Biodegradable resin and method for producing the same

An alternating copolymer of hydroxycarboxylic and amino acid units addresses moldability and heat resistance issues in biodegradable plastics, enhancing their biodegradability and applicability in diverse fields.

JP2024158605APending Publication Date: 2024-11-08OSAKA GAS CO LTD +1

Patent Information

Application Number
JP2023073948
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing biodegradable plastics like PHB have poor moldability, low mechanical properties, and insufficient heat resistance, limiting their practical application, while existing copolymers with PLA and PBS compromise crystallinity and heat resistance.

Method used

An alternating copolymer of hydroxycarboxylic acid units, particularly 3-hydroxybutyric acid, and amino acid units is developed, with protected functional groups to enhance molecular weight and improve biodegradability, heat resistance, and moldability.

Benefits of technology

The copolymer achieves high marine biodegradability, excellent heat resistance, and improved moldability, making it suitable for various applications including packaging and medical uses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158605000011
    Figure 2024158605000011
  • Figure 2024158605000012
    Figure 2024158605000012
  • Figure 2024158605000013
    Figure 2024158605000013
Patent Text Reader

Abstract

To provide a biodegradable resin with superior biodegradability, such as marine degradability, as well as high heat resistance and moldability.SOLUTION: A biodegradable resin is formed using an alternating copolymer of hydroxycarboxylic acid units, including 3-hydroxybutyrate units, and amino acid units. The 3-hydroxybutyrate units may be units derived from R-3-hydroxybutyrate. The alternating copolymer may have a repeating unit represented by the following formula (1) (where R is a hydrogen atom or an alkyl group, and n is an integer of 0 or greater).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a biodegradable resin containing 3-hydroxybutyric acid (3-hydroxybutanoic acid or 3HB) units and a method for producing the same. [Background technology]

[0002] From the perspective of environmental conservation and the realization of a sustainable society, efforts are being made to convert some or all of plastic raw materials into biomass, and the use of bio-based plastics (or biodegradable plastics) is increasing. Plastic is an essential material in human life, but plastic released into the environment drifts on the ocean and breaks down and fragments due to ultraviolet rays and other factors, generating microplastics with diameters of 5 mm or less. There are also concerns that if these microplastics are ingested into the living organisms of birds, fish, and other animals, they may cause endocrine disruption.

[0003] In recent years, efforts have been made to impart biodegradability to garbage bags, for example, in order to solve the above-mentioned microplastic problem. Examples of biodegradable plastics include polylactic acid (PLA), polyhydroxyalkanoate (PHA), polybutylene succinate (PBS), and polycaprolactone (PCL). However, although many of these biodegradable plastics have high biodegradability under compost conditions, they have low biodegradability under anaerobic conditions and in the ocean. In addition, since the biodegradable plastics have a high density and sink in the ocean, the development of plastics that have high biodegradability in the ocean is necessary to solve the microplastic problem.

[0004] Global Challenge 2017,1,1700048 (Non-Patent Document 1) evaluates the biodegradability of various biodegradable polyesters in the ocean, and discloses that poly-3-hydroxybutyrate (PHB) exhibits high biodegradability in the ocean compared to PLA, PCL, etc.

[0005] In addition, JP 2017-25138 A (Patent Document 1) discloses that a biodegradable copolymer in which 3-hydroxybutyric acid (3HB) units are randomly introduced has high biodegradability under aerobic and anaerobic conditions. In addition, Patent Document 1 also describes that the biodegradation rate can be controlled by changing the ratio of 3HB units in the copolymer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-25138 A [Non-patent literature]

[0007] [Non-Patent Document 1] Global Challenge 2017,1,1700048 Summary of the Invention [Problem to be solved by the invention]

[0008] PHB described in Non-Patent Document 1 is produced by microorganisms and has excellent biodegradability, but has low moldability. That is, since the glass transition temperature is low and the crystallization rate is slow, the physical properties are not stable during molding, and moldability is low. Furthermore, since it lacks the mechanical properties and heat resistance required for general-purpose plastic molded bodies and is also low in economic efficiency, it has not been widely used.

[0009] On the other hand, Patent Document 1 does not describe the marine degradability or heat resistance of the biodegradable copolymer. It is generally known that when a monomer with a different structure is copolymerized with a crystalline polymer such as PBS or PLA, the crystallinity decreases and the heat resistance derived from the crystal also decreases. It is difficult to increase the molecular weight even with the copolymer of Patent Document 1.

[0010] Therefore, an object of the present invention is to provide a biodegradable resin which has excellent biodegradability, such as marine degradability, and also has high heat resistance and moldability, and a method for producing the same. [Means for solving the problem]

[0011] As a result of intensive research aimed at solving the above problems, the present inventors discovered that by alternately copolymerizing hydroxycarboxylic acid units, including 3-hydroxybutyric acid units, and amino acid units, a biodegradable resin that has excellent biodegradability, including marine degradability, and also has high heat resistance and moldability, can be obtained, and thus completed the invention.

[0012] That is, the biodegradable resin according to embodiment [1] of the present invention is composed of an alternating copolymer of hydroxycarboxylic acid units and amino acid units, and the hydroxycarboxylic acid units contain 3-hydroxybutyric acid units.

[0013] Aspect [2] of the present invention is an aspect in which, in the aspect [1], the 3-hydroxybutyric acid unit is a unit derived from R-3-hydroxybutyric acid.

[0014] The aspect [3] of the present invention is an aspect in which the alternating copolymer of the aspect [1] or [2] has a repeating unit represented by the following formula (1):

[0015] [ka]

[0016] (In the formula, R represents a hydrogen atom or an alkyl group, and n represents an integer of 0 or more).

[0017] The embodiment [4] of the present invention relates to the compound according to the above embodiment [3], wherein R is a hydrogen atom or C 1-3 It is an alkyl group, and n is an integer of 0 to 6.

[0018] The embodiment [5] of the present invention is an embodiment in which, in formula (1) of the embodiment [3] or [4], R is a hydrogen atom or a methyl group, and n is 0.

[0019] Aspect [6] of the present invention is any one of aspects [1] to [5] above, wherein the amino acid unit is an amino acid unit derived from an L-amino acid.

[0020] Aspect [7] of the present invention is any one of aspects [1] to [6] above, wherein the amino acid unit is an amino acid unit derived from an α-amino acid.

[0021] An embodiment [8] of the present invention is any one of the above embodiments [1] to [7], wherein the alternating copolymer has a number average molecular weight of 5,000 or more.

[0022] Aspect [9] of the present invention is any one of aspects [1] to [8] above, wherein the alternating copolymer has a glass transition temperature of 50° C. or higher.

[0023] An embodiment

[10] of the present invention is an embodiment in which the biodegradable resin of any one of the above embodiments [1] to [9] has marine biodegradability.

[0024] The present invention includes, as an aspect

[11] , a monomer synthesis step of reacting a hydroxycarboxylic acid component with an amino acid component to obtain an amide monomer; and a polymerization step of polymerizing the amide monomer to obtain an alternating copolymer of a hydroxycarboxylic acid unit and an amino acid unit. The present invention also includes a method for producing a biodegradable resin according to any one of the above aspects [1] to

[10] .

[0025] The present invention relates to an embodiment

[12] of the present invention, in the monomer synthesis step of the embodiment

[11] , At least one of the hydroxycarboxylic acid component and the amino acid component is a derivative, the derivative in the hydroxycarboxylic acid component is a derivative of a hydroxycarboxylic acid in which a hydroxyl group of the hydroxycarboxylic acid is protected with a protecting group, In this embodiment, the derivative in the amino acid component is a derivative of an amino acid in which a carboxyl group of the amino acid is protected with a protecting group.

[0026] The embodiment

[13] of the present invention is an embodiment in which, in the polymerization step of the embodiment

[11] or

[12] , the amide monomer has a carboxyl group esterified with an alkyl group.

[0027] The embodiment

[14] of the present invention is an embodiment in which, in the polymerization step of any one of the embodiments

[11] to

[13] , the amide monomer is polymerized in the presence of a tin catalyst.

[0028] In the present specification and claims, the term "3-hydroxycarboxylic acid component" is used to mean not only 3-hydroxycarboxylic acid but also derivatives in which the hydroxyl and / or carboxyl groups are protected with protecting groups, and the term "amino acid component" is used to mean not only amino acids but also derivatives in which the carboxyl groups are protected with protecting groups. Effect of the Invention

[0029] The biodegradable resin of the present invention has hydroxycarboxylic acid units, including 3-hydroxybutyric acid units, copolymerized alternately with amino acid units, and therefore has improved biodegradability, including marine degradability, and also has improved heat resistance and moldability. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is a graph evaluating the biodegradability in seawater of the amide monomers obtained in Examples 1 to 5. [Diagram 2] FIG. 2 is a graph evaluating the biodegradability of the polymers obtained in Examples 1 and 2 in soil suspensions. [Diagram 3] FIG. 3 is a graph evaluating the biodegradability in seawater of the polymers obtained in Examples 1 and 2. [Figure 4] FIG. 4 is a 1H-NMR spectrum of the polymer obtained in Example 1. [Diagram 5] FIG. 5 is a 13C-NMR spectrum of the polymer obtained in Example 1. [Figure 6] FIG. 6 is a 1H-NMR spectrum of the polymer obtained in Example 2. [Figure 7] FIG. 7 is a 13C-NMR spectrum of the polymer obtained in Example 2. [Figure 8] FIG. 8 is a 1H-NMR spectrum of the polymer obtained in Example 3. [Figure 9] FIG. 9 is a 13C-NMR spectrum of the polymer obtained in Example 3. [Figure 10] FIG. 10 is a 1H-NMR spectrum of the polymer obtained in Example 4. [Figure 11] FIG. 11 is a 13C-NMR spectrum of the polymer obtained in Example 4. [Figure 12] FIG. 12 is a 1H-NMR spectrum of the polymer obtained in Example 5. [Figure 13] FIG. 13 is a 13C-NMR spectrum of the polymer obtained in Example 5. [Figure 14] FIG. 14 is a 1H-NMR spectrum of the polymer obtained in Example 6. [Figure 15] FIG. 15 is a 13C-NMR spectrum of the polymer obtained in Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] [Alternating copolymer] The biodegradable resin of the present invention is formed of an alternating copolymer of hydroxycarboxylic acid units and amino acid units. In the present invention, the hydroxycarboxylic acid contains 3-hydroxybutyric acid units as an essential unit, and such hydroxycarboxylic acid units and amino acid units are arranged alternately and regularly, thereby exhibiting biodegradability such as marine degradability, and also improving heat resistance and moldability. In the following description, since the hydroxycarboxylic acid units are derived from hydroxycarboxylic acid components and the amino acid units are derived from amino acid components, the hydroxycarboxylic acid units may be used synonymously with the hydroxycarboxylic acid components, and the amino acid units may be used synonymously with the amino acid components.

[0032] (3-hydroxybutyric acid unit) The hydroxycarboxylic acid unit contains a 3-hydroxybutyric acid unit as an essential unit. The 3-hydroxybutyric acid component corresponding to the 3-hydroxybutyric acid unit may be 3-hydroxybutyric acid (3HB) or a derivative of 3HB in which the hydroxyl group is protected with a protecting group.

[0033] 3HB (or BHB) may be an optical isomer (R or S form) or may be a racemate, but from the standpoint of biodegradability, it is preferable that it contains at least the R form (R-3-hydroxybutyric acid).

[0034] The proportion of R-isomers in 3HB, particularly the optical purity (enantiomer or optical isomer excess), is, for example, 50% ee or more (e.g., 80% ee or more), preferably 90% ee or more (e.g., 95 to 100% ee), and more preferably 98 to 100% ee (e.g., 99 to 100% ee, particularly substantially 100% ee). If the optical purity is too low, there is a risk of reduced biodegradability.

[0035] In addition, the R-form [(R)3HB] may be used in combination with the S-form [(S)3HB] and / or racemic form, but the mass proportion of the R-form in 3HB is preferably 10% by mass or more, more preferably 50% by mass or more, even more preferably 90% by mass or more, and most preferably 100% by mass.

[0036] The protecting group in the derivative may be a conventional protecting group for protecting a hydroxyl group. Examples of the conventional protecting group include alkyl groups such as methyl, ethyl, and t-butyl; cycloalkyl groups such as cyclohexyl; aryl groups such as 2,4-dinitrophenyl; aralkyl groups such as benzyl, 2,6-dichlorobenzyl, 3-bromobenzyl, p-methoxybenzyl, 2-nitrobenzyl, 4-dimethylcarbamoylbenzyl, and triphenylmethyl; acetyl, propionyl, isopropionyl, butyryl, isobutyryl, and valeryl. Examples of protecting groups include aliphatic acyl groups such as aryl, isovaleryl, and pivaloyl groups; alicyclic acyl groups such as cyclohexylcarbonyl groups; aromatic acyl groups such as benzoyl, p-phenylbenzoyl, phthaloyl, and naphthoyl groups; and silyl ether groups (silyl-based protecting groups) such as trimethylsilyl (TMS), triethylsilyl (TES), t-butyldimethylsilyl (TBS), triisopropylsilyl (TIPS), and t-butyldiphenylsilyl (TBDPS). These protecting groups can be used alone or in combination of two or more.

[0037] Among these protecting groups, silyl ether groups are preferred, trialkylsilyl groups such as TBS groups are more preferred, and triC 1-4 Alkylsilyl groups are more preferred.

[0038] The 3-hydroxybutyric acid (3HB) unit is preferably the main unit in the hydroxycarboxylic acid unit, and specifically, may be 50 mol% or more of the hydroxycarboxylic acid unit, preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 99 mol% or more, and most preferably 100 mol%. If the proportion of the 3HB unit is too small, it may be difficult to achieve a balance between biodegradability, heat resistance, and moldability of the biodegradable resin.

[0039] (Other hydroxycarboxylic acid units) The hydroxycarboxylic acid unit may further contain another hydroxycarboxylic acid unit (second hydroxycarboxylic acid unit) within the range that does not impair the effects of the present invention. The other hydroxycarboxylic acid component corresponding to the other hydroxycarboxylic acid unit may be another hydroxycarboxylic acid or a derivative of another hydroxycarboxylic acid in which the hydroxyl group is protected with a protecting group.

[0040] The other hydroxycarboxylic acid components include hydroxyalkanoic acid components other than the 3HB component (other hydroxyalkanoic acid components), hydroxycycloalkanecarboxylic acid components, hydroxyarenecarboxylic acid components, and the like.

[0041] Other hydroxyalkanoic acid components include, for example, glycolic acid, 2-hydroxypropanoic acid (lactic acid), 3-hydroxypropanoic acid, 2-hydroxybutanoic acid (2-hydroxybutyric acid), 4-hydroxybutanoic acid, 3-hydroxy-3-methyl-butanoic acid, 2-hydroxypentanoic acid (2-hydroxyvaleric acid), 3-hydroxypentanoic acid, 5-hydroxypentanoic acid, 2-hydroxy-2-methyl-pentanoic acid, 3-hydroxyhexanoic acid, 6-hydroxyheptanoic acid, 3-hydroxyheptanoic acid, 7-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 8-hydroxyoctanoic acid, 3-hydroxynananoic acid, 9-hydroxynananoic acid, 3-hydroxydecanoic acid, and 10-hydroxydecanoic acid. 1-6 Hydroxy C, optionally having an alkyl group 2-15 Alkanoic acid and the like.

[0042] The other hydroxyalkanoic acid component may be the corresponding lactone, for example, a di-C lactone such as β-propiolactone, β-dimethylpropiolactone, γ-butyrolactone, γ-dimethylbutyrolactone, δ-valerolactone, or ε-caprolactone. 1-12 C which may have an alkyl group 3-15 Lactones, etc.

[0043] Examples of hydroxycycloalkanoic acids include hydroxycyclohexanecarboxylic acid.

[0044] Hydroxyarene carboxylic acids include, for example, hydroxybenzoic acid.

[0045] These other hydroxycarboxylic acid components can be used alone or in combination of two or more. Among these, other hydroxyalkanoic acid components are preferred, and hydroxy C such as 3-hydroxypropanoic acid and 4-hydroxybutanoic acid are preferred. 3-10 Alkanoic acids are more preferred.

[0046] The protecting groups in the derivatives, including preferred embodiments, are the same as those in the derivatives of the 3HB components.

[0047] The ratio of the other hydroxycarboxylic acid units is 0.5 mol or less, preferably 0.3 mol or less, more preferably 0.1 mol or less, and even more preferably 0.01 mol or less, per mol of the 3HB units. If the ratio of the other hydroxycarboxylic acid units is too high, it may be difficult to achieve a balance between biodegradability, heat resistance, and moldability of the biodegradable resin.

[0048] (amino acid unit) The amino acid component corresponding to the amino acid unit may be an amino acid or a derivative in which the carboxyl group is protected with a protecting group.

[0049] The amino acid may be an acidic or basic amino acid, but is preferably a neutral amino acid. Examples of neutral amino acids include aliphatic α-amino acids such as glycine, α-alanine, α-valine, α-leucine, and α-isoleucine; aromatic α-amino acids such as α-phenylalanine; aliphatic β-amino acids such as β-alanine and β-leucine; aromatic β-amino acids such as β-phenylalanine; amino C acids such as 6-aminohexanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. 4-20 Alkyl-carboxylic acids and the like.

[0050] These amino acids can be used alone or in combination of two or more. Among these amino acids, α-amino acids are preferred, α-aliphatic amino acids are more preferred, and C amino acids such as glycine and alanine are more preferred, because they can improve the glass transition temperature of the polymer. 2-4 α-amino acids are more preferred, C 2-3 Alpha-amino acids are most preferred.

[0051] The α-amino acids other than glycine may be optical isomers (L- or D-forms) or racemates, but it is preferable to contain at least the L-form (L-amino acids such as L-alanine) since this can improve biodegradability as well as the molecular weight of the polymer.

[0052] The proportion of L-forms in the α-amino acids, particularly the optical purity (enantiomer or optical isomer excess), is, for example, 50% ee or more (e.g., 80% ee or more), preferably 90% ee or more (e.g., 95 to 100% ee), and more preferably 98 to 100% ee (e.g., 99 to 100% ee, particularly substantially 100% ee). If the optical purity is too low, there is a risk of biodegradability and the molecular weight of the polymer decreasing.

[0053] In addition, the α-amino acids may be used in combination with L-, D- and / or racemic forms, but the mass proportion of the L-form in the α-amino acids is preferably 10% by mass or more, more preferably 50% by mass or more, even more preferably 90% by mass or more, and most preferably 100% by mass.

[0054] The protecting group in the derivative may be a conventional protecting group for protecting a carboxyl group. Examples of the conventional protecting group include alkyl groups such as methyl, ethyl, t-butyl, and trichloroethyl; cycloalkyl groups such as cyclohexyl; aralkyl groups such as benzyl, p-nitrobenzyl, and diphenylmethyl; and phenacyl. These protecting groups may be used alone or in combination.

[0055] Among these protecting groups, alkyl groups are preferred, and C groups such as methyl and ethyl groups are preferred. 1-3 Alkyl groups are more preferred, C 1-2 Alkyl groups are more preferred.

[0056] The amino acid unit is C 2-3 α-amino acid units (especially glycine or α-alanine, including the L-form) are preferred, 2-3 The proportion of α-amino acid units is preferably a major unit in the amino acid units, and specifically, it may be 50 mol % or more, preferably 80 mol % or more, more preferably 90 mol % or more, even more preferably 99 mol % or more, and most preferably 100 mol % in the amino acid units. 2-3 If the proportion of the α-amino acid unit is too low, it may be difficult to achieve a balance between biodegradability, heat resistance, and moldability of the biodegradable resin.

[0057] (Preferred repeating unit) The biodegradable resin of the present invention may be a polymer in which units derived from a hydroxycarboxylic acid component, including the 3-hydroxybutyric acid component, and units derived from the amino acid component are alternately copolymerized, but is preferably an alternating copolymer having a repeating unit represented by formula (1).

[0058] In the formula (1), examples of the alkyl group represented by R include C groups such as a methyl group, an ethyl group, a propyl group, a butyl group, and a hexyl group. 1-12 These alkyl groups can be used alone or in combination. R is a hydrogen atom or a C 1-3 An alkyl group is preferred, and a hydrogen atom or C 1-2 An alkyl group is more preferred, and a hydrogen atom or a methyl group is even more preferred.

[0059] The repeating number n of methylene units may be an integer of 0 or more, for example, an integer of 0 to 6, preferably an integer of 0 to 3, further preferably an integer of 0 to 2, more preferably 0 or 1, and most preferably 0.

[0060] In the repeating unit represented by formula (1), R is a hydrogen atom or C 1-3 A repeating unit in which R is an alkyl group and n is an integer of 0 to 6 is preferred, and a repeating unit in which R is a hydrogen atom or a methyl group and n is 0 is more preferred.

[0061] The biodegradable resin of the present invention may maintain optical activity, and is most preferably made of an alternating copolymer having a repeating unit represented by the following formula (2).

[0062] [ka]

[0063] (In the formula, R 1 indicates a hydrogen atom or a methyl group).

[0064] The component (monomer of biodegradable resin) corresponding to the repeating unit represented by the formula (1) has excellent biodegradability, particularly marine biodegradability. The aerobic biodegradability of this monomer in seawater after 60 days at 30° C. may be 30% or more, preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more.

[0065] In this specification and claims, the aerobic biodegradability in seawater can be measured by an oxygen demand biodegradability test in accordance with the measurement conditions in ASTM D6691-17.

[0066] (Characteristics of biodegradable resin) The biodegradable resin of the present invention has excellent biodegradability, particularly marine biodegradability. The aerobic biodegradability of the biodegradable resin of the present invention in seawater after 60 days at 30° C. may be 30% or more, preferably 40% or more, more preferably 45% or more, and even more preferably 50% or more.

[0067] The biodegradable resin of the present invention is also biodegradable in a soil suspension. The aerobic biodegradability of the biodegradable resin of the present invention in a soil suspension after 60 days at 25° C. may be 10% or more, preferably 20% or more, more preferably 30% or more, and even more preferably 40% or more.

[0068] In this specification and claims, the aerobic biodegradability in a soil suspension can be measured in accordance with ISO14851:2019.

[0069] The biodegradable resin of the present invention has a large molecular weight, even though it has the biodegradability as described above. The number average molecular weight of the biodegradable resin of the present invention may be 5,000 or more, for example, 5,000 to 300,000, preferably 7,000 to 100,000, further preferably 8,000 to 80,000, more preferably 10,000 to 70,000, and most preferably 12,000 to 50,000. If the molecular weight is too small, there is a risk of the mechanical properties being reduced.

[0070] In this specification and claims, the number average molecular weight of the biodegradable resin can be measured by gel permeation chromatography (eluent: 5 mM sodium trifluoroacetate / hexafluoroisopropanol, reference resin: polymethyl methacrylate), and more specifically, by the method described in the examples below.

[0071] The biodegradable resin of the present invention may have a high glass transition temperature of 30° C. or higher (particularly 50° C. or higher), for example, 30 to 150° C., preferably 40 to 120° C., further preferably 50 to 110° C., more preferably 60 to 100° C., and most preferably 70 to 90° C. If the glass transition temperature is too low, there is a risk that the heat resistance and moldability will decrease, and conversely, if the glass transition temperature is too high, there is a risk that the moldability will decrease.

[0072] In this specification and claims, the glass transition temperature of the biodegradable resin can be measured using a dynamic viscoelasticity measuring device, and in detail, can be measured by the method described in the examples below.

[0073] The biodegradable resin of the present invention also has high heat resistance. For example, the 5% weight loss temperature (Td5%) may be 200°C or higher (e.g., 200 to 400°C), preferably 210 to 350°C, more preferably 220 to 300°C, and even more preferably 230 to 250°C.

[0074] In this specification and claims, the 5% weight loss temperature of a biodegradable resin can be measured using a thermogravimeter in a nitrogen atmosphere, and in detail, can be measured by the method described in the examples below.

[0075] The biodegradable resin of the present invention may be crystalline. The degree of crystallinity of the biodegradable resin of the present invention is, for example, 10 to 80%, preferably 20 to 70%, further preferably 30 to 50%, and further preferably 35 to 45%.

[0076] [Manufacturing method of biodegradable resin] The method for producing a biodegradable resin of the present invention includes a monomer synthesis step of reacting a hydroxycarboxylic acid component with an amino acid component to obtain an amide monomer, and a polymerization step of polymerizing the amide monomer to obtain an alternating copolymer of hydroxycarboxylic acid units and amino acid units.

[0077] (A) Monomer synthesis process In the monomer synthesis step, a hydroxycarboxylic acid component is reacted with an amino acid component to obtain an amide monomer which will become a monomer for a repeating unit of a polymer.

[0078] The hydroxycarboxylic acid component and amino acid component used as raw materials may be hydroxycarboxylic acid and amino acid, but from the viewpoint of productivity, it is preferable that at least one of them is a derivative protected with a protecting group. Specifically, it is preferable to protect the hydroxyl group of the hydroxycarboxylic acid and / or the carboxyl group of the amino acid, which are functional groups not involved in forming an amide bond, with a protecting group. In particular, it is preferable to protect at least the carboxyl group of the amino acid with a protecting group, from the viewpoints of efficiently producing an amide monomer and improving the molecular weight of the alternating copolymer in the subsequent polymerization step, and it is preferable to protect both the hydroxyl group of the hydroxycarboxylic acid and the carboxyl group of the amino acid with a protecting group.

[0079] (Method for protecting hydroxyl group of hydroxycarboxylic acid) As a method for protecting the hydroxyl group of the hydroxycarboxylic acid (particularly 3HB) with a protecting group, a method for introducing the protecting group by a conventional method depending on the type of the protecting group described above can be used. When the protecting group is a silyl ether group, the method for introducing the protecting group is preferably a method in which a silyl ether group is introduced into the hydroxyl group of the hydroxycarboxylic acid component using a silylating agent for introducing a silyl ether group in a solvent in the presence of a base catalyst.

[0080] The proportion of the silylating agent may be 1 mol or more, for example, 1 to 1.5 mol, and preferably 1.1 to 1.3 mol, per mol of the hydroxycarboxylic acid component.

[0081] The base catalyst may be an inorganic base or an organic base. Examples of inorganic bases include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; alkali metal or alkaline earth metal carbonates such as sodium carbonate, sodium hydrogen carbonate, and magnesium carbonate. Examples of organic bases include trialkylamines such as trimethylamine, triethylamine, and diisopropylethylamine; alkanolamines such as triethanolamine and dimethylaminoethanol; pyridine, imidazole, morpholine, N-methylmorpholine, and hexamethylenetetramine; heterocyclic amines such as diazabicycloundecene (DBU); diazabicyclononene (DBN), and 1,4-diazabicyclo[2.2.2]octane (DABCO). These base catalysts may be used alone or in combination. Among these, organic bases such as trialkylamines and heterocyclic amines are preferred, and heterocyclic amines such as imidazole are particularly preferred.

[0082] The proportion of the base catalyst is, for example, 0.1 to 10 mol, preferably 0.5 to 8 mol, more preferably 1 to 5 mol, and even more preferably 2 to 3 mol, per 1 mol of the hydroxycarboxylic acid component.

[0083] Examples of the solvent include ethers (e.g., cyclic ethers such as tetrahydrofuran and 1,4-dioxane), esters (e.g., ethyl acetate), ketones (e.g., chain ketones such as acetone and methyl ethyl ketone; cyclic ketones such as cyclohexanone), halogen-containing solvents (e.g., halogenated hydrocarbons such as dichloromethane and chloroform), amides (e.g., dimethylacetamide, dimethylformamide, N-methylpyrrolidone), nitriles (e.g., acetonitrile, propionitrile), sulfoxides (e.g., dimethylsulfoxide), etc. These solvents can be used alone or in combination of two or more. Among these, amides, halogen-containing solvents, and nitriles are preferred, and amides such as dimethylformamide are particularly preferred.

[0084] The volume of the solvent may be 1 or more times the volume of the hydroxycarboxylic acid component, for example, 1 to 100 times, preferably 5 to 50 times, further preferably 10 to 30 times, and further preferably 15 to 20 times.

[0085] The hydroxycarboxylic acid component to be reacted with the silylating agent may be a hydroxycarboxylic acid, but from the viewpoint of improving productivity, it may also be a derivative in which the carboxyl group of the hydroxycarboxylic acid is protected with a protecting group.

[0086] The derivative in which the carboxyl group of the hydroxycarboxylic acid is protected with a protecting group is preferably a derivative protected with an alkyl group as the protecting group. Examples of such derivatives include C-substituted esters of hydroxycarboxylic acids such as methyl esters of hydroxycarboxylic acids and ethyl esters of hydroxycarboxylic acids. 1-3 Among these, the C alkyl esters of hydroxycarboxylic acids, such as the methyl esters of hydroxycarboxylic acids, 1-2 Alkyl esters are preferred. These derivatives can be prepared by conventional methods and are commercially available.

[0087] The reaction temperature for introducing a protecting group into the hydroxyl group of the hydroxycarboxylic acid component may be 0° C. or higher, for example, 0 to 50° C., preferably 10 to 40° C., more preferably 20 to 30° C., or may be room temperature.

[0088] The hydroxycarboxylic acid component in which a protecting group has been introduced into the hydroxyl group may be separated and purified by a conventional method after adding a conventional reaction terminator such as saturated ammonium chloride.

[0089] When a derivative with a protected carboxyl group is used as the hydroxycarboxylic acid component, it is preferable to remove (deprotect) the protecting group of the carboxyl group after protecting the hydroxyl group with a protecting group. The protecting group can be removed by a conventional method depending on the type of the protecting group. When the protecting group is an alkyl group, the protecting group can be removed by hydrolysis in the presence of a base.

[0090] Examples of the base include the bases exemplified as the base catalyst in the method for introducing a silyl ether group as a protecting group described above. The bases can be used alone or in combination of two or more. Among the bases, alkali metal hydroxides such as lithium hydroxide are preferred.

[0091] The proportion of the base is, for example, 0.1 to 10 mol, preferably 0.3 to 5 mol, more preferably 0.5 to 3 mol, and even more preferably 1 to 2 mol, relative to 1 mol of the hydroxycarboxylic acid derivative.

[0092] The deprotection may be carried out by hydrolysis in the presence of water, or may be carried out in a mixed solvent of water and an organic solvent. Examples of the organic solvent include the solvents exemplified in the method for introducing a silyl ether group as a protecting group described above. Among the above solvents, ethers such as tetrahydrofuran are preferred. The volume ratio of water to the organic solvent is water / organic solvent=10 / 1 to 1 / 10, preferably 3 / 1 to 1 / 5, more preferably 1 / 1 to 1 / 3, and more preferably 1 / 1.5 to 1 / 2.5.

[0093] The total volume of water and the organic solvent may be 1 or more times the volume of the hydroxycarboxylic acid derivative, for example, 1 to 100 times, preferably 5 to 80 times, more preferably 10 to 50 times, and more preferably 30 to 40 times.

[0094] The reaction temperature for deprotecting the alkyl group may be 0° C. or higher, for example, 0 to 50° C., preferably 10 to 40° C., more preferably 20 to 30° C., and may be room temperature.

[0095] The hydroxycarboxylic acid derivative from which the carboxyl protecting group has been deprotected may be neutralized and separated or purified by a conventional method, such as filtration, transfer, salting out, distillation, solvent removal, precipitation, crystallization, recrystallization, decantation, extraction, drying, washing, chromatography, etc.

[0096] (Derivatives in which the carboxyl group of an amino acid is protected with a protecting group) The derivative in which the carboxyl group of the amino acid is protected with a protecting group is preferably a derivative protected with an alkyl group as the protecting group. Examples of such derivatives include α-amino acid C carboxylates such as glycine methyl ester hydrochloride and alanine methyl ester hydrochloride. 1-3 Among these, α-amino acid C salts such as glycine methyl ester hydrochloride and L-alanine methyl ester hydrochloride are 1-2 The inorganic acid salts of alkyl esters are preferred. These derivatives can be prepared by conventional methods and are commercially available.

[0097] (Method of synthesizing amide monomers) The amide monomer is obtained by condensing a hydroxycarboxylic acid component (particularly, a 3HB component) with an amino acid component to form an amide bond. The condensation reaction may be carried out in a solvent in the presence of a condensing agent, and is particularly preferably carried out in the presence of a condensing agent, a condensation auxiliary, and a base.

[0098] The ratio of the amino acid component can be selected from the range of about 0.5 to 1.5 moles per mole of the hydroxycarboxylic acid component, for example, 0.6 to 1.4 moles, preferably 0.8 to 1.3 moles, more preferably 0.9 to 1.2 moles, and even more preferably 1 to 1.2 moles.

[0099] The condensation agent may be a conventional condensation agent used to form an amide bond. Examples of the conventional condensation agent include carbodiimide-based condensation agents such as diisopropylcarbodiimide (DIPC), 1-ethyl-3-(3-dimethylaminopropyl)-carbodiimide (EDCI=WSCI), 1-ethyl-3-(3-dimethylaminopropyl)-carbodiimide hydrochloride (EDCI·HCl=WSCI·HCl), and dicyclohexylcarbodiimide (DCC); O-(7-azabenzotriazol-1-yl)-1,1,3,3-tetramethyluronium Examples of the fluorophosphate-based condensing agent include hexafluorophosphate, O-benzotriazol-1-yl-N,N,N',N'-tetramethyluronium hexafluorophosphate, benzotriazol-1-yl-oxy-tris-pyrrolidinophosphonium hexafluorophosphate, and benzotriazol-1-yl-tris(dimethylamino)phosphonium hexafluorophosphate salt (BOP); diphenylphosphoryl azide (DPPA), etc. These condensing agents can be used alone or in combination of two or more kinds.

[0100] Among these condensing agents, carbodiimide-based condensing agents such as EDCI and EDCI·HCl are preferred.

[0101] The ratio of the condensing agent can be selected from the range of about 0.5 to 1.5 mol per 1 mol of the hydroxycarboxylic acid component, for example, 0.6 to 1.4 mol, preferably 0.8 to 1.3 mol, further preferably 0.9 to 1.2 mol, and even more preferably 1 to 1.2 mol.

[0102] Examples of the condensation auxiliary include N-hydroxydicarboxylic acid imides such as N-hydroxysuccinimide (HONSu) and N-hydroxy-5-norbornene-2,3-dicarboxylic acid imide (HONB); N-hydroxybenzotriazoles such as 1-hydroxybenzotriazole (HOBt) and 1-hydroxy-7-azabenzotriazole (HOAt); triazines such as 3-hydroxy-4-oxo-3,4-dihydro-1,2,3-benzotriazine (HOOBt); 2-hydroxyimino-2-cyanoacetic acid ethyl ester, etc. These condensation auxiliary can be used alone or in combination of two or more kinds.

[0103] Among these condensation assistants, N-hydroxydicarboxylic acid imides such as HONSu and N-hydroxybenzotriazoles such as HOBt are preferred, and N-hydroxybenzotriazoles are particularly preferred.

[0104] The proportion of the condensation aid can be selected from the range of about 0.5 to 1.5 mol per mol of the hydroxycarboxylic acid component, for example, 0.6 to 1.4 mol, preferably 0.8 to 1.3 mol, further preferably 0.9 to 1.2 mol, and even more preferably 1 to 1.2 mol.

[0105] The base may be used to adjust the pH of the reaction system to, for example, near neutral. Examples of the base include the bases exemplified as the base catalyst in the method of introducing a silyl ether group as a protecting group described above. The bases may be used alone or in combination of two or more. Among the bases, trialkylamines such as trimethylamine, triethylamine, and diisopropylethylamine; heterocyclic tertiary amines such as N-methylmorpholine and pyridine are preferred.

[0106] The ratio of the base can be selected from the range of about 0.1 to 10 mol per 1 mol of the hydroxycarboxylic acid component, and is, for example, 1 to 5 mol, preferably 1.5 to 3 mol, further preferably 2 to 2.5 mol, and even more preferably 2.1 to 2.3 mol.

[0107] Examples of the solvent include those exemplified in the method of introducing a silyl ether group as a protecting group described above. Among the above solvents, halogen-containing solvents such as dichloromethane are preferred. The volume of the solvent may be 1 time or more, for example 1 to 300 times, preferably 10 to 200 times, more preferably 30 to 150 times, and more preferably 50 to 120 times, relative to the volume of the hydroxycarboxylic acid derivative.

[0108] The reaction temperature for forming the amide bond may be 0° C. or higher, for example, 0 to 50° C., preferably 10 to 40° C., more preferably 20 to 30° C., or may be room temperature. The obtained amide monomer may be separated or purified by a conventional method.

[0109] (Method for deprotecting amide monomer) When the amide monomer is an amide monomer obtained by a condensation reaction between a hydroxycarboxylic acid derivative having a protected hydroxyl group and an amino acid derivative having a protected carboxyl group, it is preferable to deprotect only the protecting group of the hydroxyl group, since this allows the molecular weight of the alternating copolymer to be improved in the subsequent polymerization step.

[0110] As a method for removing the protective group of the hydroxyl group of the amide monomer, a method for removing the protective group by a conventional method according to the type of the protective group can be used. When the protective group is a silyl ether group, the method for removing the protective group includes a method of deprotecting the protective group by acting a deprotecting agent. Examples of the deprotecting agent include inorganic acids such as hydrochloric acid and sulfuric acid; acetyl chloride; and fluorine compounds such as anhydrous hydrogen fluoride, trifluoromethanesulfonic acid, and trifluoroacetic acid. Among these, acetyl chloride is preferred.

[0111] The ratio of the deprotecting agent can be selected from the range of about 0.01 to 1 mol per 1 mol of the amide monomer, for example, 0.02 to 0.7 mol, preferably 0.03 to 0.5 mol, further preferably 0.05 to 0.3 mol, and even more preferably 0.1 to 0.2 mol.

[0112] The deprotection may be carried out in a solvent. Examples of the solvent include those exemplified in the method for introducing a silyl ether group as a protecting group, as well as alcohols such as methanol and ethanol. Among these, alcohols such as methanol are preferred.

[0113] The volume of the solvent may be 1 or more times the volume of the amide monomer, for example, 1 to 100 times, preferably 5 to 50 times, further preferably 10 to 40 times, and further preferably 20 to 30 times.

[0114] The amide monomer from which the hydroxyl-protecting group has been deprotected may be neutralized by a conventional method, and then separated or purified.

[0115] (Preferred embodiment) As described above, the monomer synthesis process is preferably a monomer synthesis process including four steps, namely, a first protection step of introducing a protecting group to the hydroxyl group of a derivative of a hydroxycarboxylic acid having a protected carboxyl group to obtain a first intermediate, a deprotection step of deprotecting the carboxyl group of the first intermediate to obtain a second intermediate, an amidation step of subjecting the second intermediate to a condensation reaction with a derivative of an amino acid having a protected carboxyl group to obtain a first amide monomer, and a second protection step of deprotecting the hydroxyl group of the amide monomer to obtain a second amide monomer.

[0116] (B) Polymerization process In the polymerization step, the amide monomer obtained in the monomer synthesis step is polymerized (polycondensed) to obtain an alternating copolymer of hydroxycarboxylic acid units and amino acid units. The polymerization reaction of the amide monomer may be carried out in a solvent in the presence of an esterification catalyst.

[0117] The amide monomer may have a main skeleton having an amide bond that has a hydroxyl group for forming an ester bond and a carboxyl group or an ester-forming derivative thereof, but it is preferable that the main skeleton has a hydroxyl group and a carboxyl group esterified with an alkyl group, in order to improve the molecular weight of the alternating copolymer. Examples of the alkyl group for esterifying the carboxyl group include C 1, C 2, C 3, C 4, C 5, C 6, C 7, C 8, C 9, C 10, C 11, C 12, C 13, C 14, C 15, C 16, C 17, C 18, C 19, C 20, C 21, C 22, C 23, C 24, C 25, C 36, C 26, C 37, C 28, C 38, C 29, C 39, C 40, C 50, C 61, C 72, C 83, C 94, C 105, C 116, C 22, C 23, C 24, C 25, C 38, C 25, C 39, C 41, C 25, C 26, C 37, C 28, C 38, C 29, C 39, C 41, C 25, C 16, C 21, C 22, C 23, C 24, C 25, C 37, C 25, C 38, C 26, C 39, C 18, C 25, C 37, C 26, C 38, C 27, C 28, C 39, C 19, C 21, C 22, C 23, C 24, C 25, C 26, C 27 1-4 Alkyl esters are preferred, C 1-3 Alkyl groups are more preferred, C 1-2 Alkyl groups are more preferred.

[0118] As the esterification catalyst, for example, a metal catalyst can be used. As the metal catalyst, for example, a metal compound containing an alkali metal such as sodium; an alkaline earth metal such as magnesium, calcium, barium; a transition metal such as titanium, manganese, cobalt; a metal of Group 12 of the periodic table such as zinc, cadmium; a metal of Group 13 of the periodic table such as aluminum; a metal of Group 14 of the periodic table such as germanium, tin, lead; a metal of Group 15 of the periodic table such as antimony, etc. can be used. As the metal compound, for example, alkoxide; an organic acid salt such as acetate, propionate, laurate; an inorganic acid salt such as borate, carbonate; an oxide, etc., or a hydrate thereof may be used. Examples of commonly used esterification catalysts include titanium-based catalysts such as tetrapropyl titanate, tetrabutyl titanate, and tetrastearyl titanate; tin-based catalysts such as dibutyltin dilaurate, dibutyltin dichloride, butyltin trichloride, and dibutyltin oxide; metal salts of alkylbenzenesulfonic acids such as sodium paratoluenesulfonate; alkylsulfonic acids such as methanesulfonic acid; cobalt hydroxide, manganese acetate, zinc oxide, and cobalt octylate.

[0119] These esterification catalysts can be used alone or in combination of two or more. Among these catalysts, tin-based catalysts are preferred from the viewpoint of improving the molecular weight of the alternating copolymer, and dialkyltin difatty acid esters such as dibutyltin diacetate, dibutyltin dipropionate, dibutyltin dioctate, and dibutyltin dilaurate are more preferred, and diC such as dibutyltin dilaurate are more preferred. 1-6 Alkyl tin di-C 8-16 Alkanoic acid esters are more preferred.

[0120] The proportion of the esterification catalyst may be 0.001 mol or more relative to 1 mol of the amide monomer, for example, 0.001 to 0.1 mol, preferably 0.003 to 0.05 mol, and more preferably 0.005 to 0.03 mol. If the proportion of the esterification catalyst is too small, there is a risk that the molecular weight of the alternating copolymer cannot be increased.

[0121] The polymerization reaction may be carried out in the presence of a stabilizer such as a heat stabilizer or an antioxidant, if necessary. Usually, a heat stabilizer is often used, and examples of the heat stabilizer include phosphorus compounds such as trimethyl phosphate, triethyl phosphate, triphenyl phosphate, dibutyl phosphate (dibutyl phosphate or dibutyl phosphate), phosphorous acid, trimethyl phosphite, and triethyl phosphite. Of these, dibutyl phosphate is often used. The amount of the heat stabilizer used is, for example, 0.001×10 per mole of the amide monomer. -3 ~10×10 -3 Molar, preferably 0.01 x 10 -3 ~5×10 -3 It is a mole.

[0122] The polymerization reaction may usually be carried out in an atmosphere of an inert gas, for example, nitrogen gas; or a rare gas such as helium or argon, and the ester exchange reaction may be carried out in an atmosphere of an inert gas such as nitrogen gas.

[0123] The polymerization reaction may be carried out under normal pressure or under reduced pressure. The reaction temperature can be selected depending on the polymerization method. For example, the reaction temperature in the melt polymerization method is 150 to 300°C, preferably 160 to 250°C, and more preferably 170 to 200°C.

[0124] The resulting alternating copolymer may be separated or purified by conventional methods. EXAMPLES

[0125] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The raw materials used are as follows, and the properties and evaluation of the obtained intermediate and polymer were measured as follows.

[0126] [Ingredients used] (R)3HB-OMe: (R)3HB methyl ester, manufactured by Tokyo Chemical Industry Co., Ltd. Gly-OMe-HCl: glycine methyl ester hydrochloride, manufactured by Tokyo Chemical Industry Co., Ltd. L-Ala-OMe-HCl: L-alanine methyl ester hydrochloride, manufactured by Tokyo Chemical Industry Co., Ltd. D-Ala-OMe-HCl: D-alanine methyl ester hydrochloride, manufactured by Tokyo Chemical Industry Co., Ltd. rac-Ala-OMe-HCl: rac-alanine methyl ester hydrochloride, manufactured by Tokyo Chemical Industry Co., Ltd. β-Ala-OMe-HCl: β-alanine methyl ester hydrochloride, manufactured by Tokyo Chemical Industry Co., Ltd. 6AH: 6-aminohexanoic acid, manufactured by Nacalai Tesque, Inc. TBSCl: t-butyldimethylchlorosilane, manufactured by Kanto Chemical Co., Ltd. EDCI·HCl: 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, manufactured by Tokyo Chemical Industry Co., Ltd. HOBt·H2O: 1-Hydroxybenzotriazole hydrate, manufactured by Tokyo Chemical Industry Co., Ltd.

[0127] [Biodegradability of monomers and polymers] The aerobic biodegradability (BOD; biodegradability) of the obtained monomers and polymers was measured in soil suspension at 25 ° C in accordance with ISO14851:2019, and in seawater at 30 ° C with reference to the measurement conditions in ASTM D6691-17. The soil suspension was prepared by suspending soil collected at the RIKEN (latitude 35 ° 46' 46.38 "N, longitude 139 ° 36' 52.308 "E) in pure water (0.1 g / mL) and filtering the filtrate. The seawater was collected from Hojo Beach, Tateyama City, Chiba Prefecture (latitude 35 ° 59' 49.794 "N, longitude 139 ° 51' 23.724 "E) and filtered to remove impurities. The aerobic biodegradability was calculated from the oxygen consumption measured using a BOD meter (WTW "OxiTop IDS").

[0128] [Polymer molecular weight] The number average molecular weight (Mn) of the obtained polymer was measured by gel permeation chromatography (flow rate 0.2 mL / min, eluent: 5 mM sodium trifluoroacetate / hexafluoroisopropanol, standard resin: polymethyl methacrylate) using a chromatography system ("ACQUITY Advanced Polymer Chromatography System" manufactured by Nihon Waters Co., Ltd.) and three types of separation columns ("ACQUITY APC XT BEH column 900 Å, 2.5 μm, 4.6 × 75 mm, 300K-2M" "ACQUITY APC XT BEH column 200 Å, 2.5 μm, 4.6 × 75 mm, 3K-70K" "ACQUITY APC XT BEH column 45 Å, 1.7 μm, 4.6 × 150 mm, 200K-5K" manufactured by Nihon Waters Co., Ltd.).

[0129] [Polymer glass transition temperature] The glass transition temperature (Tg) of the obtained polymer was measured using a dynamic viscoelasticity measuring device (DMA-8000 manufactured by PerkinElmer Japan Co., Ltd.) in a single cantilever mode using a stainless steel material pocket, with a frequency of 1 Hz, a strain of 0.05 mm, and a temperature rise rate of 2°C / min from -50 to 200°C.

[0130] [Polymer melting point] The melting point (Tm) of the obtained polymer was measured by heating the sample under conditions of a helium atmosphere, a measurement temperature of -50 to 200°C, and a heating rate of 10°C / min, using a differential scanning calorimeter (PerkinElmer Japan Co., Ltd., "DSC-8500"). From the obtained DSC chart (DSC curve), the peak top temperature of the endothermic peak due to melting was determined as the melting point.

[0131] [5% weight loss temperature of polymer] The 5% weight loss temperature (Td5%) of the polymer was measured using a simultaneous differential thermal / thermogravimetry analyzer (Hitachi High-Tech Science Corporation, "TG / DTA7200") in a nitrogen atmosphere by increasing the temperature from 30°C to 500°C at a heating rate of 10°C / min.

[0132] [Polymer crystallinity] The degree of crystallinity (Xc) of the obtained polymer was determined from the diffraction intensity by the Vonk method using an X-ray diffractometer (Rigaku Corporation, "RINT-2500"). The voltage was set to 40 kV and the current to 100 mA, and the radiation source used was Cu-Kα radiation with a wavelength of 0.154 nm. A silicon non-reflective sample plate was used, and measurements were made from 2θ of 4.0° to 60.0° at a scanning speed of 2.0° / min.

[0133] [Polymer NMR] The obtained polymer was dissolved in deuterated chloroform containing hexafluoroisopropanol (HFIP) or 2,2,2-trifluoroethanol (TFE) with tetramethylsilane (TMS) as an internal standard [CDCl3 / HFIP = 1 / 1 (volume ratio) or CDCl3 / TFE = 1 / 1 (volume ratio)], and analyzed by a nuclear magnetic resonance apparatus (Agilent Technologies, Inc., "Varian NMR System 500") 1 H-NMR spectrum and 13 C-NMR spectrum was measured.

[0134] In the present embodiment, the volume ratio refers to the volume ratio at a temperature of 20°C.

[0135] Example 1 (1) Preparation of hydroxycarboxylic acid derivatives (Protection step of hydroxyl group: synthesis of TBS-(R)3HB-OMe)

[0136] [ka]

[0137] As shown in the above formula, the first intermediate TBS-(R)3HB-OMe was synthesized. That is, under a nitrogen atmosphere, (R)3HB-OMe (25 mL, 224 mmol) was added to dimethylformamide DMF (450 mL), and the solution was cooled to 0°C. TBSCl (40.6 g, 269 mmol) and imidazole (36.7 g, 538 mmol) were added, and the mixture was warmed to room temperature and stirred for 24 hours. A saturated aqueous solution of ammonium chloride was added, and the mixture was extracted with diethyl ether. The organic layer was washed with saturated saline and dried over sodium sulfate. After distilling off the solvent under reduced pressure, the residue was purified by silica gel column chromatography (hexane:ethyl acetate = 19:1 (volume ratio)) to obtain TBS-(R)3HB-OMe (50.1 g, 96%) as a colorless liquid.

[0138] (Deprotection step of carboxyl group: synthesis of TBS-(R)3HB-OH)

[0139] [ka]

[0140] As shown in the above formula, the first intermediate, TBS-(R)3HB-OH, was synthesized. TBS-(R)3HB-OMe (50.0 g, 215 mmol) was dissolved in THF (645 mL) and water (323 mL) was added. The solution was cooled to 0°C, lithium hydroxide monohydrate (13.5 g, 323 mmol) was added, and the mixture was warmed to room temperature and stirred for 17 hours. The reaction mixture was concentrated under reduced pressure, neutralized with 1M hydrochloric acid, and extracted with diethyl ether. The organic layer was washed with saturated saline and dried over sodium sulfate. The solvent was removed under reduced pressure to obtain TBS-(R)3HB-OH (44.3 g, 94%) as a colorless liquid.

[0141] (2) Amidation process (Synthesis of TBS-(R)3HB-Gly-OMe)

[0142] [ka]

[0143] As shown in the above formula, the second intermediate, TBS-(R)3HB-Gly-OMe, was synthesized. That is, under a nitrogen atmosphere, TBS-(R)3HB-OH (10.9 g, 50 mmol), glycine methyl ester hydrochloride (6.9 g, 55 mmol), and HOBt·H2O (8.4 g, 55 mmol) were dissolved in dichloromethane (500 mL), and the solution was cooled to 0°C. EDCI·HCl (10.5 g, 55 mmol) and triethylamine Et3N (15.4 mL, 110 mmol) were added, and the mixture was warmed to room temperature and stirred for 20 hours. The dichloromethane layer was repeatedly washed with saturated aqueous sodium bicarbonate. The organic layer was washed with saturated aqueous ammonium chloride and saturated saline, and dried over sodium sulfate. The solvent was removed under reduced pressure, and the residue was purified by silica gel column chromatography (hexane:ethyl acetate=1:1 (volume ratio)) to obtain TBS-(R)3HB-Gly-OMe (13.0 g, 90%) as a colorless liquid.

[0144] (3) Deprotection step (Synthesis of (R)3HB-Gly-OMe)

[0145] [ka]

[0146] As shown in the above formula, R-3-hydroxybutanoylglycine methyl ester ((R)3HB-Gly-OMe), an amide monomer, was synthesized. That is, under a nitrogen atmosphere, TBS-(R)3HB-Gly-OMe (11.6 g, 40 mmol) was dissolved in dehydrated methanol (120 mL), and the solution was cooled to 0°C. Acetyl chloride AcCl (0.43 mL, 6.0 mmol) was added dropwise, and the mixture was stirred at 0°C for 3 hours. Triethylamine (0.85 mL, 6 mmol) was added to the reaction mixture, and the mixture was concentrated under reduced pressure. The residue was purified by silica gel column chromatography (ethyl acetate:methanol = 19:1 (volume ratio)) to obtain (R)3HB-Gly-OMe (6.6 g, 95%) as a white solid.

[0147] (4) Polymerization process (Synthesis of P[(R)3HB-alt-Gly])

[0148] [ka]

[0149] As shown in the above formula, P[(R)3HB-alt-Gly], an alternating copolymer (polymer) of (R)3HB and glycine, was synthesized. That is, under a nitrogen stream, 0.1 M dibutyltin dilaurate (DBTDL) toluene solution [0.2 mL, 2 mol% (0.02 mol ratio per 1 mol of (R)3HB-Gly-OMe)] was added to (R)3HB-Gly-OMe (175 mg, 1.0 mmol) and stirred at 180°C for 1 hour. The mixture was dissolved in trifluoroethanol and the solution was poured into acetone. The resulting precipitate was collected by filtration and dried under reduced pressure at 40°C to obtain the polymer P[(R)3HB-alt-Gly] (85 mg, 60%) as a white solid. The obtained polymer 1 H-NMR spectrum and 13The C-NMR spectra are shown in Figures 4 and 5, respectively. In the figures, lowercase alphabetical dashes indicate terminal structures.

[0150] In addition, "alt" in the abbreviations of the above polymers indicates that the polymers are alternating copolymers.

[0151] Example 2 (1) Amidation process (Synthesis of TBS-(R)3HB-L-Ala-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-OH (10.9 g, 50 mmol), L-alanine methyl ester hydrochloride (7.7 g, 55 mmol), and HOBt·H2O (8.4 g, 55 mmol) were dissolved in dichloromethane (500 mL) and the solution was cooled to 0°C. EDCI·HCl (10.5 g, 55 mmol) and triethylamine (15.4 mL, 110 mmol) were added, and the mixture was warmed to room temperature and stirred for 20 hours. A saturated aqueous solution of sodium bicarbonate was added to repeatedly wash the dichloromethane layer. The organic layer was washed with a saturated aqueous solution of ammonium chloride and saturated saline, and dried over sodium sulfate. After distilling off the solvent under reduced pressure, the residue was purified by silica gel column chromatography (hexane:ethyl acetate = 7:3 (volume ratio)) to obtain the second intermediate, TBS-(R)3HB-L-Ala-OMe (14.1 g, 93%) as a colorless liquid.

[0152] (2) Deprotection step (Synthesis of (R)3HB-L-Ala-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-L-Ala-OMe (12.1 g, 40 mmol) was dissolved in dehydrated methanol (120 mL), and the solution was cooled to 0°C. Acetyl chloride (0.43 mL, 6.0 mmol) was added dropwise, and the mixture was stirred at 0°C for 3 hours. Triethylamine (0.85 mL, 6 mmol) was added to the reaction mixture, which was then concentrated under reduced pressure. The residue was purified by silica gel column chromatography (ethyl acetate:methanol = 19:1 (volume ratio)) to obtain the third intermediate (monomer), R-3-hydroxybutanoyl L-alanine methyl ester ((R)3HB-L-Ala-OMe) (7.4 g, 98%) as a white solid.

[0153] (3) Polymerization process (Synthesis of P[(R)3HB-alt-L-Ala]) Under a nitrogen stream, (R)3HB-L-Ala-OMe (189 mg, 1.0 mmol) was added with 0.1 M dibutyltin dilaurate (DBTDL) toluene solution (0.2 mL, 2 mol%) and stirred at 180°C for 1 hour. The mixture was dissolved in trifluoroethanol, and the solution was poured into diethyl ether. The resulting precipitate was collected by filtration and dried under reduced pressure at 40°C to obtain P[(R)3HB-alt-L-Ala] (66 mg, 42%), which is an alternating copolymer (polymer) of (R)3HB and L-alanine, as a white solid. 1 H-NMR spectrum and 13 The C-NMR spectra are shown in Figures 6 and 7, respectively.

[0154] Example 3 (1) Amidation process (Synthesis of TBS-(R)3HB-D-Ala-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-OH (10.9 g, 50 mmol), D-alanine methyl ester hydrochloride (7.7 g, 55 mmol), and HOBt·H2O (8.4 g, 55 mmol) were dissolved in dichloromethane (500 mL) and the solution was cooled to 0°C. EDCI·HCl (10.5 g, 55 mmol) and triethylamine (15.4 mL, 110 mmol) were added, and the mixture was warmed to room temperature and stirred for 20 hours. A saturated aqueous solution of sodium bicarbonate was added to repeatedly wash the dichloromethane layer. The organic layer was washed with a saturated aqueous solution of ammonium chloride and saturated saline, and dried over sodium sulfate. After distilling off the solvent under reduced pressure, the residue was purified by silica gel column chromatography (hexane:ethyl acetate = 7:3 (volume ratio)) to obtain the second intermediate TBS-(R)3HB-D-Ala-OMe (14.0 g, 92%) as a white solid.

[0155] (2) Deprotection step (Synthesis of (R)3HB-D-Ala-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-D-Ala-OMe (12.1 g, 40 mmol) was dissolved in dehydrated methanol (120 mL), and the solution was cooled to 0°C. Acetyl chloride (0.43 mL, 6.0 mmol) was added dropwise, and the mixture was stirred at 0°C for 3 hours. Triethylamine (0.85 mL, 6 mmol) was added to the reaction mixture, which was then concentrated under reduced pressure. The residue was purified by silica gel column chromatography (ethyl acetate:methanol = 19:1 (volume ratio)) to obtain the third intermediate (monomer), R-3-hydroxybutanoyl D-alanine methyl ester ((R)3HB-D-Ala-OMe) (7.5 g, 98%) as a white solid.

[0156] (3) Polymerization process (Synthesis of P[(R)3HB-alt-D-Ala]) Under a nitrogen stream, (R)3HB-D-Ala-OMe (189 mg, 1.0 mmol) was added with a 0.1 M dibutyltin dilaurate (DBTDL) toluene solution (0.2 mL, 2 mol%) and stirred at 180°C for 1 hour. The mixture was dissolved in trifluoroethanol, and the solution was poured into acetone. The resulting precipitate was collected by filtration and dried under reduced pressure at 40°C to obtain P[(R)3HB-alt-D-Ala] (82 mg, 52%), an alternating copolymer (polymer) of (R)3HB and D-alanine, as a white solid. 1 H-NMR spectrum and 13 The C-NMR spectra are shown in Figures 8 and 9, respectively.

[0157] Example 4 (1) Amidation process (Synthesis of TBS-(R)3HB-rac-Ala-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-OH (10.9 g, 50 mmol), rac-alanine methyl ester hydrochloride (7.7 g, 55 mmol), and HOBt·HO (8.4 g, 55 mmol) were dissolved in dichloromethane (500 mL) and the solution was cooled to 0°C. EDCI·HCl (10.5 g, 55 mmol) and triethylamine (15.4 mL, 110 mmol) were added, and the mixture was warmed to room temperature and stirred for 20 hours. The dichloromethane layer was repeatedly washed with a saturated aqueous solution of sodium bicarbonate. The organic layer was washed with a saturated aqueous solution of ammonium chloride and saturated saline, and dried over sodium sulfate. After distilling off the solvent under reduced pressure, the residue was purified by silica gel column chromatography (hexane:ethyl acetate = 7:3 (volume ratio)) to obtain the second intermediate, TBS-(R)3HB-rac-Ala-OMe (14.1 g, 93%) as a colorless liquid.

[0158] In addition, "rac" in the abbreviation of the second intermediate indicates that it is a racemic mixture.

[0159] (2) Deprotection step (Synthesis of (R)3HB-rac-Ala-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-rac-Ala-OMe (12.1 g, 40 mmol) was dissolved in dehydrated methanol (120 mL), and the solution was cooled to 0°C. Acetyl chloride (0.43 mL, 6.0 mmol) was added dropwise, and the mixture was stirred at 0°C for 3 hours. Triethylamine (0.85 mL, 6 mmol) was added to the reaction mixture, which was then concentrated under reduced pressure. The residue was purified by silica gel column chromatography (ethyl acetate:methanol = 19:1 (volume ratio)) to obtain the third intermediate (monomer), R-3-hydroxybutanoyl-rac-alanine methyl ester ((R)3HB-rac-Ala-OMe) (7.1 g, 94%) as a colorless liquid.

[0160] (3) Polymerization process (Synthesis of P[(R)3HB-alt-rac-Ala]) Under a nitrogen stream, (R)3HB-rac-Ala-OMe (189 mg, 1.0 mmol) was added with a 0.1 M dibutyltin dilaurate (DBTDL) toluene solution (0.2 mL, 2 mol%) and stirred at 180°C for 1 hour. The mixture was dissolved in trifluoroethanol, and the solution was poured into diethyl ether. The resulting precipitate was collected by filtration and dried under reduced pressure at 40°C to obtain P[(R)3HB-alt-rac-Ala] (71 mg, 45%), which is an alternating copolymer (polymer) of (R)3HB and rac-alanine, as a white solid. 1 H-NMR spectrum and 13 The C-NMR spectra are shown in Figures 10 and 11, respectively.

[0161] Example 5 (1) Amidation process (Synthesis of TBS-(R)3HB-β-Ala-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-OH (10.9 g, 50 mmol), β-alanine methyl ester hydrochloride (7.7 g, 55 mmol), and HOBt·H2O (8.4 g, 55 mmol) were dissolved in dichloromethane (500 mL) and the solution was cooled to 0°C. EDCI·HCl (10.5 g, 55 mmol) and triethylamine (15.4 mL, 110 mmol) were added, and the mixture was warmed to room temperature and stirred for 20 hours. A saturated aqueous solution of sodium bicarbonate was added to repeatedly wash the dichloromethane layer. The organic layer was washed with a saturated aqueous solution of ammonium chloride and saturated saline, and dried over sodium sulfate. After distilling off the solvent under reduced pressure, the residue was purified by silica gel column chromatography (hexane:ethyl acetate = 1:1 (volume ratio)) to obtain the second intermediate, TBS-(R)3HB-β-Ala-OMe (13.7 g, 90%) as a colorless liquid.

[0162] (2) Deprotection step (Synthesis of (R)3HB-β-Ala-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-β-Ala-OMe (12.1 g, 40 mmol) was dissolved in dehydrated methanol (120 mL), and the solution was cooled to 0°C. Acetyl chloride (0.43 mL, 6.0 mmol) was added dropwise, and the mixture was stirred at 0°C for 3 hours. Triethylamine (0.85 mL, 6 mmol) was added to the reaction mixture, which was then concentrated under reduced pressure. The residue was purified by silica gel column chromatography (ethyl acetate:methanol = 19:1 (volume ratio)) to obtain the third intermediate (monomer), R-3-hydroxybutanoyl β-alanine methyl ester ((R)3HB-β-Ala-OMe) (7.4 g, 98%) as a white solid.

[0163] (3) Polymerization process (Synthesis of P[(R)3HB-alt-β-Ala]) Under a nitrogen stream, (R)3HB-β-Ala-OMe (189 mg, 1.0 mmol) was added with 0.1 M dibutyltin dilaurate (DBTDL) toluene solution (0.2 mL, 2 mol%) and stirred at 180°C for 1 hour. The mixture was dissolved in trifluoroethanol and the solution was poured into acetone. The resulting precipitate was collected by filtration and dried under reduced pressure at 40°C to obtain P[(R)3HB-alt-β-Ala] (65 mg, 41%), which is an alternating copolymer (polymer) of (R)3HB and β-alanine, as a white solid. 1 H-NMR spectrum and 13 The C-NMR spectra are shown in Figures 12 and 13, respectively.

[0164] Example 6 (1) Preparation of amino acid derivatives (Synthesis of 6AH-OMe HCl) Dehydrated methanol (300 mL) was cooled to 0°C under a nitrogen atmosphere. Acetyl chloride (12.8 mL, 180 mmol) was added dropwise and stirred at 0°C for 15 minutes. 6-Aminohexanoic acid (7.9 g, 60 mmol) was added, and the mixture was warmed to room temperature and stirred for 1 hour, and then refluxed for 15 hours. The solution cooled to room temperature was concentrated under reduced pressure, and the residue was dissolved in methanol and added dropwise to cold diethyl ether. The resulting precipitate was filtered, washed with diethyl ether, and collected to obtain 6-aminohexanoic acid methyl ester hydrochloride (6AH-OMe·HCl) (10.3 g, 94%) as a white solid.

[0165] (2) Amidation process (Synthesis of TBS-(R)3HB-6AH-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-OH (10.9 g, 50 mmol), 6AH-OMe·HCl (10.0 g, 55 mmol), and HOBt·HO (8.4 g, 55 mmol) were dissolved in dichloromethane (500 mL), and the solution was cooled to 0°C. EDCI·HCl (10.5 g, 55 mmol) and triethylamine (15.4 mL, 110 mmol) were added, and the mixture was warmed to room temperature and stirred for 20 hours. A saturated aqueous solution of sodium bicarbonate was added to repeatedly wash the dichloromethane layer. The organic layer was washed with a saturated aqueous solution of ammonium chloride and saturated saline, and dried over sodium sulfate. After distilling off the solvent under reduced pressure, the residue was purified by silica gel column chromatography (hexane:ethyl acetate = 7:3 (volume ratio)) to obtain the second intermediate, TBS-(R)3HB-6AH-OMe (16.6 g, 96%), as a colorless liquid.

[0166] (3) Deprotection step (Synthesis of (R)3HB-6AH-OMe) Under a nitrogen atmosphere, TBS-(R)3HB-6AH-OMe (13.8 g, 40 mmol) was dissolved in dehydrated methanol (120 mL), and the solution was cooled to 0°C. Acetyl chloride (0.43 mL, 6.0 mmol) was added dropwise, and the mixture was stirred at 0°C for 3 hours. Triethylamine (0.85 mL, 6 mmol) was added to the reaction mixture, which was then concentrated under reduced pressure. The residue was purified by silica gel column chromatography (ethyl acetate:methanol = 19:1 volume ratio) to obtain the third intermediate, R-3-hydroxybutanoyl 6-aminohexanoic acid methyl ester ((R)3HB-6AH-OMe) (9.0 g, 98%), as a white solid.

[0167] (4) Polymerization process (Synthesis of P[(R)3HB-alt-6AH]) Under a nitrogen stream, (R)3HB-6AH-OMe (231 mg, 1.0 mmol) was added with a 0.1 M dibutyltin dilaurate (DBTDL) toluene solution (0.2 mL, 2 mol%) and stirred at 180°C for 1 hour. The mixture was dissolved in trifluoroethanol, and the solution was poured into acetone. The resulting precipitate was collected by filtration and dried under reduced pressure at 40°C to obtain P[(R)3HB-alt-6AH] (93 mg, 46%), which is an alternating copolymer (polymer) of (R)3HB and 6-aminohexanoic acid, as a white solid. 1 H-NMR spectrum and 13 The C-NMR spectra are shown in Figures 14 and 15, respectively.

[0168] The results of evaluating the biodegradability in seawater of the monomers (third intermediates) obtained in Examples 1 to 5 are shown in the graph of Figure 1. As is clear from the results in Figure 1, all of the monomers showed high biodegradability. Among them, the monomers of Examples 1 and 2 showed particularly high biodegradability.

[0169] The results of evaluating the various physical properties of the polymers obtained in Examples 1 to 6 are shown in Table 1. For comparison, the results of the homopolymer of (R)3HB (P[(R)3HB]) and poly-L-lactic acid (PLLA) are also shown as Reference Examples 1 and 2. In Table 1, "nd" indicates that not detected.

[0170] [Table 1]

[0171] As is clear from the results in Table 1, the polymers of Examples 1 to 6 had high number average molecular weights and high glass transition temperatures, and therefore had excellent heat resistance and moldability. Among them, the polymers of Examples 1 to 2 and 4 were well-balanced.

[0172] Incidentally, no melting point Tm was detected in the polymers of Examples 2 to 4. Moreover, in the polymer obtained in Example 4, no diffraction peak of a crystalline substance was detected.

[0173] The results of evaluating the biodegradability in soil suspension of the polymers obtained in Examples 1 and 2 are shown in the graph of Figure 2. As is clear from the results in Figure 2, all of the polymers showed high biodegradability.

[0174] The results of evaluating the biodegradability in seawater of the polymers obtained in Examples 1 and 2 are shown in the graph of Figure 3. As is clear from the results in Figure 3, all of the polymers showed high biodegradability. [Industrial Applicability]

[0175] The biodegradable resin of the present invention has high biodegradability and can be used in various fields, such as paints, antistatic agents, inks, adhesives, pressure sensitive adhesives, electric and electronic materials (e.g., carrier transport agents, luminescent bodies, organic photoreceptors, etc.), electric and electronic parts or devices (e.g., optical lenses, optical films, optical disks, inkjet printers, digital paper, organic semiconductor lasers, dye-sensitized solar cells, etc.), mechanical parts or devices (e.g., automobiles, aviation and space materials, sensors, etc.). In particular, since the biodegradable resin has high mechanical properties, it can be easily molded by extrusion molding, injection molding, etc., and can be suitably used for molded members in various fields (e.g., molded bodies such as casings and housings), containers (containers for food, daily necessities, electrical and electronic devices and parts, etc.), packaging materials such as films and sheets, and garbage bags. In addition, the problem of microplastics (especially microplastics in the ocean), which has become a new problem in recent years, can also be solved by taking advantage of the high biodegradability. In addition, since the biodegradable resin of the present invention contains a skeleton derived from 3HB and has biocompatibility, it can also be used in the medical field (e.g., medical devices, etc.).

Claims

1. A biodegradable resin comprising an alternating copolymer of hydroxycarboxylic acid units and amino acid units, said hydroxycarboxylic acid units including 3-hydroxybutyric acid units.

2. 2. The biodegradable resin according to claim 1, wherein the 3-hydroxybutyric acid unit is a unit derived from R-3-hydroxybutyric acid.

3. 3. The biodegradable resin according to claim 1, wherein the alternating copolymer has a repeating unit represented by the following formula (1): [Formula 1] (In the formula, R represents a hydrogen atom or an alkyl group, and n represents an integer of 0 or more.)

4. In the formula (1), R is a hydrogen atom or C 1-3 4. The biodegradable resin according to claim 3, wherein n is an alkyl group and n is an integer of 0 to 6.

5. 4. The biodegradable resin according to claim 3, wherein in said formula (1), R is a hydrogen atom or a methyl group, and n is 0.

6. 3. The biodegradable resin according to claim 1, wherein the amino acid unit is an amino acid unit derived from an L-amino acid.

7. 3. The biodegradable resin according to claim 1, wherein the amino acid unit is an amino acid unit derived from an α-amino acid.

8. 3. The biodegradable resin according to claim 1, wherein the alternating copolymer has a number average molecular weight of 5,000 or more.

9. 3. The biodegradable resin according to claim 1, wherein the alternating copolymer has a glass transition temperature of 50° C. or higher.

10. 3. The biodegradable resin according to claim 1, which has marine biodegradability.

11. a monomer synthesis step of reacting a hydroxycarboxylic acid component with an amino acid component to obtain an amide monomer; and a polymerization step of polymerizing the amide monomer to obtain an alternating copolymer of a hydroxycarboxylic acid unit and an amino acid unit. A method for producing the biodegradable resin according to claim 1 or 2.

12. In the monomer synthesis step, At least one of the hydroxycarboxylic acid component and the amino acid component is a derivative, the derivative in the hydroxycarboxylic acid component is a derivative of a hydroxycarboxylic acid in which a hydroxyl group of the hydroxycarboxylic acid is protected with a protecting group, The method according to claim 11, wherein the derivative in the amino acid component is an amino acid derivative in which the carboxyl group of the amino acid is protected with a protecting group.

13. The method according to claim 11, wherein in the polymerization step, the amide monomer has a carboxyl group esterified with an alkyl group.

14. The method according to claim 11, wherein in the polymerization step, the amide monomer is polymerized in the presence of a tin catalyst.

Citation Information

Patent Citations

  • Polyester elastomer molded article

    JP1981041249A

  • Polylactic acid block copolymer having amide bond

    JP1999302374A

  • Lactic-acid-based biodegradable polymer

    JP2001031762A

  • Biodegradable copolymer and production process therefor as well as biodegradability improvement method

    JP2017025138A

  • Polyester amide compound

    US20130023642A1

Cited By

  • Degradable hemp tree powder material

    CN121873439A