Aqueous resin composition for heat-resistant layer of lithium-ion secondary battery separator

The use of an aqueous resin composition with specific acrylic polymers addresses the heat shrinkage and electrolyte solubility challenges of lithium-ion battery separators, enhancing safety by reducing short circuit risks.

JP2024135742AActive Publication Date: 2024-10-04DIC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023046585
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Existing lithium-ion secondary battery separators face challenges in maintaining heat shrinkage resistance and electrolyte solubility resistance, particularly under high-temperature conditions, leading to potential short circuits and safety risks.

Method used

An aqueous resin composition containing specific acrylic polymers, such as (meth)acrylamide and N-methylol (meth)acrylamide, is used to form a heat-resistant layer for the separator, enhancing its heat shrinkage resistance and electrolyte solubility.

Benefits of technology

The composition provides a separator with excellent heat shrinkage resistance and electrolyte solubility, reducing the risk of short circuits and improving safety under high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135742000001
    Figure 2024135742000001
Patent Text Reader

Abstract

To provide an aqueous resin composition for a heat-resistant layer of a lithium-ion secondary battery separator, which provides a separator with excellent resistance to heat shrinkage and electrolyte solubility.SOLUTION: An aqueous resin composition for a heat-resistant layer of a lithium-ion secondary battery separator includes an acrylic polymer (A) whose essential raw materials are (meth)acrylamide and N-methylol (meth)acrylamide, and an aqueous medium (B) in which the monomer raw material of the acrylic polymer (A) contains 90 to 99.5 mass% of (meth)acrylamide and 0.5 to 5 mass% of N-methylol (meth)acrylamide.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous resin composition for a heat-resistant layer of a separator for a lithium ion secondary battery. [Background technology]

[0002] Polyolefin porous membranes exhibit excellent electrical insulation and ion permeability, and are therefore widely used as separators in batteries, capacitors, etc. In particular, in recent years, as portable devices have become more multifunctional and lighter in weight, lithium ion secondary batteries with high output density and high capacity density have come to be used as their power sources, and polyolefin porous membranes are mainly used as separators for such batteries.

[0003] Lithium-ion secondary batteries have high power density and capacity density, but because they use organic solvents in the electrolyte, the electrolyte can decompose due to heat generated by abnormal events such as short circuits and overcharging, and in the worst case, can even catch fire. To prevent such events, lithium-ion secondary batteries have several built-in safety features, one of which is the separator shutdown feature. When the battery generates abnormal heat, the micropores in the separator are blocked by thermal melting, suppressing ionic conduction in the electrolyte and stopping the progress of the electrochemical reaction. In general, the lower the shutdown temperature, the higher the safety. One of the reasons why polyethylene is used as a separator component is that it has a moderate shutdown temperature.

[0004] However, in high-energy batteries, even if the electrochemical reaction is stopped by shutting down the battery, the temperature inside the battery continues to rise, resulting in the separator shrinking due to heat and rupturing, causing a short circuit between the two electrodes.

[0005] For the purpose of producing a highly safe battery, a technique has been proposed in which a separator is formed by laminating a heat-resistant layer on a first porous layer mainly composed of a thermoplastic resin (see, for example, Patent Document 1).

[0006] However, as the capacity of batteries has been increased, high-capacity batteries tend to generate a large amount of heat during abnormal heating and are prone to being exposed to higher temperature environments. Although the separator described in this publication is considered to be safer than a normal separator that does not have a heat-resistant layer, there is still room for improvement in terms of suppressing the thermal contraction of the separator even in a high-temperature environment and reducing the risk of short-circuiting between the two electrodes due to the separator rupture.

[0007] In response to this, an aqueous binder solution for lithium ion batteries has been proposed, which contains a water-soluble trihydroxysilyl group-containing poly(meth)acrylamide, which is a polymer of monomer groups containing 60 mol % or more of a (meth)acrylamide group-containing compound and 0.05 to 0.80 mol % of a double bond-containing trihydroxysilyl compound having a vinyl group or a (meth)acryloxy group, per 100 mol of monomer groups (see Patent Document 2).

[0008] This aqueous solution was able to suppress the thermal shrinkage of the separator at 150°C, and also had relatively good adhesion to the substrate and rate characteristics. However, in recent years, there has been a demand for even stricter heat resistance conditions (180°C), and this solution was not able to meet these demands. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 3756815 [Patent Document 2] Patent No. 7027955 Summary of the Invention [Problem to be solved by the invention]

[0010] The problem to be solved by the present invention is to provide an aqueous resin composition for a heat-resistant layer of a separator for a lithium ion secondary battery, which can provide a separator having excellent heat shrinkage resistance and resistance to solubility in an electrolyte. [Means for solving the problem]

[0011] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by using an aqueous resin composition containing a specific acrylic polymer and an aqueous medium, thereby completing the present invention.

[0012] That is, the present invention relates to an aqueous resin composition for a heat-resistant layer of a separator for a lithium ion secondary battery, which contains an acrylic polymer (A) having (meth)acrylamide and N-methylol(meth)acrylamide as essential raw materials, and an aqueous medium (B), characterized in that the monomer raw materials for the acrylic polymer (A) contain 90 to 99 mass% (meth)acrylamide and 0.5 to 5 mass% N-methylol(meth)acrylamide. Effect of the Invention

[0013] Since the aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator of the present invention can provide a separator excellent in heat shrinkage resistance and electrolyte solubility resistance, it can be suitably used as a binder for the heat-resistant layer of a lithium ion secondary battery separator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator of the present invention contains an acrylic polymer (A) having (meth)acrylamide and N-methylol(meth)acrylamide as essential raw materials, and an aqueous medium (B), in which the monomer raw materials of the acrylic polymer (A) contain 90 to 99 mass % of (meth)acrylamide and 0.5 to 5 mass % of N-methylol(meth)acrylamide.

[0015] In the present invention, "(meth)acrylamide" refers to either or both of acrylamide and methacrylamide, "(meth)acrylate" refers to either or both of acrylate and methacrylate, "(meth)acrylic acid" refers to either or both of acrylic acid and methacrylic acid, and "(meth)acryloyl" refers to either or both of acryloyl and methacryloyl.

[0016] The (meth)acrylamide content in the monomer raw material of the acrylic polymer (A) is 90 to 999.5 mass %, and from the viewpoint of further improving the heat shrinkage resistance and the resistance to solubility in an electrolyte, the content is preferably 93 to 99.5 mass %, and more preferably 95 to 99.5 mass %.

[0017] The content of N-methylol (meth)acrylamide in the monomer raw material of the acrylic polymer (A) is 0.5 to 5% by mass, and preferably 0.5 to 3% by mass in order to further improve the heat shrinkage resistance and the resistance to solubility in an electrolyte.

[0018] The acrylic polymer (A) is essentially made of (meth)acrylamide and N-methylol (meth)acrylamide, but may also use other monomers as monomer raw materials.

[0019] Examples of the other monomers include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate; unsaturated monocarboxylic acids such as (meth)acrylic acid and crotonic acid; and anhydrides. Monomers having a carboxyl group, such as unsaturated dicarboxylic acids, such as maleic acid, maleic anhydride, itaconic acid, and fumaric acid; 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate Monomers having a hydroxyl group, such as N-(2-hydroxyethyl)(meth)acrylamide, glycerin mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, and lactone-modified (meth)acrylates having a hydroxyl group at the end; (meth)acrylates having an amino group, such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, and N,N-diethylaminopropyl (meth)acrylate; monomers having a nitrogen atom, such as monomers having an N-hydroxymethylamide group, such as (meth)acrylamide, and monomers having an N-alkoxymethylamide group, such as N-butoxymethylacrylamide; (meth)acrylates having a glycidyl group, such as glycidyl (meth)acrylate;Examples of the monomer include monomers having an alkoxysilyl group such as vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropyltriethoxysilane, and 3-(meth)acryloyloxypropylmethyldimethoxysilane; polyalkylene glycol (meth)acrylates such as polyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, polybutylene glycol (meth)acrylate, and methoxypolybutylene glycol (meth)acrylate; vinyl monomers such as styrene, α-methylstyrene, paramethylstyrene, chloromethylstyrene, and vinyl acetate; tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate; and di(meth)acrylates such as ethylene glycol di(meth)acrylate and propylene glycol di(meth)acrylate. These monomers can be used alone or in combination of two or more kinds.

[0020] The content of the other monomers in the monomer raw materials of the acrylic polymer (A) is preferably less than 5% by mass.

[0021] The acrylic polymer (A) can be produced by various methods, but the underwater polymerization method is preferred because the acrylic polymer (A) can be easily obtained.

[0022] Examples of the method for obtaining the acrylic polymer (A) by the underwater polymerization method include a method in which the monomer (a1) and the like, which are raw materials for the acrylic polymer (A), are radically polymerized in an aqueous medium in the presence of a polymerization initiator at a temperature of 50 to 100°C.

[0023] Examples of the polymerization initiator include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), and azobiscyanovaleric acid; organic peroxides such as tert-butyl peroxypivalate, tert-butyl peroxybenzoate, tert-butylperoxy-2-ethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, benzoyl peroxide, and tert-butyl hydroperoxide; and inorganic peroxides such as hydrogen peroxide, ammonium persulfate, potassium persulfate, and sodium persulfate. These polymerization initiators can be used alone or in combination of two or more.

[0024] The amount of the polymerization initiator in the raw material of the acrylic polymer (A) is preferably 0.2 parts by mass or less, more preferably 0.02 to 0.18 parts by mass, and more preferably 0.05 to 0.15 parts by mass, relative to 100 parts by mass of the monomer, in order to further improve the heat shrinkage resistance and the resistance to solubility in an electrolyte solution.

[0025] The aqueous medium (B) may be water, an organic solvent miscible with water, or a mixture thereof. Examples of the organic solvent miscible with water include alcohols such as methanol, ethanol, n-propanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; polyalkylene glycols such as ethylene glycol, diethylene glycol, and propylene glycol; alkyl ethers of polyalkylene glycols; and lactams such as N-methyl-2-pyrrolidone. In the present invention, only water may be used, or a mixture of water and an organic solvent miscible with water may be used, or only an organic solvent miscible with water may be used. From the viewpoint of safety and environmental load, only water or a mixture of water and an organic solvent miscible with water is preferred, and only water is particularly preferred.

[0026] As the aqueous medium (B), it is simple and preferable to use the aqueous medium used when producing the acrylic polymer (A) by an underwater polymerization method or the like as it is.

[0027] Furthermore, by carrying out a solvent removal step as necessary, the amount of organic solvent in the resin composition of the present invention can be reduced.

[0028] The aqueous resin composition of the present invention obtained by the above method preferably contains the acrylic polymer (A) in an amount of 3 to 30 mass %, more preferably 5 to 10 mass %, based on the total amount of the aqueous resin composition, since this further improves coating workability.

[0029] In addition, the aqueous resin composition of the present invention preferably contains the aqueous medium (B) in an amount of 97 to 70 mass %, more preferably 95 to 90 mass %, based on the total amount of the aqueous resin composition, since this further improves coating workability.

[0030] The aqueous resin composition of the present invention may contain, as necessary, additives such as a curing agent, a curing catalyst, a lubricant, a filler, a thixotropic agent, a tackifier, a wax, a heat stabilizer, a light resistance stabilizer, a fluorescent whitening agent, a foaming agent, a pH adjuster, a leveling agent, a gelling inhibitor, a dispersion stabilizer, an antioxidant, a radical scavenger, a heat resistance imparting agent, an inorganic filler, an organic filler, a plasticizer, a reinforcing agent, a catalyst, an antibacterial agent, a mildew inhibitor, a rust inhibitor, a thermoplastic resin, a thermosetting resin, a pigment, a dye, an electrical conductivity imparting agent, an antistatic agent, a moisture permeability improving agent, a water repellent, an oil repellent, a hollow foam, a compound containing crystal water, a flame retardant, a water absorbing agent, a moisture absorbing agent, a deodorizer, a foam stabilizer, an antifoaming agent, an antifungal agent, an antiseptic, an anti-algae agent, a pigment dispersant, an antiblocking agent, an antihydrolysis agent, and a pigment.

[0031] The aqueous resin composition of the present invention can provide a separator having excellent heat shrinkage resistance and electrolyte solubility resistance, and therefore can be suitably used as a binder for the heat-resistant layer of a lithium ion secondary battery.

[0032] By adding an inorganic filler to the aqueous resin composition of the present invention, a heat-resistant layer having excellent heat resistance can be obtained.

[0033] Examples of the inorganic filler that can be used include oxides such as silica, alumina, titania, zirconia, magnesia, zinc oxide, and iron oxide, nitrides such as silicon nitride, titanium nitride, and boron nitride, silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, aluminum hydroxide, aluminum oxide hydroxide, potassium titanate, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, silica sand, and calcined kaolin. Among these, it is preferable to use calcined kaolin or alumina in order to form a heat-resistant layer with even better heat resistance.

[0034] It is preferable to use the inorganic filler and the aqueous resin composition of the present invention in a solid content mass ratio in the range of 1 / 1,000 to 1 / 5 in order to form a separator having communicating pores sufficient to conduct ions and having excellent heat resistance. EXAMPLES

[0035] The present invention will now be described in more detail with reference to specific examples.

[0036] Example 1 In a 2.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blower, 1000.0 parts by mass of ion-exchanged water was charged and heated to 70°C, and then a mixture of 97.0 parts by mass of acrylamide, 1.0 parts by mass of itaconic acid, 2.0 parts by mass of N-methylol acrylamide, 0.1 parts by mass of ammonium persulfate, and 200.0 parts by mass of ion-exchanged water was added dropwise over 3 hours. After 3 hours had elapsed since the end of the dropwise addition, the mixture was cooled. The non-volatile content of the resulting aqueous resin composition (1) was 7.8% by mass, and the viscosity was 5500 mPa s.

[0037] [Preparation of heat-resistant layer slurry] While stirring at 5,000 rpm with a homodisper, 37.3 parts by mass of the aqueous resin composition (1) synthesized above and 117.3 parts by mass of ion-exchanged water were gradually added with 100 parts by mass of alumina ("AKP-3000" manufactured by Sumitomo Chemical Co., Ltd.). Dispersion was carried out for 15 minutes to prepare a heat-resistant layer slurry (1).

[0038] Example 2 In a 2.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blower, 1000.0 parts by mass of ion-exchanged water was charged and heated to 70°C, and then a mixture of 99.0 parts by mass of acrylamide, 1.0 part by mass of N-methylol acrylamide, 0.1 parts by mass of ammonium persulfate, and 200.0 parts by mass of ion-exchanged water was added dropwise over 3 hours. After 3 hours had elapsed since the completion of the dropwise addition, the mixture was cooled. The non-volatile content of the resulting aqueous resin composition (2) was 7.7% by mass, and the viscosity was 3500 mPa s.

[0039] [Preparation of heat-resistant layer slurry] While stirring at 5,000 rpm with a homodisper, 37.8 parts by mass of the aqueous resin composition (2) synthesized above and 116.7 parts by mass of ion-exchanged water were gradually added with 100 parts by mass of alumina (AKP-3000 manufactured by Sumitomo Chemical Co., Ltd.). Dispersion was carried out for 15 minutes to prepare a heat-resistant layer slurry (2).

[0040] (Comparative Example 1: Synthesis and Evaluation of Aqueous Resin Composition (R1) for Heat-Resistant Layer of Lithium-Ion Secondary Battery Separator) A reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube was charged with 100 g of ion-exchanged water, 0.42 g (0.0028 mol) of vinyltrimethoxysilane ("KBM-1003" manufactured by Shin-Etsu Chemical Co., Ltd.), 1.23 g of nitric acid, and 1.00 g of methanol, and the reaction was carried out at 25°C for 0.5 hours to obtain a homogeneous aqueous solution containing a double bond-containing trihydroxysilyl compound. In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, 1011 g of ion-exchanged water, 400 g (2.81 mol) of 50% acrylamide aqueous solution, and 0.223 g (0.0014 mol) of sodium methallylsulfonate were placed. Next, the double bond-containing trihydroxysilyl compound obtained above was added to the system. At that time, the pH was 2.2. After removing oxygen from the reaction system through nitrogen gas, the temperature was raised to 50°C. 2.0 g of 2,2'-azobis-2-amidinopropane dihydrochloride ("NC-32" manufactured by Nippoh Chemical Co., Ltd.) and 30 g of ion-exchanged water were added, and the temperature was raised to 80°C and the reaction was carried out for 3.0 hours. An aqueous solution containing water-soluble trihydroxysilyl group-containing poly(meth)acrylamide with a non-volatile content of 13.1% and a viscosity (25°C) of 24,000 mPa·s was obtained.

[0041] [Preparation of heat-resistant layer slurry] While stirring at 5,000 rpm with a homodisper, 100 parts by mass of 1% by mass carboxymethylcellulose (Daicel Chemical Industries, Ltd., "DN-800H") was gradually added to 100 parts by mass of alumina (Sumitomo Chemical Industries, Ltd., "AKP-50") to carry out dispersion. After these were uniformly mixed, 68.7 parts by mass of the aqueous resin composition (R1) synthesized above and 256.3 parts by mass of ion-exchanged water were added and mixed uniformly to prepare a heat-resistant layer slurry (R1).

[0042] [Preparation of separator with heat-resistant layer] The heat-resistant layer slurry obtained above was applied to both sides of a 12 μm-thick polyethylene separator substrate using a bar coater so that the film thickness after drying would be 4 μm, to obtain a separator having a heat-resistant layer. The drying temperature was 60° C. and the drying time was 5 minutes.

[0043] [Evaluation of heat shrink resistance] The separator with the heat-resistant layer prepared above was cut into 5 cm squares, and placed between thick paper in a hot air dryer at 180°C for 1 hour to carry out a heat resistance test. After the test, the length and width of the separator were measured, and the shrinkage rate in the vertical direction (MD shrinkage rate (%)) and the shrinkage rate in the horizontal direction (TD shrinkage rate (%)) were calculated to evaluate the heat shrinkage resistance. Shrinkage rate (%) = separator length after test / separator length before test × 100 (%)

[0044] [Evaluation of resistance to electrolyte dissolution] A coating having a thickness of 150 μm was prepared from the aqueous resin composition obtained above, and the coating was immersed in an electrolyte solvent (ethylene carbonate / diethyl carbonate / ethyl methyl carbonate=40 / 20 / 40 (mass ratio)) at 60° C. for 72 hours, and then removed. The gel fraction and expansion rate (weight conversion) of the coating were calculated to evaluate the electrolyte solubility resistance. The higher the gel fraction, the better the resistance to solubility in an electrolyte solution, and the lower the expansion coefficient, the better the resistance to solubility in an electrolyte solution. Gel fraction (%) = weight of film after drying after immersion / weight of film before immersion × 100 Expansion rate (%) = (coating weight after immersion - coating weight before immersion) / coating weight before immersion × 100

[0045] The evaluation results of Examples 1 and 2 and Comparative Example 1 are shown in Table 1.

[0046] [Table 1]

[0047] It was confirmed that the heat-resistant layers obtained from the aqueous resin compositions of Examples 1 and 2 of the present invention were excellent in heat shrinkage resistance and resistance to solubility in an electrolyte solution.

[0048] On the other hand, in Comparative Example 1, acrylamide was used as the monomer raw material for the acrylic polymer (A) in an amount greater than the upper limit of the present invention, and N-methylol(meth)acrylamide was not used. It was confirmed that the heat-resistant layer obtained had poor heat shrinkage resistance and electrolyte solubility resistance.

Claims

1. The aqueous resin composition for a heat-resistant layer of a separator for a lithium ion secondary battery contains an acrylic polymer (A) having (meth)acrylamide and N-methylol(meth)acrylamide as essential raw materials, and an aqueous medium (B), wherein the monomer raw materials for the acrylic polymer (A) contain 90 to 99.5% by mass of (meth)acrylamide and 0.5 to 5% by mass of N-methylol(meth)acrylamide.

2. 2. The aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator according to claim 1, wherein the polymerization initiator in the raw material of the acrylic polymer (A) is 0.2 parts by mass or less per 100 parts by mass of the monomer raw material.

3. A slurry for a heat-resistant layer of a lithium ion secondary battery separator, comprising the aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator according to claim 1 or 2.

4. A lithium ion secondary battery separator having a heat-resistant layer obtained by using the slurry for a lithium ion secondary battery separator heat-resistant layer according to claim 3.

Citation Information

Patent Citations

  • Binder composition for electricity storage device, slurry for electricity storage device, electricity storage device electrode, separator, and electricity storage device

    JP2015118908A

  • Lithium ion secondary battery separator, method for manufacturing lithium ion secondary battery separator, and lithium ion secondary battery

    JP2018026266A

  • Binder aqueous solution for lithium ion battery, slurry for lithium ion battery, manufacturing methods thereof, electrode for lithium ion battery, separator for lithium ion battery, separator / electrode laminate for lithium ion battery, and lithium ion battery

    JP2019057487A

  • Slurry for thermal crosslinking type lithium ion battery, manufacturing method thereof, electrode for lithium ion battery, separator for lithium ion battery, separator / electrode laminate for lithium ion battery, and lithium ion battery

    JP2019057488A

  • Secondary-battery porous membrane composition, secondary-battery porous membrane and secondary battery

    WO2015122322A1