably removed until the proportion P is 4 mass % or less, and more preferably removed until the proportion P is 3 mass % or less.

[0138] However, if the acid treatment is carried out excessively, not only the carbonates are removed, but also the metal components contained in the phosphor particles are dissolved. This dissolution may cause changes in the composition and crystal structure of the phosphor, resulting in a decrease in the photoluminescence quantum yield and a shift in the spectral peak wavelength. Therefore, the acid treatment does not completely remove the carbonates from the phosphor particles, but only partially. The carbonates are preferably removed by the acid treatment so that the ratio P is 1% by mass or more, and more preferably 2% by mass or more.

[0139] Here, the ratio P is a value obtained by the following method using differential thermogravimetry (TG-DTA). That is, the differential thermogravimetry is performed on the above composite as a sample in a temperature range of room temperature to 540°C, for example, in a temperature range of 30°C to 540°C. As a result, the ratio P1 is obtained as the ratio (M1A-M1B) / M1A, which is the ratio of the difference M1A-M1B between the mass M1A of the sample before the start of heating and the mass M1B of the sample after heating to 540°C to the mass M1A of the sample. In addition, the same differential thermogravimetry as above is performed on a sample similar to the above composite except that it does not contain carbonate, for example, an unused phosphor. As a result, the ratio P0 is obtained as the ratio (M0A-M10) / M0A, which is the ratio of the difference M0A-M0B between the mass M0A of the sample before the start of heating and the mass M0B of the sample after heating to 540°C to the mass M0A of the sample before the start of heating. The proportion P is the difference P1-P0 between the ratio P1 and the ratio P0.

[0140] The ratio P after the acid treatment can be adjusted, for example, by the concentration of dilute hydrochloric acid used in the acid treatment, the temperature of the dilute hydrochloric acid, and the time of the acid treatment.

[0141] The concentration of the dilute hydrochloric acid is preferably in the range of 0.1 to 0.4 mol / L, more preferably in the range of 0.15 to 0.2 mol / L. If the concentration is high, the acid treatment can be completed in a short time. However, if the concentration is too high, it becomes difficult to adjust the ratio P.

[0142] The temperature of the dilute hydrochloric acid is preferably in the range of 15 to 35° C., more preferably in the range of 20 to 30° C. If the temperature is increased, the acid treatment can be completed in a short time. However, if the temperature is excessively increased, it becomes difficult to adjust the ratio P.

[0143] The time for the acid treatment is preferably within a range of 5 to 20 minutes, and more preferably within a range of 10 to 15 minutes. It is preferable to be able to complete the acid treatment in a short time, but if the reaction rate is increased for that purpose, it becomes difficult to adjust the ratio P.

[0144] The controller 800 controls at least one of the reaction rate and time of the acid treatment so that the carbonates are partially removed, for example, so that the proportion P after the acid treatment falls within the above range.

[0145] According to one example, under the condition that the ratio P before the acid treatment is almost constant and the concentration of the dilute hydrochloric acid is also almost constant, the relationship between the temperature of the dilute hydrochloric acid, the time of the acid treatment, and the ratio P after the acid treatment is previously examined. In this case, the controller 800 refers to the output of the temperature sensor and the ratio P to be achieved in the above relationship to determine an appropriate time for the acid treatment, and controls the operation of the acid treatment device 700A so that the acid treatment continues for this time.

[0146] Alternatively, under a situation where the ratio P before the acid treatment is almost constant and the temperature and concentration of the dilute hydrochloric acid are also almost constant, the relationship between the time of the acid treatment and the ratio P after the acid treatment is examined in advance. In this case, the controller 800 determines an appropriate time for the acid treatment by referring to the ratio P to be achieved in the above relationship, and controls the operation of the acid treatment apparatus 700A so that the acid treatment continues for this time.

[0147] The above-mentioned reference operation may be performed by an operator. In this case, the operator inputs the acid treatment time obtained by this reference operation into the controller 800. The controller 800 controls the operation of the acid treatment device 700A so that the acid treatment continues for the input time.

[0148] In the regeneration apparatus 700, the acid treatment in the acid treatment apparatus 700A is followed by cleaning in the first cleaning apparatus 700B. The liquid DHC1 discharged from the acid treatment apparatus 700A contains phosphor particles from which carbonates have been partially removed, and dilute hydrochloric acid. Metal elements contained in the carbonates are dissolved in this dilute hydrochloric acid. In the first cleaning apparatus 700B, cleaning is performed using pure water, so that the hydrochloric acid and the dissolved metal elements can be removed.

[0149] In the regeneration apparatus 700, cleaning in the first cleaning apparatus 700B is followed by cleaning in the second cleaning apparatus 700C. In the second cleaning apparatus 700C, cleaning is performed using an organic solvent, so that water is replaced with the organic solvent.

[0150] Thereafter, the slurry containing the wavelength converting material and the organic solvent is sent from the regenerator 700 via the pipeline L6 to the drying device 900. The drying device 900 removes the organic solvent from the slurry to obtain a regenerated wavelength converting material in the form of a powder.

[0151] <4> Photosensitive resin composition The photosensitive resin composition contains a wavelength converting material and a photosensitive resin.

[0152] <4.1> Wavelength conversion materials The wavelength converting material is, for example, a phosphor containing metal elements such as Sr, Ca, Al, Si, Eu, Ba, and Mg. The wavelength converting material includes not only non-agglomerated particles, but also particle agglomerates.

[0153] An example of a red phosphor particle has the general formula MAlSiN3:Eu 2+ (M is Sr or a combination of Sr and one or more selected from Mg, Ca and Ba; Eu 2+ An example of a blue phosphor particle is a phosphor particle containing a crystal represented by the general formula (Ba, Sr, Ca, Mg) 10 These are phosphor particles containing crystals represented by (PO4)6Cl2:Eu. These have high moisture resistance and do not dissolve in the developer. However, if they remain in the developer, elements such as Sr, Ca, and Ba may form carbonates on the particle surface.

[0154] An example of a green phosphor particle has the general formula MGa2S4:Eu 2+ (M is one or more selected from Sr, Ba and Ca, and Eu 2+The phosphor particles contain crystals represented by the formula (wherein represents the luminescence center). These phosphor particles contain sulfur element, and the light conversion property is inactivated by immersion in an aqueous solution such as a developer. These phosphor particles can be made moisture resistant by coating them with an oxide film containing one or more oxides of Si, Al, Ti, Zr, Sn, and Zn, or by coating them with a film made of phosphate.

[0155] In addition, the phosphor particles coated with this oxide or phosphate do not produce carbonates of the metal elements contained therein by reaction with the developer components. Therefore, a wavelength conversion layer containing such phosphor particles can be formed by the same system and method as those described with reference to Figures 2 to 5, except that the regeneration device 700 and the regeneration process using it are omitted.

[0156] The coating layer made of this oxide or phosphate can play the same optical role as that of the coating layer made of carbonate, which will be described later. The refractive index n of the oxide that the coating layer can contain is described below.

[0157] SiO2(n=1.46) Al2O3(n=1.65) TiO2(n=2.52) ZrO2(n=2.1) SnO2 (n=2.01) ZnO(n=1.9) These refractive indices are for light having a wavelength within the range of 530 to 550 nm.

[0158] The particle size distribution of the wavelength conversion material by the laser diffraction / scattering method is, for example, the difference W between the maximum particle size and the minimum particle size. orig is in the range of 1 to 20 μm, and the volume-based median diameter D 50 The particle size distribution of the wavelength converting material by a laser diffraction / scattering method is preferably such that the median diameter D is within a range of 3.5 to 4.5 μm in a volume-based cumulative distribution. 50 and has a 90% diameter D in the range of 7.0 to 8.4 μm. 90It has.

[0159] When the thickness of the partition layer 34, i.e., the height of the partition walls, is within the range of 10 to 50 μm, the particle size of the wavelength converting material is preferably 0.7 times or less the height of the partition walls. When the wavelength converting material contains aggregates, the aggregates can be at least partially eliminated by using ultrasonic or vibration stirring before coating the photosensitive resin composition. If excessively large particles are piled up in the thickness direction in the space surrounded by the partition walls, the wavelength converting layer may protrude from the partition layer 34.

[0160] <4.2> Photosensitive resin The photosensitive resin contains, for example, a polymerizable compound and a photopolymerization initiator, and may further contain at least one of a siloxane resin and a solvent.

[0161] <4.2.1> Polymerizable compounds The photopolymerizable compound is a resin that is polymerized and hardened by irradiation with active energy rays such as ultraviolet rays. As the photopolymerizable compound, for example, a monofunctional, bifunctional, or trifunctional or higher functional (meth)acrylate monomer can be used.

[0162] In this specification, "(meth)acrylate" is a general term for both acrylate and methacrylate, and "(meth)acryloyl" is a general term for both acryloyl and methacryloyl.

[0163] Examples of monofunctional (meth)acrylate compounds include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfuryl acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isobornyl (meth)acrylate. acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phosphate (meth)acrylate, ethylene oxide modified phosphate (meth)acrylate, phenoxy (meth)acrylate, ethylene oxide modified phenoxy (meth)acrylate, propylene oxide ethylene oxide modified phenoxy (meth)acrylate, nonylphenol (meth)acrylate, ethylene oxide modified nonylphenol (meth)acrylate, propylene oxide modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, p) acryloyloxyethyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hexahydrohydrogen phthalate, 2-(meth)acryloyloxypropyl tetrahydrohydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate, 2-adamantane,Examples of the mono(meth)acrylate include adamantane derivative mono(meth)acrylates such as adamantyl acrylate having a monovalent mono(meth)acrylate derived from an adamantanediol.

[0164] Examples of bifunctional (meth)acrylate compounds include di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate.

[0165] Examples of trifunctional or higher (meth)acrylate compounds include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, and glycerin tri(meth)acrylate, as well as trifunctional (meth)acrylate compounds such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate. and polyfunctional (meth)acrylate compounds having three or more functional groups such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ditrimethylolpropane hexa(meth)acrylate, as well as polyfunctional (meth)acrylate compounds in which a portion of these (meth)acrylates is substituted with an alkyl group or ε-caprolactone.

[0166] In addition, urethane (meth)acrylate can also be used as the photopolymerizable compound. Examples of the urethane (meth)acrylate include those obtained by reacting a polyester polyol with an isocyanate monomer or a prepolymer, and then reacting the resulting product with a (meth)acrylate monomer having a hydroxyl group.

[0167] Examples of urethane (meth)acrylates include pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate toluene diisocyanate urethane prepolymer, pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate isophorone diisocyanate urethane prepolymer, and the like.

[0168] The above-mentioned (meth)acrylate compounds may be used alone or in combination of two or more. In addition, the above-mentioned (meth)acrylate compounds may be monomers in the photosensitive resin composition, or may be partially polymerized oligomers.

[0169] The content of the polymerizable compound is preferably in the range of 0.01 to 20% by mass, more preferably in the range of 1 to 10% by mass, based on the total mass of the solid content of the photosensitive resin. Increasing the content of the polymerizable compound increases the transparency of the wavelength conversion layer. However, excessively increasing the content of the polymerizable compound reduces the handleability of the photosensitive resin or the photosensitive resin composition.

[0170] <4.2.2> Photopolymerization initiator A photopolymerization initiator is a compound that generates radicals when irradiated with ultraviolet light.

[0171] Examples of the photopolymerization initiator include benzoins (benzoin alkyl ethers such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether), phenyl ketones [e.g., acetophenones (e.g., acetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, and 1,1-dichloroacetophenone), alkyl phenyl ketones such as 2-hydroxy-2-methylpropiophenone, and cycloalkyl phenyl ketones such as 1-hydroxycyclohexyl phenyl ketone], aminoacetophenones {2-methyl-1-[4-(methylthio)phenyl ]-2-morpholinoaminopropanone-1, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, etc.}, anthraquinones (anthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 1-chloroanthraquinone, etc.), thioxanthones (2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone, etc.), ketals (acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.), benzophenones (benzophenone, etc.), xanthones, phosphine oxides (for example, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, etc.), etc. These photopolymerization initiators may be used alone or in combination of two or more.

[0172] The content of the photopolymerization initiator is preferably in the range of 0.01 to 20% by mass, more preferably in the range of 0.1 to 5% by mass, based on the total mass of the solid content of the photosensitive resin. By increasing the content of the photopolymerization initiator, the coating film made of the photosensitive resin composition can be cured more reliably. In addition, if the content of the photopolymerization initiator is not excessively high, the transparency of the wavelength conversion layer is unlikely to decrease due to the remaining unreacted photopolymerization initiator.

[0173] <4.2.3> Siloxane resin The photosensitive resin and the photosensitive resin composition preferably contain a siloxane resin. The siloxane resin has high heat resistance and light resistance, and the change in transmittance of short wavelengths around 400 nm caused by heat or light degradation is small. Therefore, the siloxane resin enhances the heat resistance and yellowing resistance of the wavelength conversion layer.

[0174] Examples of monomers for siloxane resins include Pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane,1,3,5,7,9,11,13-heptamethyl-15-phenyl-(CAS No.18616-10-9) and Pentacyclo[9.5.1. 13,9 .1 5,15 .1 7,13 ]octasiloxane,1,3,5,7,9,13-hexamethyl-11,15-diphenyl-(CAS No.18421-62-0) and other complete cage silsesquioxanes.

[0175] In the above photosensitive resin or photosensitive resin composition, the ratio A / C of the content A of the siloxane resin to the content C of the polymerizable compound is preferably in the range of 1 to 8000, more preferably in the range of 1 to 1000, further preferably in the range of 5 to 500, and particularly preferably in the range of 10 to 100. Increasing the ratio A / C enhances the heat resistance and yellowing resistance of the wavelength converting layer. As long as the ratio A / C is not excessively large, the transparency of the wavelength converting layer is not impaired.

[0176] <4.2.4> Solvents The photosensitive resin and the photosensitive resin composition may contain a solvent, such as an organic solvent.

[0177] Examples of organic solvents include ethers, ketones, esters, and cellosolves. Examples of ethers include dibutyl ether, dimethoxymethane, dimethoxyethane, diethoxyethane, propylene oxide, 1,4-dioxane, 1,3-dioxolane, 1,3,5-trioxane, tetrahydrofuran, anisole, and phenetole. Examples of ketones include acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, and ethylcyclohexanone. Examples of esters include ethyl formate, propyl formate, n-pentyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, n-pentyl acetate, and γ-butyrolactone. Examples of cellosolves include methyl cellosolve, cellosolve (ethyl cellosolve), butyl cellosolve, cellosolve acetate, etc. The organic solvent may be used alone or in combination of two or more kinds.

[0178] <5> Recycled wavelength conversion materials The used developer further contains wavelength conversion materials, polymerizable compounds, photopolymerization initiators, siloxane resins, etc., in addition to the inorganic components originally contained in the developer. When the wavelength conversion material recovered from the used developer contains impurities such as inorganic components, polymerizable compounds, photopolymerization initiators, and siloxane resins at high concentrations, the photosensitive layer formed from the photosensitive resin composition consisting of the wavelength conversion material recovered and the photosensitive resin is inferior in photosensitivity, developability, and curability to the photosensitive layer formed from the photosensitive resin composition consisting of unused wavelength conversion material and photosensitive resin. In addition, the wavelength conversion layer formed from the former photosensitive resin composition is inferior in wavelength conversion properties to the wavelength conversion layer formed from the latter photosensitive resin composition.

[0179] In the above-described system and method, the above-mentioned impurities are removed from the recovered wavelength conversion material by cleaning in the cleaning device 600. Therefore, the regenerated product obtained from the recovered wavelength conversion material has a low impurity content.

[0180] Moreover, the recycled wavelength converting material has a sufficiently small carbonate content, and the coating layer made of this carbonate can enhance the light scattering properties of the particles, as will be explained below. Therefore, the recycled wavelength converting material can achieve the same brightness as a new wavelength converting material without increasing the amount of the recycled wavelength converting material used.

[0181] FIG. 5 is a cross-sectional view illustrating a wavelength converting material according to one embodiment of the present invention. The wavelength converting material PP shown in Fig. 5 is an example of a regenerated product obtained by the above-mentioned system and method. This wavelength converting material PP includes phosphor particles P1 and a coating layer P2. The coating layer P2 is a carbonate residue formed on the surface of the phosphor particles P1.

[0182] 5, the wavelength converting material PP and the phosphor particles P1 are depicted as being spherical, but in reality, they are irregular in shape. The growth and dissolution of carbonate do not proceed uniformly throughout the particle. Therefore, the wavelength converting material PP has irregularities on its surface, and also has irregularities of a different shape at the interface between the phosphor particles P1 and the coating layer P2.

[0183] Therefore, in a wavelength converting layer containing a recycled wavelength converting material PP, scattering of excitation light is more likely to occur in the wavelength converting layer than in a wavelength converting layer containing a new wavelength converting material PP, i.e., in the former case, the probability that excitation light will be incident on the wavelength converting material is higher than in the latter case.

[0184] The coating layer P2 may contain, for example, one or more carbonates of strontium, calcium, and barium. The refractive index of strontium carbonate is 1.67, the refractive index of calcium carbonate is 1.65, and the refractive index of barium carbonate is 1.67. These refractive indices are smaller than the refractive index of the phosphor particles P1 and larger than the refractive index of the resin contained in the wavelength conversion layer. The refractive index of the phosphor particles P1 is, for example, in the range of 2 to 3. The refractive index of the resin contained in the wavelength conversion layer is, for example, in the range of 1.45 to 1.55. The above refractive indexes and the refractive index described later are refractive indices for light having a wavelength in the range of 530 to 550 nm.

[0185] When the refractive indexes satisfy the above relationship, the excitation light incident obliquely on the wavelength converting material PP is refracted at the interface between the resin and the coating layer P2 and at the interface between the coating layer P2 and the phosphor particles P1, and the traveling direction approaches the vertical direction. In this case, the distance from when the excitation light enters the phosphor particles P1 to when it exits is longer than when the refractive index does not satisfy the above relationship. Therefore, when the refractive indexes satisfy the above relationship, the probability that the excitation light is utilized for fluorescence is higher.

[0186] In this way, in the wavelength converting layer containing the recycled wavelength converting material PP, the excitation light is more likely to be utilized for fluorescence, and therefore, when the recycled wavelength converting material PP is used, the luminance can be equivalent to that when a new wavelength converting material is used, even though the amount of phosphor particles P1 is small.

[0187] When the refractive indexes satisfy the above relationship, the refractive index of the coating layer P2 is preferably in the range of 1.5 to 1.9. The difference between the refractive index of the coating layer P2 and the refractive index of the resin contained in the wavelength conversion layer is preferably 0.05 or more. There is no upper limit to this difference, but the smallest refractive index of a typical resin is about 1.48.

[0188] The thickness of the coating layer P2 is preferably in the range of 1 / 4 of the shortest wavelength in the visible light range to the longest wavelength in the visible light range, and more preferably in the range of 100 to 500 nm. If the coating layer P2 is made thicker, the ratio of the phosphor particles P1 in the wavelength conversion material PP decreases. If the coating layer P2 is made thin, the photoluminescence quantum yield is likely to decrease and the spectral peak wavelength is likely to shift due to the acid treatment. In addition, if the coating layer P2 is made thin, it may be difficult to obtain the optical effects described above for the coating layer P2.

[0189] The wavelength converting material PP has a particle size distribution substantially similar to that of unused wavelength converting material. Preferably, the particle size distribution of the recovered wavelength converting material measured by a laser diffraction / scattering method has a median diameter D in the range of 3.5 to 4.5 μm in a volume-based cumulative distribution. 50 and has a 90% diameter D in the range of 7.0 to 8.4 μm. 90 It has.

[0190] As described above, the wavelength converting material PP can be used as a material for the wavelength converting layer. When the wavelength converting material PP is used as a material for the wavelength converting layer, it is possible to realize excellent photosensitivity, developability, curability, and wavelength converting characteristics, similar to the case of using a new wavelength converting material. That is, the above technology makes it possible to recycle the wavelength converting material. In addition, since the wavelength converting material is expensive, it is possible to reduce the manufacturing costs of display devices and the like by reusing the wavelength converting material.

[0191] In addition, phosphor particles coated with carbonate may be used as new wavelength converting material. Such wavelength converting material does not generate new carbonate by development. Therefore, the regenerating device 700 and the acid treatment described with reference to Figs. 2 and 4 can be omitted.

[0192] In such a wavelength converting material, the carbonate is, for example, one or more of strontium carbonate, calcium carbonate, and barium carbonate. The proportion P in this wavelength converting material is preferably within the above-mentioned range. In addition, in this wavelength converting material, the thickness of the coating layer made of carbonate is preferably within the above-mentioned range.

[0193] For example, a coating layer made of carbonate can be formed on phosphor particles by stirring the phosphor particles in an aqueous solution of sodium hydroxide and sodium carbonate, or a coating layer made of carbonate can be formed on phosphor particles by stirring the phosphor particles in an aqueous solution of sodium hydroxide in which carbon dioxide gas is bubbled. EXAMPLES

[0194] Tests carried out in relation to the present invention are described below.

[0195] (1) Test A (1.1) Example 1A A black matrix substrate 3 was produced for the display device 1 shown in Fig. 1. In this example, the second wavelength conversion layer 36G and the filling layer 36B were omitted.

[0196] Specifically, the transparent substrate 31 is made of a material having a linear expansion coefficient of 3×10 -6 / ° C. and a rectangular low expansion glass plate having dimensions of 320 mm×400 mm was used.

[0197] The partition layer 34 had a two-layer structure of a resin layer and a metal layer. The resin layer had through holes at the positions of the first through holes. The resin layer was formed to a thickness of 20 μm. The metal layer was made of an Al-Nd alloy containing 2 mass % Nd, and had a thickness of 200 nm. The metal layer was formed so as to cover the upper surface of the resin layer and the side walls of the through holes provided in the resin layer.

[0198] The first wavelength conversion layer 36R was formed by the following method: First, a wavelength conversion material was mixed with a photosensitive resin containing an acrylic-siloxane resin, a photopolymerization initiator, and a polymerizable compound to prepare a photosensitive resin composition.

[0199] The wavelength conversion material is (Sr,Ca)AlSiN3:Eu 2+ The phosphor used was one that converts light with a wavelength of 450 nm into light with a wavelength of 636 nm.

[0200] The photosensitive layer made of the photosensitive resin composition was formed to a thickness of 14 μm. For pattern exposure of the photosensitive layer, a light-transmitting photomask was used in the region corresponding to the first wavelength conversion layer 36R and the region corresponding to the alignment mark, etc., and exposure was performed with ihg rays.

[0201] The development of the photosensitive layer and the acquisition of the regenerated wavelength converting material were carried out by the method described with reference to FIGS.

[0202] A sodium bicarbonate solution was used as the developer. A nozzle tip 222 that sprays the developer in a fan shape was used. Spray development was performed at a spray pressure of 0.2 MPa so that droplets with an average particle size of 20 to 100 μm as measured by the laser Doppler method were discharged from the nozzle tip 222.

[0203] In the cleaning device 600, the used developer and the like were filtered by pressure filtration. In these filtrations, a filter paper (product name: No. 5C, manufactured by Kiriyama Seisakusho) made of cellulose fiber and having a retention particle size of 1 μm was used as the filter.

[0204] In the cleaning device 600, the cycle of cleaning with pure water and filtration was repeated until the pH of the filtrate became 8 or less.

[0205] In addition, acetone was used as the organic solvent in the cleaning device 600. A cycle of cleaning with acetone and filtration was repeated multiple times to remove impurities soluble in acetone. In each cycle, the mass of acetone was 5 times the mass of the filter cake.

[0206] In the regeneration device 700, dilute hydrochloric acid with a hydrochloric acid concentration of 1% (0.3 mol / L) was used for the acid treatment. The acid treatment was carried out for 20 minutes with the temperature of the dilute hydrochloric acid set to 25° C. Cleaning in the regeneration device 700 was carried out in the same manner and under the same conditions as cleaning in the cleaning device 600.

[0207] The above-mentioned differential thermogravimetric analysis was performed on each of the thus obtained regenerated wavelength converting material and the new wavelength converting material to determine the proportion P of carbon dioxide derived from the carbonate in the complex of the carbonate and the phosphor particles. The differential thermogravimetric analysis was performed in the temperature range of 30 to 540°C using a differential thermogravimetric analyzer STA7200RV manufactured by Hitachi High-Tech Science Corporation. The above-mentioned ratio (M0A-M10) / M0A for the new wavelength converting material was 2%. As a result, the proportion P of the regenerated wavelength converting material was 1 mass % as shown in Table 1 below.

[0208] The emission characteristics of the recycled wavelength converting material and the new wavelength converting material were also investigated. Light with a wavelength of 450 nm was used as the excitation light, and the emission characteristics were examined using a luminance meter manufactured by Topcon Corporation. As a result, the emission intensity of the recycled wavelength converting material was about 4% lower than that of the new wavelength converting material, as shown in Table 1 below. Furthermore, the emission peak wavelength of the recycled wavelength converting material was 636 nm, the same as that of the new wavelength converting material.

[0209] (1.2) Example 2A A regenerated wavelength converting material was obtained in the same manner as in Example 1A, except that the time of the acid treatment was shortened to 15 minutes. The proportion P of this regenerated wavelength converting material was also determined, and the luminescence characteristics were examined. As a result, the proportion P of this regenerated wavelength converting material was 2 mass % as shown in Table 1 below. Furthermore, the luminescence intensity of this regenerated wavelength converting material was about 2% lower than that of a new wavelength converting material, as shown in Table 1 below. The luminescence peak wavelength of this regenerated wavelength converting material was 636 nm, which was the same as the luminescence peak wavelength of the new wavelength converting material.

[0210] (1.3) Example 3A A regenerated wavelength converting material was obtained in the same manner as in Example 1A, except that the time of the acid treatment was shortened to 10 minutes. The proportion P of this regenerated wavelength converting material was also determined, and the luminescence characteristics were examined. As a result, the proportion P of this regenerated wavelength converting material was 3 mass % as shown in Table 1 below. Furthermore, the luminescence intensity of this regenerated wavelength converting material was equal to that of a new wavelength converting material, as shown in Table 1 below. The luminescence peak wavelength of this regenerated wavelength converting material was 636 nm, which was the same as that of the new wavelength converting material.

[0211] (1.4) Example 4A A regenerated wavelength converting material was obtained in the same manner as in Example 1A, except that the time of the acid treatment was shortened to 6 minutes. The proportion P of this regenerated wavelength converting material was also determined, and the luminescence characteristics were examined. As a result, the proportion P of this regenerated wavelength converting material was 4 mass %, as shown in Table 1 below. Furthermore, the luminescence intensity of this regenerated wavelength converting material was equal to that of a new wavelength converting material, as shown in Table 1 below. The luminescence peak wavelength of this regenerated wavelength converting material was 636 nm, which was the same as that of the new wavelength converting material.

[0212] (1.5) Comparative Example 1A A recycled wavelength converting material was obtained by carrying out the same method as in Example 1A, except that the treatment by the regenerating device 700 was omitted. The proportion P of this recycled wavelength converting material was also determined, and the luminescence characteristics were examined. As a result, the proportion P of this recycled wavelength converting material was 6 mass % as shown in Table 1 below. Furthermore, the luminescence intensity of this recycled wavelength converting material was equal to that of a new wavelength converting material, as shown in Table 1 below. The peak luminescence wavelength of this recycled wavelength converting material was 636 nm, the same as that of the new wavelength converting material.

[0213] (1.6) Comparative example 2A A regenerated wavelength converting material was obtained in the same manner as in Example 1A, except that the acid cleaning time was extended to 25 minutes. The proportion P of this regenerated wavelength converting material was also determined, and the luminescence characteristics were examined. As a result, the proportion P of this regenerated wavelength converting material was 0 mass %, as shown in Table 1 below. Furthermore, the luminescence intensity of this regenerated wavelength converting material was about 6% lower than that of a new wavelength converting material, as shown in Table 1 below. Furthermore, the luminescence peak wavelength of this regenerated wavelength converting material shifted to 630 nm from 636 nm, which is the luminescence peak wavelength of the new wavelength converting material.

[0214] [Table 1]

[0215] (2) Test B (2.1) Example 1B A black matrix substrate 3 was produced for the display device 1 shown in Fig. 1. In this example, the second wavelength conversion layer 36G and the filling layer 36B were omitted.

[0216] Specifically, the transparent substrate 31 is made of a material having a linear expansion coefficient of 3×10 -6 / ° C. and a rectangular low expansion glass plate having dimensions of 320 mm×400 mm was used.

[0217] The partition layer 34 had a two-layer structure of a resin layer and a metal layer. The resin layer had through holes at the positions of the first through holes. The resin layer was formed to a thickness of 15 μm. The metal layer was made of an Al-Nd alloy containing 2 mass % Nd, and had a thickness of 200 nm. The metal layer was formed so as to cover the upper surface of the resin layer and the side walls of the through holes provided in the resin layer.

[0218] The first wavelength conversion layer 36R was formed by the following method: First, a wavelength conversion material was mixed with a photosensitive resin containing an acrylic-siloxane resin, a photopolymerization initiator, and a polymerizable compound to prepare a photosensitive resin composition.

[0219] The wavelength conversion material is (Sr,Ca)AlSiN3:Eu 2+ The phosphor particles represented by the formula (I) were coated with a coating layer made of strontium carbonate. The phosphor particles convert light with a wavelength of 450 nm to light with a wavelength of 636 nm. The coating layer was formed by stirring the phosphor particles in an aqueous solution of sodium hydroxide and sodium carbonate for one day, filtering and washing the solution. The coating layer had a thickness of 300 nm and a ratio P of 2%. The particle size of the wavelength conversion material was distributed in the range of 1 to 20 μm.

[0220] The photosensitive layer made of the photosensitive resin composition was formed to a thickness of 14 μm. For pattern exposure of the photosensitive layer, a light-transmitting photomask was used in the region corresponding to the first wavelength conversion layer 36R and the region corresponding to the alignment mark, etc., and exposure was performed with ihg rays. The photosensitive layer was developed by the method described with reference to FIG. 2.

[0221] The first wavelength conversion layer 36R of the black matrix substrate 3 thus obtained was irradiated with light having a wavelength of 450 nm as excitation light, and the emission intensity was measured using a CS-1000 manufactured by Konica Minolta, Inc. As a result, the emission intensity was 0.129 cd / m 2 It was.

[0222] (2.2) Comparative example 1B A black matrix substrate 3 of the display device 1 shown in FIG. 1 was produced in the same manner as in Example 1B, except that the covering layer was omitted from the wavelength converting material. Note that the second wavelength conversion layer 36G and the filling layer 36B were also omitted in this example. The particle size of the wavelength converting material used in this example was distributed in the range of 1 to 20 μm. The luminous intensity of the first wavelength conversion layer 36R of the black matrix substrate 3 thus obtained was measured in the same manner as in Example 1B. As a result, the luminous intensity was 0.114 cd / m 2 It was.

[0223] (3) Test C (3.1) Reference example 1C A black matrix substrate 3 for the display device 1 shown in Fig. 1 was produced. In this example, the first wavelength conversion layer 36R and the filling layer 36B were omitted.

[0224] Specifically, the transparent substrate 31 is made of a material having a linear expansion coefficient of 3×10 -6 / ° C. and a rectangular low expansion glass plate having dimensions of 320 mm×400 mm was used.

[0225] The partition layer 34 had a two-layer structure of a resin layer and a metal layer. The resin layer had through holes at the positions of the first through holes. The resin layer was formed to a thickness of 15 μm. The metal layer was made of an Al-Nd alloy containing 2 mass % Nd, and had a thickness of 200 nm. The metal layer was formed so as to cover the upper surface of the resin layer and the side walls of the through holes provided in the resin layer.

[0226] The second wavelength conversion layer 36G was formed by the following method: First, a wavelength conversion material was mixed with a photosensitive resin containing an acrylic-siloxane resin, a photopolymerization initiator, and a polymerizable compound to prepare a photosensitive resin composition.

[0227] The wavelength conversion material is (Sr,Ba)Ga2S4:Eu 2+The phosphor particles represented by the formula (I) were coated with a coating layer made of phosphate (refractive index n=1.63) and used. The phosphor particles convert light with a wavelength of 450 nm to light with a wavelength of 540 nm. The coating layer was formed by stirring an aqueous solution of phosphate radical containing the phosphor particles, filtering it, and then baking and drying it. The thickness of the coating layer was 200 nm. The particle size of the wavelength conversion material was distributed within the range of 1 to 18 μm.

[0228] The photosensitive layer made of the photosensitive resin composition was formed to a thickness of 14 μm. For pattern exposure of the photosensitive layer, a light-transmitting photomask was used in the region corresponding to the second wavelength conversion layer 36G and the region corresponding to the alignment mark, etc., and exposure was performed with ihg rays. The photosensitive layer was developed by the method described with reference to FIG. 2.

[0229] The second wavelength conversion layer 36G of the black matrix substrate 3 thus obtained was irradiated with light having a wavelength of 450 nm as excitation light, and the emission intensity was measured using a CS-1000 manufactured by Konica Minolta, Inc. As a result, the emission intensity was 0.250 cd / m 2 It was.

[0230] In addition, a recovered wavelength converting material was obtained by carrying out the same method as that described with reference to Figures 2 to 4, except that the processing by the regenerating device 700 was omitted. The luminescence characteristics of this recycled wavelength converting material were also investigated. As a result, luminescence brightness comparable to that of a new wavelength converting material was obtained.

[0231] (3.2) Comparative example 1C A black matrix substrate 3 of the display device 1 shown in FIG. 1 was produced in the same manner as in Reference Example 1C, except that the covering layer was omitted from the wavelength converting material. Note that the first wavelength conversion layer 36R and the filling layer 36B were also omitted in this example. The particle size of the wavelength converting material used in this example was distributed in the range of 1 to 20 μm. The luminous intensity of the second wavelength conversion layer 36G of the black matrix substrate 3 thus obtained was measured in the same manner as in Reference Example 1C. As a result, the luminous intensity was 0.220 cd / m 2 It was.

[0232] In addition, a recovered wavelength conversion material was obtained by carrying out the same method as that described with reference to Figures 2 to 4, except that the processing by the regeneration device 700 was omitted. The luminescence characteristics of this recycled wavelength conversion material were also examined. As a result, no luminescence was generated. [Explanation of symbols]

[0233] 1...display device, 2...light control device, 3...black matrix substrate, 4...adhesive layer, 21...substrate, 22...multilayer wiring layer, 23...light emitting diode, 31...transparent substrate, 32...black matrix, 33B...undercoat layer, 33G...second colored layer, 33R...first colored layer, 34...partition wall layer, 36B...filling layer, 36G...second wavelength conversion layer, 36R...first wavelength conversion layer, 100...regeneration system, 200...spray developing device, 210...developing container, 220...spray nozzle assembly, 221...header, 222... nozzle tip, 230... transport device, 231... transport roller, 300... developer storage tank, 400... circulation pump, 500... filtration device, 600... cleaning device, 600A... filtration device, 600B... first cleaning device, 600C... second cleaning device, 610A... container, 610B... container, 610C... container, 620A... filter, 620B... filter, 620C... filter, 630B... valve, 630C... valve, 640B... pump, 640C... pump, 700... regeneration device, 700A ...acid treatment device, 700B...first cleaning device, 700C...second cleaning device, 710A...container, 710B...container, 710C...container, 720A...filter, 720B...filter, 720C...filter, 730B...valve, 730C...valve, 740B...pump, 740C...pump, 800...controller, 900...drying device, DHC1...liquid, DHC2...liquid, DL1...developing solution, DL2...liquid, DL3...developing solution, L1...pipe, L2...pipe, L3...pipe, L4...pipe, L5...pipe , L6...Pipeline, L7A...Pipeline, L8A...Pipeline, L8B...Pipeline, L8C...Pipeline, L9B...Pipeline, L9C...Pipeline, L10...Pipeline, L11...Pipeline, L14...Pipeline, L17A...Pipeline, L18A...Pipeline, L18B...Pipeline, L18C...Pipeline, L 19B...pipe, L19C...pipe, L20...pipe, P1...phosphor particles, P2...coating layer, PP...wavelength conversion material, WL1B...liquid, WL1C...liquid, WL2B...liquid, WL2C...liquid, WL3B...liquid, WL3C...liquid, WL4B...liquid, WL4C...liquid.

Claims

1. A wavelength conversion material comprising phosphor particles and a coating layer coating the phosphor particles, the coating layer being made of a metal carbonate containing one or more selected from the group consisting of strontium, calcium and barium, and a proportion of carbon dioxide in the total of the phosphor particles and the carbonate being within a range of 1 to 4 mass %.

2. 2. The wavelength converting material according to claim 1, which is a recycled product obtained by recycling particles recovered from a used developer after exposure and development of a photosensitive layer containing phosphor particles and a photosensitive resin.

3. The wavelength converting material according to claim 1 , wherein the refractive index of the coating layer is smaller than the refractive index of the phosphor particles.

4. The phosphor particles have the general formula MAlSiN 3 :Eu 2+ (M is Sr or a combination of Sr and one or more selected from Mg, Ca, and Ba; Eu 2+ represents a luminescence center), and a red phosphor particle containing a crystal represented by the general formula (Ba, Sr, Ca, Mg) 10 (P.O. 4 ) 6 C 2 2. The wavelength converting material according to claim 1, comprising blue phosphor particles containing crystals represented by: Eu.

5. The particle size distribution by the laser diffraction / scattering method shows that the median diameter D is in the range of 3.5 to 4.5 μm in the cumulative distribution based on the volume. 50 and a 90% diameter D in the range of 7.0 to 8.4 μm. 90 The wavelength converting material according to claim 1 ,

6. A method for manufacturing a display device, comprising sequentially exposing and developing a photosensitive layer containing the wavelength converting material according to claim 1 and a photosensitive resin.

7. A display device comprising the wavelength converting material according to any one of claims 1 to 5.

8. 8. The display device according to claim 7, comprising a plurality of wavelength conversion layers, one or more of the plurality of wavelength conversion layers containing the wavelength conversion material, the phosphor particles contained therein being red or blue phosphor particles, and one or more of the plurality of wavelength conversion layers containing a wavelength conversion material having green phosphor particles and a coating layer made of an oxide or phosphate coating the green phosphor particles.

9. a photosensitive layer including phosphor particles and a photosensitive resin, the phosphor particles including one or more selected from the group consisting of strontium, calcium, and barium, and then spray-developing the photosensitive layer; filtering the developer used in the spray development to recover the phosphor particles contained therein; treating the recovered phosphor particles with dilute hydrochloric acid to partially remove carbonates formed on the surfaces of the phosphor particles by reaction with components contained in the developer; A method for producing a regenerated wavelength conversion material comprising the steps of:

10. 10. The method for producing a regenerated wavelength conversion material according to claim 9, wherein the carbonate is partially removed so that a ratio of carbon dioxide in the total of the phosphor particles and the carbonate is within a range of 1 to 4 mass %.

11. a spray developing device that spray-develops the exposed photosensitive layer, the photosensitive layer including phosphor particles and a photosensitive resin; a filtering device for filtering the developer used in the spray development to recover phosphor particles contained therein; a regeneration device for treating the recovered phosphor particles with dilute hydrochloric acid to partially remove carbonates formed on the surfaces of the phosphor particles by reaction with components contained in the developer; A playback system with

12. The regeneration system described in claim 11, further comprising a controller that controls the operation of the regeneration device so that the proportion of carbon dioxide in the total of the phosphor particles and the carbonate is within the range of 1 to 4 mass % by partially removing the carbonate.

Citation Information

Patent Citations

  • Full color LED display panel

    JP2019028380A

  • Full color LED display panel and manufacturing method thereof

    JP2019140361A