Substrate processing method, substrate processing apparatus, semiconductor device manufacturing method, and semiconductor manufacturing apparatus

By using an organic solvent with uniformly dispersed water to generate a treatment liquid for SAM formation without ultrasonic waves, the method efficiently forms a dense and protective self-assembled monolayer on substrates, addressing the inefficiencies of conventional methods.

JP2024135393APending Publication Date: 2024-10-04SCREEN HOLDINGS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023046049
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional methods struggle to form a self-assembled monolayer (SAM) with high density and protective performance efficiently and in a short time, particularly in semiconductor manufacturing, due to challenges in film formation efficiency and positioning accuracy.

Method used

A substrate processing method involving the use of an organic solvent with uniformly dispersed water, generating a treatment liquid through a hydrolysis reaction without ultrasonic waves, allowing SAM molecules to chemically adsorb onto the substrate surface, thereby forming a dense SAM efficiently.

Benefits of technology

The method enables the formation of a self-assembled monolayer with high density and protective performance in a shorter time, reducing film defects and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135393000001_ABST
    Figure 2024135393000001_ABST
Patent Text Reader

Abstract

To provide a substrate processing method, a substrate processing apparatus, a semiconductor device manufacturing method, and a semiconductor manufacturing apparatus that can efficiently form a self-assembled monolayer with excellent density and protective performance on a substrate surface in a short period of time by suppressing or reducing the occurrence of film defects.SOLUTION: A substrate processing method according to the present invention includes a dispersion liquid generation step S101 of generating a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent, a treatment liquid generation step S102 of adding an SAM-forming material to the dispersion liquid to generate a treatment liquid containing SAM molecules, and a film formation step S103 of contacting the treatment liquid with a surface to chemically adsorb the SAM molecules and form an SAM. The dispersion liquid generation step S101 is a step of generating a dispersion liquid by mixing an organic solvent and water while applying ultrasound, or by mixing an organic solvent and water and then applying ultrasound, and the treatment liquid generation step S102 is a step of generating a treatment liquid without applying ultrasound.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a substrate processing method and substrate processing apparatus capable of efficiently forming a self-assembled monolayer having excellent density and protective performance in a short time, as well as a semiconductor device manufacturing method and semiconductor manufacturing apparatus. [Background technology]

[0002] In the manufacture of semiconductor devices, photolithography is widely used as a technique for selectively forming a film on a specific surface region of a substrate. For example, after forming a lower layer wiring, an insulating film is formed, and a dual damascene structure having trenches and via holes is formed by photolithography and etching, and a conductive film such as Cu is embedded in the trenches and via holes to form wiring.

[0003] However, in recent years, semiconductor devices have become increasingly miniaturized, and there are cases where the alignment accuracy of photolithography is insufficient. For this reason, there is a demand for an alternative to photolithography to selectively form a film in a specific region on the substrate surface with high accuracy.

[0004] For example, Patent Document 1 discloses a method for selectively etching a silicon nitride (SiN) film and a silicon oxide (SiO2) film on a substrate, in which a thermal phosphoric acid resistant material is formed as a SAM on the surface of the silicon oxide film in advance in order to selectively etch the silicon nitride film.

[0005] In order to adequately protect the silicon oxide film from the etching solution, it is necessary to form a highly dense SAM. However, with conventional SAM deposition methods, it is difficult to deposit such a highly dense SAM in a short time, resulting in poor production efficiency. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent No. 5490071 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a substrate processing method and substrate processing apparatus, as well as a semiconductor device manufacturing method and semiconductor manufacturing apparatus, which are capable of efficiently forming a self-assembled monolayer having excellent density and protective performance on a substrate surface in a short time by suppressing or reducing the occurrence of film defects. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems, the substrate processing method according to the present invention is a substrate processing method for forming a self-assembled monolayer on a surface of a substrate, the method comprising: a dispersion generating step of generating a dispersion in which water is uniformly dispersed in an organic solvent as a main solvent; a treatment liquid generating step of adding a material containing a molecule having a functional group exhibiting hydrolysis reactivity and capable of forming the self-assembled monolayer to the dispersion, and generating a treatment liquid containing the molecules having a hydroxyl group and in which the molecules having the hydroxyl group are present without being aggregated by hydrolysis reaction between the water dispersed in the dispersion and the functional group; and a film forming step of forming the self-assembled monolayer by supplying the treatment liquid to the surface of the substrate, the dispersion generating step being a step of mixing the organic solvent and the water while applying ultrasonic waves, or mixing the organic solvent and the water and then applying ultrasonic waves to generate the dispersion, and the treatment liquid generating step being a step performed without applying ultrasonic waves to the dispersion.

[0009] According to the above configuration, in the dispersion liquid generating step, the organic solvent and water are mixed while applying ultrasonic waves, or the organic solvent and water are mixed and then ultrasonic waves are applied to generate a dispersion liquid. As a result, in the dispersion liquid generating step, a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent can be obtained. Furthermore, in the treatment liquid generating step, a material (hereinafter sometimes referred to as a "SAM forming material") containing a molecule (hereinafter sometimes referred to as a "SAM molecule") capable of forming a self-assembled monolayer (hereinafter sometimes referred to as a "SAM") is added to the dispersion liquid obtained in the dispersion liquid generating step without applying ultrasonic waves to generate a treatment liquid. Here, the SAM molecule has a functional group exhibiting hydrolysis reactivity, and water molecules are uniformly dispersed and present in the dispersion liquid. Therefore, when the SAM forming material is added to the dispersion liquid, the functional group exhibiting hydrolysis reactivity in the SAM molecule undergoes a hydrolysis reaction with the water molecules in the dispersion liquid to become a hydroxyl group (OH group). As a result, a treatment liquid containing a SAM molecule having a hydroxyl group can be generated. In addition, in the treatment liquid generating step, the treatment liquid is generated so that the SAM molecules having a hydroxyl group are present without being aggregated with each other. In the treatment liquid generation step, the treatment liquid can be generated without applying ultrasonic waves, so that the SAM molecules having hydroxyl groups are present without agglomerating with each other. By generating the treatment liquid so that the SAM molecules having hydroxyl groups are present without agglomerating with each other, a self-assembled monolayer can be formed satisfactorily in the film formation step.

[0010] Furthermore, in the film formation process, by contacting the surface of the substrate with the treatment liquid, a dehydration condensation reaction occurs between the hydroxyl groups of the SAM molecules and those present on the substrate surface, causing the SAM molecules to be chemically adsorbed. The chemically adsorbed SAM molecules then self-organize to form the SAM.

[0011] In this manner, in the above-mentioned configuration, the SAM molecules to be chemically adsorbed on the substrate surface are hydrolyzed in advance at the stage of generating the treatment liquid to introduce hydroxyl groups. Therefore, compared to forming a SAM using SAM molecules without introducing hydroxyl groups, the hydrolysis reaction of the SAM molecules, which is a rate-limiting step in the SAM film formation process, can be omitted. In addition, since the treatment liquid contains SAM molecules having hydroxyl groups without agglomeration, the dehydration condensation reaction between the SAM molecules having hydroxyl groups and the hydroxyl groups on the substrate surface, which is a rate-limiting step in the SAM film formation process, can be effectively generated. Therefore, the SAM molecules can be chemically adsorbed on the substrate surface at a high density. As a result, in the above-mentioned configuration, even if the SAM molecules are not kept in contact with the substrate surface for a long time to form a dense SAM as in the conventional substrate processing method, the occurrence of film defects can be suppressed, and a SAM with excellent density and protective performance can be efficiently formed in a short time.

[0012] In the above-mentioned configuration, the amount of water added in the dispersion producing step is preferably within a range of 50 ppm or more and 200 ppm or less in the dispersion.

[0013] By adding 50 ppm or more of water, the hydrolysis reaction of the functional groups exhibiting hydrolysis reactivity in the SAM molecules can be prevented from becoming insufficient, and a sufficient amount of SAM molecules with hydroxyl groups introduced can be present in the treatment solution. As a result, it is possible to suppress the occurrence of film defects and form a SAM with excellent density, even without contacting the SAM molecules with the substrate surface for a long time to form a dense SAM, as in the conventional substrate treatment method. On the other hand, by adding 200 ppm or less of water, it is possible to suppress excessive aggregation of SAM molecules having hydroxyl groups due to a dehydration condensation reaction. As a result, it is possible to suppress the decrease in density of the SAM molecules chemically adsorbed on the substrate surface, and to form a SAM with excellent density.

[0014] In the above-mentioned configuration, it is preferable that the treatment liquid generating step includes adding a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid that is left standing.

[0015] When the SAM-forming material is added to the dispersion, if mechanical force such as stirring or shaking is applied to the dispersion, the SAM molecules having hydroxyl groups may aggregate with each other. However, by preparing a treatment liquid by adding the SAM-forming material to a dispersion in a stationary state as in the above configuration, it is possible to produce a treatment liquid in which the aggregation of the SAM molecules having hydroxyl groups with each other is further suppressed.

[0016] In order to solve the above-mentioned problems, the method for manufacturing a semiconductor device of the present invention is a method for manufacturing a semiconductor device, which includes processing a substrate having a laminate on its surface, the laminate including an alternately laminated layer to be protected during etching and an etched layer to be etched, the method including a step of selectively forming a self-assembled monolayer on at least the surface of the protected layer, and a step of selectively etching the etched layer using the self-assembled monolayer as a protective layer, the step of forming the self-assembled monolayer including a dispersion liquid generation step of generating a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent, and a step of selectively etching the self-assembled monolayer having a functional group exhibiting hydrolysis reactivity and a functional group exhibiting hydrolysis reactivity. The method includes a treatment liquid generating step of adding a material containing molecules capable of forming a molecular film to the dispersion liquid, and hydrolyzing the functional groups with water dispersed in the dispersion liquid to generate a treatment liquid containing the molecules in a state having hydroxyl groups and in which the molecules having the hydroxyl groups exist without agglomerating, and a film forming step of forming the self-assembled monolayer by supplying the treatment liquid to the surface of the substrate, wherein the dispersion liquid generating step is a step of mixing the organic solvent and the water while applying ultrasonic waves, or mixing the organic solvent and the water and then applying ultrasonic waves to generate the dispersion liquid, and the treatment liquid generating step is a step performed without applying ultrasonic waves to the dispersion liquid.

[0017] According to the above-mentioned configuration, in the dispersion liquid generating step, the organic solvent and water are mixed while applying ultrasonic waves, or the organic solvent and water are mixed and then ultrasonic waves are applied to generate the dispersion liquid. As a result, in the dispersion liquid generating step, a dispersion liquid in which water is uniformly dispersed in the organic solvent as the main solvent can be obtained. Furthermore, in the treatment liquid generating step, a SAM-forming material containing SAM molecules is added to the dispersion liquid obtained in the dispersion liquid generating step without applying ultrasonic waves to generate the treatment liquid. Here, the SAM molecules have functional groups that exhibit hydrolysis reactivity, and water molecules are uniformly dispersed and present in the dispersion liquid. Therefore, when the SAM-forming material is added to the dispersion liquid, the functional groups that exhibit hydrolysis reactivity in the SAM molecules undergo a hydrolysis reaction with the water molecules in the dispersion liquid to become hydroxyl groups (OH groups). As a result, a treatment liquid containing SAM molecules having hydroxyl groups can be generated. In the treatment liquid generating step, the treatment liquid is generated so that the SAM molecules having hydroxyl groups exist without aggregating with each other. In the treatment liquid generating step, the treatment liquid is generated so that the SAM molecules having hydroxyl groups exist without aggregating with each other by generating the treatment liquid without applying ultrasonic waves. By producing a treatment liquid in which SAM molecules having hydroxyl groups are present without agglomerating with each other, a good self-assembled monolayer can be formed in the film formation step.

[0018] Furthermore, in the film formation process, by contacting the surface of the substrate with the treatment liquid, a dehydration condensation reaction occurs between the hydroxyl groups of the SAM molecules and those present on the substrate surface, causing the SAM molecules to be chemically adsorbed. The chemically adsorbed SAM molecules then self-organize to form the SAM.

[0019] In this manner, in the above-mentioned configuration, the SAM molecules to be chemically adsorbed on the substrate surface are hydrolyzed in advance at the stage of generating the treatment liquid to introduce hydroxyl groups. Therefore, compared to forming a SAM using SAM molecules without introducing hydroxyl groups, the hydrolysis reaction of the SAM molecules, which is a rate-limiting step in the SAM film formation process, can be omitted. In addition, since the treatment liquid contains SAM molecules having hydroxyl groups without agglomeration, the dehydration condensation reaction between the SAM molecules having hydroxyl groups and the hydroxyl groups on the substrate surface, which is a rate-limiting step in the SAM film formation process, can be effectively generated. Therefore, the SAM molecules can be chemically adsorbed on the substrate surface at a high density. As a result, in the above-mentioned configuration, even if the SAM molecules are not kept in contact with the substrate surface for a long time to form a dense SAM as in the conventional semiconductor device manufacturing method, the occurrence of film defects can be suppressed, and a SAM with excellent denseness and protective performance can be efficiently formed in a short time.

[0020] In the above-mentioned configuration, the amount of water added in the dispersion producing step is preferably within a range of 50 ppm or more and 200 ppm or less in the dispersion.

[0021] By adding 50 ppm or more of water, the hydrolysis reaction of the functional group exhibiting hydrolysis reactivity in the SAM molecule can be prevented from becoming insufficient, and a sufficient amount of SAM molecules with hydroxyl groups introduced therein can be present in the treatment solution. As a result, it is possible to suppress the occurrence of film defects and form a SAM with excellent density, even without contacting the SAM molecule with the substrate surface for a long time to form a dense SAM, as in the conventional semiconductor device manufacturing method. On the other hand, by adding 200 ppm or less of water, it is possible to suppress excessive aggregation of SAM molecules having hydroxyl groups due to a dehydration condensation reaction. As a result, it is possible to suppress the decrease in density of the SAM molecules chemically adsorbed on the substrate surface, and to form a SAM with excellent density.

[0022] In the above-mentioned configuration, it is preferable that the treatment liquid generating step includes adding a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid that is left standing.

[0023] When the SAM-forming material is added to the dispersion, if mechanical force such as stirring or shaking is applied to the dispersion, the SAM molecules having hydroxyl groups may aggregate with each other. However, by preparing a treatment liquid by adding the SAM-forming material to a dispersion in a stationary state as in the above configuration, it is possible to produce a treatment liquid in which the aggregation of the SAM molecules having hydroxyl groups with each other is further suppressed.

[0024] In order to solve the above-mentioned problems, the substrate processing apparatus of the present invention is a substrate processing apparatus for forming a self-assembled monolayer on a surface of a substrate, comprising: a processing liquid generation unit for generating a processing liquid containing molecules capable of forming the self-assembled monolayer; an ultrasonic application unit; and a processing liquid supply unit for forming the self-assembled monolayer by supplying the processing liquid generated in the processing liquid generation unit to the surface of the substrate, wherein the processing liquid generation unit generates a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent, and further adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid, and generates the processing liquid containing the molecules having hydroxyl groups and in which the molecules having the hydroxyl groups exist without agglomerating by hydrolysis reaction between the water dispersed in the dispersion liquid and the functional groups, and the ultrasonic application unit applies ultrasonic waves in the processing liquid generation unit when or after mixing the organic solvent and the water to generate the dispersion liquid.

[0025] According to the above configuration, the treatment liquid generating unit generates a mixed liquid by mixing an organic solvent as a main solvent with water. The ultrasonic application unit applies ultrasonic waves when the treatment liquid generating unit mixes the organic solvent with water, or to the mixed liquid generated by mixing the organic solvent with water. As a result, the treatment liquid generating unit can generate a dispersion liquid in which water is uniformly dispersed in the organic solvent. Furthermore, the treatment liquid generating unit generates a treatment liquid by adding a material containing SAM molecules (SAM forming material) to the generated dispersion liquid without applying ultrasonic waves. Here, the SAM molecules have functional groups that exhibit hydrolysis reactivity, and water molecules are uniformly dispersed and present in the dispersion liquid. Therefore, when the SAM forming material is added to the dispersion liquid, the functional groups that exhibit hydrolysis reactivity in the SAM molecules undergo a hydrolysis reaction with the water molecules in the dispersion liquid to become hydroxyl groups (OH groups). As a result, a treatment liquid containing SAM molecules having hydroxyl groups can be generated. The treatment liquid generating unit generates the treatment liquid so that the SAM molecules having hydroxyl groups exist without coagulating with each other. Furthermore, the treatment liquid generating unit can generate the treatment liquid without applying ultrasonic waves, so that the treatment liquid is generated so that the SAM molecules having hydroxyl groups are present without agglomerating with each other. By generating the treatment liquid so that the SAM molecules having hydroxyl groups are present without agglomerating with each other, a self-assembled monolayer can be satisfactorily formed on the surface of the substrate.

[0026] Furthermore, the processing liquid supply unit supplies the processing liquid to the surface of the substrate, thereby bringing the SAM molecules into contact with the substrate surface, which causes a dehydration condensation reaction between the hydroxyl groups of the SAM molecules and the hydroxyl groups present on the substrate surface. As a result, the SAM molecules can be chemically adsorbed onto the substrate surface, and the chemically adsorbed SAM molecules can self-assemble to form a SAM.

[0027] In this manner, in the above-mentioned configuration, the SAM molecules to be chemically adsorbed on the substrate surface are hydrolyzed in advance at the stage of generating the treatment liquid to introduce hydroxyl groups. Therefore, compared to forming a SAM using SAM molecules without introducing hydroxyl groups, the hydrolysis reaction of the SAM molecules, which is a rate-limiting step in the SAM film formation process, can be omitted. In addition, since the treatment liquid contains SAM molecules having hydroxyl groups without agglomeration, the dehydration condensation reaction between the SAM molecules having hydroxyl groups and the hydroxyl groups on the substrate surface, which is a rate-limiting step in the SAM film formation process, can be effectively generated. Therefore, the SAM molecules can be chemically adsorbed on the substrate surface at a high density. As a result, in the above-mentioned configuration, even if the SAM molecules are not kept in contact with the substrate surface for a long time to form a dense SAM as in the conventional substrate processing apparatus, the occurrence of film defects can be suppressed, and a SAM with excellent density and protective performance can be efficiently formed in a short time.

[0028] In the above configuration, it is preferable that the amount of water added when the organic solvent and the water are mixed in the treatment liquid production section is within a range of 50 ppm or more and 200 ppm or less.

[0029] By adding 50 ppm or more of water, the hydrolysis reaction of the functional groups exhibiting hydrolysis reactivity in the SAM molecules can be prevented from becoming insufficient, and a sufficient amount of SAM molecules with hydroxyl groups introduced can be present in the treatment solution. As a result, it is possible to suppress the occurrence of film defects and form a SAM with excellent density, even without contacting the SAM molecules with the substrate surface for a long time to form a dense SAM, as in the conventional substrate treatment apparatus. On the other hand, by adding 200 ppm or less of water, it is possible to suppress excessive aggregation of SAM molecules having hydroxyl groups due to a dehydration condensation reaction. As a result, it is possible to suppress the decrease in density of the SAM molecules chemically adsorbed on the substrate surface, and to form a SAM with excellent density.

[0030] In the above-mentioned configuration, it is preferable that the treatment liquid generating unit adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid that is left standing.

[0031] When adding a SAM-forming material to a dispersion, if mechanical force such as stirring or shaking is applied to the dispersion, there is a possibility that SAM molecules having hydroxyl groups may aggregate with each other. However, as in the above configuration, the treatment liquid generator prepares a treatment liquid by adding a SAM-forming material to a stationary dispersion, so that a treatment liquid can be generated with further suppression of aggregation of SAM molecules having hydroxyl groups with each other.

[0032] In order to solve the above-mentioned problems, the semiconductor manufacturing apparatus of the present invention is a semiconductor manufacturing apparatus for processing a substrate having a laminate provided on its surface, the laminate including an alternately laminated layer to be protected during etching and an etched layer to be etched, the apparatus including a processing solution generating unit for generating a processing solution including molecules capable of forming the self-assembled monolayer, an ultrasonic application unit, a processing solution supply unit for forming the self-assembled monolayer by supplying the processing solution generated in the processing solution generating unit to the surface of the substrate, and a processing solution supply unit for selectively etching the etched layer using the self-assembled monolayer as a protective layer. and an etching unit which removes the water by etching, wherein the treatment liquid generating unit generates a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent, and further adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid, and generates the treatment liquid containing the molecules in a state having hydroxyl groups and in which the molecules having the hydroxyl groups exist without agglomerating by causing a hydrolysis reaction between the water dispersed in the dispersion liquid and the functional groups, and the ultrasonic application unit applies ultrasonic waves when or after mixing the organic solvent and the water in the treatment liquid generating unit to generate the dispersion liquid.

[0033] According to the above configuration, the treatment liquid generating unit generates a mixed liquid by mixing an organic solvent as a main solvent with water. The ultrasonic application unit applies ultrasonic waves when the treatment liquid generating unit mixes the organic solvent with water, or to the mixed liquid generated by mixing the organic solvent with water. As a result, the treatment liquid generating unit can generate a dispersion liquid in which water is uniformly dispersed in the organic solvent. Furthermore, the treatment liquid generating unit generates a treatment liquid by adding a material containing SAM molecules (SAM forming material) to the generated dispersion liquid without applying ultrasonic waves. Here, the SAM molecules have functional groups that exhibit hydrolysis reactivity, and water molecules are uniformly dispersed and present in the dispersion liquid. Therefore, when the SAM forming material is added to the dispersion liquid, the functional groups that exhibit hydrolysis reactivity in the SAM molecules undergo a hydrolysis reaction with the water molecules in the dispersion liquid to become hydroxyl groups (OH groups). As a result, a treatment liquid containing SAM molecules having hydroxyl groups can be generated. The treatment liquid generating unit generates the treatment liquid so that the SAM molecules having hydroxyl groups exist without coagulating with each other. Furthermore, the treatment liquid generating unit can generate the treatment liquid without applying ultrasonic waves, so that the treatment liquid is generated so that the SAM molecules having hydroxyl groups are present without agglomerating with each other. By generating the treatment liquid so that the SAM molecules having hydroxyl groups are present without agglomerating with each other, a self-assembled monolayer can be satisfactorily formed on the surface of the substrate.

[0034] Furthermore, the processing liquid supply unit supplies the processing liquid to the surface of the substrate to bring the SAM molecules into contact with the substrate surface, thereby causing a dehydration condensation reaction between the hydroxyl groups of the SAM molecules and the hydroxyl groups present on the substrate surface. As a result, the SAM molecules can be chemically adsorbed onto the substrate surface, and the chemically adsorbed SAM molecules can self-assemble to form a SAM. Furthermore, the etching unit selectively etches the layer to be etched using the SAM as a protective layer.

[0035] In this manner, in the above-mentioned configuration, the SAM molecules to be chemically adsorbed on the substrate surface are hydrolyzed in advance at the stage of generating the treatment liquid to introduce hydroxyl groups. Therefore, compared to forming a SAM using SAM molecules without introducing hydroxyl groups, the hydrolysis reaction of the SAM molecules, which is a rate-limiting step in the SAM film formation process, can be omitted. In addition, since the treatment liquid contains SAM molecules having hydroxyl groups without agglomeration, the dehydration condensation reaction between the SAM molecules having hydroxyl groups and the hydroxyl groups on the substrate surface, which is a rate-limiting step in the SAM film formation process, can be effectively generated. Therefore, the SAM molecules can be chemically adsorbed on the substrate surface at a high density. As a result, in the above-mentioned configuration, even if the SAM molecules are not kept in contact with the substrate surface for a long time to form a dense SAM as in the conventional semiconductor manufacturing apparatus, the occurrence of film defects can be suppressed, and a SAM with excellent denseness and protective performance can be efficiently formed in a short time. And, since the protected layer can be protected by the SAM with excellent denseness and protective performance, the semiconductor manufacturing apparatus of the above-mentioned configuration can perform selective etching of the etched layer well.

[0036] In order to achieve the above object, another semiconductor manufacturing apparatus of the present invention is a semiconductor manufacturing apparatus for processing a substrate having a laminate provided on a surface thereof, the laminate including a layer to be protected by etching and a layer to be etched which is to be etched which are alternately laminated, the apparatus including a substrate processing unit for selectively forming a self-assembled monolayer on at least a surface of the layer to be protected, and an etching processing unit for selectively etching and removing the layer to be etched using the self-assembled monolayer as a protective layer, the substrate processing unit including a processing liquid generating unit for generating a processing liquid including molecules capable of forming the self-assembled monolayer, an ultrasonic application unit, and an etching unit for selectively etching and removing the layer to be etched using the self-assembled monolayer as a protective layer. and a treatment liquid supply unit which forms the self-assembled monolayer by supplying the treatment liquid having been uniformly dispersed in an organic solvent as a main solvent to the surface of the substrate, the treatment liquid generation unit generates a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent, and further adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid, and generates the treatment liquid containing the molecules having hydroxyl groups and in which the molecules having the hydroxyl groups exist without agglomerating by causing a hydrolysis reaction between the water dispersed in the dispersion liquid and the functional groups, and the ultrasonic application unit applies ultrasonic waves when or after mixing the organic solvent and the water in the treatment liquid generation unit to generate the dispersion liquid.

[0037] According to the above configuration, the processing liquid generating section in the substrate processing unit generates a mixed liquid by mixing an organic solvent as a main solvent with water. The ultrasonic application section applies ultrasonic waves when the processing liquid generating section mixes the organic solvent with water, or to the mixed liquid generated by mixing the organic solvent with water. As a result, the processing liquid generating section can generate a dispersion liquid in which water is uniformly dispersed in the organic solvent. Furthermore, the processing liquid generating section adds a material containing SAM molecules (SAM forming material) to the generated dispersion liquid without applying ultrasonic waves to generate a processing liquid. Here, the SAM molecules have functional groups that exhibit hydrolysis reactivity, and water molecules are uniformly dispersed and present in the dispersion liquid. Therefore, when the SAM forming material is added to the dispersion liquid, the functional groups that exhibit hydrolysis reactivity in the SAM molecules undergo a hydrolysis reaction with the water molecules in the dispersion liquid to become hydroxyl groups (OH groups). As a result, a processing liquid containing SAM molecules having hydroxyl groups can be generated. The processing liquid generating section generates the processing liquid so that the SAM molecules having hydroxyl groups exist without coagulating with each other. Furthermore, the treatment liquid generating unit can generate the treatment liquid without applying ultrasonic waves, so that the treatment liquid is generated so that the SAM molecules having hydroxyl groups are present without agglomerating with each other. By generating the treatment liquid so that the SAM molecules having hydroxyl groups are present without agglomerating with each other, a self-assembled monolayer can be satisfactorily formed on the surface of the substrate.

[0038] Furthermore, the processing liquid supply unit brings the SAM molecules into contact with the substrate surface by supplying the processing liquid to the substrate surface, thereby causing a dehydration condensation reaction between the hydroxyl groups of the SAM molecules and the hydroxyl groups present on the substrate surface. As a result, the SAM molecules can be chemically adsorbed onto the substrate surface, and the chemically adsorbed SAM molecules can self-assemble to form a SAM. Furthermore, the etching processing unit selectively etches the layer to be etched using the SAM as a protective layer.

[0039] In this manner, in the above-mentioned configuration, the SAM molecules to be chemically adsorbed on the substrate surface are hydrolyzed in advance at the stage of generating the treatment liquid to introduce hydroxyl groups. Therefore, compared to forming a SAM using SAM molecules without introducing hydroxyl groups, the hydrolysis reaction of the SAM molecules, which is a rate-limiting step in the SAM film formation process, can be omitted. In addition, since the treatment liquid contains SAM molecules having hydroxyl groups without agglomeration, the dehydration condensation reaction between the SAM molecules having hydroxyl groups and the hydroxyl groups on the substrate surface, which is a rate-limiting step in the SAM film formation process, can be effectively generated. Therefore, the SAM molecules can be chemically adsorbed on the substrate surface at a high density. As a result, in the above-mentioned configuration, even if the SAM molecules are not kept in contact with the substrate surface for a long time to form a dense SAM as in the conventional semiconductor manufacturing apparatus, the occurrence of film defects can be suppressed, and a SAM with excellent denseness and protective performance can be efficiently formed in a short time. And, since the protected layer can be protected by the SAM with excellent denseness and protective performance, the semiconductor manufacturing apparatus of the above-mentioned configuration can perform selective etching of the etched layer well.

[0040] In the above configuration, it is preferable that the amount of water added when the organic solvent and the water are mixed in the treatment liquid production section is within a range of 50 ppm or more and 200 ppm or less.

[0041] By adding 50 ppm or more of water, the hydrolysis reaction of the functional groups exhibiting hydrolysis reactivity in the SAM molecules can be prevented from becoming insufficient, and a sufficient amount of SAM molecules with hydroxyl groups introduced can be present in the treatment solution. As a result, it is possible to suppress the occurrence of film defects and form a SAM with excellent density, even without contacting the SAM molecules with the substrate surface for a long time to form a dense SAM, as in conventional semiconductor manufacturing equipment. On the other hand, by adding 200 ppm or less of water, it is possible to suppress excessive aggregation of SAM molecules having hydroxyl groups due to a dehydration condensation reaction. As a result, it is possible to suppress the decrease in density of the SAM molecules chemically adsorbed on the substrate surface, and to form a SAM with excellent density.

[0042] In the above-mentioned configuration, it is preferable that the treatment liquid generating unit adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid that is left standing.

[0043] When adding a SAM-forming material to a dispersion, if mechanical force such as stirring or shaking is applied to the dispersion, there is a possibility that SAM molecules having hydroxyl groups may aggregate with each other. However, as in the above configuration, the treatment liquid generator prepares a treatment liquid by adding a SAM-forming material to a stationary dispersion, so that a treatment liquid can be generated with further suppression of aggregation of SAM molecules having hydroxyl groups with each other. Effect of the Invention

[0044] According to the present invention, it is possible to provide a substrate processing method and substrate processing apparatus, as well as a semiconductor device manufacturing method and semiconductor manufacturing apparatus, which are capable of forming a self-assembled monolayer on a substrate surface which has high film density and excellent compactness, in which the occurrence of film defects is effectively suppressed or reduced, and which has excellent protective performance, in a shorter time and more efficiently than before. [Brief description of the drawings]

[0045] [Figure 1] 1A and 1B are cross-sectional views each showing a schematic representation of a laminate provided on a substrate, in which FIG. 1A shows the state before an etching step, and FIG. 1B shows the state after the etching step. [Diagram 2] FIG. 2(a) is a partial enlarged view of the portion surrounded by A in the laminate in FIG. 1(a), FIG. 2(b) is a partial enlarged view showing the formation of a SAM on the surface of the SiO2 layer, and FIG. 2(c) is a partial enlarged view of the portion surrounded by B in the laminate in FIG. 1(b), showing the etching of the SiN layer. [Diagram 3] 3 is a flowchart showing an example of an overall flow of a method for manufacturing a semiconductor device according to a first embodiment of the present invention. [Figure 4]FIG. 4(a) is a schematic diagram showing how a treatment liquid is supplied to the surface of a SiO2 layer in the first embodiment, FIG. 4(b) is a schematic diagram showing how a SAM molecule is chemically adsorbed onto the surface of the SiO2 layer, and FIG. 4(c) is a schematic diagram showing how the SAM molecule self-organizes on the surface of the SiO2 layer to form a SAM. [Diagram 5] Figure 5(a) is a schematic diagram showing how excess SAM molecules are removed from the surface of the SiO2 layer in the removal process, and Figure 5(b) is a partially enlarged view showing the state in which a SAM has been formed on the surface of the SiO2 layer. [Figure 6] 1 is an explanatory diagram illustrating a schematic configuration of a semiconductor manufacturing apparatus according to a first embodiment of the present invention. [Figure 7] 1 is an explanatory diagram illustrating a schematic configuration of a processing liquid storage unit and an ultrasonic wave application unit in a processing liquid supply unit in a semiconductor manufacturing apparatus according to a first embodiment of the present invention. [Figure 8] 2 is an explanatory diagram illustrating a schematic configuration of a removing liquid reservoir provided in a removing liquid supply unit in the semiconductor manufacturing apparatus according to the first embodiment of the present invention. FIG. [Figure 9] 1 is a block diagram showing a schematic configuration of an inert gas reservoir in an inert gas supply unit in a semiconductor manufacturing apparatus according to a first embodiment of the present invention. [Figure 10] FIG. 2 is an explanatory diagram illustrating a schematic configuration of an etching liquid storage section in an etching liquid supply section in the first embodiment of the present invention. [Figure 11] 10 is a flowchart showing an example of an overall flow of a method for manufacturing a semiconductor device according to a second embodiment of the present invention. [Figure 12] 11 is a side view showing a schematic configuration of a lifter in a semiconductor manufacturing apparatus according to a second embodiment of the present invention. FIG. [Figure 13] FIG. 11 is a cross-sectional view showing a state in which a plurality of substrates on which a SAM is formed are immersed in an etching solution in a second embodiment of the present invention. [Figure 14] 1 is a graph showing the relationship between the amount of water added (ppm) and the area ratio (%) of film defects in the SAM in each sample of Examples 1 to 3 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0046] (First embodiment) A first embodiment of the present invention will be described below.

[0047] [Substrate Processing Method (Semiconductor Device Manufacturing Method)] First, a substrate processing method according to the present embodiment will be described below with reference to the drawings. The substrate processing method of the present embodiment provides a technique for enabling good selective etching when forming a three-dimensional structure, such as a three-dimensional NAND structure, on the surface of a substrate.

[0048] The substrate processing method of this embodiment is applicable to a part of a process for forming a three-dimensional NAND structure on a substrate W made of silicon or the like. Therefore, hereinafter, an example in which the substrate processing method of this embodiment is applied to a manufacturing method of a semiconductor device, more specifically, a case in which processing is performed on a substrate W provided with a three-dimensional stack 3 as shown in Fig. 1 will be described. Fig. 1 is a cross-sectional view that shows a schematic representation of a stack provided on a substrate W, where Fig. 1(a) shows a state before an etching process and Fig. 1(b) shows a state after the etching process.

[0049] 2(a), the laminate 3 includes a structure in which SiO2 layers 1 functioning as interlayer insulating layers and SiN layers 2 functioning as sacrificial layers are alternately laminated on a substrate W. The laminate 3 also includes a plurality of memory trenches 4 extending through the laminate 3 in a direction perpendicular to the surface of the substrate W. FIG. 2(a) is a partial enlarged view of a portion surrounded by A in the laminate in FIG.

[0050] As shown in FIG. 3, the method for manufacturing a semiconductor device according to this embodiment includes at least a self-assembled monolayer (hereinafter referred to as "SAM") forming step S1 and an etching step S2, and enables selective etching of the SiN layer 2 through the memory trench 4 to form a recess on the side surface of the memory trench 4 in the laminate 3. FIG. 3 is a flowchart showing an example of the overall flow of the method for manufacturing a semiconductor device according to this embodiment.

[0051] <SAM Formation Step> The SAM forming step S1 is a step of selectively forming a SAM as a protective layer on the surface of the SiO2 layer 1 as a layer to be protected. As shown in FIG. 3, the SAM forming step S1 includes at least a dispersion liquid generating step S101, a treatment liquid generating step S102, a film forming step S103, a removing step S104, and a drying step S105. Note that the SAM forming step S1 corresponds to the substrate processing method of the present invention.

[0052] 1.Dispersion liquid generation process The dispersion liquid generating step S101 is a step of generating a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent. The fact that water is uniformly dispersed in the organic solvent means, for example, that water exists in the organic solvent in an emulsion state. The "main solvent" means a solvent having the largest volume ratio when using a mixed solvent composed of a plurality of solvents.

[0053] Examples of the organic solvent that is the main solvent include ether solvents, aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, fluorine solvents, and ketone solvents. The ether solvent is not particularly limited, and examples thereof include tetrahydrofuran (THF). The aromatic hydrocarbon solvent is not particularly limited, and examples thereof include toluene. The aliphatic hydrocarbon solvent is not particularly limited, and examples thereof include decane. The fluorine solvent is not particularly limited, and examples thereof include 1,3-bis(trifluoromethyl)benzene. The ketone solvent is not particularly limited, and examples thereof include methyl ethyl ketone. These solvents can be used alone or in combination of two or more. Among the solvents exemplified above, from the viewpoint of affinity with water, aromatic hydrocarbon solvents are preferred, and toluene is particularly preferred.

[0054] In addition, the organic solvent as the main solvent is preferably one having a low solubility in water. This allows water to be well dispersed in the organic solvent. Examples of organic solvents having a low solubility in water include the above-mentioned toluene.

[0055] Methods for producing a dispersion include a method of mixing an organic solvent and water while applying ultrasonic waves, and a method of mixing an organic solvent and water and then applying ultrasonic waves. By applying ultrasonic waves, it is possible to prevent the production of a mixture in which the organic solvent phase and the water phase are separated. That is, by applying ultrasonic waves, cavitation is generated in the organic solvent, and the interface between the organic solvent and the water is disturbed, thereby finely dividing the water. As a result, compared to stirring and mixing with mechanical force such as stirring or shaking, it is possible to produce a dispersion in which fine particles of water are uniformly dispersed in the organic solvent and have excellent dispersion stability. In addition, in the present invention, the addition of an emulsifier can be omitted when applying ultrasonic waves.

[0056] The amount of water added in the dispersion is preferably in the range of 50 ppm or more and 200 ppm or less, and more preferably in the range of 50 ppm or more and 150 ppm or less. By making the amount of water added 50 ppm or more, it is possible to prevent the hydrolysis reaction of the functional group exhibiting hydrolysis reactivity in the SAM molecule added in the treatment liquid generation step S102 described later from becoming insufficient. That is, at the stage of generating the treatment liquid, a sufficient amount of SAM molecules to which hydroxyl groups have been introduced can be present in the treatment liquid. As a result, it is possible to suppress the occurrence of film defects and form a SAM with excellent density, even if the SAM molecules are not brought into contact with the substrate surface for a long time to form a dense SAM, as in the conventional substrate processing method. On the other hand, by making the amount of water added 200 ppm or less, it is possible to suppress the excessive aggregation of SAM molecules having hydroxyl groups by a dehydration condensation reaction. As a result, it is possible to suppress the decrease in density of the SAM molecules to be chemically adsorbed on the substrate surface and form a SAM with excellent density.

[0057] In addition, the dispersion liquid production step S101 is preferably performed in an atmosphere of an inert gas such as nitrogen gas. If this step is performed in an environment in which moisture is present in the atmosphere, the moisture in the atmosphere will dissolve in the mixed liquid (or dispersion liquid), and as a result, a dispersion liquid with a predetermined moisture content cannot be obtained, which is not preferable.

[0058] The conditions for applying ultrasonic waves in the dispersion liquid generating step S101, specifically, for example, application time, frequency, and sonic intensity, are not particularly limited as long as the water is dispersed in the organic solvent, and can be set appropriately as necessary. The method for applying ultrasonic waves is also not particularly limited, but examples thereof include a method in which an ultrasonic vibrator is immersed in the mixed liquid and the ultrasonic vibrator is vibrated to apply ultrasonic waves.

[0059] 2. Processing solution production process The treatment liquid generating step S102 is a step of generating a treatment liquid containing SAM molecules. The treatment liquid is used to form a SAM on the surface of the SiO2 layer 1, which is the layer to be protected. Specifically, the treatment liquid is generated by adding a material capable of forming a SAM (hereinafter referred to as a "SAM-forming material") to the dispersion liquid prepared in the dispersion liquid generating step S101. In this step, it is preferable to perform the process without applying ultrasonic waves when adding the SAM-forming material to the dispersion liquid and after adding the SAM-forming material to the dispersion liquid. By not applying ultrasonic waves, the treatment liquid can be generated so that the SAM molecules exist without aggregating with each other. By generating the treatment liquid so that the SAM molecules exist without aggregating with each other, a self-assembled monolayer can be formed well in the film forming step.

[0060] The SAM-forming material is not particularly limited as long as it has a functional group exhibiting hydrolysis reactivity and contains a molecule capable of forming a SAM. In addition, the SAM-forming material is preferably one having high affinity (solubility) for the above-mentioned organic solvent. Specifically, the SAM-forming material is, for example, an organic silane compound such as octadecyltrichlorosilane. Octadecyltrichlorosilane is a compound having a trichlorosilyl group as a functional group exhibiting hydrolysis reactivity.

[0061] Before being added to the treatment liquid, the SAM molecule has a functional group that exhibits hydrolysis reactivity. Therefore, when the SAM-forming material is added to the dispersion liquid, the functional group undergoes a hydrolysis reaction with the water molecules that are uniformly dispersed in the dispersion liquid. As a result, the functional group that exhibits hydrolysis reactivity in the SAM molecule becomes a hydroxyl group (OH group). For example, when the SAM molecule is octadecyltrichlorosilane, the following reaction occurs: C 18 H 37 SiCl3+ 3H2O → C 18 H 37 Si(OH)3+ 3HCl3 As a result, a treatment liquid can be obtained in which the SAM molecules with hydroxyl groups are present without agglomeration. By preparing a treatment liquid containing SAM molecules with hydroxyl groups in advance, the hydrolysis reaction, which is the rate-limiting step in the SAM film formation process, can be omitted. As a result, it becomes possible to form a SAM film in a shorter time than with conventional treatment liquids.

[0062] The amount of the SAM-forming material added is preferably within a range of 0.05% by mass or more and 5% by mass or less with respect to the total mass of the treatment liquid.

[0063] The treatment liquid may contain known additives as long as they do not impair the effects of the present invention. The additives are not particularly limited, and examples thereof include stabilizers and surfactants.

[0064] The treatment liquid generation step is preferably carried out in a stationary state. More specifically, when the SAM-forming material is added to the dispersion, it is not preferable to apply mechanical force such as stirring and shaking to the dispersion. When the SAM-forming material is added to the dispersion, if mechanical force such as stirring and shaking is applied to the dispersion, the SAM molecules may aggregate with each other. However, by adding the SAM-forming material to the dispersion in a stationary state to prepare the treatment liquid, it is possible to further suppress the aggregation of the SAM molecules with each other and generate the treatment liquid.

[0065] As described in the description of the dispersion producing step, the water content in the treatment liquid is preferably within the range of 50 ppm or more and 200 ppm or less, and more preferably within the range of 50 ppm or more and 150 ppm or less.

[0066] The treatment liquid generating step S102 can be carried out, for example, at room temperature and normal pressure.

[0067] 3. Film formation process The film formation step S103 is a step of bringing a treatment liquid containing a SAM-forming material into contact with the surface of the substrate W to form a SAM.

[0068] The method for contacting the processing liquid with the substrate W is not particularly limited, and examples thereof include a method in which the processing liquid is applied to the surface of the substrate W, a method in which the processing liquid is sprayed onto the surface of the substrate W, and a method in which the substrate W is immersed in the processing liquid.

[0069] An example of a method for applying the processing liquid to the surface of the substrate W is to supply the processing liquid to the center of the surface of the substrate W while rotating the substrate W at a constant speed around its center as an axis. In this way, the processing liquid supplied to the surface of the substrate W flows from near the center of the surface of the substrate W toward the peripheral edge of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and is spread over the entire surface of the substrate W. As a result, the entire surface of the substrate W is covered with the processing liquid, and a liquid film of the processing liquid is formed.

[0070] The conditions for contacting the treatment liquid with the substrate W are not particularly limited. However, the film formation step S103 of this embodiment can shorten the contact time of the treatment liquid compared to the case of forming a SAM film by a conventional method. Specifically, depending on the type of SAM-forming material, its concentration, type of solvent, etc., the time required for the SAM formation step S1 (the immersion time when the substrate W is immersed in the treatment liquid) can be appropriately set within the range of 1 minute to 1440 minutes, preferably 1 minute to 60 minutes, and more preferably 1 minute to 30 minutes.

[0071] Next, the process of forming a SAM will be described in more detail using an example in which the SAM-forming material is octadecyltrichlorosilane.

[0072] As shown in Fig. 4(a), when a processing liquid is supplied to the surface of a substrate W, SAM molecules 5 in which a hydroxyl group has been introduced into octadecyltrichlorosilane are dispersed in the processing liquid at the beginning of the supply. Fig. 4(a) is a schematic diagram showing a state in which the processing liquid is supplied to the surface of a SiO2 layer 1.

[0073] Next, when hydroxyl groups (OH groups) 6 are present on the surface of the SiO2 layer 1, the SAM molecules 5 undergo a dehydration condensation reaction with the hydroxyl groups 6, as shown in FIG. 4(b). More specifically, the hydroxyl groups of the SAM molecules 5 and the hydroxyl groups 6 on the surface of the SiO2 layer 1 undergo a dehydration condensation reaction to form siloxane bonds, and the SAM molecules 5 are chemically adsorbed to the surface of the SiO2 layer 1. The SAM molecules 5 exist in the treatment solution in a state in which they are inhibited from aggregating with each other. This can promote the dehydration condensation reaction between the hydroxyl groups of the SAM molecules 5 and the hydroxyl groups on the surface of the SiO2 layer 1, which is the rate-determining step in the SAM film formation process. In addition, the SAM molecules 5 can be chemically adsorbed to the surface of the SiO2 layer 1 at a high density. FIG. 4(b) is a schematic diagram showing the state in which the SAM molecules 5 are chemically adsorbed to the surface of the SiO2 layer 1.

[0074] Next, when the SAM molecules 5 are chemically adsorbed at a high density on the surface of the SiO2 layer 1, an island-like structure of the SAM molecules 5 appears on the surface. Furthermore, in each island, the SAM molecules 5 self-organize and grow (expand) due to hydrophobic and electrostatic interactions between them, and finally form a SAM9 (see Figure 4(c)). Figure 4(c) is a schematic diagram showing how the SAM molecules 5 self-organize on the surface of the SiO2 layer 1 to form a SAM9.

[0075] 4.Removal process The removal step S104 is a step of removing the treatment liquid remaining on the surface of the SiO2 layer 1 after the film formation step S103. This makes it possible to remove excess SAM molecules 5 that do not contribute to the formation of the SAM 9, more specifically, SAM molecules 5 that are not chemically adsorbed on the surface of the SiO2 layer 1. As a result, it is possible to prevent a film made of unadsorbed SAM molecules 5 from being formed on the SAM 9, and to form a good monolayer.

[0076] The method for removing the processing liquid from the surface of the SiO2 layer 1 is not particularly limited, and examples thereof include a method of applying the removal liquid to the surface of the substrate W, a method of spraying the removal liquid onto the surface of the substrate W, and a method of immersing the substrate W in the removal liquid.

[0077] An example of a method for applying the removing liquid to the surface of the substrate W is to supply the removing liquid to the center of the surface of the substrate W while rotating the substrate W at a constant speed around its center as an axis. In this way, the removing liquid supplied to the surface of the substrate W flows from near the center of the surface of the substrate W toward the peripheral edge of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and is spread over the entire surface of the substrate W. As a result, the processing liquid on the surface of the substrate W is replaced with the removing liquid, and the entire surface of the substrate W is covered with the removing liquid, forming a liquid film of the removing liquid.

[0078] When the SAM-forming material is octadecyltrichlorosilane, the surface of the SiO2 layer 1 in the removal step S104 is as shown in Fig. 5(a). As shown in the figure, SAM molecules 5 that do not contribute to the formation of a SAM 9 are removed from the surface of the SiO2 layer 1 of the substrate W by the removal liquid 10. Fig. 5(a) is a schematic diagram showing the state in which excess SAM molecules 5 are removed from the surface of the SiO2 layer 1 in the removal step S104.

[0079] The removal liquid is not particularly limited, but an organic solvent that dissolves the SAM-forming material and has low water solubility is preferred. If the removal liquid can dissolve the SAM-forming material, the excess SAM molecules 5 that do not contribute to the formation of the SAM can be effectively removed from the surface. More specifically, examples of the removal liquid include toluene, decane, and 1,3-bis(trifluoromethyl)benzene. These solvents can be used alone or in combination of two or more.

[0080] 5.Drying process The drying step S105 is intended to remove the removing liquid remaining on the surface of the substrate W. The drying method is not particularly limited, and examples thereof include a method of spraying an inert gas such as nitrogen gas onto the surface of the substrate W. The drying conditions such as the drying time and drying temperature are not particularly limited as long as the removing liquid is removed, and can be set appropriately as necessary.

[0081] As a result, in the SAM formation step S1, as shown in FIG. 5(b), a SAM9 having excellent denseness and protective performance can be formed on the surface of the SiO2 layer 1. FIG. 5(b) is a partially enlarged view showing a state in which the SAM9 is formed on the surface of the SiO2 layer 1. In the SAM formation step S1, a treatment liquid containing a SAM molecule to which a hydroxyl group has been introduced in advance is used to form the SAM9 on the surface of the SiO2 layer 1. This makes it possible to prevent the hydrolysis reaction of the SAM molecule, which is the rate-limiting step in the formation of the SAM9, from occurring in the formation stage of the SAM9. In addition, since the SAM molecules 5 in the treatment liquid are present without agglomeration, the dehydration condensation reaction with the hydroxyl group on the surface of the SiO2 layer 1, which is the rate-limiting step in the formation of the SAM9, can also be efficiently caused. As a result, even if the SAM molecules 5 are not kept in contact with the surface of the SiO2 layer 1 for a long time in order to form a dense film, the occurrence of film defects can be suppressed, and the SAM9 having excellent denseness and protective performance can be efficiently formed in a short time.

[0082] In this embodiment, a rinsing step and another drying step may be performed immediately after the drying step S105. By performing the rinsing step, the removing liquid can be removed from the surface of the SiO2 layer 1. Also, by performing another drying step, the rinsing liquid used in the rinsing step can be removed.

[0083] The rinse liquid in the rinse step is not particularly limited, and may be, for example, DIW, etc. The method of supplying the rinse liquid to the surface of the substrate W is not particularly limited, and may be, for example, a method of applying the rinse liquid to the surface of the substrate W, a method of spraying the rinse liquid onto the surface of the substrate W, a method of immersing the substrate W in the rinse liquid, etc.

[0084] An example of a method for applying the rinse liquid to the surface of the substrate W is to supply the rinse liquid to the central portion of the surface of the substrate W while rotating the substrate W at a constant speed around its central portion as an axis. In this way, the rinse liquid supplied to the surface of the substrate W flows from near the center of the surface of the substrate W toward the peripheral portion of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and is spread over the entire surface of the substrate W. As a result, the removing liquid on the surface of the substrate W is replaced with the rinse liquid, and the entire surface of the substrate W is covered with the rinse liquid, forming a liquid film of the rinse liquid.

[0085] The other drying step is intended to remove the rinsing liquid remaining on the surface of the substrate W. The drying method is not particularly limited, and examples thereof include a method of spraying an inert gas such as nitrogen gas onto the surface of the substrate W. The drying conditions such as the drying time and drying temperature are not particularly limited as long as the rinsing liquid is removed, and can be set appropriately as necessary.

[0086] <Etching process> The etching step S2 is a step of selectively etching the SiN layer 2, which is a sacrificial layer and a layer to be etched. More specifically, this is a step of bringing an etching solution into contact with the SiN layer 2 through the memory trench 4 and removing the SiN layer 2. In this step, the SAM 9 functions as a protective layer to protect the SiO2 layer 1. This makes it possible to effectively prevent the SiO2 layer 1 from being etched.

[0087] An example of a method for applying the etching liquid to the surface of the substrate W is to rotate the substrate W at a constant speed around its central portion as an axis and supply the etching liquid to the central portion of the surface of the substrate W. In this way, the etching liquid supplied to the surface of the substrate W flows from near the center of the surface of the substrate W toward the peripheral portion of the substrate W due to the centrifugal force generated by the rotation of the substrate W, and is spread over the entire surface of the substrate W. As a result, the entire surface of the substrate W is covered with the etching liquid, and a liquid film of the etching liquid is formed.

[0088] The etching liquid can be appropriately set in consideration of the constituent material of the layer to be etched, the etching rate, etc. When the layer to be etched is a SiN layer 2 as in this embodiment, for example, an aqueous solution of phosphoric acid (H3PO4) or hydrofluoric acid (for example, HF:DIW=1:100 in volume ratio) can be used as the etching liquid. The concentration of the etching liquid can also be appropriately set in consideration of the constituent material of the layer to be etched, the etching rate, etc.

[0089] Furthermore, the etching temperature (that is, the temperature of the etching solution) and the etch rate for the layer to be etched can be appropriately set in consideration of the constituent material of the layer to be etched.

[0090] It is preferable to sequentially perform a rinsing step for removing the etching liquid and a drying step immediately after the etching step S2. The rinsing method in the rinsing step is not particularly limited, and examples thereof include a method of supplying a rinsing liquid to the surface of the substrate W and a method of immersing the substrate W in the rinsing liquid. The rinsing liquid is not particularly limited, and examples thereof include DIW. In addition, cleaning conditions such as the rinsing time and the temperature of the rinsing liquid are not particularly limited, and can be set appropriately as needed. The drying step is intended to remove the rinsing liquid remaining on the surface of the substrate W. The drying method is not particularly limited, and examples thereof include a method of spraying an inert gas such as nitrogen gas onto the surface of the substrate W. Drying conditions such as the drying time and the drying temperature are not particularly limited, and can be set appropriately as needed.

[0091] As a result, in the etching step S2, only the SiN layer 2 can be selectively removed as shown in FIG. 2(c). In addition, the SAM9, which has excellent density and protective performance, covers and protects the surface of the SiO2 layer 1, so that the SiO2 layer 1 is prevented from being etched and the etched silicon component is prevented from precipitating and adhering to the surface of the SiO2 layer 1. Furthermore, the tolerance range of the silicon concentration contained in the etching solution such as phosphoric acid can be increased. FIG. 2(c) is a partial enlarged view of the portion surrounded by B in the laminate in FIG. 1(b), showing the state in which the SiN layer 2 has been etched.

[0092] [Substrate processing equipment (semiconductor manufacturing equipment)] Next, the substrate processing apparatus according to this embodiment will be described below by taking as an example a case where it is applied to a semiconductor manufacturing apparatus.

[0093] The semiconductor manufacturing apparatus 100 of this embodiment is a single-wafer processing unit used to form a SAM and etch a layer to be etched, and includes, as shown in FIG. 6, a substrate holding unit 110 for holding a substrate W, a processing liquid supply unit 120 for supplying a processing liquid to the surface Wf of the substrate W, an ultrasonic wave application unit, a removing liquid supply unit 140 for supplying a removing liquid, an inert gas supply unit 150 for supplying an inert gas, an etching liquid supply unit 160, a chamber 170 which is a container for accommodating the substrate W, a splash prevention cup 180 for collecting the processing liquid, a swivel drive unit 190 for independently swivel-driving the arms of each unit, which will be described later, and a control unit 300. The semiconductor manufacturing apparatus 100 may also include a loading / unloading unit (not shown) for loading or unloading the substrate W. FIG. 6 is an explanatory diagram showing a schematic configuration of the semiconductor manufacturing apparatus 100 according to this embodiment. In the figure, XYZ orthogonal coordinate axes are appropriately displayed in order to clarify the directional relationship of the objects shown in the figure. Here, the XY plane represents the horizontal plane, and the +Z direction represents the vertical upward direction.

[0094] <Substrate holding part> The substrate holding unit 110 is a means for holding the substrate W, and as shown in Fig. 6, holds and rotates the substrate W in a substantially horizontal position with the surface Wf of the substrate W facing upward. The substrate holding unit 110 has a spin chuck 113 in which a spin base 111 and a rotation support shaft 112 are integrally connected. The spin base 111 has a substantially circular shape in a plan view, and a hollow rotation support shaft 112 extending substantially vertically is fixed to the center of the spin base 111. The rotation support shaft 112 is connected to a rotation shaft of a chuck rotation mechanism 114 including a motor. The chuck rotation mechanism 114 is housed in a cylindrical casing 115, and the rotation support shaft 112 is supported by the casing 115 so as to be rotatable about a vertical rotation axis J1.

[0095] The chuck rotation mechanism 114 can rotate the rotation support shaft 112 around the rotation axis J1 by being driven by a chuck drive unit (not shown) of the control unit 300. This causes the spin base 111 attached to the upper end of the rotation support shaft 112 to rotate around the rotation axis J1 at a constant speed. The control unit 300 can adjust the rotation speed of the spin base 111 by controlling the chuck rotation mechanism 114 via the chuck drive unit.

[0096] A plurality of chuck pins 116 for gripping the peripheral edge of the substrate W are provided upright near the peripheral edge of the spin base 111. The number of chuck pins 116 to be provided is not particularly limited, but it is preferable to provide at least three or more in order to reliably hold the circular substrate W. In this embodiment, three chuck pins 116 are arranged at equal intervals along the peripheral edge of the spin base 111. Each chuck pin 116 includes a substrate support pin that supports the peripheral edge of the substrate W from below, and a substrate holding pin that holds the substrate W by pressing against the outer circumferential end face of the substrate W supported by the substrate support pin.

[0097] <Processing liquid supply unit> The processing liquid supply unit 120 according to this embodiment is a unit that supplies a processing liquid to the front surface Wf of the substrate W. As shown in FIG. 6, the processing liquid supply unit 120 includes a processing liquid storage unit 121, a nozzle 122, and an arm 123.

[0098] 7, the treatment liquid storage section 121 includes an organic solvent supply section 124, a water supply section 125, a SAM-forming material supply section 126, a treatment liquid tank 127, a temperature adjustment section 128, and an inert gas supply section 129. Note that, Fig. 7 is an explanatory diagram showing a schematic configuration of the treatment liquid storage section 121 and the ultrasonic wave application section 130 in the treatment liquid supply section 120.

[0099] The organic solvent supply unit 124 includes an organic solvent storage unit 124a for storing an organic solvent, an organic solvent supply pipe 124b for supplying the organic solvent to the treatment liquid tank 127, and a valve 124c provided in the middle of the organic solvent supply pipe 124b. The valve 124c is electrically connected to the control unit 300. This allows the valve 124c to be opened and closed by an operation command from the control unit 300. When the valve 124c is opened by an operation command from the control unit 300, the organic solvent is supplied to the treatment liquid tank 127 through the organic solvent supply pipe 124b. The organic solvent in the organic solvent storage unit 124a is pressurized by a pressurizing means (not shown) and sent to the organic solvent supply pipe 124b. The pressurizing means is not particularly limited, and a known means such as a pump can be used.

[0100] The water supply unit 125 includes a water storage unit 125a for storing water, a water supply pipe 125b for supplying water to the treatment liquid tank 127, and a valve 125c provided midway along the path of the water supply pipe 125b. The valve 125c is electrically connected to the control unit 300. This allows the valve 125c to be controlled to be opened and closed by an operation command from the control unit 300. When the valve 125c is opened by an operation command from the control unit 300, water is supplied to the treatment liquid tank 127 via the water supply pipe 125b. The water in the water storage unit 125a is pressurized by a pressurizing means (not shown) and sent to the water supply pipe 125b. The pressurizing means is not particularly limited, and a known means such as a pump can be used.

[0101] The SAM-forming material supply unit 126 includes a SAM-forming material storage unit 126a for storing the SAM-forming material, a SAM-forming material supply pipe 126b for supplying the SAM-forming material to the treatment liquid tank 127, and a valve 126c provided in the middle of the SAM-forming material supply pipe 126b. The valve 126c is electrically connected to the control unit 300. This allows the valve 126c to be opened and closed by an operation command from the control unit 300. When the valve 126c is opened by an operation command from the control unit 300, the SAM-forming material is supplied to the treatment liquid tank 127 through the SAM-forming material supply pipe 126b. The SAM-forming material in the SAM-forming material storage unit 126a is pressurized by a pressurizing means (not shown) and sent to the SAM-forming material supply pipe 126b. The pressurizing means is not particularly limited, and a known means such as a pump can be used.

[0102] The treatment liquid tank 127 mixes the organic solvent supplied from the organic solvent supply unit 124 with the water supplied from the water supply unit 125, and the ultrasonic application unit 130 applies ultrasonic waves to the resulting mixture to generate a dispersion in which water is uniformly dispersed in the organic solvent. Alternatively, the ultrasonic application unit 130 can apply ultrasonic waves while mixing the organic solvent supplied from the organic solvent supply unit 124 with the water supplied from the water supply unit 125 to generate the dispersion. Furthermore, a treatment liquid can be generated by supplying a SAM-forming material from the SAM-forming material supply unit 126 while storing the generated dispersion.

[0103] The processing liquid tank 127 may include a temperature adjustment unit 128 for adjusting the temperature of the dispersion liquid and processing liquid stored therein. The temperature adjustment unit 128 is electrically connected to the control unit 300. The control unit 300 issues an operation command to the temperature adjustment unit 128, thereby making it possible to control the liquid temperature of the dispersion liquid when the dispersion liquid is generated. This makes it possible to prevent water in the dispersion liquid from evaporating (evaporating) and causing a change in the composition of the dispersion liquid.

[0104] The inert gas supply unit 129 includes an inert gas supply source 129a which is a supply source for supplying an inert gas into the processing liquid tank 127, a pump (not shown) for pressurizing the inert gas, an inert gas supply pipe 129b, and a valve 129c provided midway along the inert gas supply pipe 129b.

[0105] The inert gas supply pipe 129b is connected to the treatment liquid tank 127. The valve 129c is electrically connected to the control unit 300, and the opening and closing of the valve 129c can be controlled by an operation command from the control unit 300. When the valve is opened by an operation command from the control unit 300, the inert gas can be supplied to the treatment liquid tank 127. This allows the dispersion liquid and the treatment liquid to be generated under an inert gas atmosphere. The inert gas is not particularly limited, and examples thereof include nitrogen gas.

[0106] Furthermore, a discharge pipe 127a for supplying the processing liquid to the nozzle 122 is connected to the processing liquid tank 127. A discharge valve 127b is provided on the middle of the discharge pipe 127a. The discharge valve 127b is also electrically connected to the control unit 300. This allows the opening and closing of the discharge valve 127b to be controlled by an operation command from the control unit 300. When the discharge valve 127b and the valve 129c are opened and the valves 124c, 125c, and 126c are closed by an operation command from the control unit 300, the processing liquid is pressure-fed to the nozzle 122 via the discharge pipe 127a.

[0107] The nozzle 122 is attached to the tip of an arm 123 that extends horizontally, and is disposed above the spin base 111 when discharging the processing liquid. The arm 123 is connected to a rotation drive unit 190 via a rotation shaft (not shown). The rotation drive unit 190 is electrically connected to a control unit 300, and rotates the arm 123 in response to an operation command from the control unit 300. As the arm 123 rotates, the nozzle 122 also moves.

[0108] <Ultrasonic application unit> 7, the ultrasonic wave application unit 130 is a means for applying ultrasonic waves when generating a dispersion liquid in the processing liquid tank 127 of the processing liquid supply unit 120. The ultrasonic wave application unit 130 is electrically connected to the control unit 300, and the application of ultrasonic waves can be controlled by an operation command from the control unit 300.

[0109] The ultrasonic wave application unit 130 includes, for example, an ultrasonic vibrator provided in the treatment liquid tank 127, and an oscillator that applies a drive voltage to the ultrasonic vibrator (neither is shown). An example of the ultrasonic vibrator includes a piezoelectric body such as piezoelectric ceramics and a pair of electrodes provided on the piezoelectric body. The pair of electrodes are in contact with the piezoelectric body and are also electrically connected to the oscillator. When the oscillator outputs, for example, a high-frequency voltage as a drive voltage to the ultrasonic vibrator in response to an operation command from the control unit 300, the drive voltage is applied between the pair of electrodes, and the drive voltage is thereby applied to the piezoelectric body. The piezoelectric body to which the drive voltage is applied vibrates by alternately repeating contraction and expansion in response to the drive voltage from the oscillator. This allows ultrasonic waves to be applied to the mixture of water and organic solvent stored in the treatment liquid tank 127.

[0110] <Removal liquid supply section> The removing liquid supply unit 140 according to this embodiment is a unit that supplies a removing liquid to the front surface Wf of the substrate W. As shown in FIG. 6, the removing liquid supply unit 140 includes a removing liquid storage unit 141, a nozzle 142, and an arm 143.

[0111] 8, the removing liquid storage unit 141 has a function of supplying the removing liquid to the nozzle 142, and includes a pressurizing unit 144 and a removing liquid tank 145. Fig. 8 is an explanatory diagram showing a schematic configuration of the removing liquid storage unit 141 in the removing liquid supply unit 140.

[0112] The pressurizing unit 144 includes a nitrogen gas supply source 144a which is a source of gas for pressurizing the inside of the removal liquid tank 145, a pump (not shown) for pressurizing the nitrogen gas, a nitrogen gas supply pipe 144b, and a valve 144c provided midway along the nitrogen gas supply pipe 144b.

[0113] The nitrogen gas supply pipe 144b is connected to the removal liquid tank 145. The valve 144c is electrically connected to the control unit 300, and the opening and closing of the valve 144c can be controlled by an operation command from the control unit 300. When the valve 144c is opened by an operation command from the control unit 300, nitrogen gas can be supplied to the removal liquid tank 145.

[0114] The removal liquid tank 145 may include an agitation unit that agitates the removal liquid in the removal liquid tank 145, and a temperature adjustment unit that adjusts the temperature of the removal liquid (neither is shown). The agitation unit may include a rotation unit that agitates the removal liquid in the removal liquid tank 145, and an agitation control unit that controls the rotation of the rotation unit. The agitation control unit is electrically connected to the control unit 300, and the rotation unit is provided with, for example, a propeller-shaped agitation blade at the lower end of the rotation shaft. The control unit 300 issues an operation command to the agitation control unit to rotate the rotation unit, thereby agitating the removal liquid with the agitation blade. As a result, the concentration and temperature of the removal liquid can be made uniform in the removal liquid tank 145.

[0115] Furthermore, a discharge pipe 145a for supplying the removal liquid to the nozzle 142 is connected to the removal liquid tank 145. A discharge valve 145b is provided midway along the discharge pipe 145a. The discharge valve 145b is electrically connected to the control unit 300. This allows the opening and closing of the discharge valve 145b to be controlled by an operation command from the control unit 300. When the discharge valve 145b is opened by an operation command from the control unit 300, the removal liquid is pressure-fed to the nozzle 142 via the discharge pipe 145a.

[0116] The nozzle 142 is attached to the tip of an arm 143 that extends horizontally, and is positioned above the spin base 111 when discharging the removal liquid. The arm 143 is connected to a rotation drive unit 190 via a rotation shaft (not shown). The rotation drive unit 190 is electrically connected to a control unit 300, and rotates the arm 143 in response to an operation command from the control unit 300. As the arm 143 rotates, the nozzle 142 also moves.

[0117] <Inert gas supply section> The inert gas supply unit 150 is a means for supplying an inert gas to the front surface Wf of the substrate W. The inert gas supply unit 150 includes an inert gas storage unit 151, a nozzle 152, and an arm 153, as shown in FIG.

[0118] 9, the inert gas storage unit 151 has a function of supplying an inert gas to the nozzle 152, and includes an inert gas tank 154 for storing the inert gas, an inert gas temperature adjustment unit 155 for adjusting the temperature of the inert gas stored in the inert gas tank 154, and a pipe 156. An example of the inert gas stored in the inert gas tank 154 is nitrogen gas. FIG. 9 is a block diagram showing a schematic configuration of the inert gas storage unit 151 in the inert gas supply unit 150.

[0119] The inert gas temperature adjustment unit 155 is electrically connected to the control unit 300, and adjusts the temperature by heating or cooling the inert gas stored in the inert gas tank 154 according to an operation command from the control unit 300. The inert gas temperature adjustment unit 155 is not particularly limited, and any known temperature adjustment mechanism such as a Peltier element or a pipe through which temperature-adjusted water flows can be used.

[0120] The inert gas storage unit 151 is connected to the nozzle 152 through a pipe 156, and a valve 157 is inserted in the middle of the pipe 156. The inert gas in the inert gas tank 154 is pressurized by a pressurizing means (not shown) and sent to the pipe 156. The pressurizing means can be realized by compressing and storing the inert gas in the inert gas tank 154, in addition to pressurization by a pump or the like.

[0121] The valve 157 is electrically connected to the control unit 300 and is normally closed. Opening and closing of the valve 157 is controlled by an operation command from the control unit 300. When the valve 157 is opened by an operation command from the control unit 300, an inert gas is supplied from the nozzle 152 through the piping 156 to the front surface Wf of the substrate W.

[0122] Nozzle 152 is attached to the tip of arm 153 that extends horizontally, and is disposed above spin base 111 when discharging inert gas. Arm 153 is connected to a rotation drive unit 190 via a rotation shaft (not shown). Rotation drive unit 190 is electrically connected to control unit 300, and rotates arm 153 in response to an operation command from control unit 300. As arm 153 rotates, nozzle 152 also moves.

[0123] <Etching solution supply unit> The etching liquid supply unit 160 is a means for supplying an etching liquid to the front surface Wf of the substrate W. The etching liquid supply unit 160 has an etching liquid storage unit 161, a nozzle 162, and an arm 163, as shown in FIG.

[0124] 10, the etching liquid storage unit 161 includes at least an etching liquid tank 164, a temperature regulator 165, a liquid delivery pump 166, and a particle filter 167. Note that, FIG. 10 is an explanatory diagram showing a schematic configuration of the etching liquid storage unit 161 in the etching liquid supply unit 160.

[0125] The etching solution tank 164 may include an agitation unit (not shown) that agitates the etching solution in the etching solution tank 164. The agitation unit may include a rotation unit that agitates the etching solution and an agitation control unit that controls the rotation of the rotation unit. The agitation control unit is electrically connected to the control unit 300, and the rotation unit includes, for example, a propeller-shaped agitation blade at the lower end of the rotation shaft. The control unit 300 issues an operation command to the agitation control unit to rotate the rotation unit, thereby agitating the etching solution with the agitation blade. As a result, the concentration and temperature of the etching solution in the etching solution tank 164 can be made uniform.

[0126] The etching solution tank 164 is provided with a mixer 168 capable of mixing an etching solution with a chemical and DIW from an external supply source (not shown) to prepare an etching solution of a predetermined concentration. The chemical is a solute that functions as an etchant. Examples of the chemical include the aforementioned phosphoric acid and hydrogen fluoride.

[0127] Further, the etching solution tank 164 is connected to a discharge pipe 169 for supplying the etching solution to the nozzle 162. A temperature regulator 165, a liquid delivery pump 166, and a particle filter 167 are sequentially interposed in the middle of the discharge pipe 169 from upstream to downstream. The temperature regulator 165 and the liquid delivery pump 166 are electrically connected to the control unit 300. This allows the temperature of the etching solution to be supplied to the nozzle 162 to be controlled by an operation command from the control unit 300. Furthermore, when the liquid delivery pump 166 is controlled by an operation command from the control unit 300, the etching solution can be pressure-fed to the nozzle 162 through the discharge pipe 169. The particle filter 167 can remove foreign matter such as particles in the etching solution.

[0128] The nozzle 162 is attached to the tip of an arm 163 that extends horizontally, and is positioned above the spin base 111 when discharging the etching liquid. The arm 163 is connected to a rotation drive unit 190 via a rotation shaft (not shown). The rotation drive unit 190 is electrically connected to a control unit 300, and rotates the arm 163 according to an operation command from the control unit 300. As the arm 163 rotates, the nozzle 162 also moves.

[0129] <Shatterproof cup> The splash prevention cup 180 is provided so as to surround the spin base 111. The splash prevention cup 180 is connected to a lift drive mechanism (not shown) and can be raised and lowered in the vertical direction. When supplying a processing liquid or the like to the front surface Wf of the substrate W, the splash prevention cup 180 is positioned at a predetermined position by the lift drive mechanism and surrounds the substrate W held by the chuck pins 116 from a lateral position. This makes it possible to collect the processing liquid or the like splashed from the substrate W or the spin base 111.

[0130] <Control Unit> The control unit 300 is electrically connected to each part of the semiconductor manufacturing equipment and controls the operation of each part. The control unit 300 is composed of a computer having an arithmetic unit and a storage unit. The arithmetic unit uses a CPU that performs various arithmetic processing. The storage unit also includes a ROM, which is a read-only memory that stores a substrate processing program and an etching processing program, a RAM, which is a readable and writable memory that stores various information, and a magnetic disk that stores control software, data, and the like. The magnetic disk stores processing conditions in advance, including the generation (mixing) conditions of the dispersion liquid and the processing liquid, the supply conditions of the processing liquid, the removal liquid, the inert gas, and the etching liquid, the application conditions of ultrasonic waves, the rinsing conditions, the drying conditions, the film formation conditions of the SAM, and the etching conditions. The CPU reads the processing conditions into the RAM and controls each part of the semiconductor manufacturing equipment according to the contents.

[0131] Second embodiment A second embodiment of the present invention will now be described. This embodiment differs from the first embodiment in that the etching process is performed in a batch manner instead of a single-wafer manner. Even with this configuration, a SAM with high film density and excellent compactness, in which the occurrence of film defects is effectively suppressed or reduced, and excellent protective performance can be formed on the substrate surface more efficiently in a shorter time than with conventional film formation methods.

[0132] [Substrate Processing Method (Semiconductor Device Manufacturing Method)] A substrate processing method (semiconductor device manufacturing method) according to this embodiment will be described below with reference to Fig. 11. Fig. 11 is a flow chart showing an example of an overall flow of a substrate processing method according to a second embodiment of the present invention. Note that the SAM formation step S1 (dispersion liquid generation step S101, treatment liquid generation step S102, film formation step S103, removal step S104, and drying step S105) shown in Fig. 11 are the same as those in the first embodiment, and therefore detailed descriptions of these steps will be omitted.

[0133] <Etching process> The etching step S2' is a step of selectively etching the SiN layer 2, which is the layer to be etched, by immersing the substrate W after the SAM formation in an etching solution.

[0134] The method of immersing the substrate W in the etching solution is, for example, performed with the substrate W in an upright position. Here, the "upright position" refers to a position in which the surface of the substrate W is aligned in a direction substantially perpendicular to a horizontal plane, and includes a vertical position. The etching solution may be the same as that described in the first embodiment. In addition, the etching temperature (i.e., the liquid temperature of the etching solution) and the etch rate for the layer to be etched may be appropriately set in consideration of the constituent material of the layer to be etched, as in the first embodiment.

[0135] [Substrate processing equipment (semiconductor manufacturing equipment)] Next, the semiconductor manufacturing apparatus according to this embodiment will be described below by taking as an example a case where it is applied to a semiconductor manufacturing apparatus.

[0136] The semiconductor manufacturing apparatus of this embodiment differs from the substrate processing apparatus of the first embodiment in that it is equipped with at least a single-wafer substrate processing unit for forming a SAM and a batch-type etching processing unit for etching the layer to be etched.

[0137] <Substrate processing unit> The substrate processing unit may have a similar configuration to that of the semiconductor manufacturing apparatus 100 of the first embodiment, and therefore a detailed description thereof will be omitted.

[0138] <Etching processing unit> The etching processing unit of this embodiment is a batch-type processing unit used for etching a layer to be etched, and performs an etching step S2' on a substrate W on which a SAM has been formed in the substrate processing unit. As shown in Figs. 12 and 13, the etching processing unit at least includes a substrate transport section (not shown), a lifter 210, and a processing tank 220 for storing an etching solution. Fig. 12 is a side view showing a schematic configuration of the lifter 210 in the semiconductor manufacturing apparatus of this embodiment. Fig. 13 is a cross-sectional view showing a state in which a plurality of substrates W on which a SAM has been formed in this embodiment are immersed in an etching solution.

[0139] The substrate transport unit transports the substrate W on which the SAM has been formed in the substrate processing unit to the etching processing unit. The substrate transport unit includes, for example, an articulated robot capable of transporting the substrate W. The tip of the articulated robot includes a transport arm capable of loading the substrates W all at once in a horizontal position.

[0140] As shown in FIG. 12, the lifter 210 includes a flat back plate 211, a plurality (three) of holding bars 212, and a lifting mechanism (not shown). The back plate 211 stands upright, and at its lower end, the holding bars 212 extend in one direction so as to be perpendicular to the back plate 211. The holding bars 212 are provided with a plurality of grooves 213 arranged in the extending direction. The plurality of grooves 213 are arranged at equal intervals and spaced apart from each other. Each groove 213 extends in a direction perpendicular to the extending direction of the holding bar 212, and can fit a plurality of substrates W in an upright position. This allows the holding bar 212 to abut against and support the group of substrates W from below in an upright position, and to hold them collectively. The number of holding bars 212 is not particularly limited as long as it is plural. Furthermore, the number of grooves 213 provided in the holding rod 212 is not particularly limited and may be set appropriately depending on the number of substrates W to be held. Furthermore, the lifting mechanism can raise or lower the lifter 210 in the Z direction shown in Fig. 13. This allows the lifter 210, which is collectively holding the group of substrates W, to be moved into or removed from the processing bath 220.

[0141] 13, the processing tank 220 includes an injection pipe 222 for supplying the etching liquid into the processing tank 220, an inner tank 223 for storing the etching liquid, and an outer tank 224 provided on the periphery of the upper opening of the inner tank 223. The injection pipe 222 is provided on the bottom of the inner tank 223, and enables the etching liquid to be supplied in an upflow manner to the inner tank 223. In addition, the outer tank 224 enables the etching liquid that has overflowed from the inner tank 223 to be collected.

[0142] (Other matters) In the above description, the most preferred embodiment of the present invention has been described. However, the present invention is not limited to this embodiment. The configurations in the above-described embodiment and each modified example can be changed, modified, substituted, added, deleted, and combined within a range that does not contradict each other. EXAMPLES

[0143] Preferred examples of the present invention are described in detail below. However, the materials, amounts, conditions, etc. described in the examples are not intended to limit the scope of the present invention unless otherwise specified.

[0144] Example 1 First, in a sealed container in a stationary state, 50 ppm of water was added to toluene as an organic solvent under conditions of a temperature of 23°C and normal pressure. Furthermore, ultrasonic waves were applied to the mixture of toluene and water in a stationary state for 30 minutes. As a result, a dispersion liquid in which water was uniformly dispersed in toluene as a main solvent was prepared (dispersion liquid generation process). The ultrasonic wave application conditions were a frequency of 45 Hz.

[0145] Next, octadecyltrichlorosilane as a SAM-forming material was added to the dispersion liquid in a stationary state under conditions of a temperature of 23°C and normal pressure to prepare a treatment liquid (treatment liquid generation step). The content (concentration) of octadecyltrichlorosilane was 5% by mass with respect to the total mass of the treatment liquid.

[0146] Separately from the preparation of the treatment solution, a substrate with a SiO2 film (thickness 100 nm) formed on its surface was prepared and immersed in a hydrogen fluoride aqueous solution for 1 minute. The volume ratio of hydrogen fluoride to DIW used was hydrogen fluoride:DIW=1:100.

[0147] Next, the substrate was removed from the hydrogen fluoride aqueous solution and immersed in a treatment liquid containing a SAM-forming material for 5 minutes to form a SAM (approximately 1 nm thick) on the surface of the SiO2 film of the substrate (film formation process).

[0148] Next, the substrate was removed from the treatment solution and immersed in toluene as a removal solution for 1 minute to remove any unadsorbed SAM-forming material remaining on the surface of the substrate (removal step).

[0149] Next, the surface of the substrate on which the SAM was formed was dried by blowing nitrogen gas onto it after it was removed from the toluene (drying step). The temperature of the nitrogen gas was room temperature, and the drying time was 1 minute.

[0150] Furthermore, the dried substrate was immersed in DIW to remove toluene (rinsing process), and then nitrogen gas was sprayed onto the surface on which the SAM was formed to dry it (drying process). The temperature of the nitrogen gas was room temperature. In this way, a sample according to this embodiment was produced.

[0151] Next, the obtained sample was subjected to an etching process. Specifically, the substrate was immersed in an etching solution, and the area on the substrate surface that was not protected by the SAM was etched. The etching conditions were set to 195 seconds for immersion time in the etching solution (etching process time) so that the amount of SiO2 etched was about 10 nm. An aqueous hydrogen fluoride solution was used as the etching solution, and the volume ratio of hydrogen fluoride to DIW was hydrogen fluoride:DIW=1:100.

[0152] Next, the substrate was removed from the etching solution and immersed in DIW, and then removed from the DIW (rinsing process with DIW). The etched surface was then dried by spraying nitrogen gas on it (drying process). The temperature of the nitrogen gas was room temperature.

[0153] Example 2 In this example, the amount of water added when preparing the dispersion was changed to 100 ppm. Except for this, samples were prepared in the same manner as in Example 1, and the obtained samples were subjected to an etching treatment.

[0154] Example 3 In this example, the amount of water added when preparing the dispersion was changed to 200 ppm. Except for this, samples were prepared in the same manner as in Example 1, and the obtained samples were subjected to an etching treatment.

[0155] Comparative Example 1 In this comparative example, water was not added when preparing the dispersion liquid, but otherwise, samples were prepared in the same manner as in Example 1, and the obtained samples were subjected to an etching treatment.

[0156] Comparative Example 2 In this comparative example, the amount of water added when preparing the dispersion was changed to 300 ppm. Except for this, samples were prepared in the same manner as in Example 1, and the obtained samples were subjected to an etching treatment.

[0157] (SAM compactness evaluation) For each of the samples according to Examples 1 to 3 and Comparative Examples 1 and 2, the area of ​​film defects in the SAM was calculated to evaluate the denseness of the SAM.

[0158] That is, the SAM of each sample was imaged using an atomic force microscope (AFM) (trade name: Dimension Icon, manufactured by Bruker Japan Co., Ltd.), and an observation image (AFM image) of 500 nm square was obtained. Next, each obtained observation image was binarized, and then image processing was performed to map the film defects, and the site (region) of the film defect of the SAM was identified. In order to identify the site (region) of the film defect of the SAM by mapping, image processing was performed so that defects located at a depth of less than 1 nm from the SAM surface were mapped, taking into consideration that the film thickness of the SAM was about 1 nm. As a result, the site (region) at a depth of more than 1 nm from the SAM surface, more specifically, the etched site, was mapped as the region of the film defect of the SAM, and was not included in the area. Next, the area of ​​the film defect region of the SAM identified by image processing was calculated, and the ratio to the area of ​​the entire region in the observation image was calculated. The results are shown in Table 1 and FIG. 14. FIG. 14 is a graph showing the relationship between the amount of water added (ppm) and the area ratio (%) of film defects in the SAM in each sample of Examples 1 to 3 and Comparative Examples 1 and 2.

[0159] 14, the area ratios of film defects in the SAMs in Examples 1 to 3 were 38.0%, 19.2%, and 45.1%, respectively. On the other hand, the area ratios of film defects in the SAMs in Comparative Examples 1 and 2 were both 100%. This confirmed that the SAMs obtained using the treatment solutions of Examples 1 to 3 all had good density and protective performance.

[0160] [Table 1] [Explanation of symbols]

[0161] 1 SiO2 layer 2 SiN layer 3. Laminate 4. Memory Trench 5 SAM (self-assembled monolayer) molecule 6 Hydroxyl groups 9 SAM (Self-assembled monolayer) 100 Semiconductor manufacturing equipment 110 Board holding part 120 Processing liquid supply unit 121 Processing liquid storage section 124 Organic Solvent Supply Section 125 Water supply section 126 SAM (self-assembled monolayer) forming material supply section 127 Processing liquid tank 129 Inert gas supply section 130 Ultrasonic application unit 140 Removal liquid supply section 150 Inert gas supply unit 160 Etching solution supply unit 190 Swivel drive unit 210 Lifter 220 Treatment tank 300 Control section S1 SAM (self-assembled monolayer) formation process S2, S2' Etching process S101 Dispersion liquid generation process S102 Processing solution generation process S103 Film formation process S104 Removal process S105 Drying process W substrate Surface of Wf substrate

Claims

1. A substrate processing method for forming a self-assembled monolayer on a surface of a substrate, comprising: a dispersion producing step of producing a dispersion in which water is uniformly dispersed in an organic solvent as a main solvent; a treatment liquid generating step of adding a material containing a molecule having a functional group exhibiting hydrolysis reactivity and capable of forming the self-assembled monolayer to the dispersion liquid, and generating a treatment liquid containing the molecule having a hydroxyl group and in which the molecule having the hydroxyl group is present without being aggregated by hydrolysis reaction between the functional group and water dispersed in the dispersion liquid; a film formation step of forming the self-assembled monolayer by supplying the treatment liquid onto the surface of the substrate; Including, the dispersion generating step is a step of mixing the organic solvent and the water while applying ultrasonic waves, or mixing the organic solvent and the water and then applying ultrasonic waves to generate the dispersion, The treatment liquid generating step is a step performed without applying ultrasonic waves to the dispersion liquid. A method for processing a substrate.

2. 2. The substrate processing method according to claim 1, wherein the amount of water added in the dispersion generating step is within a range of 50 ppm to 200 ppm in the dispersion.

3. 2. The substrate processing method according to claim 1, wherein the processing liquid generating step comprises adding a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid that is left stationary.

4. 1. A method for manufacturing a semiconductor device, comprising processing a substrate having a laminate provided on a surface thereof, the method comprising: The laminate includes a layer to be protected from etching and a layer to be etched that are alternately laminated, selectively forming a self-assembled monolayer on at least a surface of the layer to be protected; and selectively etching the layer to be etched using the self-assembled monolayer as a protective layer, The step of forming a self-assembled monolayer includes: a dispersion producing step of producing a dispersion in which water is uniformly dispersed in an organic solvent as a main solvent; a treatment liquid generating step of adding a material containing a molecule having a functional group exhibiting hydrolysis reactivity and capable of forming the self-assembled monolayer to the dispersion liquid, and generating a treatment liquid containing the molecule having a hydroxyl group and in which the molecule having the hydroxyl group is present without being aggregated by hydrolysis reaction between the functional group and water dispersed in the dispersion liquid; a film formation step of forming the self-assembled monolayer by supplying the treatment liquid onto the surface of the substrate; Including, the dispersion generating step is a step of mixing the organic solvent and the water while applying ultrasonic waves, or mixing the organic solvent and the water and then applying ultrasonic waves to generate the dispersion, The treatment liquid generating step is a step performed without applying ultrasonic waves to the dispersion liquid. A method for manufacturing a semiconductor device.

5. 5. The method for manufacturing a semiconductor device according to claim 4, wherein the amount of water added in the dispersion liquid preparation step is within a range of 50 ppm to 200 ppm in the dispersion liquid.

6. 5. The method for manufacturing a semiconductor device according to claim 4, wherein the treatment liquid generating step comprises adding a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid that has been left standing.

7. A substrate processing apparatus for forming a self-assembled monolayer on a surface of a substrate, comprising: a treatment liquid generating unit for generating a treatment liquid containing molecules capable of forming the self-assembled monolayer; An ultrasonic wave application unit; a treatment liquid supplying unit that supplies the treatment liquid generated in the treatment liquid generating unit onto the surface of the substrate to form the self-assembled monolayer; Equipped with the treatment liquid generating unit generates a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent, further adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid, and generates the treatment liquid containing the molecules in a state having hydroxyl groups and in which the molecules having hydroxyl groups are present without being aggregated by causing a hydrolysis reaction between the water dispersed in the dispersion liquid and the functional groups, The ultrasonic application unit applies ultrasonic waves when or after mixing the organic solvent and the water in the processing liquid generation unit to generate the dispersion liquid.

8. 8. The substrate processing apparatus according to claim 7, wherein an amount of water added when the organic solvent and the water are mixed in the processing liquid generating section is within a range of 50 ppm to 200 ppm.

9. The substrate processing apparatus according to claim 7 , wherein the processing liquid generating unit adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid that is left stationary.

10. A semiconductor manufacturing apparatus for processing a substrate having a laminate on a surface thereof, comprising: The laminate includes a layer to be protected from etching and a layer to be etched which are alternately laminated, a treatment liquid generating unit for generating a treatment liquid containing molecules capable of forming the self-assembled monolayer; An ultrasonic wave application unit; a treatment liquid supplying unit that supplies the treatment liquid generated in the treatment liquid generating unit onto the surface of the substrate to form the self-assembled monolayer; an etching unit that selectively etches and removes the layer to be etched using the self-assembled monolayer as a protective layer; Equipped with the treatment liquid generating unit generates a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent, further adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid, and generates the treatment liquid containing the molecules in a state having hydroxyl groups and in which the molecules having hydroxyl groups are present without being aggregated by causing a hydrolysis reaction between the water dispersed in the dispersion liquid and the functional groups, The semiconductor manufacturing apparatus, wherein the ultrasonic application unit applies ultrasonic waves when or after mixing the organic solvent and the water in the treatment liquid production unit to produce the dispersion liquid.

11. A semiconductor manufacturing apparatus for processing a substrate having a laminate on a surface thereof, comprising: The laminate includes a layer to be protected from etching and a layer to be etched which are alternately laminated, a substrate processing unit for selectively forming a self-assembled monolayer on at least a surface of the layer to be protected; an etching processing unit that selectively etches and removes the layer to be etched using the self-assembled monolayer as a protective layer; The substrate processing unit includes: a treatment liquid generating unit for generating a treatment liquid containing molecules capable of forming the self-assembled monolayer; An ultrasonic wave application unit; a treatment liquid supplying unit that supplies the treatment liquid generated in the treatment liquid generating unit onto the surface of the substrate to form the self-assembled monolayer; Equipped with the treatment liquid generating unit generates a dispersion liquid in which water is uniformly dispersed in an organic solvent as a main solvent, further adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid, and generates the treatment liquid containing the molecules in a state having hydroxyl groups and in which the molecules having hydroxyl groups are present without being aggregated by causing a hydrolysis reaction between the water dispersed in the dispersion liquid and the functional groups, The semiconductor manufacturing apparatus, wherein the ultrasonic application unit applies ultrasonic waves when or after mixing the organic solvent and the water in the treatment liquid production unit to produce the dispersion liquid.

12. 12. The semiconductor manufacturing apparatus according to claim 10, wherein an amount of water added when mixing the organic solvent and the water in the treatment liquid producing section is within a range of 50 ppm or more and 200 ppm or less.

13. 12. The semiconductor manufacturing apparatus according to claim 10, wherein the treatment liquid generating section adds a material containing molecules capable of forming the self-assembled monolayer to the dispersion liquid that is left standing.

Citation Information

Patent Citations

  • Substrate for manufacturing organic semiconductor device, organic semiconductor device, and method for manufacturing same

    JP2007019121A

  • Siloxane-based molecular membrane, method for producing the same and organic device using the membrane

    JP2007145984A

  • Method for manufacturing substrate with single particle film etching mask and for formation of fine uneven surface structure

    JP2013030805A

  • Etching method

    JP2013062278A

  • Etching method, etching device and storage medium

    JP2013251379A