Film and application of the same

A film with a thermoplastic resin, organic antibacterial agent, and oil combination addresses decomposition and appearance issues, offering superior antibacterial and mechanical properties for packaging.

JP2024135654APending Publication Date: 2024-10-04MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023046447
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing antibacterial sheets using dehydroacetic acid or sodium dehydroacetate face issues with decomposition at high temperatures during resin molding and generate foreign matter affecting film appearance when increased amounts are used.

Method used

A film composed of a thermoplastic resin, an organic antibacterial agent with an average particle size of 20 μm or less, and an oil, which suppresses foreign substance generation and maintains good appearance while providing antibacterial properties.

Benefits of technology

The film achieves excellent antibacterial properties and high tensile elongation at break, ensuring a good appearance without foreign matter, suitable for food packaging and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135654000001
    Figure 2024135654000001
Patent Text Reader

Abstract

To provide a film having both excellent antibacterial property and good appearance.SOLUTION: A film contains a thermoplastic resin (A), an organic antibacterial agent (B) and oil and fat (C), wherein an average particle diameter of the organic antibacterial agent (B) contained in the film is 20 μm or less. A food packaging material contains the film.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film having both antibacterial properties and good appearance, and applications thereof. [Background technology]

[0002] In recent years, food waste has become a food issue. Food waste occurs when food spoils and is discarded, but it can also occur when food that has passed its expiration date or best-before date is discarded. Food waste is an issue when food that could have been eaten is discarded without being eaten, and to solve this problem, antibacterial films have been developed as a way to extend the expiration date or best-before date of food. Furthermore, with growing awareness of environmental conservation, there are also studies being conducted on making products thinner, reducing the amount of raw materials used, and improving recyclability.

[0003] For example, Patent Document 1 discloses an antibacterial sheet made of a thermoplastic resin to which 0.5 to 5.0% of dehydroacetic acid or sodium dehydroacetate has been added. Here, it has been investigated whether a sheet that exerts an antibacterial effect can be obtained by using dehydroacetic acid or sodium dehydroacetate as an antibacterial agent. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-267451 Summary of the Invention [Problem to be solved by the invention]

[0005] The antibacterial sheet disclosed in Patent Document 1 uses dehydroacetic acid or sodium dehydroacetate as an antibacterial agent, but when dehydroacetic acid is used, there is a problem that the antibacterial agent decomposes during resin molding because decomposition begins at 150°C or higher. In addition, when sodium dehydroacetate is used, there is a problem that if the amount of antibacterial agent used is increased to obtain the desired antibacterial properties, foreign matter is generated, which impairs the appearance of the film. If foreign matter (such as aggregates of antibacterial particles) is generated in the film, the film may break from these foreign matter, which causes problems in film formation.

[0006] In view of the above problems in the prior art, an object of the present invention is to provide a film having both excellent antibacterial properties and good appearance. [Means for solving the problem]

[0007] Examples of specific embodiments of the present invention are given below. [1] A film comprising a thermoplastic resin (A), an organic antibacterial agent (B), and an oil (C), wherein the average particle size of the organic antibacterial agent (B) contained in the film is 20 μm or less. [2] The film according to [1], wherein the thermoplastic resin (A) has a melting point of 180°C or lower or a glass transition temperature of 180°C or lower. [3] The film according to [1] or [2], wherein the thermoplastic resin (A) is a polyolefin resin. [4] The film according to [3], wherein the polyolefin resin is at least one selected from the group consisting of polyethylene, polypropylene, and ethylene-vinyl acetate copolymer. [5] The film according to any one of [1] to [4], wherein the organic antibacterial agent (B) is an organic acid salt. [6] The film according to [5], wherein the organic acid salt is at least one selected from the group consisting of sorbates, dehydroacetates, propionates, acetates, and benzoates. [7] The film according to any one of [1] to [6], wherein the content of the organic antibacterial agent (B) is 0.1 to 30 mass % relative to the total mass of the film. [8] The film according to any one of [1] to [7], wherein the oil (C) is a hydrogenated oil. [9] The film according to any one of [1] to [8], wherein the oil (C) is a highly hydrogenated oil.

[10] The film according to any one of [1] to [9], wherein the content of the oil or fat (C) is 0.01 to 10 mass % relative to the total mass of the film.

[11] The film according to any one of [1] to

[10] , which has a tensile elongation at break in at least one direction of 300% or more, as measured in accordance with JIS K7127 (1999).

[12] The film according to any one of [1] to

[11] , which is for food packaging.

[13] A food packaging material comprising the film according to any one of [1] to

[12] . Effect of the Invention

[0008] According to the present invention, a film having both excellent antibacterial properties and good appearance can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described below as an example of an embodiment of the present invention. However, the scope of the present invention is not limited to the embodiment described below. In this specification, when "X to Y" (X and Y are arbitrary numbers) is expressed, unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number) is expressed, it also includes the meaning of "preferably greater than X" or "preferably less than Y". In addition, "film" and "sheet" used in the following description are not clearly distinguished from each other, and "film" includes "sheet", and "sheet" includes "film".

[0010] [Antibacterial film] The film of the present invention contains a thermoplastic resin (A), an organic antibacterial agent (B), and a fat or oil (C). In the present invention, the average particle size of the organic antibacterial agent (B) contained in the film is 20 μm or less. The film of the present invention (hereinafter also referred to as "the present film") contains the fat or oil (C) in addition to the organic antibacterial agent (B), and thus can achieve both antibacterial properties and good appearance. The present film is a film that exhibits excellent antibacterial properties, and is therefore sometimes called an antibacterial film.

[0011] In addition, the film has high tensile elongation at break. When foreign matter (such as an aggregate of antibacterial particles) occurs in the film, the foreign matter may become the starting point for breaking the film, but in the present invention, an organic antibacterial agent having an average particle size of 20 μm or less is used as the organic antibacterial agent (B), and further, by containing oil (C) in addition to the organic antibacterial agent (B), the generation of foreign matter (such as an aggregate of antibacterial particles) can be suppressed, and therefore a high tensile elongation at break can be achieved.

[0012] As described above, in this film, a specific organic antibacterial agent is used in combination with fats and oils, and then composited with a thermoplastic resin, making it possible to produce an antibacterial film that combines antibacterial properties, good appearance, and high tensile elongation at break. The present invention will be described in detail below.

[0013] <Thermoplastic resin (A)> The film contains a thermoplastic resin (A). Examples of the thermoplastic resin include polyolefin resins, polyester resins, polyamide resins, polystyrene resins, acrylic resins, polyether resins, polyurethane resins, and ethylene-vinyl alcohol copolymer resins. Among them, the thermoplastic resin (A) is preferably a resin having heat sealability. In this specification, examples of the resin having heat sealability include resins having a melting point of 180° C. or less or a glass transition temperature of 180° C. or less. When the resin having heat sealability has a melting point, the melting point is more preferably 170° C. or less, even more preferably 160° C. or less, and particularly preferably 150° C. or less. When the resin having heat sealability has a glass transition temperature, the glass transition temperature is more preferably 150° C. or less, even more preferably 120° C. or less, and particularly preferably 100° C. or less. By setting the melting point or glass transition temperature within the above range, heat sealing at a lower temperature is possible, and the heat sealability is improved. By using a resin having heat sealability as the thermoplastic resin (A), the composition can be preferably used for, for example, food packaging applications.

[0014] In this embodiment, the thermoplastic resin (A) is preferably a polyolefin resin. The polyolefin resin is not particularly limited, but examples thereof include polymers containing α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, or 1-decene as structural units. The polyolefin resin may be a homopolymer containing only one of the above monomers as structural units, a copolymer containing two or more of the above monomers as structural units, or a copolymer containing other copolymerizable monomers as structural units. The copolymer contains the above monomers as main structural units.

[0015] Among them, from the viewpoints of appearance, tensile elongation at break, versatility, economy, etc., the polyolefin resin is preferably a polyethylene resin containing ethylene as the main monomer component, or a polypropylene resin containing propylene as the main monomer component, and is particularly preferably a polyethylene resin. Here, the main monomer component refers to a monomer component that is a structural unit that occupies 50% by mass or more and 100% by mass or less in the polyolefin resin. In this embodiment, the polyolefin resin is preferably at least one selected from the group consisting of polyethylene, polypropylene, and an ethylene-vinyl acetate copolymer.

[0016] The content of the thermoplastic resin (A) in the film of this embodiment is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 75% by mass or more, and particularly preferably 80% by mass or more, based on the total mass of the film. The content of the thermoplastic resin (A) is preferably 99% by mass or less, based on the total mass of the film. By setting the content of the thermoplastic resin (A) within the above range, the generation of foreign matter (such as aggregates of antibacterial particles) can be suppressed, making it easier to obtain good appearance and high tensile elongation at break.

[0017] (Polyethylene resin) The polyethylene resin is not particularly limited as long as it is a resin containing ethylene as the main monomer component, and examples thereof include low density polyethylene, linear low density polyethylene, linear very low density polyethylene, medium density polyethylene, and high density polyethylene. The polyethylene resin may be an ethylene homopolymer, or a copolymer containing ethylene as the main monomer component and other copolymerizable monomer components. Examples of the copolymer include a copolymer or multicomponent copolymer containing ethylene as the main monomer component and one or more comonomers selected from other copolymerizable monomer components, or a mixed composition thereof. The polyethylene resin may be used alone, or two or more types of copolymerizable monomer components, which have different compositions and physical properties, may be used in combination.

[0018] Examples of other copolymerizable monomer components (comonomers) include α-olefins having 3 to 10 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, and 1-octene; vinyl esters, such as vinyl acetate and vinyl propionate; unsaturated carboxylic acid esters, such as methyl (meth)acrylate and ethyl (meth)acrylate, and ionomers thereof; and unsaturated compounds, such as conjugated dienes and non-conjugated dienes. The proportion of the structural unit derived from the copolymerizable monomer contained in the polyethylene resin is not particularly limited, but is usually preferably 30% by mass or less, and more preferably 15% by mass or less. The inclusion of a copolymerizable monomer component in the polyethylene resin can increase the flexibility and transparency of the film.

[0019] Among these, the polyethylene resin is preferably low-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, ethylene-vinyl acetate copolymer (EVA), ethylene-(meth)acrylic acid ester copolymer or ionomer resin, more preferably linear low-density polyethylene or ethylene-vinyl acetate copolymer (EVA), and particularly preferably linear low-density polyethylene.

[0020] The linear low density polyethylene is preferably a linear low density polyethylene containing at least one α-olefin selected from the group consisting of 1-butene, 1-hexene, and 4-methyl-1-pentene as a comonomer. The proportion of the comonomer component is not particularly limited, but is usually preferably 30% by mass or less, and more preferably 15% by mass or less. The inclusion of the comonomer component in the linear low density polyethylene can increase the flexibility and transparency of the film.

[0021] The method for producing the polyethylene resin is not particularly limited, and any known polymerization method using an olefin polymerization catalyst can be used. For example, there are a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, etc. using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst, and a bulk polymerization method using a radical initiator.

[0022] The melting point of the polyethylene resin is preferably 70 to 130° C., and more preferably 80 to 120° C. If the melting point of the polyethylene resin is within this range, the tensile strength (for example, tensile breaking strength and tensile breaking elongation) and dimensional stability of the film tend to be improved. Here, the melting point of a polyethylene-based resin is the crystalline melting peak temperature (Tm) (°C) determined from a thermogram measured using a differential scanning calorimeter (DSC) by heating approximately 10 mg of resin from -50°C to 200°C at a heating rate of 10°C / min, holding it at 200°C for 1 minute, then cooling it to -50°C at a cooling rate of 10°C / min, and again heating it to 200°C at a heating rate of 10°C / min.

[0023] The melt flow rate (MFR) of the polyethylene resin is not particularly limited, but is usually preferably 0.1 to 20 g / 10 min or more, more preferably 0.5 to 18 g / 10 min, and even more preferably 1 to 15 g / 10 min. If the MFR is 0.1 g / 10 min or more, extrusion processability is stable, and if it is 20 g / 10 min or less, stable film formation during molding is possible and thickness unevenness, reduction or variation in mechanical strength, etc. are reduced, which is preferable. Here, MFR is a value measured in accordance with JIS K7210-1 (2014), and the measurement conditions are 190°C and a load of 2.16 kg.

[0024] The density of polyethylene resin is 0.880 to 0.980 g / cm 3 It is preferable that the density is 0.890 to 0.960 g / cm 3 More preferably, it is 0.900 to 0.940 g / cm 3It is particularly preferable that the density is 0.880 to 0.980 g / cm 3 It is preferable that the density is within this range because it has an excellent balance of transparency, strength, adhesion, and flexibility. Here, the density is a value measured in accordance with JIS K6922-1 (2018).

[0025] (Polypropylene resin) The polypropylene-based resin is not particularly limited as long as it is a resin containing propylene as the main monomer component, and may be a propylene homopolymer, or a copolymer containing propylene as the main monomer component and other copolymerizable monomer components. Examples of the copolymer include a copolymer or multicomponent copolymer containing propylene as the main monomer component and one or more comonomers selected from other copolymerizable monomer components, or a mixed composition thereof. The polypropylene-based resin may be used alone, or two or more types of copolymerizable monomer components, which have different compositions and physical properties, may be used in combination.

[0026] Examples of other copolymerizable monomer components (comonomers) include α-olefins having 2 to 20 carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, and 1-octene; dienes, such as divinylbenzene, 1,4-cyclohexadiene, dicyclopentadiene, cyclooctadiene, and ethylidene norbornene; vinyl acetate, (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylic acid glycidyl, vinyl alcohol, ethylene glycol, maleic anhydride, styrene, and cyclic olefins. The proportion of the structural unit derived from the copolymerizable monomer contained in the polypropylene-based resin is not particularly limited, but is usually preferably 30% by mass or less, and more preferably 15% by mass or less. The inclusion of a copolymerizable monomer component in the polypropylene-based resin can increase the flexibility and transparency of the film.

[0027] The polypropylene resin may be a block copolymer, a random copolymer, or a graft copolymer.

[0028] The method for producing the polypropylene resin is not particularly limited, and any known polymerization method using an olefin polymerization catalyst can be used. For example, there are a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, etc. using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst, and a bulk polymerization method using a radical initiator.

[0029] The melting point of the polypropylene resin is preferably 70 to 170° C., and more preferably 80 to 160° C. If the melting point of the polypropylene resin is in this range, the film will have a good balance of flexibility, strength, and heat resistance, which is preferable. Here, the melting point of a polypropylene-based resin is the crystalline melting peak temperature (Tm) (°C) determined from a thermogram measured using a differential scanning calorimeter (DSC) by heating approximately 10 mg of resin from -50°C to 200°C at a heating rate of 10°C / min, holding it at 200°C for 1 minute, then cooling it to -50°C at a cooling rate of 10°C / min, and again heating it to 200°C at a heating rate of 10°C / min.

[0030] The melt flow rate (MFR) of the polypropylene resin is not particularly limited, but is usually preferably 0.2 to 20 g / 10 min or more, more preferably 0.5 to 18 g / 10 min, and even more preferably 1 to 15 g / 10 min. If the MFR is 0.2 g / 10 min or more, the extrusion processability is stable, and if it is 20 g / 10 min or less, stable film formation during molding is possible and thickness unevenness, decrease or variation in mechanical strength, etc. are reduced, which is preferable. Here, MFR is a value measured in accordance with JIS K7210-1 (2014), and the measurement conditions are 230°C and a load of 2.16 kg.

[0031] <Organic antibacterial agents (B)> This film contains an organic antibacterial agent (B). In this film, the organic antibacterial agent (B) is uniformly dispersed throughout the film. For example, when the film is divided into three parts in the thickness direction, the content of the organic antibacterial agent (B) in each part is approximately uniform. In this specification, "the content of the organic antibacterial agent (B) is approximately uniform" means that there is no difference of 10% by mass or more in the content of the organic antibacterial agent (B) in each part.

[0032] The average particle size of all organic antibacterial agents (B) contained in the present film is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less, even more preferably 8 μm or less, and particularly preferably 5 μm or less. The average particle size of the organic antibacterial agent (B) is preferably 0.01 μm or more. By setting the average particle size of all organic antibacterial agents (B) contained in the present film within the above range, the antibacterial agent is easily exposed to the film surface, good antibacterial properties are obtained, and defects in the film caused by foreign matter (lumps) can be reduced, and the tensile breaking elongation and appearance can be improved. The average particle size in this specification is the particle size measured using a laser diffraction type particle size measuring device (CILAS 1190 manufactured by CILAS Corporation) and the arithmetic average value is calculated.

[0033] The D90 particle size of all organic antibacterial agents (B) contained in the present film is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 5 μm or less, and particularly preferably 2 μm or less. The D90 particle size of the organic antibacterial agent (B) is preferably 0.3 μm or more. By making the D90 particle size of all organic antibacterial agents (B) contained in the present film within the above range, the antibacterial agent is easily exposed to the film surface, good antibacterial properties are obtained, and defects in the film caused by foreign matter (lumps) can be reduced, and the tensile breaking elongation and appearance can be improved. The D90 particle size in this specification is calculated according to JIS Z 8825 (2013) by measuring the particle size using a laser diffraction particle size measuring device (CILAS 1190 manufactured by Cirrus Corporation).

[0034] The D50 particle size of the all-organic antibacterial agent (B) contained in the present film is preferably 0.05 to 1 μm, more preferably 0.08 to 0.8 μm, and even more preferably 0.1 to 0.5 μm. If the D50 particle size is within the above range, antibacterial properties can be imparted without impairing the tensile elongation at break or the appearance. The D50 particle size in this specification is measured using a laser diffraction particle size measuring device (CILAS 1190 manufactured by CILAS Corporation) and calculated in accordance with JIS Z 8825 (2013).

[0035] The D10 particle size of the all-organic antibacterial agent (B) contained in the present film is preferably 0.01 to 0.2 μm, more preferably 0.02 to 0.1 μm. If the D10 particle size is within the above range, antibacterial properties can be easily imparted without impairing the tensile elongation at break or the appearance. The D10 particle size in this specification is calculated in accordance with JIS Z 8825 (2013) by measuring the particle size using a laser diffraction particle size measuring device (CILAS 1190 manufactured by CILAS Corporation).

[0036] The maximum diameter of the organic antibacterial agent (B) contained in the present film is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The maximum diameter of the organic antibacterial agent (B) is preferably 0.5 μm or more. By setting the maximum diameter of the organic antibacterial agent (B) within the above range, the antibacterial agent is easily exposed on the film surface, good antibacterial properties are obtained, and defects in the film caused by foreign matter (lumps) can be reduced, and the effect of increasing the tensile breaking elongation and improving the appearance can be easily obtained.

[0037] Various grinding methods may be used as a method for controlling the particle size of the organic antibacterial agent (B) within the above range. Examples of grinding methods include rotary grinding using a ball mill, a bead mill, a jet mill, an attritor, a vibration mill, a planetary mill, a rotary mill, a stone mill, etc. These grinding methods may be dry or wet, and the temperature during grinding may be appropriately adjusted from extremely low to high temperatures so as to obtain the desired particle size. In addition, these grinding steps may be a combination of multiple grinding methods, may be ground in stages, or may be classified as necessary. Among these, rotary grinding using a bead mill, a jet mill, a stone mill, etc. is preferred from the viewpoint of productivity and grindability.

[0038] The organic antibacterial agent (B) used in the present invention can be used without any particular limitation as long as it has an average particle size within the above range and is an organic antibacterial agent. For example, monocarboxylic acids such as benzoic acid, dehydroacetic acid, sorbic acid, propionic acid, acetic acid, formic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, and stearic acid, salts of the above monocarboxylic acids such as sodium dehydroacetate, potassium sorbate, sodium propionate, and sodium benzoate; oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, Organic acids such as dicarboxylic acids, such as azelaic acid and sebacic acid, and their salts; hydroxy acids, such as lactic acid, gluconic acid, glycolic acid, glyceric acid, malic acid, citric acid, tartaric acid, hydroxyacetic acid, hydroxybutyric acid, tartronic acid, salicylic acid, (m-, p-)hydroxybenzoic acid, 12-hydroxydodecanoic acid, 12-hydroxyisobutyric acid, (o-, m-, p-)hydroxyphenylacetic acid, 4-hydroxyphthalic acid, and 12-hydroxystearic acid, and their salts. Antibacterial agents; amino acid-based antibacterial agents such as glycine; quaternary ammonium salt-based antibacterial agents such as hexadecylpyridinium chloride, diisobutylphenoxydimethylbenzoylammonium chloride, benzalkonium chloride, benzethonium chloride, methylbenzethonium chloride, cetylpyridinium chloride, cetrimonium, dophanium chloride, didecyldimethylammonium chloride, and domiphen bromide; surfactant-based antibacterial agents such as alkyldiaminoethylglycine hydrochloride, sodium alkylbenzenesulfonate, polyoxyethylene nonylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene stearylamine, and lauryldimethylbenzylammonium chloride; halogen-based antibacterial agents such as diiodomethyl-p-trisulfone and polyvinylpyrrolidone iodide; peroxide-based antibacterial agents such as peracetic acid; ester-based antibacterial agents such as glyceryl laurate and ethyl hydroxybenzoate; aldehyde-based antibacterial agents such as formaldehyde;Cresol, o-phenylphenol, 2-isopropyl-5-methylphenol, ethanol, ethyl-2,4-dihydroxy-6-methylbenzoate, methyl-2,4-dihydroxy-3,6-dimethylbenzoate, isopropyl-2,4-dihydroxy-6-methylbenzoate, 3-methoxy-5-methylphenyl-2,4-dihydroxy-6-methylbenzoate, ethyl-2,4-dihydroxy-3,6-dimethylbenzoate, ethyl-3-formyl-2,4-dihydroxy-6-methylbenzoate, iso Examples of the phenol-alcohol antibacterial agents include propyl-3-formyl-2,4-dihydroxy-6-methylbenzoate, 3-hydroxy-5-methylphenyl-2,4-dihydroxy-6-methylbenzoate, 3-methyl-4 isopropylphenol, 3-hydroxy-5-methylphenyl-2-dihydroxy-4-methoxy-6-methylbenzoate, 3-methoxy-5-methylphenyl-2-hydroxy-4-methoxy-6-methylbenzoate, and 3-chloro-2,6-dihydroxy-4-methylbenzoate. Only one of these organic antibacterial agents may be contained, or two or more types may be contained.

[0039] The organic antibacterial agent is preferably an organic acid salt having a salt form among organic antibacterial agents, because of its thermal stability, compatibility with thermoplastic resins, and ease of handling. Furthermore, from the viewpoints of safety to living organisms, ease of availability, cost, etc., the organic acid salt is preferably at least one selected from the group consisting of sorbates, dehydroacetates, propionates, acetates, and benzoates. These sorbates, dehydroacetates, propionates, acetates, and benzoates are listed in the Official Specification of Food Additives established by the Ministry of Health, Labor, and Welfare, and are preferably used from the viewpoint of safety when used in applications such as food packaging.

[0040] The content of the organic antibacterial agent (B) in the film of this embodiment is preferably 0.1 to 30 mass % relative to the total mass of the film, more preferably 0.5 to 20 mass %, and particularly preferably 1 to 15 mass %. By setting the content of the organic antibacterial agent (B) within the above range, it is possible to impart superior antibacterial properties to the film.

[0041] <Oil (C)> The film contains fats and oils (C). The fats and oils used in the present invention have the effect of dispersing the antibacterial agent uniformly in the thermoplastic resin, and can improve the appearance of the film. The fats and oils refer to ester compounds of fatty acids and glycerin, and examples thereof include vegetable fats and oils, animal fats and oils obtained by hardening these fats and oils. Specific examples of vegetable fats and oils include rapeseed oil, soybean oil, rice oil, palm oil, palm kernel oil, coconut oil, corn oil, cottonseed oil, peanut oil, castor oil, sunflower oil, olive oil, etc. Examples of animal fats and oils include chicken oil, lard, beef tallow, milk fat, mutton tallow, horse fat, and fish oil. Examples of hardened oils include hardened rapeseed oil, extremely hardened rapeseed oil, hardened soybean oil, extremely hardened soybean oil, hardened rice oil, extremely hardened rice oil, hardened palm oil, extremely hardened palm oil, hardened palm kernel oil, hardened coconut oil, hardened corn oil, hardened cottonseed oil, hardened castor oil, hardened sunflower oil, hardened olive oil, hardened chicken fat oil, extremely hardened chicken fat oil, hardened lard oil, extremely hardened lard oil, hardened beef tallow oil, extremely hardened beef tallow oil, extremely hardened fish oil, and extremely hardened fish oil. Among these oils, hardened oil or extremely hardened oil is preferably used from the viewpoint of handling and heat resistance, and extremely hardened oil is more preferably used. Among them, extremely hardened soybean oil, extremely hardened rapeseed oil, extremely hardened rice oil, and extremely hardened palm oil are particularly preferable from the viewpoint of large distribution amount, price, and high heat resistance. These oils may be used alone or in a mixture of two or more types.

[0042] Here, the hardening treatment of fats and oils refers to a treatment in which hydrogen is added to fats and oils, and unsaturated fatty acids contained in normal fats and oils are converted to saturated fatty acids. Since the ratio of saturated fatty acids in highly hardened oils is high, they have a high affinity with thermoplastic resins and can effectively disperse organic antibacterial agents.

[0043] The fat (C) is preferably solid at 15° C. By using such fat (C), the handleability of the fat (C) during film production can be improved, and the production efficiency of the film can be increased. In addition, by using a solid fat (C), the antibacterial agent can be more uniformly dispersed in the thermoplastic resin, and the appearance of the film can be more effectively improved. Examples of fats and oils that are solid at 15°C include palm oil, palm kernel oil, chicken oil, lard, beef tallow, milk fat, mutton tallow, horse tallow, hardened rapeseed oil, extremely hardened rapeseed oil, hardened soybean oil, extremely hardened soybean oil, hardened rice oil, extremely hardened rice oil, hardened palm oil, extremely hardened palm oil, hardened palm kernel oil, hardened coconut oil, hardened corn oil, hardened cottonseed oil, hardened castor oil, hardened sunflower oil, hardened olive oil, hardened chicken fat oil, extremely hardened chicken fat oil, hardened lard oil, extremely hardened lard oil, hardened beef tallow oil, extremely hardened beef tallow oil, hardened fish oil and extremely hardened fish oil.

[0044] The content of the fat (C) in the film of this embodiment is preferably 0.01 to 10% by mass, more preferably 0.02 to 8% by mass, and particularly preferably 0.03 to 5% by mass, based on the total mass of the film. By setting the content of the fat (C) within the above range, the generation of foreign matter (lumps) caused by the antibacterial agent can be reduced, and the appearance of the film can be improved. In addition, by reducing the generation of foreign matter (lumps), the decrease in the tensile elongation at break of the film can be suppressed. In addition, by setting the content of the fat (C) to the above upper limit value or less, the fat can be suppressed from bleeding out of the film and becoming cloudy, and by setting the content of the fat (C) to the above lower limit value or more, the effect of dispersing the antibacterial agent can be enhanced, and the generation of foreign matter (lumps) can be reduced.

[0045] In order to reduce the amount of oil (C) used and improve the dispersibility of the organic antibacterial agent, the oil (C) may be used by coating the particle surface of the organic antibacterial agent (B). When the oil (C) is used by coating the particle surface of the organic antibacterial agent (B), it is preferable to provide a step of coating the particles of the organic antibacterial agent (B) with the oil (C) in advance. The method of coating the particles of the organic antibacterial agent (B) with the oil (C) is not particularly limited, but includes a method of heating the oil (C) to the melting point or higher while stirring the particles of the organic antibacterial agent (B), a method of dissolving the oil (C) in a solvent to make it liquid and spraying the oil (C) evenly onto the particles of the organic antibacterial agent (B), a method of putting the particles of the organic antibacterial agent (B) into the oil (C) that has been heated to the melting point or higher to make it liquid or into the oil (C) that has been dissolved in a solvent to make it liquid, and a method of cooling or removing the solvent while stirring the particles of the organic antibacterial agent (B) and the like.

[0046] <Optional ingredients> The present film may further contain optional components in addition to the above-mentioned components. Examples of optional components include colorants, inorganic fillers, organic fillers, ultraviolet absorbers, light stabilizers, heat stabilizers, antioxidants, lubricants (slip agents), anti-blocking agents, hydrolysis inhibitors, plasticizers, flame retardants, anti-fogging agents, and adhesives. These optional components may be directly mixed with the resin constituting the film, or a master batch containing the resin and optional components may be prepared before forming the film. The present film may contain two or more optional components in appropriate combination. The content of the optional components is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the film.

[0047] The film may also contain a sugar alcohol as an optional component. Examples of sugar alcohols include chain sugar alcohols such as glycerol with three carbon atoms; sugar alcohols with four carbon atoms, such as erythritol and threitol, obtained by reducing monosaccharides; sugar alcohols with five carbon atoms, such as ribitol, arabitol and xylitol; and sugar alcohols with six carbon atoms, such as glucitol, mannitol, iditol, talitol and galactitol. Examples of sugar alcohols include cyclic sugar alcohols, such as cyclitols, such as inositol. Examples of sugar alcohols include disaccharide alcohols, such as maltitol, lactitol and reduced isomaltulose, obtained by reducing disaccharides.

[0048] The film may contain an organic acid as an optional component. Examples of the organic acid include monocarboxylic acids such as acetic acid, formic acid, propionic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, and stearic acid; dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid; hydroxy acids such as lactic acid, gluconic acid, glycolic acid, glyceric acid, malic acid, citric acid, tartaric acid, hydroxyacetic acid, hydroxybutyric acid, tartronic acid, salicylic acid, (m-, p-)hydroxybenzoic acid, 12-hydroxydodecanoic acid, 12-hydroxyisobutyric acid, (o-, m-, p-)hydroxyphenylacetic acid, 4-hydroxyphthalic acid, and 12-hydroxystearic acid; and inositol phosphates such as phytic acid.

[0049] (Laminated film) The film may be a single layer film, or a laminated film with other resin layers. In the laminated film, when the layer containing the thermoplastic resin (A), the organic antibacterial agent (B) and the oil (C) is called "Layer A" and the other resin layer is called "Layer B", the laminated film may have a two-layer structure of Layer A / Layer B, or a multi-layer structure such as Layer A / Layer B / Layer A or Layer B / Layer A / Layer B. In addition, when the laminated film has Layer A and Layer B, and further another resin layer C (hereinafter referred to as "Layer C"), it may have a three-layer structure of Layer A / Layer B / Layer C, or a three-type five-layer structure such as Layer A / Layer B / Layer C / Layer B / Layer A. Furthermore, when the laminated film has layers A to C and another resin layer D (hereinafter referred to as "layer D"), it may have a four-layer structure of layer A / layer B / layer C / layer D, or a four-type seven-layer structure of layer A / layer B / layer C / layer D / layer C / layer B / layer A. Note that, in the laminated film, there is no limitation on the number of layers, the order of layers, or the type and number of layers other than layer A, but it is preferable that layer A is provided on the front and / or back surface of the film. Note that the laminated film may have a structure in which a plurality of layers A are laminated. When the laminated film is used for food packaging, it is preferable that layer A containing thermoplastic resin (A), organic antibacterial agent (B) and oil (C) is disposed on the surface of the laminated film and is the innermost layer (the layer in contact with food).

[0050] Specific examples of the configuration of the laminate film include a laminate film having at least three layers: a layer containing a thermoplastic resin (A), an organic antibacterial agent (B) and a sugar alcohol (C), a base layer of polyester, polyamide, polypropylene, polystyrene (syndiotactic polystyrene) or the like, and a gas barrier layer having gas barrier properties of polytetrafluoroethylene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, etc. In this case, the layer containing the thermoplastic resin (A), the organic antibacterial agent (B) and the sugar alcohol (C) is preferably disposed on one surface layer (the innermost layer) of the laminate film.

[0051] When the present film is a laminated film, examples of the other resin layer include layers containing polyester, polyamide, polypropylene, polystyrene (syndiotactic polystyrene), polymethylpentene, polyimide, polytetrafluoroethylene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyethylene, etc. The other resin layer may be provided depending on the required function, and for example, the provision of the other resin layer can impart gas barrier properties, heat resistance, and moisture resistance. The laminated film may also have a layer containing a metal such as aluminum or iron.

[0052] When a laminated film is to be produced, it may be produced according to a conventional method, among which a method of co-extrusion using a plurality of extruders through a lamination die is preferred.

[0053] (Film manufacturing method) The present film can be produced by a known method. For example, the present film can be produced by using an inflation method, an extrusion T-die method, or the like. Specifically, the present film can be produced by melt-kneading the thermoplastic resin (A), the organic antibacterial agent (B), and the oil (C), and forming the molten resin composition into a film (sheet). The present film may be a non-stretched film or a stretched film.

[0054] When the present film is a laminated film, the laminated film can be manufactured by adopting the above-mentioned known method using the resin composition forming each layer. Alternatively, the laminated film may be manufactured by laminating previously obtained films by a lamination method or the like. Among them, it is preferable to use the co-extrusion T-die method, since the film-forming process is the same even when the number of layers of the film is large, and thickness control is relatively easy.

[0055] The manufacturing process of the present film may include a step of winding the obtained film into a roll. That is, the present embodiment may relate to a rolled body (film roll) obtained by winding the present film into a roll. When winding the film, it is preferable to wind the film around a core. It is preferable to use a core having a width equal to or greater than the width of the film.

[0056] <Film properties> The present film preferably has the following physical properties:

[0057] (Tensile breaking strength) In this film, the tensile strength at break in at least one direction measured in accordance with JIS K7127 (1999) is preferably 3 MPa or more, more preferably 5 MPa or more, even more preferably 7 MPa or more, and particularly preferably 9 MPa or more. The upper limit of the tensile strength at break is not particularly limited, but is preferably 100 MPa or less. The tensile strength at break is a value measured in accordance with JIS K7127 (1999) using a tensile tester using a test piece having a length of 50 mm in the measurement direction and a width of 10 mm under the conditions of a measurement temperature of 23±2°C, a chuck distance of 20 mm, and a test speed of 200 mm / min.

[0058] More specifically, the MD tensile breaking strength of the present film, measured in accordance with JIS K7127 (1999), is preferably 3 MPa or more, more preferably 5 MPa or more, even more preferably 7 MPa or more, and particularly preferably 9 MPa or more. The upper limit of the MD tensile breaking strength is not particularly limited, but is preferably 100 MPa or less. The TD tensile strength at break, measured in accordance with JIS K7127 (1999), is preferably 3 MPa or more, more preferably 5 MPa or more, even more preferably 7 MPa or more, and particularly preferably 9 MPa or more. The upper limit of the TD tensile strength at break is not particularly limited, but is preferably 100 MPa or less. In this embodiment, it is preferable that the tensile breaking strength in either the MD or TD is within the above range, and it is particularly preferable that the tensile breaking strength in both the MD and TD is within the above range.

[0059] (Tensile elongation at break) In this film, the tensile elongation at break in at least one direction measured in accordance with JIS K7127 (1999) is preferably 300% or more, more preferably 310% or more, and even more preferably 320% or more. The upper limit of the tensile elongation at break is not particularly limited, but is preferably 2000% or less. The tensile elongation at break is a value measured in accordance with JIS K7127 (1999) using a tensile tester using a test piece having a length of 50 mm in the measurement direction and a width of 10 mm under the conditions of a measurement temperature of 23±2°C, a chuck distance of 20 mm, and a test speed of 200 mm / min.

[0060] More specifically, the MD tensile elongation at break of the film, measured in accordance with JIS K7127 (1999), is preferably 300% or more, more preferably 310% or more, and even more preferably 320% or more. The upper limit of the MD tensile elongation at break is not particularly limited, but is preferably 2000% or less. The TD tensile elongation at break measured in accordance with JIS K7127 (1999) is preferably 300% or more, more preferably 310% or more, and even more preferably 320% or more. The upper limit of the TD tensile elongation at break is not particularly limited, but is preferably 2000% or less. In this embodiment, it is preferable that the tensile elongation at break in either the MD or TD is within the above range, but it is particularly preferable that the tensile elongation at break in both the MD and TD is within the above range.

[0061] (Total light transmittance) In this film, the antibacterial agent has high dispersibility, and the generation of foreign matter (lumps) is suppressed, so that this film has high transparency. Specifically, the total light transmittance of this film measured in accordance with JIS K7361-1 (1997) is preferably 50% or more, more preferably 65% ​​or more, and even more preferably 75% or more. Since the higher the total light transmittance, the more preferable it is, the upper limit is not particularly limited, but it may be, for example, 100% or less, 98% or less, or 95% or less. By setting the total light transmittance within the above range, the visibility of the contents can be improved when used as a packaging film, etc. The total light transmittance was measured using a haze meter conforming to JIS K7361-1 (1997) at five measurement points (n=5), and the arithmetic average value was calculated.

[0062] (Hayes) The haze of the present film measured according to JIS K7136 (2000) is preferably 60% or less, more preferably 55% or less. The lower limit of the haze is not particularly limited, and may be 0%. By keeping the haze within the above range, the visibility of the contents can be improved when the film is used as a packaging film or the like. The haze was measured using a haze meter conforming to JIS K7136 (2000) at five measurement points (n=5), and the arithmetic average value was calculated.

[0063] (Area ratio of foreign matter (lumps)) This film has excellent appearance with little generation of foreign matter (lumps) originating from antibacterial agents, etc. The appearance of a film can be evaluated, for example, by calculating the area ratio of foreign matter (lumps) in the film. The area ratio of foreign matter (lumps) occurring in a film can be measured using a digital microscope. Specifically, the reflected field is observed with a ring light, and the brightness range of the lump is extracted from the brightness histogram of the observed image to determine the area of ​​the lump. The area ratio of the lump is then calculated as a percentage by dividing the area of ​​the lump by the observed area. The smaller the area ratio of foreign matter (lumps) is, the more preferable; it is preferably 1.00% or less, more preferably 0.80% or less, and particularly preferably 0.50% or less.

[0064] (Antibacterial performance) This film exhibits excellent antibacterial properties. For example, the antibacterial properties of the film can be evaluated by the following method. Specifically, in the antibacterial property test described in JIS Z2801 (2012), the bacteria used in the test is changed to baker's yeast (dry yeast) and the antibacterial property test is performed. The test medium is SDA (Sabouraud dextrose agar) medium, and the bacterial liquid is prepared by adding 0.1 g of baker's yeast to 9 ml of PSB (phosphate buffered saline) and stirring well, and then diluting it by 10 to the power of 6 to about 100 CFU / mL. Next, 0.2 mL of the bacterial liquid is dropped onto a film cut into a size of 5 cm x 5 cm, and then a cover film of 4 cm x 4 cm is placed on the film, the bacterial liquid is adhered to the film, and the film is placed in a sterilized petri dish and cultured in a thermo-hygrostat at 35 ± 1 ° C and a relative humidity of 90% for 24 hours. The bacterial solution on the evaluation film is then spread on the SDA medium, spread evenly over the entire medium with a platinum loop, and cultured in a thermo-hygrostat at 35±1°C and 90% relative humidity for 72 hours, after which the viable bacterial count is measured. The viable bacterial count is 9×10 6 Preferably less than 5 × 10 6 More preferably, it is less than 3×10 6 It is even more preferable that it is less than 1000 .mu.m.

[0065] (Thickness) The thickness of the present film is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The thickness of the present film is preferably 500 μm or less, more preferably 400 μm or less, and even more preferably 300 μm or less. By making the thickness of the present film within the above range, the processability and handling properties during film production can be more effectively improved.

[0066] (peel strength) After the film is used as a lid material and heat sealed to a base material (tray), the easy peel strength when the lid material is opened is preferably 1.0 N / mm to 20.0 N / mm when the test piece is 15 mm wide and at 23° C. By setting the easy peel strength to be equal to or higher than the above lower limit, the hermeticity of the package can be maintained. Also, by setting the easy peel strength to be equal to or lower than the above upper limit, the ease of opening can be improved.

[0067] <Application> The present film can be used for various purposes, and is preferably used for packaging food, packaging medicines such as tablets, packaging medical instruments such as syringes and needles, and packaging sanitary materials such as gauze and masks. In particular, the present film is preferably used for packaging food. This embodiment may also relate to a food packaging material. When the present film is used for packaging food, for example, the present film is formed into a bag shape, food is contained therein, and then the film is heat-sealed to obtain a package.

[0068] The present film can also be used as a lid material. In this case, for example, the present film (lid material) can be heat-sealed to a glass or resin container to seal the container and obtain a package. Examples of containers include cups and trays. EXAMPLES

[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. In the following, various measurements and evaluations of the film and its materials were performed as follows. Here, the flow direction of the film from the extruder is called the machine direction (MD), and the direction perpendicular to the machine direction is called the transverse direction or width direction (TD).

[0070] [Evaluation method] (1) Thickness According to JIS K7130 (1999), measurements were taken at 10 random points using a stand-type constant pressure thickness gauge, and the average value was taken as the film thickness.

[0071] (2) Tensile strength and tensile elongation at break The tensile strength and elongation at break in the MD and TD of the film were measured according to a method in accordance with JIS K7127 (1999). The measurement conditions were a pulling speed of 200 mm / min and an atmospheric temperature of 23°C. The measurement device used was a tensile tester (product name: Autograph AG-X, manufactured by Shimadzu Corporation). The test specimen was a rectangle cut from the film with a length of 50 mm in the measurement direction and a width of 10 mm. Both ends of the test specimen in the longitudinal direction were chucked with a chuck distance of 20 mm and pulled at a crosshead speed of 200 mm / min, and the tensile strength and elongation in the MD and TD were measured three times each, and the average values ​​were calculated.

[0072] (3) Area ratio of the bumps The area ratio of foreign matter (lumps) occurring in the film was calculated using a digital microscope. First, the reflected field of view was observed with a ring light, and the brightness range of the foreign matter (lumps) was extracted from the brightness histogram of the observed image to determine the area of ​​the foreign matter (lumps). The area ratio of the foreign matter (lumps) was calculated as a percentage by dividing the area of ​​the foreign matter (lumps) by the observed area.

[0073] (4) Transparency (total light transmittance) The total light transmittance of the film was measured using a haze meter (NDH-7000II, manufactured by Nippon Denshoku Industries Co., Ltd.) according to the light transmittance measuring method described in JIS K7361-1 (1997).

[0074] (5) Transparency (haze) The haze of the film was measured using a haze meter (NDH-7000II, manufactured by Nippon Denshoku Industries Co., Ltd.) according to the haze measurement method described in JIS K7136 (2000).

[0075] (6) Simple antibacterial activity test The antibacterial performance was measured in accordance with the antibacterial test described in JIS Z2801 (2012), except that the bacteria used in the test was changed to baker's yeast. Baker's yeast (dry yeast) was prepared as the test bacteria, and SDA (Sabouraud dextrose agar) medium was prepared as the test medium. The bacteria liquid was prepared by adding 0.1 g of baker's yeast to 9 ml of PSB (phosphate buffered saline) and stirring well, and then diluting it by 10 to the power of 6 to make about 100 CFU / mL. The films obtained in each Example and Comparative Example were cut into a size of 5 cm x 5 cm to be used as evaluation films. After dropping 0.2 mL of the prepared bacterial solution on one surface of each evaluation film, a 4 cm x 4 cm cover film was placed over it, the bacterial solution was attached to the evaluation film, and the film was placed in a sterilized petri dish and cultured in a thermo-hygrostat at 35 ± 1 ° C. and a relative humidity of 90% for 24 hours. Next, the bacterial solution on the evaluation film was spread on the SDA medium, spread evenly over the entire medium with a platinum loop, and cultured in a thermo-hygrostat at 35 ± 1 ° C. and a relative humidity of 90% for 72 hours. After that, the viable bacteria count after culture was measured. The measured viable bacteria count was evaluated for simple antibacterial properties according to the following evaluation criteria. A: Viable bacteria count is 0-5×10 6 less than B: The number of live bacteria is 5 x 10 6 More than 9×10 6 less than C: The number of live bacteria is 9 x 10 6 End

[0076] (7) Particle size The particle size of the organic antibacterial agent (B) was measured using a laser diffraction particle size analyzer (CILAS 1190 manufactured by CILAS Corporation), and the D90, D50, and D10 particle sizes were evaluated according to JIS Z 8825 (2013). The maximum value of the measured particle size distribution was taken as the maximum particle size, and the arithmetic mean was taken as the average particle size.

[0077] (Organic antibacterial agent) In the examples and comparative examples, the following organic antibacterial agents were used. Antibacterial agent B1: Sodium dehydroacetate with a mean particle size of 0.22 μm, a D90 particle size of 0.42 μm, a D50 particle size of 0.17 μm, and a D10 particle size of 0.04 μm Antibacterial agent B2: Sodium dehydroacetate with a mean particle size of 1.6 μm, a D90 particle size of 6.06 μm, a D50 particle size of 0.24 μm, and a D10 particle size of 0.05 μm Antibacterial agent B3: Sodium dehydroacetate with a mean particle size of 68.75 μm, a D90 particle size of 151 μm, a D50 particle size of 52.4 μm, and a D10 particle size of 0.33 μm

[0078] [Example 1] Antibacterial agent B1 was used as an organic antibacterial agent. While stirring 400 g of antibacterial agent B1 with a piccolo mixer heated to 60 ° C, a liquid mixture of 4 g of extremely hardened soybean oil and 30 g of hexane heated to 60 ° C was dropped from above to prepare a coated antibacterial agent coated with extremely hardened soybean oil. Then, a polyethylene resin (linear low density polyethylene, ethylene / 1-butene = 93 / 7 (mass ratio), density 0.924 g / cm3, MFR 2.0 g / 10 minutes, melting point 123 ° C) was dry blended with the above coated antibacterial agent so that the mass ratio was 96 mass % and 4 mass %, and melt kneaded at a temperature of 200 ° C for 5 minutes using a tabletop melt kneader. Then, the melt-kneaded resin composition was put into a tabletop film forming machine to obtain a film with a thickness of 30 μm. The evaluation results of the obtained film are shown in Table 1.

[0079] [Example 2] Polyethylene resin (linear low density polyethylene, ethylene / 1-butene=93 / 7 (mass ratio), density 0.924g / cm3, MFR 2.0g / 10 min, melting point 123°C) as polyolefin resin, antibacterial agent B1 as organic antibacterial agent, and hardened soybean oil as fat were dry blended to have mass ratios of 95 mass%, 4 mass%, and 1 mass%, respectively, and melt-kneaded at a temperature of 200°C for 5 minutes using a tabletop melt kneader. The melt-kneaded resin composition was then put into a tabletop film-forming machine to obtain a film with a thickness of 40 μm. The evaluation results of the obtained film are shown in Table 1.

[0080] [Example 3] A film having a thickness of 30 μm was produced in the same manner as in Example 2, except that the mass ratios of the polyolefin resin, the organic antibacterial agent (antibacterial agent B1), and the oil and fat were changed to 93.5 mass%, 4 mass%, and 2.5 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.

[0081] [Example 4] A film having a thickness of 40 μm was produced in the same manner as in Example 2, except that the mass ratios of the polyolefin resin, the organic antibacterial agent (antibacterial agent B2), and the oil and fat were changed to 93.5 mass%, 4 mass%, and 2.5 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.

[0082] [Comparative Example 1] A film having a thickness of 30 μm was produced in the same manner as in Example 2, except that no oil or fat was used and the mass ratio of the polyethylene resin to the organic antibacterial agent (antibacterial agent B1) was changed to 96 mass% and 4 mass%, respectively, to obtain a film. The evaluation results of the obtained film are shown in Table 1.

[0083] [Comparative Example 2] A film having a thickness of 40 μm was produced in the same manner as in Example 2, except that antibacterial agent B2 was used as the organic antibacterial agent and the mass ratio of the polyethylene resin to the organic antibacterial agent was changed to 96 mass% and 4 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.

[0084] [Comparative Example 3] A film having a thickness of 40 μm was produced in the same manner as in Example 2, except that antibacterial agent B3 was used as the organic antibacterial agent and the mass ratio of the polyethylene resin to the organic antibacterial agent was changed to 96 mass% and 4 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.

[0085] [Comparative Example 4] A film having a thickness of 40 μm was produced in the same manner as in Comparative Example 3, except that the mass ratio of the polyethylene resin to the organic antibacterial agent (antibacterial agent B3) was changed to 98 mass% and 2 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.

[0086] [Comparative Example 5] An oil-coated organic antibacterial agent and a film were prepared in the same manner as in Example 1, except that antibacterial agent B3 was used as the organic antibacterial agent, and a film having a thickness of 40 μm was obtained.

[0087] [Comparative Example 6] A film having a thickness of 40 μm was produced in the same manner as in Example 2, except that antibacterial agent B3 was used as the organic antibacterial agent.

[0088] [Comparative Example 7] A film having a thickness of 40 μm was produced in the same manner as in Comparative Example 4, except that antibacterial agent B1 was used as the organic antibacterial agent.

[0089] [Table 1]

[0090] In the examples, the generation of foreign matter (lumps) was suppressed, and a film with excellent appearance was obtained. In addition, in the examples, a film with excellent antibacterial properties was obtained. Furthermore, in the examples, the tensile elongation at break of the film was large. On the other hand, in the comparative example, inhibition of the generation of foreign matter (lumps) and antibacterial properties were not achieved at the same time. [Industrial Applicability]

[0091] The thermoplastic resin film of the present invention has antibacterial properties, good appearance and high tensile elongation at break, and therefore can be suitably used for applications such as food packaging films, storage containers, building materials, miscellaneous goods and home appliances.

Claims

1. A film comprising a thermoplastic resin (A), an organic antibacterial agent (B) and an oil (C), The organic antibacterial agent (B) contained in the film has an average particle size of 20 μm or less.

2. The film according to claim 1, wherein the thermoplastic resin (A) has a melting point of 180°C or lower or a glass transition temperature of 180°C or lower.

3. The film according to claim 1 , wherein the thermoplastic resin (A) is a polyolefin resin.

4. 4. The film according to claim 3, wherein the polyolefin resin is at least one selected from the group consisting of polyethylene, polypropylene, and ethylene-vinyl acetate copolymer.

5. The film according to any one of claims 1 to 4, wherein the organic antibacterial agent (B) is an organic acid salt.

6. 6. The film according to claim 5, wherein the organic acid salt is at least one selected from the group consisting of sorbates, dehydroacetates, propionates, acetates, and benzoates.

7. The film according to any one of claims 1 to 4, wherein the content of the organic antibacterial agent (B) is 0.1 to 30 mass% based on the total mass of the film.

8. The film according to any one of claims 1 to 4, wherein the oil (C) is a hardened oil.

9. The film according to any one of claims 1 to 4, wherein the oil (C) is a highly hydrogenated oil.

10. The film according to any one of claims 1 to 4, wherein the content of the oil (C) is 0.01 to 10 mass% based on the total mass of the film.

11. The film according to any one of claims 1 to 4, which has a tensile elongation at break in at least one direction of 300% or more, as measured in accordance with JIS K7127 (1999).

12. The film according to any one of claims 1 to 4, which is for food packaging.

13. A food packaging material comprising the film according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Tectosilicate-based antimicrobial agent

    JP1991120204A

  • Antimicrobial sheet material

    JP1996283500A

  • Starch-based composite resin composition and its molded product

    JP2004002613A

  • Antibacterial film and package

    JP2015189138A

  • Antibacterial film

    JP2023004163A

Cited By