Molded body for thermal processing
A poly(3-hydroxyalkanoate) resin composition with specific monomer ratios and molecular weights addresses mold releasability and surface smoothness issues, enhancing thermoformability and productivity.
Patent Information
- Application Number
- JP2023046449
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing poly(3-hydroxyalkanoate) resin sheets for thermoforming face issues with mold releasability and surface smoothness, leading to reduced productivity due to sticking, holes, or wrinkles during thermoforming.
A molded article containing a poly(3-hydroxyalkanoate) resin component composed of specific ratios and molecular weights of 3-hydroxybutyrate copolymers, including copolymers (A) and (C) with 4-7 mol% and 24 mol% other hydroxyalkanoate units, respectively, and a weight average molecular weight of 450,000 or more, ensuring smoothness and processability.
The solution provides a molded article with a smooth surface and improved thermoformability, allowing for efficient mold release without wrinkles or holes, thereby enhancing productivity.
Smart Images

Figure 2024135656000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a molded article for thermal processing that contains a poly(3-hydroxyalkanoate)-based resin component. [Background technology]
[0002] Large amounts of petroleum-derived plastics are discarded every year, and environmental pollution caused by these large amounts of waste has been raised as a serious issue. In recent years, microplastics have also become a major problem in the marine environment.
[0003] Poly(3-hydroxyalkanoate) resins have excellent seawater degradability and are materials that can solve the environmental problems caused by discarded plastics. For example, the mechanical properties of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), a type of poly(3-hydroxyalkanoate) resin, can be flexibly controlled by changing the composition ratio of 3-hydroxyhexanoate.
[0004] On the other hand, a method is known in which a resin sheet is subjected to a secondary thermoforming process such as vacuum forming or press forming to mold the sheet into a container having a central recess, such as tableware.
[0005] Patent Document 1 discloses a resin sheet for thermoforming, which contains a poly(3-hydroxyalkanoate) resin, and discloses that by setting the heat shrinkage rate of the resin sheet to a specific value or more, the resin sheet can be thermoformed into a molded product having a relatively uniform thickness. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2022-10543 Summary of the Invention [Problem to be solved by the invention]
[0007] The resin sheet for heat processing described in Patent Document 1 can be heat molded into a molded product having a relatively uniform thickness, but the releasability after heat molding may be insufficient. In particular, if the cooling time in the mold is set to be short, the solidification of the resin does not proceed sufficiently, and part of the resin sticks to the mold, making it impossible to release the molded product, or even if it can be released, the molded product may have holes or wrinkles. Therefore, it is difficult to increase the productivity of heat molding.
[0008] On the other hand, when trying to improve the release properties after thermoforming by adjusting the composition of the resin sheet, melt fracture can occur during the production of the resin sheet for thermal processing (e.g., calendar molding), resulting in unevenness on the sheet surface, making it difficult to obtain a sheet with a smooth surface.
[0009] In view of the above-mentioned current situation, the present invention aims to provide a molded body for heat processing that contains a poly(3-hydroxyalkanoate)-based resin component and that has both good surface smoothness and good processability during heat molding. [Means for solving the problem]
[0010] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have discovered that by forming a poly(3-hydroxyalkanoate) resin component from at least two types of 3-hydroxybutyrate copolymers having specific monomer ratios, and by setting the content ratio and weight average molecular weight of the copolymer, as well as the weight average molecular weight of the entire resin component, within specific ranges, it is possible to provide a molded body for thermal processing which has a good smoothness of the molded body surface and also has good processability during thermal molding, and have thus completed the present invention.
[0011] That is, the present invention provides a molded article for thermal processing containing a poly(3-hydroxyalkanoate)-based resin component, The poly(3-hydroxyalkanoate) resin component comprises a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 4 mol% or more and less than 7 mol%, and a copolymer (C) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 24 mol% or more, the proportion of the copolymer (A) in the entire poly(3-hydroxyalkanoate)-based resin component is 20% by weight or more and 95% by weight or less; The weight average molecular weight (Mw) of each of the copolymer (A) and the copolymer (C) is 450,000 or more; The present invention relates to a molded article for thermal processing, wherein the weight average molecular weight (Mw) of the entire poly(3-hydroxyalkanoate) resin component is 450,000 or more. The present invention also relates to a molded product obtained by imparting a predetermined shape to the molded article for thermal processing by thermal molding. Effect of the Invention
[0012] According to the present invention, it is possible to provide a molded body for heat processing that contains a poly(3-hydroxyalkanoate)-based resin component, and that has both good surface smoothness and good processability during heat molding. The molded product for thermal processing according to the present invention has a sheet surface with few irregularities and can have a smooth surface.
[0013] In addition, the molded body for heat processing according to the present invention can be processed into a molded product having a predetermined shape by heat molding (for example, molding by vacuum molding or press molding). When the molded body for heat processing according to the present invention is used for heat molding, it can be released from the mold without generating holes or wrinkles even if the cooling time in the mold is short, so that the productivity of the heat molding can be increased. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment. The present embodiment relates to a molded article for thermal processing that contains a poly(3-hydroxyalkanoate)-based resin component.
[0015] (Poly(3-hydroxyalkanoate) resin component) The poly(3-hydroxyalkanoate) resin component contains at least two types of poly(3-hydroxyalkanoate) resins having different content ratios of constituent monomers. Each poly(3-hydroxyalkanoate) resin is a copolymer of 3-hydroxybutyrate (hereinafter sometimes referred to as 3HB) units and other hydroxyalkanoate units.
[0016] The other hydroxyalkanoate units may be 3-hydroxyalkanoate units other than 3HB units, or may be hydroxyalkanoate units other than 3-hydroxyalkanoate units (e.g., 4-hydroxyalkanoate units).The other hydroxyalkanoate units may include only one type, or may include two or more types.
[0017] As the poly(3-hydroxyalkanoate)-based resin, a poly(3-hydroxyalkanoate)-based resin produced from a microorganism is particularly preferred. In the poly(3-hydroxyalkanoate)-based resin produced from a microorganism, all of the 3-hydroxyalkanoate units are contained as (R)-3-hydroxyalkanoate units.
[0018] Specific examples of poly(3-hydroxyalkanoate) resins include poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (abbreviation: P3HB3HV), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviation: P3HB3HH), poly(3-hydroxy Examples of such poly(3-hydroxybutyrate-co-3-hydroxyheptanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxynonanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyundecanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (abbreviation: P3HB4HB), etc. In particular, from the viewpoint of productivity and mechanical properties of the thermal processing molded body, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate) is preferred, and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is particularly preferred.
[0019] The poly(3-hydroxyalkanoate)-based resin component contains at least the following copolymer (A) and the following copolymer (C). In addition to these two copolymers, it is preferable that the following copolymer (D) is further contained. Copolymer (A): A copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 4 mol% or more and less than 7 mol%. Copolymer (C): A copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 24 mol% or more. Copolymer (D): A copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 1 mol % or more and less than 4 mol %.
[0020] Copolymer (A) is a highly crystalline poly(3-hydroxyalkanoate) resin, whereas copolymer (C) is a poly(3-hydroxyalkanoate) resin having lower crystallinity than copolymer (A).
[0021] In general, highly crystalline poly(3-hydroxyalkanoate) resins have excellent productivity but poor mechanical properties, while low-crystalline poly(3-hydroxyalkanoate) resins have poor productivity but excellent mechanical properties. By using the above-mentioned resins in combination, it is possible to provide a molded product for thermal processing that has both good surface smoothness and good processability during thermal molding.
[0022] The content of other hydroxyalkanoate units in the copolymer (A) is 4 mol% or more and less than 7 mol%. The lower limit of the content may be 4.5 mol% or more, or 5 mol% or more. The upper limit may be 6.5 mol% or less, or 6 mol% or less.
[0023] The copolymer (A) is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0024] The content of other hydroxyalkanoate units in the copolymer (C) is 24 mol% or more. The lower limit of the ratio may be 25 mol% or more, or 26 mol% or more. From the viewpoint of productivity, the upper limit of the ratio is preferably 99 mol% or less, more preferably 50 mol% or less, even more preferably 40 mol% or less, and particularly preferably 30 mol% or less.
[0025] The copolymer (C) is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0026] The content of other hydroxyalkanoate units in the copolymer (D) is 1 mol% or more and less than 4 mol%. The lower limit of the content is preferably 2 mol% or more. By using the copolymer (D) in combination, the productivity of the molded article for thermal processing can be improved.
[0027] The copolymer (D) is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0028] The proportion of the copolymer (A) in the entire poly(3-hydroxyalkanoate)-based resin components contained in the molded article for heat processing according to this embodiment is 20% by weight or more and 95% by weight or less. Within this range, both the smoothness of the molded article surface and the processability during heat molding can be improved. If the proportion of copolymer (A) is less than 20% by weight, it takes a long time for the resin to solidify in the mold after heat molding, and it is not possible to release the resin from the mold by cooling for a short time, or even if it is possible to release the resin from the mold, holes or wrinkles are likely to occur. If the proportion of copolymer (A) is more than 95% by weight, the phenomenon of melt fracture is likely to occur during the production of a molded product for heat processing, and the molded product surface becomes uneven, making it difficult to obtain a molded product with a smooth surface. The lower limit of the proportion of the copolymer (A) is preferably 30% by weight or more, more preferably 40% by weight or more, and may be 50% by weight or more, or may be 60% by weight or more. The upper limit of the proportion is preferably 90% by weight or less, and may be 80% by weight or less.
[0029] The proportion of copolymer (C) in the entire poly(3-hydroxyalkanoate)-based resin component is preferably 5% by weight or more and 50% by weight or less. When the proportion of copolymer (C) is 5% by weight or more, it becomes easier to produce a molded product for thermal processing having a smooth surface. When the proportion of copolymer (C) is 50% by weight or less, it becomes easier to release the molded product from the mold without generating holes or wrinkles even if the cooling time in the mold after thermoforming is short. The lower limit of the proportion of the copolymer (C) may be 8% by weight or more, or 10% by weight or more. The upper limit is preferably 45% by weight or less. It may be 40% by weight or less, or 30% by weight or less.
[0030] When copolymer (D) is blended, the proportion of copolymer (D) in the entire poly(3-hydroxyalkanoate)-based resin component is preferably 3% by weight or more and 35% by weight or less. When the proportion of copolymer (D) is 3% by weight or more, it becomes easier to produce a molded product for thermal processing having a smooth surface. Also, when the proportion of copolymer (D) is 35% by weight or less, it becomes easier to release the molded product from the mold without generating holes or wrinkles even if the cooling time in the mold after thermoforming is short. The lower limit of the proportion of the copolymer (D) may be 5% by weight or more, or 8% by weight or more. The upper limit is preferably 30% by weight or less. It may be 25% by weight or less, or 20% by weight or less.
[0031] The poly(3-hydroxyalkanoate)-based resin component may be composed only of copolymer (A) and copolymer (C), or may be composed only of copolymer (A), copolymer (C), and copolymer (D). It may further contain other poly(3-hydroxyalkanoate)-based resins that do not fall into any of copolymer (A), copolymer (C), and copolymer (D). The proportion of such other resins in the poly(3-hydroxyalkanoate)-based resin component is preferably 10% by weight or less, more preferably 5% by weight or less.
[0032] The average content ratio of 3-hydroxybutyrate units and other hydroxyalkanoate units in all monomer units constituting the poly(3-hydroxyalkanoate) resin component contained in the heat-processable molded body is preferably 3-hydroxybutyrate units / other hydroxyalkanoates=96 / 4 to 90 / 10 (mol % / mol %), more preferably 95 / 5 to 91 / 9 (mol % / mol %), and even more preferably 94 / 6 to 92 / 8 (mol % / mol %), from the viewpoint of achieving both smoothness of the surface of the heat-processable molded body and processability during heat molding.
[0033] The average content ratio of each monomer unit in all monomer units constituting the poly(3-hydroxyalkanoate)-based resin component can be determined by a method known to those skilled in the art, for example, the method described in paragraph
[0047] of WO 2013 / 147139. The average content ratio means the molar ratio of each monomer unit in all monomer units constituting the poly(3-hydroxyalkanoate)-based resin component, and when the poly(3-hydroxyalkanoate)-based resin component is a mixture of two types of poly(3-hydroxyalkanoate)-based resins, it means the molar ratio of each monomer unit contained in the entire mixture.
[0034] In this embodiment, the weight average molecular weight (Mw) of the copolymer (A) and the weight average molecular weight (Mw) of the copolymer (C) are each set to 450,000 or more. By setting the weight average molecular weight of each copolymer to a specific value or more in this way, even if the cooling time in the mold after thermoforming is short, the molded product can be released from the mold without generating holes or wrinkles. However, if the weight average molecular weight of the copolymer (A) or the copolymer (C) is less than 450,000, the resin component has a low viscosity, so that drawdown becomes large during thermoforming and wrinkles are likely to occur. The upper limits of the weight average molecular weight of the copolymer (A) and the weight average molecular weight of the copolymer (C) can be set in consideration of the melt viscosity described later, but from the viewpoint of the smoothness of the surface of the molded product for thermal processing, it is preferably 1.2 million or less, more preferably 1 million or less, and even more preferably 900,000 or less. The lower limit is preferably 500,000 or more, and more preferably 550,000 or more.
[0035] In addition, when the copolymer (D) is used, the weight average molecular weight (Mw) of the copolymer (D) is preferably set to 450,000 or more, similar to the weight average molecular weights (Mw) of the copolymer (A) and the copolymer (C). The preferred range of the weight average molecular weight (Mw) of the copolymer (D) is the same as above.
[0036] In addition, the weight average molecular weight (Mw) of the entire poly(3-hydroxyalkanoate) resin component is set to 450,000 or more. By setting the weight average molecular weight of the entire resin component to a specific value or more in this way, the molded product can be released from the mold without generating holes or wrinkles, even if the cooling time in the mold after thermoforming is short. The upper limit of the weight average molecular weight of the entire poly(3-hydroxyalkanoate) resin component can be set in consideration of the melt viscosity described later, but from the viewpoint of the smoothness of the surface of the molded article for thermal processing, it is preferably 1.2 million or less, more preferably 1 million or less, and even more preferably 900,000 or less. The lower limit is preferably 500,000 or more, and more preferably 550,000 or more.
[0037] The weight average molecular weight of the poly(3-hydroxyalkanoate) resin component, copolymer (A), copolymer (C), or copolymer (D) can be measured in terms of polystyrene using gel permeation chromatography (HPLC GPC system manufactured by Shimadzu Corporation) using a chloroform solution. As the column for the gel permeation chromatography, a column suitable for measuring the weight average molecular weight may be used.
[0038] The method for producing the poly(3-hydroxyalkanoate) resin is not particularly limited, and may be a production method by chemical synthesis or a production method using a microorganism. Among them, a production method using a microorganism is preferable. A known method can be applied to the production method using a microorganism. For example, Aeromonas caviae, which produces P3HB3HV and P3HB3HH, and Alcaligenes eutrophus, which produces P3HB4HB, are known as bacteria that produce copolymers of 3-hydroxybutyrate and other hydroxyalkanoates. In particular, with regard to P3HB3HH, in order to increase the productivity of P3HB3HH, it is more preferable to use Alcaligenes eutrophus AC32 (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, pp. 4821-4830 (1997)) or the like, into which genes of P3HA synthase group have been introduced, and microbial cells in which P3HB3HH has been accumulated in the cells by culturing these microorganisms under appropriate conditions are used. In addition to the above, genetically modified microorganisms into which various poly(3-hydroxyalkanoate) resin synthesis-related genes have been introduced may be used according to the poly(3-hydroxyalkanoate) resin to be produced, or the culture conditions, including the type of substrate, may be optimized.
[0039] The molded body for thermal processing according to this embodiment does not need to contain an inorganic filler, but it is preferable that it contains an inorganic filler, since this can improve the strength of the molded body and the processability during thermal molding.
[0040] The inorganic filler is not particularly limited as long as it is an inorganic filler that can be added to the resin material for molding, and examples thereof include quartz, fumed silica, silicic anhydride, fused silica, crystalline silica, amorphous silica, inorganic fillers obtained by condensing alkoxysilanes, silica-based inorganic fillers such as ultrafine amorphous silica, alumina, zircon, iron oxide, zinc oxide, titanium oxide, silicon nitride, boron nitride, aluminum nitride, silicon carbide, glass, silicone rubber, silicone resin, titanium oxide, carbon fiber, mica, graphite, carbon black, ferrite, graphite, diatomaceous earth, clay, clay, talc, calcium carbonate, manganese carbonate, magnesium carbonate, barium sulfate, silver powder, etc. These may be used alone or in combination of two or more.
[0041] In this embodiment, among inorganic fillers, inorganic fillers belonging to silicates are preferred because they can improve the strength of the molded body and the processability during thermal molding. Furthermore, among silicates, one or more selected from the group consisting of talc, mica, kaolinite, montmorillonite, and smectite are preferred because they have a large effect of improving the strength of the molded body for thermal processing, have a small particle size distribution, and are less likely to impair the surface smoothness of the molded body. Two or more silicates may be used in combination, and in this case, the type and use ratio of the silicate can be appropriately adjusted.
[0042] Examples of the talc include general-purpose talc and surface-treated talc. Specific examples include "Microace" (registered trademark) from Nippon Talc Co., Ltd., "Talcan Powder" (registered trademark) from Hayashi Kasei Co., Ltd., and talc manufactured by Takehara Chemical Industry Co., Ltd. and Maruo Calcium Co., Ltd.
[0043] Examples of the mica include wet-ground mica and dry-ground mica, and specific examples include mica manufactured by Yamaguchi Mica Co., Ltd. and Keiwa Rozai Co., Ltd.
[0044] Examples of the kaolinite include dry kaolin, calcined kaolin, wet kaolin, etc., and specific examples include "TRANSLINK" (registered trademark), "ASP" (registered trademark), "SANTINTONE" (registered trademark), and "ULTREX" (registered trademark) manufactured by Hayashi Kasei Corporation, and kaolinite manufactured by Keiwa Rozai Co., Ltd.
[0045] When an inorganic filler is blended, the blending amount is preferably more than 0 parts by weight and not more than 30 parts by weight per 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate)-based resin component. When the blending amount of the inorganic filler is within the above range, a molded product for thermal processing having excellent strength and processability can be obtained. The upper limit may be not more than 20 parts by weight, not more than 10 parts by weight, or not more than 8 parts by weight. The lower limit is preferably not less than 1 part by weight, and more preferably not less than 3 parts by weight, since the effect of blending the inorganic filler can be more strongly realized.
[0046] The molded article for heat processing according to the present embodiment may not contain a plasticizer, but may contain a plasticizer. By blending a plasticizer, the crack resistance of the molded article for heat processing can be improved.
[0047] The plasticizer is not particularly limited, but from the viewpoint of compatibility with the poly(3-hydroxyalkanoate)-based resin component, it is preferable to use an ester compound having an ester bond in the molecule.
[0048] Examples of ester compounds that can be used as plasticizers include modified glycerin compounds, dibasic acid ester compounds, adipate compounds, polyether ester compounds, benzoate compounds, citrate compounds, isosorbide ester compounds, and polycaprolactone compounds. Among them, modified glycerin compounds, dibasic acid ester compounds, adipate compounds, polyether ester compounds, and isosorbide ester compounds are preferred, and modified glycerin compounds are particularly preferred. In addition, the ester compounds can be used alone or in combination of two or more. When using two or more in combination, the mixing ratio of the ester compounds can be appropriately adjusted.
[0049] As the modified glycerin compound, a glycerin ester compound is preferred. As the glycerin ester compound, any of glycerin monoester, diester, and triester can be used, but from the viewpoint of compatibility with poly(3-hydroxyalkanoate) resin components, a glycerin triester is preferred. Among the glycerin triesters, glycerin diacetomonoester is particularly preferred. Specific examples of glycerin diacetomonoester include glycerin diacetomonolaurate, glycerin diacetomonooleate, glycerin diacetomonostearate, glycerin diacetomonocaprylate, and glycerin diacetomonodecanoate, and mixtures of two or more of these can be used. For example, the modified glycerin compound includes Riken Vitamin Co., Ltd.'s "Rikemal" PL series and "BIOCIZER".
[0050] Specific examples of dibasic acid ester compounds include dibutyl adipate, diisobutyl adipate, bis(2-ethylhexyl) adipate, diisononyl adipate, diisodecyl adipate, bis[2-(2-butoxyethoxy)ethyl]adipate, bis[2-(2-butoxyethoxy)ethyl]adipate, bis(2-ethylhexyl)azelate, dibutyl sebacate, bis(2-ethylhexyl)sebacate, diethyl succinate, and mixed-group dibasic acid ester compounds.
[0051] Examples of the adipate compounds include diethylhexyl adipate, dioctyl adipate, and diisononyl adipate.
[0052] Examples of the polyether ester compounds include polyethylene glycol dibenzoate, polyethylene glycol dicaprylate, and polyethylene glycol diisostearate.
[0053] As the ester compound, a modified glycerin compound is preferred from the viewpoints of cost, versatility, and high biomass degree. In particular, from the viewpoint of food contact, a glycerin triester is more preferred, a glycerin diacetomonoester is further preferred, and glycerin diacetomonolaurate is particularly preferred.
[0054] When a plasticizer is blended, the blending amount of the plasticizer is preferably more than 0 part by weight and less than 20 parts by weight relative to 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate)-based resin component. The upper limit may be less than 10 parts by weight, less than 5 parts by weight, or less than 2 parts by weight.
[0055] (Other resins) The molded article for heat processing according to the present embodiment may contain other resins than the poly(3-hydroxyalkanoate) resin, as long as the effect of the invention is not impaired. Examples of such other resins include aliphatic polyester resins such as polybutylene succinate adipate, polybutylene succinate, polycaprolactone, and polylactic acid, and aliphatic aromatic polyester resins such as polybutylene adipate terephthalate, polybutylene sebacate terephthalate, and polybutylene azelate terephthalate. Only one type of other resin may be contained, or two or more types may be contained.
[0056] The content of the other resin is not particularly limited, but is preferably 30 parts by weight or less, more preferably 20 parts by weight or less, and even more preferably 10 parts by weight or less, based on 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate)-based resin component. It may be 5 parts by weight or less, or 1 part by weight or less. The lower limit of the content of the other resin is not particularly limited, and may be 0 parts by weight.
[0057] (Additives) The molded article for thermal processing according to this embodiment may contain other additives as long as they do not impair the effects of the invention. Examples of other additives that can be used depending on the purpose include crystallization nucleating agents, lubricants, antistatic agents, flame retardants, conductive agents, heat insulating agents, crosslinking agents, antioxidants, ultraviolet absorbers, colorants, organic fillers, and hydrolysis inhibitors. In particular, additives having biodegradability are preferred.
[0058] Examples of the crystallization nucleating agent include pentaerythritol, orotic acid, aspartame, cyanuric acid, glycine, zinc phenylphosphonate, and boron nitride. Among them, pentaerythritol is preferred because it is particularly effective in promoting the crystallization of the poly(3-hydroxyalkanoate) resin component. The amount of the crystallization nucleating agent used is not particularly limited, but is preferably 0.1 to 5 parts by weight, more preferably 0.3 to 3 parts by weight, and even more preferably 0.5 to 1.5 parts by weight, relative to 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate) resin component. In addition, one type of crystallization nucleating agent may be used, or two or more types may be used, and the usage ratio can be appropriately adjusted depending on the purpose.
[0059] Examples of the lubricant include behenamide, oleamide, erucamide, stearamide, palmitamide, N-stearylbehenamide, N-stearylerucamide, ethylenebisstearamide, ethylenebisoleamide, ethylenebiserucamide, ethylenebislauricamide, ethylenebiscapricamide, p-phenylenebisstearamide, and polycondensates of ethylenediamine, stearic acid, and sebacic acid. Among them, behenamide and erucamide are preferred because of their particularly excellent lubricant effect on poly(3-hydroxyalkanoate)-based resin components. The amount of the lubricant used is not particularly limited, but is preferably 0.01 to 5 parts by weight, more preferably 0.01 to 3 parts by weight, and even more preferably 0.01 to 1.5 parts by weight, relative to 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate)-based resin components. Furthermore, one type of lubricant may be used, or two or more types may be used, and the ratio of use can be appropriately adjusted depending on the purpose.
[0060] The molded product for heat processing according to this embodiment preferably has a melt viscosity of 5000 poise or more and 8100 poise or less, measured under conditions of a heating temperature of 150°C and a shear rate of 1216 / sec. If the melt viscosity is 5000 poise or more, it becomes easier to release the molded product from the mold without generating holes or wrinkles, even if the cooling time in the mold after heat molding is short. Also, if the melt viscosity is 8100 poise or less, it becomes easier to produce a molded product for heat processing having a smooth surface. The lower limit of the melt viscosity is preferably 5,500 poise or more, and the upper limit may be 8,000 poise or less.
[0061] The molded article for heat processing according to the present embodiment preferably has a melt flow rate (MFR) of 0.1 g / 10 min or more and 6.0 g / 10 min or less. The melt flow rate is a value measured at 165° C. and a load of 5.0 kgf according to JIS K 7210 for the molded article for heat processing cut into a size of 3 mm×3 mm. When the melt flow rate is 0.1 g / 10 min or more, it becomes easier to produce a molded product for thermal processing having a smooth surface. Also, when the melt flow rate is 6.0 g / 10 min or less, it becomes easier to release the molded product from the mold without generating holes or wrinkles, even if the cooling time in the mold after the thermoforming process is short. The lower limit of the melt flow rate is preferably 0.3 g / 10 min or more, and more preferably 0.5 g / 10 min or more.
[0062] The heat-processable molded body according to the present embodiment preferably has a drawdown time of 20 sec or more and 65 sec or less. The drawdown time refers to the time required for the center of the heat-processable molded body to sag 7 cm in the vertical direction when the heat-processable molded body cut to a size of 35 cm x 35 cm is fixed horizontally on a frame having an opening in a square shape of 28 cm x 28 cm and heated at a temperature of 350°C. If the drawdown time is within this range, the smoothness of the molded body surface and the processability during heat molding can be improved. The lower limit of the drawdown time is more preferably 25 seconds or more, and even more preferably 30 seconds or more, and the upper limit is even more preferably 60 seconds or less.
[0063] The molded article for heat processing according to this embodiment preferably has a drawdown ratio defined as drawdown time [sec] / melt flow rate [g / 10 min] / thickness of the molded article for heat processing [mm] of 0.1 [sec / (g / 10 min) / mm] or more and 300 [sec / (g / 10 min) / mm] or less. The drawdown time and melt flow rate used in the calculation of the drawdown ratio are as described above. When the drawdown ratio is 0.1 [sec / (g / 10 min) / mm] or more, it becomes easier to release the molded product from the mold without generating holes or wrinkles even if the cooling time in the mold after the thermoforming process is short. Also, when the drawdown ratio is 300 [sec / (g / 10 min) / mm] or less, it becomes easier to produce a thermoformable molded product having a smooth surface. The lower limit of the drawdown ratio is more preferably 10 [sec / (g / 10min) / mm] or more, and even more preferably 30 [sec / (g / 10min) / mm] or more. The upper limit is more preferably 270 [sec / (g / 10min) / mm] or less, and even more preferably 250 [sec / (g / 10min) / mm] or less. It may also be 200 [sec / (g / 10min) / mm] or less, or 100 [sec / (g / 10min) / mm] or less.
[0064] The thickness of the molded article for heat processing according to this embodiment is not particularly limited, but is preferably 0.01 mm or more and 1.0 mm or less before the heat molding process is performed. The lower limit may be 0.1 mm or more, or 0.2 mm or more. The upper limit may be 0.8 mm or less, or 0.7 mm or less.
[0065] The shape of the molded article for heat processing according to this embodiment is not particularly limited, but it is preferably a sheet before being subjected to heat molding.
[0066] (Method of manufacturing a molded body for thermal processing) The method for obtaining a blend of the copolymer (A), the copolymer (C) and the optional copolymer (D) is not particularly limited, and may be a method for obtaining a blend by microbial production or a method for obtaining a blend by chemical synthesis. In addition, the blend may be obtained by melt-kneading two or more resins using an extruder, kneader, Banbury mixer, roll, etc., or by dissolving two or more resins in a solvent, mixing and drying the mixture. In addition, the above-mentioned methods may be combined in combination.
[0067] The heat-processable molded article according to the present embodiment can be produced as a calendar molded article by melt-kneading the resin components and various additives as necessary, and then rolling and sheet-molding with a calendar roll. It may also be produced by an extrusion molding method in which a molten resin raw material is extruded from a T-die. It may also be produced by an inflation molding method in which a molten resin is extruded in a tubular shape from an extruder equipped with a cylindrical die at the tip, and immediately after that, gas is blown into the tube to inflate it into a balloon shape to form a film. The rolling sheet forming using the calender rolls will be described in detail below.
[0068] The rolled sheet molding using a calendar roll is a production method in which a resin composition that has been melt-kneaded and extruded in an extruder equipped with a Banbury mixer or a planetary mixer is further melt-kneaded with two or more rolls, the molten and kneaded resin composition is rolled with a calendar roll, and then formed into a sheet by cooling on one or more cooling rolls, passing between two or more cooling rolls, pressing, or other means.
[0069] The temperature of the extruder is preferably 140 to 180° C. The temperature when melt kneading with two or more rolls is preferably 90 to 150° C. The temperature when rolling with a calendar roll is preferably 90 to 150° C. The temperature for cooling the resin composition is preferably 10 to 100° C.
[0070] The take-off speed in the calender sheet molding is determined by the film thickness and width of the molded product and the amount of resin discharged, but can be adjusted within a range that maintains the stability of the calender sheet molding. In general, a take-off speed of 1 to 50 m / min is preferred.
[0071] After the calender sheet molding, a step of stretching the sheet in the MD and / or TD may be carried out. The stretching step can be carried out by pulling the sheet in the MD by making a difference in the rotation speed between the rolls and / or by clamping the width direction end of the sheet and pulling it in the TD. By carrying out the stretching step, a molded product having a relatively uniform thickness can be obtained by the subsequent thermoforming process.
[0072] The stretching ratio in the stretching step is preferably 1.1 times or more, more preferably 1.2 times or more, even more preferably 1.3 times or more, and particularly preferably 1.4 times or more. The upper limit of the stretching ratio is not particularly limited, but is preferably 3.0 times or less, more preferably 2.5 times or less, and even more preferably 2.0 times or less.
[0073] After the calender sheet molding, before winding, a step of coating the surface of the molded body for heat processing with a coating material according to desired characteristics may be performed. The coating material is not particularly limited, but may be a release agent, an anti-fogging agent, or an antistatic agent. The coating method is not particularly limited, but may be a gravure reverse method, a double-sided coating method, or a single-sided coating printing method.
[0074] (Thermoforming processing) The heat-processable molded article according to the present embodiment can be used for secondary processing into a molded article having a concave portion and / or a convex portion, such as a container, by heat molding. The heat molding process can be performed by pressing the heat-processable molded article softened by preheating, or by aligning it with a mold using vacuum or compressed air. Specific examples of the heat molding process include press molding, vacuum molding, compressed air molding, vacuum-pressure molding, matched mold molding, plug-assist molding, plug-assist vacuum molding, plug-assist vacuum-pressure molding, and TOM molding. Of these, press molding, vacuum molding, vacuum-pressure molding, plug-assist vacuum molding, and plug-assist vacuum-pressure molding are preferred because they are simple and require low mold costs.
[0075] The preheating before the thermal molding process is a step of fixing the ends of the molded article for thermal processing with clamps or pins and heating the molded article for thermal processing using a far-infrared heater, etc. The temperature of the molded article achieved by the preheating can be appropriately set by those skilled in the art, but it is preferably a temperature between the melting peak temperature and the end temperature on the higher side of the melting peak in differential scanning calorimetry of the poly(3-hydroxybutyrate)-based resin component.
[0076] The device used to preheat the molded body for heat processing to the above temperature is not particularly limited, and examples thereof include a far-infrared heater, a hot-wire heater, and a hot air heater. However, a far-infrared heater is preferred because it is easy to heat the molded body quickly and uniformly. When using a far-infrared heater, the temperature of the heater is generally set higher than the target molded body temperature, and the temperature of the molded body can be controlled by the distance between the heater and the molded body and the preheating time. For example, a method in which a far-infrared heater set to 300 to 350°C is placed at a distance of 10 to 50 cm from the molded body and heated for 5 to 30 seconds can be mentioned. The actual temperature of the molded body can be measured by a non-contact thermometer using infrared rays, or a method in which a thermo label (registered trademark) that changes color depending on temperature is attached to the molded body to set the preheating conditions can be mentioned.
[0077] The molded body for heat processing according to this embodiment has good processability during heat molding. Therefore, even if the cooling time in the mold is short after the molded body for heat processing is heat molded, it can be released from the mold without generating holes or wrinkles. Therefore, it is possible to increase the productivity of the heat molding process.
[0078] The molded article for heat processing according to the present embodiment has excellent biodegradability, and therefore can be suitably used in the fields of agriculture, fisheries, forestry, horticulture, medicine, sanitary products, food industry, clothing, non-clothing, packaging, automobiles, building materials, and other fields. For example, it can be used for food containers (lids, trays) and agricultural materials (seedling pots, trays).
[0079] In particular, the molded body for heat processing according to this embodiment can be preferably used for secondary processing into a molded product having a concave portion and / or a convex portion by heat molding. Specifically, it can be preferably heat molded into a container having a concave portion in the center, a container having a partition, a container having a folded portion around the opening, etc. Although there is no particular limitation on the more specific aspect, the molded body for heat processing according to this embodiment can be particularly preferably used for heat molding into a food container (lid, tray) or an agricultural material (seedling pot, tray).
[0080] The following items enumerate preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] A molded article for thermal processing containing a poly(3-hydroxyalkanoate)-based resin component, The poly(3-hydroxyalkanoate) resin component comprises a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 4 mol% or more and less than 7 mol%, and a copolymer (C) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 24 mol% or more, the proportion of the copolymer (A) in the entire poly(3-hydroxyalkanoate)-based resin component is 20% by weight or more and 95% by weight or less; The weight average molecular weight (Mw) of each of the copolymer (A) and the copolymer (C) is 450,000 or more; The poly(3-hydroxyalkanoate) resin component as a whole has a weight average molecular weight (Mw) of 450,000 or more. [Item 2] 2. The molded article for thermal processing according to item 1, wherein the proportion of the copolymer (C) in the entire poly(3-hydroxyalkanoate)-based resin component is 5% by weight or more and 50% by weight or less. [Item 3] 3. The molded article for thermal processing according to item 1 or 2, wherein the poly(3-hydroxyalkanoate)-based resin component further contains a copolymer (D) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 1 mol% or more and less than 4 mol%. [Item 4] 4. The molded body for thermal processing according to any one of items 1 to 3, wherein the molded body for thermal processing has a drawdown ratio measured of 0.1 [sec / (g / 10 min) / mm] or more and 300 [sec / (g / 10 min) / mm] or less. Drawdown ratio: Drawdown time [sec] / Melt flow rate [g / 10 min] / Thickness of the molded product for heat processing [mm] Drawdown time [sec]: The heat-processable molded product cut to a size of 35 cm x 35 cm was fixed horizontally to a frame having a square opening of 28 cm x 28 cm, and heated at a temperature of 350°C. The time required for the center of the heat-processable molded product to sag 7 cm in the vertical direction. Melt flow rate [g / 10 min]: The value measured on the above-mentioned heat-processable molded product cut into a size of 3 mm x 3 mm at 165°C and a load of 5.0 kgf according to JIS K 7210. [Item 5] 5. The molded article for thermal process according to any one of items 1 to 4, wherein the molded article for thermal process has a melt viscosity of 5000 poise or more and 8100 poise or less, as measured under conditions of a heating temperature of 150° C. and a shear rate of 1216 / sec. [Item 6] 6. The molded article for thermal process according to any one of items 1 to 5, wherein the melt flow rate measured on the molded article for thermal process is 0.1 g / 10 min or more and 6.0 g / 10 min or less. [Item 7] 7. The molded product for thermal process according to any one of items 1 to 6, wherein the drawdown time measured for the molded product for thermal process is 20 seconds or more and 65 seconds or less. [Item 8] 8. The molded article for thermal processing according to any one of items 1 to 7, wherein the molded article for thermal processing is a sheet having a thickness of 0.01 mm or more and 1.0 mm or less. [Item 9] 9. The molded article for thermal processing according to any one of items 1 to 8, comprising more than 0 and 30 parts by weight or less of an inorganic filler relative to 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate)-based resin component. [Item 10] 10. The molded body for thermal processing according to item 9, wherein the inorganic filler comprises one or more selected from the group consisting of talc, mica, kaolinite, montmorillonite, and smectite. [Item 11] 11. The molded article for thermal process according to any one of items 1 to 10, wherein the molded article for thermal process is a calender molded article. [Item 12] 12. The molded body for thermal processing according to any one of items 1 to 11, wherein the thermal processing is press molding or vacuum molding. [Item 13] 13. A molded product obtained by imparting a predetermined shape to the molded article for thermal processing according to any one of items 1 to 12 by thermal molding. [Item 14] Item 14. The molded product according to item 13, which is a food container or an agricultural material. EXAMPLES
[0081] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0082] (Raw materials used) Copolymer (A-2): Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) having a 3-hydroxyhexanoate (3HH) composition of 5.1 mol% and a weight average molecular weight of 760,000, produced according to the method described in International Publication No. 2008 / 010296. Copolymer (A-8): Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) having a 3-hydroxyhexanoate (3HH) composition of 5.2 mol% and a weight average molecular weight of 380,000, produced according to the method described in International Publication No. 2008 / 010296. Copolymer (A-10): Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) having a 3-hydroxyhexanoate (3HH) composition of 5.8 mol% and a weight average molecular weight of 610,000, obtained according to the method described in International Publication No. 2008 / 010296.
[0083] Copolymer (B-1): Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) having a 3HH composition of 10.5 mol% and a weight average molecular weight of 580,000, produced according to the method described in International Publication No. 2013 / 147139.
[0084] Copolymer (C-1): Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) having a 3HH composition of 28.0 mol% and a weight average molecular weight of 580,000, obtained according to the method described in International Publication No. 2019 / 142845. Copolymer (C-2): Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) having a 3HH composition of 28.0 mol% and a weight average molecular weight of 380,000, obtained according to the method described in International Publication No. 2019 / 142845.
[0085] Copolymer (D-1): Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) having a 3HH composition of 2.9 mol% and a weight average molecular weight of 580,000, obtained according to the method described in International Publication No. 2004 / 041936. Copolymer (D-2): Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) having a 3HH composition of 2.9 mol% and a weight average molecular weight of 380,000, obtained according to the method described in International Publication No. 2004 / 041936.
[0086] (Method of measuring weight average molecular weight) The weight average molecular weight of each copolymer, or the weight average molecular weight of the entire poly(3-hydroxyalkanoate) resin component, was measured by first dissolving the resin to be measured in chloroform and heating it in a hot water bath at 60°C for 0.5 hours, filtering the soluble matter through a disposable PTFE filter with a pore size of 0.45 μm, and then performing GPC measurement using the filtrate under the following conditions. GPC measuring device: Hitachi RI monitor (L-3000) Columns: Showa Denko KG (1 column), K-806L (2 columns) Sample concentration: 3mg / ml Free solution: Chloroform solution Free liquid flow rate: 1.0ml / min Sample injection volume: 100 μL Analysis time: 30 minutes Standard sample: Standard polystyrene
[0087] (Melt Viscosity) The sheets produced in each of the Examples and Comparative Examples were cut into pieces of approximately 3 mm x 3 mm, and approximately 5 g of the cut samples were used to measure the melt viscosity at a shear rate of 1216 / sec 5 minutes after the cut sheets were placed in the barrel of a Capillograph 1D manufactured by Toyo Seiki Seisakusho, which had been heated to a set temperature of 150°C.
[0088] (Sheet Melt Flow Rate (MFR) value) The sheets produced in each of the Examples and Comparative Examples were cut into pieces of about 3 mm x 3 mm, and about 30 g of each cut sample was used to measure the melt flow rate value in accordance with JIS K 7210. The measurement was performed under a load of 5.0 kgf and at a measurement temperature of 165°C.
[0089] (Sheet drawdown time) The sheets produced in each Example and Comparative Example were cut to approximately 35 cm x 35 cm and used for the measurements. The sheets were fixed horizontally to a frame with a 28 cm x 28 cm square opening in a vacuum forming machine (FVS-500 manufactured by Wakisaka Engineering Co., Ltd.), and the time until the center of the sheet sagged 7 cm (the vertical distance from the fixed surface of the sheet to the lowest point) was measured under the condition of a heating temperature of 350°C. This time was taken as the drawdown time.
[0090] (Sheet drawdown ratio) The drawdown ratio was calculated by dividing the ratio of the drawdown time to the melt flow rate value (drawdown time / melt flow rate value) by the sheet thickness.
[0091] (Seat appearance) The surface appearance of the sheets produced in each of the Examples and Comparative Examples was visually observed and evaluated according to the following criteria. ◯: The surface of the sheet is smooth and free of irregularities. △: The surface of the sheet is not smooth and has bumps.
[0092] (Thermoforming processability of sheets) The sheets produced in each of the Examples and Comparative Examples were thermoformed by the method described below, and the obtained molded products were visually evaluated according to the following criteria. Using a vacuum molding machine (FVS-500 manufactured by Wakisaka Engineering Co., Ltd.), the sheet was heated at a heating temperature of 350°C for about 20 seconds, and vacuum molding (thermoforming) was performed in a mold kept at about 30 to 50°C [mold shape: truncated cone, dimensions: depth 2 cm x diameter 9 cm at the bottom of the truncated cone and diameter 7 cm at the top of the truncated cone; arrangement in the mold frame: four truncated cone-shaped molds are arranged in a 25 cm x 25 cm mold frame (one truncated cone-shaped mold is arranged in the center of each 12.5 cm x 12.5 cm square)]. After cooling in the mold for about 5 seconds, the molded product was released from the mold within about 1 second and evaluated according to the following criteria. ○: The molded product has no wrinkles or holes after demolding. △: The molded product has wrinkles or holes after demolding. ×: The sheet is not solidified and cannot be released from the mold. If an attempt is made to release the sheet forcibly, the sheet sticks to the mold and a molded product cannot be obtained.
[0093] Example 1 A powder was prepared by blending 30 parts by weight of copolymer (A-10), 42 parts by weight of copolymer (C-1), 28 parts by weight of copolymer (D-1), and 5 parts by weight of inorganic filler (Microace K1 manufactured by Nippon Talc Co., Ltd.). The weight-average molecular weight of the powder was evaluated and found to be 600,000. The powder thus produced was placed in a Φ8 inch x L20 roll (manufactured by Kansai Roll Co., Ltd.) heated to a set temperature of 145°C, melted and kneaded for 3 minutes, and rolled to a sheet thickness of 0.28 mm and a sheet width of approximately 35 cm. The sheet was then stretched in the MD direction at a stretch ratio of 1.0 to 1.5 times while being cooled to produce a sheet with a width of 30 to 35 cm. The produced sheets were measured for melt viscosity, MFR value, drawdown time, and sheet thickness, and the drawdown ratio was calculated. In addition, the appearance of the sheets was evaluated. The results are shown in Table 1. The prepared sheets were vacuum molded and the thermoforming processability was evaluated by the method described above. The results are shown in Table 1.
[0094] (Examples 2 to 5, Comparative Examples 1 to 6) Powders and sheets were produced in the same manner as in Example 1, except that the formulation was changed as shown in Table 1, and evaluations were carried out in the same manner as in Example 1. The results are summarized in Table 1. However, in Comparative Example 3, an attempt was made to produce a sheet by the above-mentioned method, but the sheet could not be produced.
[0095] [Table 1]
[0096] It can be seen from Table 1 that the sheets of Examples 1 to 5 had good appearances, and by vacuum forming the sheets, molded products without wrinkles or holes were obtained. On the other hand, in Comparative Example 1, which did not contain copolymer (C) or (D), the surface of the produced sheet was uneven and had a poor appearance. In Comparative Example 2, the content of copolymer (A) was as low as 10% by weight, and wrinkles and holes were generated in the molded product obtained by vacuum molding. In Comparative Example 3, which did not contain the copolymer (A), the resin stuck to the roll during sheet production and could not be peeled off from the roll, so that a sheet could not be produced. In Comparative Example 4, copolymer (C) was not used, and in addition, the Mw of copolymer (A) was low at 380,000, and the Mw of the entire P3HA-based resin component was low at 440,000, and wrinkles and holes were generated in the molded product obtained by vacuum molding. In Comparative Example 5, no copolymer (C) was used, and the sheet in the mold was not sufficiently solidified within the above-mentioned cooling time, and it was impossible to release the sheet from the mold, so that no molded product was obtained. The composition in Comparative Example 5 is similar to the composition disclosed in the examples of Patent Document 1. In Comparative Example 6, the Mw of copolymer (C) and copolymer (D) was low at 380,000, and the sheet was prone to sagging during vacuum molding, so the molded product obtained by vacuum molding had molding defects such as wrinkles and holes.
Claims
1. A molded article for thermal processing containing a poly(3-hydroxyalkanoate)-based resin component, The poly(3-hydroxyalkanoate) resin component comprises a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 4 mol% or more and less than 7 mol%, and a copolymer (C) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 24 mol% or more, the proportion of the copolymer (A) in the entire poly(3-hydroxyalkanoate)-based resin component is 20% by weight or more and 95% by weight or less; The weight average molecular weight (Mw) of each of the copolymer (A) and the copolymer (C) is 450,000 or more; The poly(3-hydroxyalkanoate) resin component as a whole has a weight average molecular weight (Mw) of 450,000 or more.
2. 2. The molded article for thermal processing according to claim 1, wherein the proportion of said copolymer (C) in the entire poly(3-hydroxyalkanoate)-based resin component is 5% by weight or more and 50% by weight or less.
3. The molded article for thermal processing according to claim 1 or 2, wherein the poly(3-hydroxyalkanoate)-based resin component further contains a copolymer (D) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of which is 1 mol % or more and less than 4 mol %.
4. 3. The molded body for thermal processing according to claim 1 or 2, wherein the drawdown ratio measured for the molded body for thermal processing is 0.1 [sec / (g / 10 min) / mm] or more and 300 [sec / (g / 10 min) / mm] or less. Drawdown ratio: Drawdown time [sec] / Melt flow rate [g / 10 min] / Thickness of the molded article for heat processing [mm] Drawdown time [sec]: The heat-processable molded product cut to a size of 35 cm x 35 cm was fixed horizontally on a frame having a square opening of 28 cm x 28 cm, and heated at a temperature of 350°C. The time required for the center of the heat-processable molded product to sag 7 cm in the vertical direction. Melt flow rate [g / 10 min]: a value measured on the molded product for heat processing cut into a size of 3 mm x 3 mm under conditions of 165°C and a load of 5.0 kgf in accordance with JIS K 7210
5. 3. The molded product for thermal processing according to claim 1 or 2, wherein the molded product for thermal processing has a melt viscosity of 5000 poise or more and 8100 poise or less, measured under conditions of a heating temperature of 150°C and a shear rate of 1216 / sec.
6. 3. The molded article for thermal processing according to claim 1, wherein the melt flow rate measured for the molded article for thermal processing is 0.1 g / 10 min or more and 6.0 g / 10 min or less.
7. 3. The molded product for thermal process according to claim 1, wherein the drawdown time measured for the molded product for thermal process is 20 sec or more and 65 sec or less.
8. The molded article for thermal processing according to claim 1 or 2, which is a sheet having a thickness of 0.01 mm or more and 1.0 mm or less.
9. 3. The molded article for thermal processing according to claim 1, further comprising more than 0 and not more than 30 parts by weight of an inorganic filler per 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate)-based resin component.
10. The molded article for thermal processing according to claim 9 , wherein the inorganic filler comprises at least one selected from the group consisting of talc, mica, kaolinite, montmorillonite, and smectite.
11. The molded article for thermal processing according to claim 1 or 2, which is a calender molded article.
12. The molded article for thermal processing according to claim 1 or 2, wherein the thermal processing is press molding or vacuum molding.
13. 3. A molded product, which is obtained by imparting a predetermined shape to the molded article for thermal processing according to claim 1 or 2 by thermal molding.
14. The molded product according to claim 13, which is a food container or an agricultural material.
Citation Information
Patent Citations
Resin sheet for thermoforming, method for producing the same, and method for producing molding
JP2022010543A