Adhesive composition, laminate, adhesive film, adhesive layer for optical film, image display device and polarizing plate
The adhesive composition with a biomass-derived acrylic copolymer addresses the need for high adhesive strength and water vapor barrier properties, enhancing performance in image display devices and polarizing plates.
Patent Information
- Application Number
- JP2023046238
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing adhesive compositions face challenges in achieving high adhesive strength and water vapor barrier properties while reducing the use of fossil resource-based materials, particularly in applications like organic EL displays.
An adhesive composition using an acrylic copolymer with a glass transition temperature of 10°C or less, derived from at least 30% biomass, incorporating components (A1) like isobornyl acrylate and (A2) alkyl (meth)acrylate, which provide high adhesive strength and water vapor barrier properties.
The adhesive composition exhibits high adhesive strength to various substrates and low water vapor permeability, supporting applications in image display devices and polarizing plates.
Smart Images

Figure 2024135515000001 
Figure 2024135515000002 
Figure 2024135515000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition, a laminate, a pressure-sensitive adhesive film, a pressure-sensitive adhesive layer for an optical film, an image display device, and a polarizing plate. [Background technology]
[0002] In recent years, carbon dioxide emissions from the combustion of petroleum-derived products have become a problem, and there is a demand to reduce the use of fossil resource materials such as petroleum. Accordingly, in the field of adhesives, attempts are being made to conserve the use of petroleum resources by using bio-derived materials instead of petroleum-derived materials.
[0003] For example, Patent Document 1 discloses a pressure-sensitive adhesive sheet containing an acrylic polymer. 50% or more of the total carbon atoms contained in the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet disclosed in Patent Document 1 are biomass-derived carbon. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-105309 A Summary of the Invention [Problem to be solved by the invention]
[0005] As disclosed in Patent Document 1, in consideration of environmental issues, attempts have been made to further increase the biomass content of pressure-sensitive adhesive compositions. Furthermore, for example, when used for certain pharmaceuticals or electronic components such as organic electroluminescence displays, the pressure-sensitive adhesive sheet is required to have high water vapor barrier properties.
[0006] The present invention has been made in consideration of the above circumstances, and aims to provide a pressure-sensitive adhesive composition which uses a biological material and can exhibit high adhesive strength and water vapor barrier properties, and a laminate, a pressure-sensitive adhesive film, a pressure-sensitive adhesive layer for an optical film, an image display device, and a polarizing plate which use the same. [Means for solving the problem]
[0007] That is, the present invention employs the following configuration. [1] A pressure-sensitive adhesive composition comprising an acrylic copolymer, the acrylic copolymer having a glass transition temperature of 10°C or lower, 30% or more of the total carbon number of the acrylic copolymer being biomass-derived carbon, the acrylic copolymer containing a component (A), the component (A) having a component (A1) represented by the following general formula (1), and a content of the component (A1) relative to the total amount of monomers of the component (A) being 25 parts by weight or more. [ka] (In general formula (1), R 1 is a hydrogen atom or a methyl group. 2 R is a polycyclic hydrocarbon group having 7 to 12 carbon atoms. 2 is an alkyl group derived from biomass. [2] The pressure-sensitive adhesive composition according to [1], wherein the component (A1) is isobornyl acrylate. [3] The pressure-sensitive adhesive composition according to [1] or [2], wherein the (A) component includes an (A2) component, and the (A2) component is an alkyl (meth)acrylate having an alkyl group having 1 to 20 carbon atoms at an ester terminal. [4] The pressure-sensitive adhesive composition according to any one of [1] to [3], wherein the acrylic copolymer has a component (B), and the component (B) is a hydroxyalkyl (meth)acrylate. [5] A laminate having a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of [1] to [4]. [6] A pressure-sensitive adhesive film comprising a resin film and a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of [1] to [4] on one or both sides thereof. [7] A pressure-sensitive adhesive layer for an optical film, which is formed from the pressure-sensitive adhesive composition according to any one of [1] to [4]. [8] An image display device in which the pressure-sensitive adhesive layer for an optical film according to [7] is used for bonding an optical film. [9] A polarizing plate having a pressure-sensitive adhesive layer, which uses the pressure-sensitive adhesive layer for an optical film according to [7]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a pressure-sensitive adhesive composition which uses a biological material and is capable of exhibiting high adhesive strength and water vapor barrier property, and a laminate, a pressure-sensitive adhesive film, a pressure-sensitive adhesive layer for an optical film, an image display device, and a polarizing plate which use the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Adhesive composition> The present embodiment is a pressure-sensitive adhesive composition containing an acrylic copolymer. In the present embodiment, the term "adhesive" refers to a liquid in which an adhesive composition is dissolved in a solvent. In this embodiment, the "adhesive composition" refers to a material that is in a soft solid (viscoelastic) state in a temperature range around room temperature (20°C) and has the property of easily adhering to an adherend by the application of pressure.
[0010] In this specification, the term "a pressure-sensitive adhesive composition capable of exerting high adhesive strength" refers to a pressure-sensitive adhesive composition having adhesive strength to a plurality of types of adherends each of which is equal to or greater than a predetermined value. Specifically, it means a pressure-sensitive adhesive composition having an adhesive strength to an acrylic plate of 5 N / 25 mm or more, an adhesive strength to a glass plate of 2 N / 25 mm or more, an adhesive strength to a stainless steel plate of 3 N / 25 mm or more, and an adhesive strength to a cycloolefin polymer film of 16 N / 25 mm or more, as measured by the method described in the examples described later.
[0011] In this specification, "having high water vapor barrier properties" means that the water vapor transmission rate is 300 g / (m 2 This means that the time is less than or equal to 100 ms.
[0012] Acrylic copolymer In this embodiment, the acrylic copolymer has a glass transition temperature of 10° C. or lower. The glass transition temperature is calculated by the following FOX formula. (FOX formula) 1 / Tg=W1 / Tg1+W2 / Tg2+···W N / Tg N Tg: Glass transition temperature of the acrylic copolymer Tg N : Glass transition temperature of homopolymer W N : weight fraction of monomer
[0013] The acrylic copolymer having a glass transition temperature of 10° C. or less is a basic property for functioning as a pressure-sensitive adhesive composition.
[0014] In this embodiment, 30% or more of the total carbon number of the acrylic copolymer is derived from biomass. A high biomass carbon ratio in the acrylic copolymer means that the amount of fossil resource-based materials, such as petroleum, used is small.
[0015] From the viewpoint of reducing the amount of fossil resource-based materials used, a higher biomass carbon ratio is preferable. In this embodiment, it is preferable that the biomass-derived carbon accounts for 30% to 100% of the total carbon number of the acrylic copolymer.
[0016] The biomass ratio can be measured by measuring the proportion of carbon isotope with mass number 14 using accelerator mass spectrometry (AMS).
[0017] In this embodiment, the biomass degree of the acrylic copolymer can be measured by removing the solvent component contained in the pressure-sensitive adhesive composition and measuring the solid content by accelerator mass spectrometry (AMS method).
[0018] Component (A) The acrylic copolymer contains a component (A), which has a component (A1) represented by the following general formula (1).
[0019] [ka] (In general formula (1), R 1 is a hydrogen atom or a methyl group. 2 R is a polycyclic hydrocarbon group having 7 to 12 carbon atoms. 2 is an alkyl group derived from biomass.
[0020] The monomer represented by the general formula (1) is R 1 may be an alkyl acrylate in which R is a hydrogen atom; 1 is a methyl group.
[0021] In general formula (1), R 2 is a polycyclic hydrocarbon group having 7 to 12 carbon atoms. A polycyclic hydrocarbon group is a hydrocarbon group having two or more rings, and R 2 Examples of the alkyl group include a norbornyl group, an isobornyl group, and an adamantyl group, and among these, an isobornyl group is preferable.
[0022] The component (A1) represented by general formula (1) is preferably isobornyl acrylate.
[0023] The bulky side chain R of the (A1) component 2 Since the steric hindrance inhibits the permeation of water molecules, the adhesive layer formed using the adhesive composition of this embodiment exhibits high water vapor barrier properties.
[0024] ·(A2) Component The component (A) preferably contains a component (A2) in addition to the component (A1). The component (A2) is an alkyl (meth)acrylate having an alkyl group having 1 to 20 carbon atoms at the ester terminal. The alkyl group in the component (A2) may be an alkyl group derived from biomass or may be an alkyl group derived from non-biomass.
[0025] When the alkyl group in the component (A2) has 3 or more carbon atoms, the alkyl group may be linear or branched. 2 may be a cyclic alkyl group.
[0026] The alkyl group contained in the component (A2) is preferably an alkyl group having 8 or more carbon atoms, and more preferably an alkyl group having 10 or more carbon atoms.
[0027] Examples of the linear or branched alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, an s-butyl group, a t-butyl group, a pentyl group, an isopentyl group, a hexyl group, a heptyl group, an octyl group, a 2-ethylhexyl group, an isooctyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, a stearyl group, an isostearyl group, and a lauryl group.
[0028] Examples of the cyclic alkyl group include a cyclohexyl group, an isobornyl group, and a dicyclopentanyl group.
[0029] When the number of carbon atoms in the alkyl group of the component (A2) is within the above range, high adhesive strength can be achieved.
[0030] The acrylic copolymer is preferably a copolymer of the components (A1) and (A2). In this case, the (A1) component and the (A2) component may each be one of the above-mentioned alkyl (meth)acrylates, or two or more of them may be used in combination.
[0031] The content of the component (A1) relative to the total amount of the monomers of the component (A) is 25 parts by weight or more, more preferably 30 parts by weight or more, and even more preferably 35 parts by weight or more. The content of the component (A1) relative to the total amount of the monomers of the component (A) is preferably 50 parts by weight or less, more preferably 48 parts by weight or less, and even more preferably 45 parts by weight or less.
[0032] The content of the (A1) component relative to the total amount of the monomers of the (A) component is, for example, 25 parts by weight or more and 50 parts by weight or less, 30 parts by weight or more and 48 parts by weight or less, or 35 parts by weight or more and 45 parts by weight or less.
[0033] When the ratio of the (A1) component is equal to or greater than the above lower limit, the R 2 Since the steric hindrance of the above is exerted and the permeation of water molecules is inhibited, an adhesive layer exhibiting high water vapor barrier properties is obtained. When the proportion of the component (A1) is equal to or less than the above upper limit, the glass transition temperature of the adhesive does not become too high, and the adhesive composition can maintain an appropriate hardness.
[0034] ·(B) Component The component (B) is a hydroxyalkyl (meth)acrylate.
[0035] Although the component (B) is an optional component, by copolymerizing the component (B), crosslinking points can be introduced into the acrylic copolymer. Specific examples of the (B) component include at least one of 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and other polyalkylene glycol mono(meth)acrylates.
[0036] Furthermore, the proportion of the (B) component in the acrylic copolymer is preferably 10.0 parts by weight or less, more preferably 7.5 parts by weight or less, even more preferably 6.0 parts by weight or less, particularly preferably 5.0 parts by weight or less, and even more preferably 3.0 parts by weight or less, relative to the total amount (100 parts by weight) of the (A) component. Furthermore, the proportion of the (B) component in the acrylic copolymer may be 0.1 parts by weight or more, 1.0 parts by weight or more, or 1.5 parts by weight or more, relative to the total amount (100 parts by weight) of the (A) component.
[0037] The ratio of the (B) component in the acrylic copolymer relative to the total amount (100 parts by weight) of (A) is, for example, 0.1 parts by weight or more and 10.0 parts by weight or less, 1.0 parts by weight or more and 7.5 parts by weight or less, 1.0 parts by weight or more and 6.0 parts by weight or less, 1.0 parts by weight or more and 5.0 parts by weight or less, or 1.5 parts by weight or more and 3.0 parts by weight or less.
[0038] The weight average molecular weight of the acrylic copolymer is not particularly limited, but is preferably 200,000 or more and 5,000,000 or less, more preferably 300,000 or more and 4,000,000 or less, and particularly preferably 500,000 or more and 2,000,000 or less. When the weight average molecular weight of the acrylic copolymer is within this range, the obtained adhesive composition can exhibit excellent adhesive strength. In this specification, the weight average molecular weight means a polystyrene-equivalent molecular weight determined by GPC (gel permeation chromatography) measurement.
[0039] The presence of ethyl acrylate, component (A1), component (A2), and component (B) in the acrylic copolymer can be confirmed by a Fourier transform infrared spectrophotometer (FTIR), a gas chromatograph mass spectrometer (GCMS), a nuclear magnetic resonance (NMR) device, or the like.
[0040] The synthesis of the acrylic copolymer may be carried out by polymerizing the above-mentioned alkyl (meth)acrylate monomer by radical reaction in the presence of a polymerization initiator by a conventionally known method. The detailed polymerization method is not particularly limited, and a conventionally known method may be used. For example, solution polymerization is preferred.
[0041] The pressure-sensitive adhesive composition of the present embodiment can be produced by mixing the acrylic copolymer with, as required, a solvent, a crosslinking agent, a tackifier, a silane coupling agent, and the like.
[0042] Examples of crosslinking agents that may be contained in the pressure-sensitive adhesive composition of the present embodiment include trifunctional or higher isocyanate compounds. Specifically, diisocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, and pentamethylene diisocyanate are preferred, and TMP adducts of tolylene diisocyanate and isocyanurates of pentamethylene diisocyanate are particularly preferred.
[0043] <Laminate> The laminate of the present embodiment is a two-layer laminate of substrate / adhesive layer, in which the adhesive composition is laminated on the substrate. It may also be a three-layer laminate in which substrate / adhesive layer / substrate are laminated in this order. Here, the adhesive layer means a layer of the adhesive composition after the adhesive composition of the present embodiment is applied to the substrate and dried.
[0044] Examples of the substrate include a resin film, a glass plate, an acrylic plate, and a metal foil. The pressure-sensitive adhesive composition of the present embodiment can exhibit high adhesive strength to a variety of substrates.
[0045] The resin film is preferably at least one selected from the group consisting of modified polyimide resin films, polyester resin films, liquid crystal polymer films, cyclic olefin resin films, polyphenylene ether resin films, polyphenylene sulfide resin films, polyether ether ketone resin films, bismaleimide resin films, triazine resin films, and benzocyclobutene resin films.
[0046] Examples of the metal foil include stainless steel foil, copper foil, and aluminum foil.
[0047] In the laminate of the present embodiment, the thickness of the pressure-sensitive adhesive layer is, for example, 1 μm or more and 200 μm or less, and the thickness of the substrate is, for example, 20 μm or more and 200 μm or less.
[0048] <Adhesive film> The pressure-sensitive adhesive film of the present embodiment includes a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition of the present embodiment on one or both sides of a resin film.
[0049] <Adhesive layer for optical film> The pressure-sensitive adhesive layer for optical films of the present embodiment can be formed by applying the pressure-sensitive adhesive composition of the present embodiment to a substrate or a release film, and then crosslinking the pressure-sensitive adhesive composition. The gel fraction of the pressure-sensitive adhesive layer for optical films after crosslinking is preferably 60 to 90%.
[0050] When the pressure-sensitive adhesive layer for an optical film of this embodiment is used for bonding between layers of optical members, it is desirable for the pressure-sensitive adhesive layer to be thin. The thickness of the pressure-sensitive adhesive layer for an optical film is preferably 5 to 25 μm.
[0051] <Image display device> The present embodiment is an image display device in which the pressure-sensitive adhesive layer for an optical film of the present embodiment is used for bonding an optical film. The pressure-sensitive adhesive layer for an optical film of the present embodiment can be used for bonding glass plates and the like of an image display device.
[0052] Examples of the image display device of the present embodiment include a liquid crystal display device (liquid crystal panel), an organic EL display device (liquid crystal panel), a touch panel, and electronic paper, but are not limited to these.
[0053] <Polarizing plate> The present embodiment is a polarizing plate in which the pressure-sensitive adhesive layer for an optical film of the present embodiment is used for bonding an optical film. The pressure-sensitive adhesive layer for an optical film of the present embodiment has sufficient transparency and is therefore suitable for use in laminating a polarizing plate. EXAMPLES
[0054] The present invention will be explained more specifically below with reference to examples, but the present invention is not limited to these examples.
[0055] <Preparation of Pressure-Sensitive Adhesive Composition> Example 1 (1) Manufacture of acrylic copolymer Nitrogen gas was introduced into a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, and the air in the reactor was replaced with nitrogen gas. Then, 40 parts by weight of isobornyl acrylate, 60 parts by weight of 2-ethylhexyl acrylate, 1.0 part by weight of 4-hydroxybutyl (meth)acrylate, and a solvent (ethyl acetate) were added to the reactor. Then, 0.1 parts by weight of azobisisobutyronitrile as a polymerization initiator was dropped over 2 hours, and the mixture was reacted at 65°C for 6 hours to obtain an acrylic copolymer solution.
[0056] The weight average molecular weight (Mw) and molecular weight dispersity (Mw / Mn) of the acrylic copolymer, calculated as standard polystyrene by GPC measurement, are shown in Table 1.
[0057] (2) Production of adhesive composition To 100 parts by weight of the obtained acrylic copolymer, 0.3 parts by mass of a crosslinking agent (Takenate (registered trademark) D-101E, manufactured by Mitsui Chemicals, Inc.) was added and mixed with stirring to obtain a pressure-sensitive adhesive composition of Example 1.
[0058] (3) Manufacturing of adhesive sheets This adhesive composition was applied onto a release film consisting of a silicone resin-coated polyethylene terephthalate (PET) film, and then dried at 90°C to remove the solvent, yielding an adhesive sheet with an adhesive layer thickness of 25 μm.
[0059] [Measurement of biomass degree] The biomass ratios shown in Table 1 were calculated using the following method. The content of carbon isotope with mass number 14 was measured by accelerator mass spectrometry (AMS) in accordance with ASTM D6866 to measure the biomass degree of the acrylic copolymer contained in the pressure-sensitive adhesive composition. Specifically, for the adhesive sheet obtained in "(3) Production of adhesive sheet" above, the content ratio of carbon isotope with mass number 14 was measured by accelerator mass spectrometry (AMS method) measured in accordance with ASTM D6866, thereby measuring the biomass degree of the acrylic copolymer contained in the adhesive composition. The pressure-sensitive adhesive sheet obtained in the above "(3) Production of pressure-sensitive adhesive sheet" corresponds to the solid content from which the solvent component of the pressure-sensitive adhesive composition has been removed, and therefore the biomass degree of the pressure-sensitive adhesive sheet can be regarded as the biomass degree of the acrylic copolymer contained in the pressure-sensitive adhesive composition.
[0060] [Calculation of glass transition temperature] The glass transition temperature was calculated by the following FOX formula. (FOX formula) 1 / Tg=W1 / Tg1+W2 / Tg2+···W N / Tg N Tg: Glass transition temperature of the acrylic copolymer Tg N : Glass transition temperature of homopolymer W N : weight fraction of monomer
[0061] Examples 2 to 3 and Comparative Examples 1 to 8 In the same manner as in Example 1, pressure-sensitive adhesive compositions of Examples 2 to 3 and Comparative Examples 1 to 8 shown in Table 1 below were prepared.
[0062] [Table 1]
[0063] In Table 1, each symbol represents the following material. The numbers in brackets indicate the blend amount (parts by weight). IBOA: Isobornyl acrylate 2EHA: 2 Ethylhexyl Acrylate LMA: Lauryl methacrylate OCA: Octyl acrylate LA: Lauryl acrylate THFA: Tetrahydrofuryl acrylate BHA: Behenyl acrylate 4HBA: 4-Hydroxybutyl acrylate
[0064] [Adhesive strength measurement 1] The adhesive sheet obtained in the above "(3) Production of adhesive sheet" was transferred onto one side of a 50 μm thick polyester film substrate to obtain a sample adhesive film (optical film with adhesive layer). The obtained adhesive film was attached to the surface of a 1 mm thick stainless steel foil (SUS304 BA plate) that had been washed with acetone using a pressure roller, and left for 20 minutes in an atmosphere of 23°C x 50% RH. As a method for measuring the adhesive strength when peeling the adhesive film from the surface of the stainless steel foil, the peel strength of the adhesive film was measured using a tensile tester in accordance with JIS Z0237 (Test method for adhesive tapes and adhesive sheets), and the peel strength when peeled in a 180° direction at a speed of 300 mm / min was taken as the adhesive strength (N / 25 mm) of the adhesive layer of the adhesive film to the stainless steel foil. When the adhesive strength was 3 N / 25 mm or more, it was evaluated as having high adhesive strength to the stainless steel foil.
[0065] [Adhesive strength measurement 2] The adhesive sheet obtained in the above "(3) Production of adhesive sheet" was transferred onto one side of a 50 μm thick polyester film substrate to obtain a sample adhesive film (optical film with adhesive layer). The obtained adhesive film was attached to the surface of a 2 mm thick acrylic plate (trade name Paraglass (registered trademark)) using a pressure roller, and left for 20 minutes in an atmosphere of 23°C x 50% RH. As a method for measuring the adhesive strength when peeling the adhesive film from the surface of the acrylic plate, the peel strength of the adhesive film was measured using a tensile tester in accordance with JIS Z0237 (Test method for adhesive tapes and adhesive sheets), and the peel strength when peeled in a 180° direction at a speed of 300 mm / min was taken as the adhesive strength (N / 25 mm) of the adhesive layer of the adhesive film to the acrylic plate. When the adhesive strength was 5 N / 25 mm or more, it was evaluated as having high adhesive strength to the acrylic plate.
[0066] [Adhesive strength measurement 3] The adhesive sheet obtained in the above "(3) Production of adhesive sheet" was transferred onto one side of a polyester film substrate having a thickness of 50 μm to obtain an adhesive film (optical film with adhesive layer) as a sample. The obtained adhesive film was attached to the surface of the non-tin side of an alkali-free glass (trade name Eagle XG (registered trademark)) having a thickness of 1 mm, which had been washed with acetone, using a pressure roller, and left for 20 minutes in an atmosphere of 23 ° C × 50% RH. As a method for measuring the adhesive strength when peeling the adhesive film from the surface of the glass plate, the peel strength of the adhesive film was measured using a tensile tester in accordance with JIS Z0237 (Test method for adhesive tape and adhesive sheet), and the peel strength when peeled in a 180 ° direction at a speed of 300 mm / min was taken as the adhesive strength (N / 25 mm) of the adhesive layer of the adhesive film to the glass plate. When the adhesive strength was 2 N / 25 mm or more, it was evaluated that the adhesive film exhibited high adhesive strength to the glass plate.
[0067] [Adhesive strength measurement 4] The adhesive sheet obtained in the above "(3) Production of adhesive sheet" was transferred onto one side of a 50 μm thick polyester film substrate to obtain an adhesive film (optical film with adhesive layer) as a sample. The obtained adhesive film was attached to the surface of a 50 μm thick cycloolefin copolymer film (trade name Zeonor (registered trademark) ZF-16) fixed with double-sided tape on the surface of a 1 mm thick stainless steel foil (SUS304 BA plate) using a pressure roller, and left for 20 minutes in an atmosphere of 23 ° C x 50% RH. As a method for measuring the adhesive strength when peeling the adhesive film from the surface of the cycloolefin copolymer film, the peel strength of the adhesive film was measured using a tensile tester in accordance with JIS Z0237 (Test method for adhesive tape and adhesive sheet), and the peel strength when peeled in the 180 ° direction at a speed of 300 mm / min was taken as the adhesive strength (N / 25 mm) of the adhesive layer of the adhesive film to the cycloolefin copolymer film. An adhesive strength of 16 N / 25 mm or more was evaluated as having high adhesive strength to the glass plate. In Table 2, cycloolefin copolymer film is abbreviated as "COP."
[0068] [Water vapor transmission rate measurement] Water vapor permeability [g / (m 2 The water vapor transmission rate (g / day) was calculated by the infrared sensor method based on JIS K7129 B method using a MOCON (registered trademark) water vapor transmission rate measuring device PERMATRAN-W (registered trademark) 3 / 34G manufactured by Hitachi High-Tech Science Corporation, at 32°C and 90% RH, and calculated from the amount of water vapor (g) that permeated over 24 hours at 1 m2 of area. 2 The measured value was 890g / (m 2 ·day), the measurement limit of the measuring device is reached, so the measurement value is not specified and it is assumed to be "890g / (m 2 1-day or more".
[0069] [Table 2]
[0070] As shown in Table 2, Examples 1 to 3, which used an acrylic copolymer containing a predetermined amount of component (A1), had a water vapor permeability of 300 g / (m 2 ·day), demonstrating high water vapor barrier properties. This is presumably because the side chains of component (A1) inhibit the permeation of water molecules through steric hindrance.
[0071] Moreover, Examples 1 to 3 exhibited high adhesive strength to all of the acrylic plate, glass plate, stainless steel foil, and cycloolefin polymer film.
[0072] On the other hand, Comparative Examples 1 to 6 and 8, which did not contain the component (A1), had high water vapor transmission rate and low adhesion. Furthermore, Comparative Example 7, in which the content of the component (A1) was less than 25 parts by weight based on the total amount of the component (A), had a higher water vapor transmission rate than Examples 1 to 3, and had insufficient adhesion to the cycloolefin polymer film.
Claims
1. A pressure-sensitive adhesive composition comprising an acrylic copolymer, The glass transition temperature of the acrylic copolymer is 10° C. or lower, 30% or more of the total carbon number of the acrylic copolymer is biomass-derived carbon, The acrylic copolymer contains a component (A), The component (A) has a component (A1) represented by the following general formula (1), A pressure-sensitive adhesive composition, wherein the content of the component (A1) is 25 parts by weight or more based on the total amount of the monomers of the component (A). [Formula 1] (In general formula (1), R 1 is a hydrogen atom or a methyl group. 2 is a polycyclic hydrocarbon group having 7 to 12 carbon atoms. 2 is an alkyl group derived from biomass.
2. The pressure-sensitive adhesive composition according to claim 1 , wherein the component (A1) is isobornyl acrylate.
3. 3. The pressure-sensitive adhesive composition according to claim 1, wherein the component (A) comprises a component (A2), and the component (A2) is an alkyl (meth)acrylate having an alkyl group having 1 to 20 carbon atoms at an ester terminal.
4. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the acrylic copolymer comprises a component (B), and the component (B) is a hydroxyalkyl (meth)acrylate.
5. A laminate having a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to claim 1 or 2.
6. A pressure-sensitive adhesive film comprising a resin film and a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to claim 1 or 2 on one or both sides thereof.
7. A pressure-sensitive adhesive layer for an optical film, which is formed from the pressure-sensitive adhesive composition according to claim 1 or 2.
8. An image display device, in which the pressure-sensitive adhesive layer for an optical film according to claim 7 is used for bonding an optical film.
9. A polarizing plate with a pressure-sensitive adhesive layer, comprising the pressure-sensitive adhesive layer for an optical film according to claim 7 .
Citation Information
Patent Citations
Adhesive composition
JP2016079256A
Pressure-sensitive adhesive and pressure-sensitive adhesive sheet
JP2018145368A
Aqueous pigment dispersion, aqueous inkjet ink and dry film
JP2022133936A
Adhesive composition, adhesive layer, and adhesive sheet
JP2023016418A
Adhesive agent, adhesive tape, and method for affixing electronic components or vehicle-mounted components
WO2019244595A1