Secondary battery, battery pack and vehicle
The integration of a fluororesin and acrylic resin binder in the electrodes of a secondary battery with an aqueous electrolyte addresses water electrolysis issues, enhancing cycle life performance by reducing side reactions and maintaining electrode integrity.
Patent Information
- Application Number
- JP2023046714
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Non-aqueous lithium secondary batteries using lithium titanium oxide and lithium manganese oxide as electrode materials face challenges with water electrolysis and gas generation in aqueous electrolytes, leading to reduced energy density and cycle life performance.
A secondary battery with an aqueous electrolyte and electrodes containing a first binder composed of a fluororesin and an acrylic resin, which suppresses contact between active materials and water, thereby reducing side reactions and improving cycle life performance.
The use of a fluororesin and acrylic resin binder enhances the cycle life performance of the secondary battery by minimizing water electrolysis and side reactions, maintaining electrode flexibility and coverage, and ensuring sufficient hydrophobicity.
Smart Images

Figure 2024135832000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to a secondary battery, a battery pack, and a vehicle. [Background technology]
[0002] Non-aqueous electrolyte batteries, particularly lithium secondary batteries, using a carbon material or lithium titanium oxide as the negative electrode active material and a layered oxide containing nickel, cobalt, manganese, etc. as the positive electrode active material have already been put to practical use as power sources in a wide range of fields. The form of such non-aqueous electrolyte batteries is diverse, ranging from small ones for various electronic devices to large ones for electric vehicles.
[0003] Meanwhile, the use of aqueous electrolytes has been studied. In aqueous electrolytes, the potential range in which the battery is charged and discharged must be limited to a potential range in which the electrolysis reaction of water contained as a solvent does not occur. For example, by using lithium manganese oxide as the positive electrode active material and lithium vanadium oxide as the negative electrode active material, the electrolysis of water can be avoided. Although these combinations can obtain an electromotive force of about 1 to 1.5 V, it is difficult to obtain a sufficient energy density for a battery.
[0004] Lithium manganese oxide is used as the positive electrode active material, and LiTi2O4 and Li4Ti5O are used as the negative electrode active material. 12 Theoretically, the use of lithium titanium oxide such as the above can provide an electromotive force of about 2.6 V to 2.7 V, making it an attractive battery from the viewpoint of energy density. Non-aqueous lithium secondary batteries that use such combinations of positive and negative electrode materials provide excellent life performance, and such batteries have already been put to practical use. However, in aqueous electrolytes, the lithium insertion / extraction potential of lithium titanium oxide is approximately 1.5 V (vs. Li / Li) based on the lithium potential. + ), water is easily electrolyzed. On the other hand, the lithium manganese oxide used in the positive electrode also has the problem of gas generation due to oxidation of anions in the aqueous solution, making satisfactory charging and discharging impossible. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2017 / 135323 [Non-patent literature]
[0006] [Non-Patent Document 1] Nature Energy volume 7, pages 186-193 (2022) Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in view of the above circumstances, and has an object to provide a secondary battery having excellent cycle life performance, a battery pack including this secondary battery, and a vehicle including this battery pack. [Means for solving the problem]
[0008] According to an embodiment, a secondary battery is provided. The secondary battery includes an aqueous electrolyte, a positive electrode, and a negative electrode. At least one of the positive electrode and the negative electrode includes a first binder. The first binder includes a fluorine-based resin and an acrylic resin.
[0009] According to another embodiment, a battery pack including a secondary battery according to the embodiment is provided.
[0010] According to another embodiment, a vehicle is provided that includes a battery pack according to an embodiment. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Diagram 2] 2 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 1. [Diagram 3]FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Figure 4] 4 is an enlarged cross-sectional view of part B of the secondary battery shown in FIG. 3. [Diagram 5] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 6] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 7] 7 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. 6. [Figure 8] 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 9] 1 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the embodiments will be described with reference to the drawings as appropriate. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Also, each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.
[0013] (First embodiment) In a secondary battery containing an aqueous electrolyte, electrolysis of water in the aqueous electrolyte may occur as a side reaction, which may cause deterioration of the aqueous electrolyte.
[0014] For example, when water electrolysis occurs in a lithium ion secondary battery, lithium ions released from the positive electrode may not contribute to the battery reaction because the insertion of lithium ions and the generation of hydrogen compete with each other at the negative electrode. In addition, when hydrogen is generated at the negative electrode, lithium ions may be simultaneously desorbed from the negative electrode. Therefore, when water electrolysis occurs, lithium ions are consumed from both the negative electrode and the positive electrode, and the amount of lithium ions available for charging and discharging may decrease. As a result, the battery capacity may deteriorate with the charge and discharge cycle.
[0015] In addition, in the side reactions, for example, solid components may be generated as decomposition products of the aqueous electrolyte. These solid components may deposit on the electrodes, for example, and may cause an increase in resistance.
[0016] As a result of extensive research, the present inventors have realized the secondary battery according to the first embodiment.
[0017] According to a first embodiment, a secondary battery is provided. The secondary battery includes an aqueous electrolyte, a positive electrode, and a negative electrode. At least one of the positive electrode and the negative electrode includes a first binder. The first binder includes a fluorine-based resin and an acrylic resin.
[0018] Acrylic resins have a high ability to coat active material particles, making it possible to prevent contact between the active material in the electrode and water in the aqueous electrolyte.
[0019] Fluorine-based resins are highly hydrophobic, which can prevent contact between the active material in the electrode and the water in the aqueous electrolyte, thereby suppressing side reactions, thereby contributing to improved cycle life performance.
[0020] Since fluororesin has high hydrophobicity, the molecules of the fluororesin tend to aggregate with each other. As a result, for example, the fluororesin tends to fibrillate. The fibrillated fluororesin may have poor coverage on particulate active materials (active material particles). Therefore, it is difficult to improve coverage on active material particles by using the fluororesin alone.
[0021] Since the acrylic resin and the fluorine-based resin may be compatible with each other, they may be mixed and used as the first binder.
[0022] The first binder contains an acrylic resin that has high coverage on active material particles and a fluorine-based resin that has high hydrophobicity. Therefore, the first binder can ensure sufficient coverage and hydrophobicity to suppress side reactions even in an aqueous electrolyte battery in which electrolysis of water is more likely to occur than in a nonaqueous electrolyte battery. As a result, the cycle life performance can be further improved.
[0023] The secondary battery according to the embodiment will be further described below.
[0024] In such a secondary battery, at least one of the positive electrode and the negative electrode contains a first binder. The electrode may include a current collector and an active material-containing layer formed on the current collector. The active material-containing layer includes an active material and a first binder. The active material may be, for example, active material particles having a particle shape. The electrode may further include a coating. The coating may be included in the active material-containing layer.
[0025] The first binder can cover at least a part of the surface of the active material particles, thereby preventing contact between the active material and the aqueous electrolyte and thus preventing side reactions, thereby contributing to an improvement in cycle life performance.
[0026] The first binder has a viscosity of 0.01≦A F / (A F +A O +2A N )≦0.95. O is the amount of oxygen atoms, and A F is the amount of fluorine atoms, and A N is the amount of nitrogen atoms. O +A N >0, A F >0.
[0027] The first binder may contain oxygen atoms and fluorine atoms. The oxygen atoms may be contained, for example, in the acrylic resin in the first binder. The fluorine atoms may be contained, for example, in the fluorine resin in the first binder. The first binder may further contain nitrogen atoms. The nitrogen atoms may be contained, for example, in the acrylic resin such as acrylonitrile.
[0028] The first binder has an amount of oxygen atoms A O , the amount of fluorine atoms A F and the amount of nitrogen atoms A N However, 0.01≦A F / (A F +A O +2A N )≦0.95. O +A N As long as it satisfies >0, A O Or A N may be 0. In other words, the first binder does not have to contain either an oxygen atom or a nitrogen atom.
[0029] When the ratio of the acrylic resin in the first binder is high or the ratio of the fluororesin is low, A F / (A F +A O +2A N The higher the ratio of the acrylic resin to the first binder, or the lower the ratio of the fluorine-based resin, the higher the coverage of the active material particles with the first binder tends to be. F / (A F +A O +2A N ) is preferably 0.95 or less, particularly preferably 0.8 or less.
[0030] When the ratio of the acrylic resin in the first binder is low or when the ratio of the fluorine resin is high, A F / (A F +A O +2A NThe smaller the ratio of the acrylic resin to the first binder, or the larger the ratio of the fluorine-based resin, the higher the hydrophobicity and the more flexible the electrode tends to be. F / (A F +A O +2A N ) is preferably 0.01 or more, more preferably 0.05 or more, particularly preferably 0.5 or more, and even more preferably 0.6 or more. O , the amount of fluorine atoms A F and the amount of nitrogen atoms A N However, 0.5≦A F / (A F +A O +2A N )≦0.8 is more preferable.
[0031] 0.01≦A F / (A F +A O +2A N )≦0.95 is satisfied, the atomic ratio can be satisfied when the ratio of the acrylic resin to the first binder is 5% by mass or more and 70% by mass or less, which is preferable. When the ratio of the acrylic resin to the first binder is 5% by mass or more, the coverage rate of the first binder on the active material particles can be increased. When the ratio is 70% by mass or less, sufficient hydrophobicity can be ensured and the flexibility of the electrode can be maintained. When the electrode is flexible, cracking of the electrode due to expansion and contraction of the electrode accompanying charge and discharge cycles can be suppressed. Therefore, the adverse effect of resistance increase can be suppressed. It is more preferable that the ratio of the acrylic resin to the first binder is within the range of 15% by mass or more and 45% by mass or less.
[0032] The acrylic resin may be a polymer containing at least one selected from the group consisting of acrylic acid esters, methacrylic acid esters, and acrylonitrile. At least one selected from the group consisting of acrylic acid esters, methacrylic acid esters, and acrylonitrile may be included in the polymer as a monomer, for example. The type of monomer contained in the polymer may be one or more types. The polymer may be a polymer consisting of one type of monomer, or may be a copolymer containing two or more types of monomers. Specific examples of the polymer include acrylic acid ester polymers, methacrylic acid ester polymers, and acrylonitrile polymers, and copolymers thereof. The type of acrylic resin may be one or more types.
[0033] Of the above, the acrylic resin preferably contains a methacrylic acid ester polymer from the viewpoint of compatibility with the fluorine-based resin.
[0034] In the Fourier transform infrared spectroscopy (FT-IR) measurement, the infrared absorption spectrum of the surface of the electrode provided in the secondary battery according to this embodiment is 1710 cm -1 over 1740cm -1 It may have an absorption peak within the range of 1120 cm -1 More than 1160cm -1 The absorption peak may be in the range of
[0035] Infrared absorption spectrum, 1710cm -1 over 1740cm -1 The absorption peaks in the following range are assigned to C=O bonds: 1120 cm -1 More than 1160cm -1 The absorption peaks in the range of are assigned to C-O bonds. These bonds can be assigned to carboxylic acid esters. Examples of carboxylic acid esters include acrylic resins. The infrared absorption spectrum of the surface of an electrode containing an acrylic resin can have the absorption peaks as described above.
[0036] The infrared absorption spectrum of the surface of the electrode included in the secondary battery according to this embodiment has an absorption peak at 2800 cm in addition to the absorption peak that the surface of the electrode containing the acrylic resin may have. -1 More than 3000cm -1 It may have an absorption peak within the range of 1800 cm -1 More than 2500cm -1 The absorbance can be low over the following range: The infrared absorption spectrum of the surface of an electrode comprising a polymer containing acrylate or methacrylate esters has the above characteristics.
[0037] The infrared absorption spectrum of the surface of an electrode containing a polymer containing an acrylate or methacrylate ester is, for example, 2900 / A 2000 ≧2, A 1725 / A 2000 ≧4 and A 1145 / A 2000 ≧4, where A λ is the wavelength of infrared absorption in λcm -1 This refers to the absorbance at
[0038] The infrared absorption spectrum of the surface of the electrode of the secondary battery according to this embodiment is 1800 cm -1 More than 2500cm -1 In the infrared absorption spectrum, the peaks can be defined, for example, as follows, since the absorbance can be low over the following range: 2900 / A 2000 Infrared absorption spectrum that satisfies ≧2 is 2800 cm -1 More than 3000cm -1 It can be said that the peak is within the following range: 1725 / A 2000 Infrared absorption spectrum that satisfies ≧4 is 1710 cm -1 over 1740cm -1 It can be said that the peak is within the following range: 1145 / A 2000 Infrared absorption spectrum that satisfies ≧4 is 1120 cm -1 More than 1160cm -1It can be said to have a peak within the following range:
[0039] The infrared absorption spectrum of the surface of the electrode included in the secondary battery according to this embodiment has an absorption peak at 2240 cm in addition to the absorption peak that the surface of the electrode containing the acrylic resin may have. -1 More than 2260cm -1 The absorption peak may be attributable to a C≡N bond, which may be attributable to, for example, acrylonitrile. -1 More than 2200cm -1 The absorbance can be low over the following range: The infrared absorption spectrum of the surface of an electrode containing a polymer containing acrylonitrile has the above characteristics.
[0040] The infrared absorption spectrum of the surface of an electrode containing a polymer containing acrylonitrile is, for example, 2250 / A 2000 ≧4 may be satisfied.
[0041] As explained earlier, A 2250 / A 2000 Infrared absorption spectrum that satisfies ≧4 is 1800 cm -1 More than 2200cm -1 It can be said to have a peak within the following range:
[0042] The ratio of the fluororesin to the first binder is preferably within the range of 30% by mass to 95% by mass. At 30% by mass or more, sufficient hydrophobicity can be ensured and the flexibility of the electrode can be maintained, thereby suppressing the adverse effect of an increase in resistance. At 95% by mass or less, the coverage rate of the first binder on the active material particles can be increased. The ratio of the fluororesin is more preferably within the range of 55% by mass to 85% by mass.
[0043] The fluororesin may be a polymer containing vinylidene fluoride. For example, vinylidene fluoride may be included in the polymer as a monomer. Specifically, the fluororesin may be polyvinylidene fluoride (PVDF) or a copolymer containing vinylidene fluoride and another monomer.
[0044] The X-ray photoelectron spectroscopy (XPS) spectrum of the surface of the electrode included in the secondary battery according to this embodiment may have a peak in the range of 292 eV to 294 eV. The peak appearing in this range is an absorption peak attributable to a C-F bond. The C-F bond may be attributable to a fluororesin. The XPS spectrum of the surface of the electrode containing the fluororesin may have the above peak.
[0045] The electrode preferably further includes a coating. The form of the coating is not particularly limited. The coating may be formed on the surface of the electrode, or may be formed inside the active material-containing layer. In these cases, the electrode is generally said to include a coating. The coating may be exposed on the electrode surface. The electrode surface refers to the main surface of the active material-containing layer that is not in contact with the current collector. The coating may be formed, for example, on the outside of the first binder that covers at least a part of the active material particle surface. The coating may cover the part of the active material particle surface that is not covered by the first binder. Therefore, when the electrode further includes a coating in addition to the first binder, the contact between the active material and the aqueous electrolyte can be further suppressed, thereby suppressing side reactions.
[0046] Therefore, when the electrode includes a coating, for example, when active material particles that are prone to side reactions are used in combination with an aqueous electrolyte, side reactions can be further suppressed. Examples of active material particles that are prone to side reactions include active material particles with small particle sizes. Active material particles with small particle sizes have a large surface area. Therefore, although output performance can be improved, they tend to be prone to side reactions. When the electrode includes a coating, such active material particles that are prone to side reactions can be used, so that both suppression of side reactions and improvement of output performance can be achieved.
[0047] The coating includes at least one selected from the group consisting of cyanates, sulfates, metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide. Examples of cyanates include cyanate compounds and isocyanate compounds. Examples of isocyanate compounds include, for example, lithium isocyanate. Examples of sulfates include sulfates and sulfites. Specific examples of sulfates and sulfites include lithium sulfate and lithium sulfite, respectively.
[0048] Cyanates and sulfates can exist stably in aqueous electrolyte batteries and have excellent lithium ion conductivity, which makes it possible to suppress side reactions and maintain low resistance.
[0049] The XPS spectrum of the surface of the electrode included in the secondary battery according to this embodiment may have a peak in the range of 398 eV to 402 eV. The XPS spectrum of the surface of the electrode including the coating containing cyanates has the above-mentioned characteristics.
[0050] The XPS spectrum of the surface of the electrode included in the secondary battery according to this embodiment may have a peak in the range of 168 eV to 173 eV. The XPS spectrum of the surface of the electrode including the coating containing sulfates has the above characteristics.
[0051] Metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide have high hydrogen overvoltage. Therefore, an electrode including a coating containing at least one of the above substances can suppress the electrolysis of water. Therefore, hydrogen generation can be suppressed and the absorption and release of lithium ions in the negative electrode can be facilitated. Therefore, the cycle life performance of the secondary battery can be improved. Of the positive electrode and the negative electrode, it is more preferable that the coating containing at least one selected from the group consisting of metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide is formed on the negative electrode.
[0052] The XPS spectrum of the surface of the electrode included in the secondary battery according to this embodiment may have a peak in the range of 1020.6 eV to 1023.2 eV. The XPS spectrum of the surface of the electrode including a coating containing at least one selected from the group consisting of metallic zinc, zinc oxide, and zinc hydroxide has the above-mentioned characteristics.
[0053] The coating containing metallic zinc may also contain zinc oxide or zinc hydroxide. Zinc oxide may be produced, for example, by oxidation of the surface of metallic zinc.
[0054] Metallic zinc, zinc oxide, and zinc hydroxide can be distinguished from one another by fitting the peak shapes within the range of 1020.7 eV to 1023.2 eV. For example, in the XPS spectrum of an electrode surface including a coating containing metallic zinc and zinc oxide, a peak can be detected within the range of 1020.7 eV to 1021.3 eV and a peak can be detected within the range of 1021.8 eV to 1022.6 eV by fitting the peak shapes.
[0055] The peaks in the range of 1020.7 eV to 1021.3 eV can be attributed to, for example, metallic zinc. The peaks in the range of 1021.8 eV to 1022.6 eV can be attributed to, for example, zinc oxide.
[0056] In addition, in the XPS spectrum of the electrode surface including a coating containing zinc hydroxide, a peak can be detected in the range of 1022.4 eV to 1023.2 eV by peak shape fitting.
[0057] The XPS spectrum of the surface of the electrode included in the secondary battery according to this embodiment may have a peak in the range of 484.4 eV to 485.3 eV. The XPS spectrum of the surface of the electrode including the coating containing metal tin has the above characteristics.
[0058] The XPS spectrum of the surface of the electrode included in the secondary battery according to this embodiment may have a peak in the range of 136.2 eV to 137.1 eV. The XPS spectrum of the surface of the electrode including the coating containing metallic lead has the above characteristics.
[0059] The XPS spectrum of the surface of the electrode included in the secondary battery according to this embodiment may have a peak in the range of 684.7 eV to 685.4 eV. The XPS spectrum of the surface of the electrode including the coating containing lithium fluoride has the above characteristics.
[0060] The XPS spectrum of the surface of the electrode included in the secondary battery according to this embodiment may have a peak in the range of 55.2 eV to 55.8 eV. The XPS spectrum of the surface of the electrode including the coating containing lithium oxide has the above characteristics.
[0061] The secondary battery according to the embodiment will be described in detail below.
[0062] The secondary battery may be, for example, a lithium secondary battery (lithium ion secondary battery) that uses lithium ions as carrier ions. The secondary battery includes an aqueous electrolyte secondary battery that contains an aqueous electrolyte (for example, an aqueous electrolyte). In other words, the secondary battery may be an aqueous electrolyte lithium ion secondary battery.
[0063] Such a secondary battery may further include a separator disposed between the positive electrode and the negative electrode.
[0064] In the secondary battery, the negative electrode, the positive electrode, and the separator may constitute an electrode group, and the aqueous electrolyte may be retained in the electrode group.
[0065] The secondary battery may further include an exterior member capable of housing the electrode group and the aqueous electrolyte, and may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.
[0066] The negative electrode, positive electrode, separator, aqueous electrolyte, exterior member, negative electrode terminal, and positive electrode terminal will be described in detail below. Parts of the description of the negative electrode and positive electrode that overlap with the electrodes described above will be omitted.
[0067] 1) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode active material-containing layer may be formed on one or both sides of the negative electrode current collector. The negative electrode active material-containing layer may include a negative electrode active material, and optionally a conductive agent and a negative electrode binder. The negative electrode may further include a coating.
[0068] The negative electrode active material-containing layer may contain the first binder described above as a negative electrode binder. That is, the negative electrode may be the electrode described above. When the negative electrode is the electrode described above, the negative electrode current collector, the negative electrode active material-containing layer, the negative electrode active material, and the negative electrode binder may be the current collector, the active material-containing layer, the active material, and the first binder described above, respectively.
[0069] When the positive electrode to be combined with the negative electrode contains a first binder, the negative electrode does not need to contain the first binder.
[0070] Examples of the negative electrode active material include lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), titanium dioxide (TiO2), anatase type titanium dioxide, rutile type titanium dioxide, niobium pentoxide (Nb2O5), hollandite type titanium composite oxide, orthorhombic titanium composite oxide, and monoclinic type niobium titanium oxide.
[0071] As an example of the above-mentioned orthorhombic titanium-containing composite oxide, Li 2+a M I 2-b Ti 6-c M II d O 14+σ In this case, the compound represented by MI is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb and K. II is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).
[0072] As an example of the monoclinic niobium titanium oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium oxide include Li x Examples include Nb2TiO7 (0≦x≦5).
[0073] Another example of monoclinic niobium titanium oxide is Li x Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0074] The negative electrode active material may be in the form of, for example, particles. The negative electrode active material may be in the form of primary particles, secondary particles formed by aggregation of primary particles, or a mixture of primary particles and secondary particles.
[0075] The average particle size of the negative electrode active material particles is preferably 5 μm or less. The average particle size of the negative electrode active material particles is more preferably in the range of 0.5 μm to 5 μm. By using negative electrode active material particles with an average particle size of 5 μm or less, the solid diffusion resistance of lithium ions can be sufficiently reduced, so that the output performance can be improved. If the average particle size of the negative electrode active material particles is less than 0.5 μm, an excessive amount of resin needs to be added to suppress side reactions caused by contact between the negative electrode active material particles and the aqueous electrolyte, which is disadvantageous in terms of resistance increase.
[0076] The conductive agent is blended to improve current collection performance and reduce contact resistance between the negative electrode active material and the negative electrode current collector. Examples of the conductive agent include carbonaceous materials such as vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanotubes, and carbon nanofibers. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coat or an electronically conductive inorganic material coat may be applied to the surface of the negative electrode active material particles.
[0077] The negative electrode binder is mixed to fill the gaps between the dispersed negative electrode active material and to bind the negative electrode active material and the negative electrode current collector. The negative electrode binder may include the first binder described above. The negative electrode binder may include another binder other than the first binder. The negative electrode binder may consist of only the first binder described above, may be a mixture of the first binder and another binder, or may consist of only the other binder. As the other binder, the above-mentioned fluorine-based resin or acrylic resin may be used alone.
[0078] Examples of other binders include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the negative electrode binder, or two or more may be used in combination as the negative electrode binder.
[0079] The mixing ratio of the negative electrode active material, the conductive agent, and the negative electrode binder in the negative electrode active material-containing layer can be appropriately changed. For example, it is preferable to mix the negative electrode active material, the conductive agent, and the negative electrode binder in a ratio of 68% by mass or more and 96% by mass or less, 2% by mass or more and 30% by mass or less, and 2% by mass or more and 30% by mass or less, respectively. By making the amount of the conductive agent 2% by mass or more, the current collection performance of the negative electrode active material-containing layer can be improved. In addition, by making the amount of the negative electrode binder 2% by mass or more, the binding property between the negative electrode active material-containing layer and the negative electrode current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and the negative electrode binder 30% by mass or less, respectively, in order to achieve high capacity.
[0080] When the negative electrode binder contains the first binder, the proportion of the first binder in the negative electrode binder is preferably 1 mass% or more. The proportion of the first binder in the negative electrode binder may be 100 mass%. The proportion of the first binder refers to the sum of the proportion of the fluorine-based resin and the proportion of the acrylic resin in the negative electrode binder.
[0081] The negative electrode preferably further includes a coating. The form of the coating is not particularly limited. The coating may be formed on the surface of the negative electrode, or may be formed inside the negative electrode active material-containing layer. The coating may be exposed on the negative electrode surface. The negative electrode surface refers to the main surface of the negative electrode active material-containing layer that is not in contact with the negative electrode current collector. The coating may be formed, for example, on the outside of the first binder that covers at least a part of the surface of the negative electrode active material particles. The coating may be formed, for example, on the first binder that covers at least a part of the surface of the negative electrode active material particles. The coating may cover, for example, a part of the surface of the negative electrode active material particles that is not covered by the negative electrode binder.
[0082] When the negative electrode further includes a coating film in addition to the first binder, contact between the negative electrode active material and the aqueous electrolyte can be further suppressed, and side reactions can be suppressed, which is preferable.
[0083] The negative electrode preferably contains a first binder as a negative electrode binder, and the surface of the negative electrode preferably contains at least one selected from the group consisting of metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide. At least one selected from the group consisting of metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide may be contained in, for example, a coating.
[0084] The density of the negative electrode active material-containing layer (excluding the negative electrode current collector) is 1.8 g / cm 3 More than 2.8g / cm 3 A negative electrode having a density of the negative electrode active material-containing layer within this range is excellent in energy density and water-based electrolyte retention. The density of the negative electrode active material-containing layer is preferably 2.1 g / cm or less. 3 More than 2.6g / cm 3 It is more preferable that:
[0085] The negative electrode current collector is made of a material that is electrochemically stable at a potential at which lithium (Li) is inserted and removed from the negative electrode active material. For example, the negative electrode current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the negative electrode current collector is preferably 5 μm or more and 20 μm or less. A negative electrode current collector having such a thickness can balance the strength and weight reduction of the negative electrode.
[0086] The negative electrode current collector may also include a portion on the surface of which the negative electrode active material-containing layer is not formed, and this portion can function as a negative electrode current collecting tab.
[0087] The negative electrode can be produced, for example, by the following method. First, a negative electrode active material, a conductive agent, and a negative electrode binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a negative electrode current collector. Next, the applied slurry is dried to obtain a laminate of a negative electrode active material-containing layer and a negative electrode current collector. Then, this laminate is pressed. In this manner, a negative electrode is produced.
[0088] Alternatively, the negative electrode may be prepared by the following method: First, the negative electrode active material, the conductive agent, and the negative electrode binder are mixed to obtain a mixture. Then, the mixture is molded into pellets. Then, the pellets are placed on the negative electrode current collector to obtain the negative electrode.
[0089] When the negative electrode includes a coating, the coating can be formed, for example, by directly forming a coating on the negative electrode using a coating precursor, or by adding the coating precursor to an aqueous electrolyte. Examples of the coating precursor include a material containing at least one selected from the group consisting of Zn, Sn, and Pb, a metal containing the aforementioned element, a metal oxide containing the aforementioned element, cyanates, sulfates, amide compounds, and organic sulfur compounds. The coating precursor may be a material containing a substance that constitutes the coating itself, or may be a material containing a substance that generates a coating by electrolysis or the like.
[0090] When the coating precursor is added to the aqueous electrolyte, the coating can be formed, for example, by electrolyzing the coating precursor on the negative electrode during the initial charge. In this case, the initial charge current is preferably less than 1C (hourly discharge rate) and the temperature is preferably 25°C or higher.
[0091] Examples of the method for directly forming a coating on the negative electrode include a method for forming a coating by a solution method, a vapor deposition method, a spray method, etc. Examples of coating precursors suitable for the method for directly forming a coating on the negative electrode include materials containing at least one selected from the group consisting of cyanates, sulfates, metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide.
[0092] The solution method is, for example, a method in which a coating precursor is added in a solution or solid state to an electrode slurry, and dried at a predetermined temperature when the electrode is coated to form a coating. The vapor deposition method is, for example, a method in which an electrode slurry is coated on a current collector, and a coating precursor is vapor-deposited to a predetermined thickness on the electrode after drying to form a coating. For example, a vacuum vapor deposition method can be used as a vapor deposition method. The spray method is, for example, a method in which an electrode slurry is coated on a current collector, and a coating precursor solution is wet-sprayed on the electrode after drying, and then dried to form a coating.
[0093] The method of adding the coating precursor to the aqueous electrolyte will be described later.
[0094] 2) Positive electrode The positive electrode can include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer can be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer can include a positive electrode active material, and optionally a conductive agent and a positive electrode binder. The positive electrode may further include a coating film.
[0095] The positive electrode active material-containing layer can include the first binder described above as the positive electrode binder. That is, the positive electrode can be the electrode described above. When the positive electrode is the electrode described above, the positive electrode current collector, the positive electrode active material-containing layer, the positive electrode active material, and the positive electrode binder can be the current collector, the active material-containing layer, the active material, and the first binder described above, respectively.
[0096] When the negative electrode combined with the positive electrode contains the first binder, the positive electrode may not contain the first binder.
[0097] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain a single compound as the positive electrode active material, or may contain a combination of two or more compounds. Examples of the oxide and the sulfide can include compounds into which Li or Li ions can be inserted and desorbed.
[0098] Examples of such compounds include, for example, manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (for example, Li x Mn2O4 or Li x MnO2; 0 <x ≦ 1), lithium nickel composite oxide (for example, Li x NiO2; 0 <x ≦ 1), lithium cobalt composite oxide (for example, Li x CoO2; 0 <x ≦ 1), lithium nickel cobalt composite oxide (for example, Li x Ni 1-y Co y O2; 0 <x ≦ 1, 0 <y <1), lithium manganese cobalt composite oxide (for example, Li x Mn y Co 1-yO2; 0 < x ≤ 1, 0 < y < 1), a lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), a lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≤ 1, Li x Fe 1-y Mn y PO4; 0 < x ≤ 1, 0 < y ≤ 1, Li x CoPO4; 0 < x ≤ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and a lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included.
[0099] Among the above, examples of more preferred compounds as the positive electrode active material include a lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≤ 1), a lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≤ 1), a lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), a lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), a lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), a lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≤ 1), and a lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn zO2; where 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, and y + z < 1 is included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.
[0100] The positive electrode active material can be, for example, in the form of particles. The positive electrode active material particles may be in the form of primary particles, may be in the form of secondary particles in which the primary particles are aggregated, or may be a mixture of primary particles and secondary particles.
[0101] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material with a primary particle size of 1 μm or less can allow the solid-state diffusion of lithium ions to proceed smoothly.
[0102] The positive electrode binder is formulated to fill the gaps between the dispersed positive electrode active materials and to bind the positive electrode active material and the positive electrode current collector. The positive electrode binder can include the first binder described above. The positive electrode binder may include other binders other than the first binder. The positive electrode binder may consist only of the first binder described above, may be a mixture of the first binder and other binders, or may consist only of other binders. As other binders, the aforementioned fluororesin or acrylic resin may be used alone.
[0103] Examples of other binders include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), fluororubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the positive electrode binder, or two or more of them may be combined and used as the positive electrode binder.
[0104] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0105] In the positive electrode active material-containing layer, the positive electrode active material and the positive electrode binder are preferably mixed in proportions of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.
[0106] By making the amount of the positive electrode binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the positive electrode binder can function as an insulator. Therefore, by making the amount of the positive electrode binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0107] When a conductive agent is added, the positive electrode active material, the positive electrode binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.
[0108] By setting the amount of the conductive agent to 3% by mass or more, the above-mentioned effects can be achieved. Also, by setting the amount of the conductive agent to 15% by mass or less, the ratio of the conductive agent in contact with the aqueous electrolyte can be reduced. If this ratio is low, decomposition of the aqueous electrolyte during high-temperature storage can be reduced.
[0109] When the positive electrode binder contains the first binder, the proportion of the first binder in the positive electrode binder is preferably 1 mass% or more. The proportion of the first binder in the positive electrode binder may be 100 mass%. The proportion of the first binder refers to the sum of the proportion of the fluorine-based resin and the proportion of the acrylic resin in the positive electrode binder.
[0110] The positive electrode preferably further includes a coating. The form of the coating is not particularly limited. The coating may be formed on the surface of the positive electrode, or may be formed inside the positive electrode active material-containing layer. The coating may be exposed on the positive electrode surface. The positive electrode surface refers to the main surface of the positive electrode active material-containing layer that is not in contact with the positive electrode current collector. The coating may be formed, for example, on the outside of the first binder that covers at least a part of the positive electrode active material particle surface. The coating may be formed, for example, on the first binder that covers at least a part of the positive electrode active material particle surface. The coating may cover, for example, a part of the positive electrode active material particle surface that is not covered by the positive electrode binder. When the positive electrode further includes a coating in addition to the first binder, the contact between the positive electrode active material and the aqueous electrolyte can be further suppressed, and side reactions can be suppressed, which is preferable.
[0111] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.
[0112] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.
[0113] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.
[0114] The positive electrode can be produced, for example, by the following method. First, a positive electrode active material, a conductive agent, and a positive electrode binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a positive electrode current collector. Next, the applied slurry is dried to obtain a laminate of a positive electrode active material-containing layer and a positive electrode current collector. Then, the laminate is pressed. In this manner, a positive electrode is produced.
[0115] Alternatively, the positive electrode may be prepared by the following method: First, a positive electrode active material, a conductive agent, and a positive electrode binder are mixed to obtain a mixture. Then, the mixture is formed into pellets. Then, the pellets are placed on a positive electrode current collector to obtain a positive electrode.
[0116] When the positive electrode includes a coating, the coating can be formed, for example, by forming a coating directly on the positive electrode, or by adding a coating precursor to an aqueous electrolyte. When the coating precursor is added to an aqueous electrolyte, the coating can be formed, for example, by electrolyzing the coating precursor on the positive electrode during the first charge. In this case, the first charge current is preferably less than 1C (hourly discharge rate), and the temperature is preferably 25°C or higher.
[0117] Examples of the method for directly forming a coating on a positive electrode include a method for forming a coating by a solution method, a vapor deposition method, or a spray method using a coating precursor. Examples of the coating precursor include those described for the negative electrode. Examples of the coating precursor suitable for the method for directly forming a coating on a positive electrode include a material containing at least one selected from the group consisting of cyanates, sulfates, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide.
[0118] The solution method, vapor deposition method and spray method can be carried out in the same manner as described for the negative electrode.
[0119] The method of adding the coating precursor to the aqueous electrolyte will be described later.
[0120] 3) Water-based electrolyte The aqueous electrolyte contains an aqueous solvent and an electrolyte salt. As the aqueous solvent, a solution containing water can be used. The solution containing water may be pure water, or a mixed solution or mixed solvent of water and a substance other than water.
[0121] The aqueous electrolyte is, for example, an aqueous solution prepared by dissolving an electrolyte salt in an aqueous solvent. The aqueous electrolyte may be a gel-like aqueous electrolyte prepared by compounding the aqueous solution with a polymer material. Examples of the polymer material include polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), and polyethylene oxide (PEO).
[0122] The aqueous solution preferably contains 1 mol or more of an aqueous solvent per mol of an electrolyte salt as a solute, and more preferably contains 3.5 mol or more of an aqueous solvent per mol of an electrolyte salt.
[0123] The presence of water in aqueous electrolytes can be confirmed by GC-MS (Gas Chromatography - Mass Spectrometry) measurements. The salt concentration and water content in aqueous electrolytes can be calculated, for example, by ICP (Inductively Coupled Plasma) emission spectrometry. The molar concentration (mol / L) can be calculated by weighing a specified amount of aqueous electrolyte and calculating the salt concentration. The number of moles of solute and solvent can also be calculated by measuring the specific gravity of the aqueous electrolyte.
[0124] Examples of the electrolyte salt include lithium salts such as LiCl, LiBr, LiOH, Li2SO4, LiNO3, LiN(SO2CF3)2 (LiTFSI: lithium bis(trifluoromethanesulfonyl)imide), LiN(SO2F)2 (LiFSI: lithium bis(fluorosulfonyl)imide), and LiB[(OCO)2]2 (LiBOB: lithium bis(oxalatoborate). The type of lithium salt used may be one type or two or more types.
[0125] The aqueous electrolyte preferably contains LiCl or LiTFSI as an electrolyte salt. LiCl is inexpensive and has high electrical conductivity, so it is preferable from the viewpoint of cost and rate characteristics of the battery. LiTFSI is preferable because it can function as a coating precursor as described later.
[0126] The pH of the aqueous electrolyte is preferably 3 to 14. This pH can be appropriately changed, and from the viewpoint of increasing hydrogen overvoltage, it is considered preferable to be on the alkaline side. When the pH is on the alkaline side, hydrogen generation can be further suppressed. As a method for adjusting the pH of the aqueous solution to the alkaline side, for example, LiOH can be added. However, a pH of more than 12 is not preferable because it advances corrosion of the positive electrode current collector. The pH of the aqueous solution is preferably in the range of 3 to 14, more preferably in the range of 3 to 9.
[0127] The aqueous electrolyte may further include an additive.
[0128] Examples of the additive include, for example, a salt containing at least one metal selected from the group consisting of Zn, Sn, and Pb, an amide compound, and an organic sulfur compound.
[0129] Each of the salt containing at least one metal selected from the group consisting of Zn, Sn, and Pb, the amide compound, and the organic sulfur compound can be a coating precursor.
[0130] Examples of salts containing at least one metal selected from the group consisting of Zn, Sn, and Pb include ZnCl2, SnCl2, and PbCl2. The salt may be one or more kinds. The salt may be dissolved or suspended in the aqueous electrolyte.
[0131] When the aqueous electrolyte contains a salt containing at least one metal selected from the group consisting of Zn, Sn, and Pb, a metal, metal oxide, or metal hydroxide containing Zn, Sn, or Pb may be formed on the electrode. The metal may be, for example, a simple metal precipitated by reducing a metal ion derived from the salt contained in the aqueous electrolyte. The metal oxide may be, for example, generated by oxidizing the precipitated metal.
[0132] Examples of metals or metal oxides containing Zn, Sn, or Pb include, for example, metallic zinc, metallic tin, metallic lead, zinc oxide, and zinc hydroxide. That is, when the aqueous electrolyte contains a salt containing at least one metal selected from the group consisting of Zn, Sn, and Pb, a coating can be formed on the electrode. This contributes to improving cycle life performance.
[0133] Examples of the amide compound include urea, methylurea, ethylurea, acetamide, N-methylacetamide, trifluoroacetamide, etc. One or more types of amide compounds can be used.
[0134] An example of the organic sulfur compound is dimethyl sulfone.
[0135] When the aqueous electrolyte contains an amide compound or an organic sulfur compound, the lithium salt contained in the aqueous electrolyte may cause a drop in the melting point of the amide compound and the organic sulfur compound. Therefore, the amide compound and the organic sulfur compound may be in a liquid state at room temperature in the aqueous electrolyte. Therefore, the aqueous electrolyte containing at least one selected from the group consisting of an amide compound and an organic sulfur compound may have a smaller proportion of water in the liquid components in the aqueous electrolyte compared to an aqueous electrolyte containing neither an amide compound nor an organic sulfur compound. Therefore, the contact between the active material and water can be suppressed, and as a result, the electrolysis of water can be suppressed.
[0136] In addition, the amide compound and the organic sulfur compound themselves can be electrolyzed in the battery. When the amide compound is electrolyzed, cyanates can be formed on the electrode. When the organic sulfur compound is electrolyzed, sulfates can be formed on the electrode. That is, the coating described above can be formed on the electrode. Therefore, when the aqueous electrolyte contains at least one selected from the group consisting of the amide compound and the organic sulfur compound, the resistance can be kept low while suppressing the electrolysis of water in the electrode.
[0137] A coating containing sulfates can be formed by decomposing an electrolyte salt containing sulfur atoms, in addition to the addition of additives. Examples of electrolyte salts containing sulfur atoms include Li2SO4, LiN(SO2CF3)2 (LiTFSI: lithium bis(trifluoromethanesulfonyl)imide), and LiN(SO2F)2 (LiFSI: lithium bis(fluorosulfonyl)imide). Therefore, electrolyte salts containing sulfur atoms can function as coating precursors. The aqueous electrolyte preferably further contains an amide compound in addition to the electrolyte salt containing sulfur atoms. The aqueous electrolyte having the above-mentioned structure is easy to form a coating containing both sulfates and cyanates. Such a coating is preferable because it can achieve both stability and low resistance.
[0138] In addition, the lithium ions contained in the lithium salt may react with a material containing fluorine atoms or a material containing oxygen atoms contained in the aqueous electrolyte to produce lithium fluoride or lithium oxide, respectively. Examples of materials containing fluorine atoms and materials containing oxygen atoms include electrolyte salts and aqueous solvents. In addition, when the aqueous electrolyte further contains an amide compound, it may react with the amide compound to produce cyanates. For example, lithium isocyanate may be produced. Therefore, the lithium salt may function as a coating precursor. An aqueous electrolyte containing LiTFSI is preferable because it is easy to form a coating containing lithium fluoride.
[0139] When the aqueous electrolyte contains a coating precursor, the coating can be formed on the electrode by, for example, electrolyzing the coating precursor on the electrode during the initial charge. In this case, the initial charge current is preferably less than 1C (hourly discharge rate) and the temperature is preferably 25°C or higher.
[0140] 4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVDF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.
[0141] Also, as the separator, a membrane containing at least inorganic solid particles, an aggregate or sintered body of inorganic solid particles, a membrane containing inorganic solid particles and a polymer material, for example, a composite membrane of inorganic solid particles and a polymer material, or an ion exchange membrane can be used. The inorganic solid particles can be, for example, particles of a solid electrolyte, and the membrane can be a solid electrolyte membrane. The solid electrolyte membrane can be, for example, a solid electrolyte composite membrane formed by forming solid electrolyte particles into a membrane using a polymer material.
[0142] Examples of inorganic solid particles include particles of ceramics such as alumina, and inorganic solid electrolytes. Inorganic solid electrolytes are solid substances that have Li-ion conductivity. Here, having Li-ion conductivity means a Li-ion conductivity of 1×10 at 25° C. -6 It means that the inorganic solid electrolyte has a lithium ion conductivity of 1.0 S / cm or more. Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes. Specific examples of the inorganic solid electrolyte are as follows.
[0143] As the oxide-based solid electrolyte, it is preferable to use a lithium phosphate solid electrolyte having a NASICON (Sodium (Na) Super Ionic Conductor) type structure and represented by the general formula Li 1+x Mα2(PO4)3. In the above general formula, Mα is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is in the range of 0 ≦ x ≦ 2.
[0144] Specific examples of the lithium phosphate solid electrolyte having a NASICON type structure include LATP compounds represented by Li 1+x Al x Ti 2-x (PO4)3 with 0.1 ≦ x ≦ 0.5; compounds represented by Li 1+x Al y Mβ 2-y (PO4)3 where Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca and 0 ≦ x ≦ 1 and 0 ≦ y ≦ 1; compounds represented by Li 1+x Al x Ge 2-x (PO4)3 with 0 ≦ x ≦ 2; and compounds represented by Li 1+x Al x Zr 2-x (PO4)3 with 0 ≦ x ≦ 2; Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 where Mγ is one or more selected from the group consisting of Ti and Ge and 0 < x ≦ 2, 0 ≦ y < 3; compounds represented by Li 1+2x Zr 1-x Ca x (PO4)3 with 0 ≦ x < 1 can be mentioned.
[0145] In addition, as the oxide-based solid electrolyte, in addition to the above lithium phosphate solid electrolyte, Li x PO y N zand 2.6≦x≦3.5, 1.9≦y≦3.8, and 0.1≦z≦1.3. 2.9 PO 3.3 N 0.46 ); Garnet-type structure La 5+x A x La 3-x MδO 12 A is 1 or more selected from the group consisting of Ca, Sr, and Ba, Mδ is 1 or more selected from the group consisting of Nb and Ta, and 0≦x≦0.5; Li3Mδ 2-x L2O 12 wherein Mδ is at least one selected from the group consisting of Nb and Ta, and L may contain Zr, and 0≦x≦0.5; Li 7-3x Al x La3Zr3O 12 and 0≦x≦0.5; Li 5+x La3Mδ 2-x Zr x O 12 where Mδ is at least one selected from the group consisting of Nb and Ta, and 0≦x≦2. LLZ compounds (e.g., Li7La3Zr2O 12 ); and La 2 / 3-x Li x Examples of such compounds include those represented by TiO3, where x is 0.3≦x≦0.7.
[0146] The inorganic solid particles may be of a single type or a mixture of two or more types.
[0147] The polymeric material may be a polymer made of a single monomer unit, a copolymer made of multiple monomer units, or a mixture of these. The polymeric material preferably contains a monomer unit made of a hydrocarbon having a functional group containing one or more selected from the group consisting of oxygen (O), sulfur (S), nitrogen (N), and fluorine (F). As the polymeric material, a single type may be used, or multiple types may be mixed and used.
[0148] The separator may contain a plasticizer and an electrolyte salt in addition to the inorganic solid particles and the polymer material. For example, when the separator contains an electrolyte salt, the ionic conductivity of the separator can be further increased.
[0149] The separator may be, for example, a plurality of separators each disposed between a positive electrode and a negative electrode, or may be a single separator folded zigzag, in which case the positive electrodes and negative electrodes are alternately disposed in the spaces created by folding the separator.
[0150] 5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.
[0151] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0152] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0153] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0154] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.
[0155] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin-shaped, or button-shaped. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.
[0156] In such a secondary battery, side reactions can be suppressed, and therefore gas generation due to the side reactions can be reduced. Therefore, the shape of the exterior member may be a sealed type, a semi-sealed type, or an open type. From the viewpoint of preventing the intrusion of water from the outside, the exterior member is preferably a sealed type.
[0157] 6) Negative terminal The negative electrode terminal has a potential range of 1V to 3V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.
[0158] 7) Positive terminal The positive electrode terminal has a potential range of 3V to 4.5V with respect to the redox potential of lithium (vs. Li / Li +) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.
[0159] Next, the secondary battery according to the embodiment will be described more specifically with reference to the drawings.
[0160] Fig. 1 is a cross-sectional view showing an example of a secondary battery, and Fig. 2 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 1.
[0161] The secondary battery 100 shown in Figures 1 and 2 includes a bag-shaped exterior member 2 shown in Figure 1, an electrode group 1 shown in Figures 1 and 2, and an aqueous electrolyte (not shown). The electrode group 1 and the aqueous electrolyte are stored in the bag-shaped exterior member 2. The aqueous electrolyte (not shown) is held in the electrode group 1.
[0162] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0163] As shown in Fig. 1, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 2, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.
[0164] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 2. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.
[0165] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.
[0166] As shown in FIG. 1, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.
[0167] The secondary battery according to the embodiment is not limited to the secondary battery having the configuration shown in FIGS. 1 and 2, but may be a battery having the configuration shown in FIGS.
[0168] Fig. 3 is a partially cutaway perspective view showing a schematic diagram of another example of a secondary battery, and Fig. 4 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 3.
[0169] The secondary battery 100 shown in Figures 3 and 4 includes an electrode group 1 shown in Figures 3 and 4, an exterior member 2 shown in Figure 3, and an aqueous electrolyte (not shown). The electrode group 1 and the aqueous electrolyte are housed in the exterior member 2. The aqueous electrolyte is held in the electrode group 1.
[0170] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0171] The electrode group 1 is a laminated type electrode group, as shown in Fig. 4. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.
[0172] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0173] The negative electrode current collector 3a of each negative electrode 3 includes a portion on one side where the negative electrode active material-containing layer 3b is not supported on any surface. This portion serves as a negative electrode current collector tab 3c. As shown in FIG. 4, the negative electrode current collector tab 3c does not overlap with the positive electrode 5. The negative electrode current collector tabs 3c are electrically connected to a belt-shaped negative electrode terminal 6. The tip of the belt-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.
[0174] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. Just as the negative electrode current collector tab 3c does not overlap with the positive electrode 5, the positive electrode current collector tab does not overlap with the negative electrode 3. The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab 3c. The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side to the negative electrode terminal 6 and is drawn out to the outside of the exterior member 2.
[0175] <Measurement method> The analysis of such a secondary battery can be carried out as follows.
[0176] (Extraction of electrodes) When analyzing electrodes contained in a secondary battery, the secondary battery is disassembled and the electrodes are taken out. The electrodes are washed with dimethyl carbonate and then dried to obtain electrodes for measurement.
[0177] (Measurement of the amount of the first binder) The amount of the first binder contained in the electrode can be measured as follows.
[0178] The active material-containing layer is peeled off from the measurement electrode obtained by performing the washing and drying described above, and the mass is measured in advance. The active material-containing layer is dispersed in a solvent such as N-methylpyrrolidone (NMP), and the first binder is dissolved in the solvent. The precipitated active material and insoluble components such as the conductive agent are collected by filtration, and the mass is measured. The difference between the mass of the active material and the mass of the precipitate can be measured as the amount of the first binder.
[0179] (FT-IR analysis) Fourier transform infrared spectroscopy (FT-IR) analysis of the electrode surface can be carried out as follows.
[0180] The measurement electrode is subjected to FT-IR analysis by the ATR (Attenuated Total Reflection) method. An example of an FT-IR device is VERTEX70v / HYPERION3000 manufactured by BRUKER or a device having equivalent functions. The resolution is 4 cm -1 The number of integration times is 128. In this manner, an infrared absorption spectrum of the electrode surface can be obtained. From the obtained infrared absorption spectrum, it is possible to determine that the electrode contains an acrylic resin and to identify the type of acrylic resin contained in the electrode.
[0181] For example, if the obtained infrared absorption spectrum has an absorption peak that is present in the infrared absorption spectrum of the electrode surface containing an acrylic resin described above, it can be determined that the electrode contains an acrylic resin.
[0182] As another example, if the obtained infrared absorption spectrum has similar characteristics to the infrared absorption spectrum of the electrode surface containing the polymer containing acrylate or methacrylate described above, it can be determined that the electrode contains a polymer containing acrylate or methacrylate. Similarly, it can be determined that the electrode contains a polymer containing acrylonitrile.
[0183] (XPS analysis of electrode surface) XPS analysis of the electrode surface can be carried out as follows.
[0184] The XPS device used may be a Quantera SXM manufactured by ULVAC-PHI, Inc., or a device with equivalent functions. Single crystal spectroscopic Al-Kα radiation (1486.6 eV) is used as the excitation X-ray source. The X-ray output is 4 kW (13 kV x 310 mA), the photoelectron detection angle is 45°, and the analysis area is approximately 4 mm x 0.2 mm. Scanning is performed at 0.10 eV / step.
[0185] The spectrum data obtained by XPS analysis of the measurement electrode is processed by smoothing and horizontal axis correction. Smoothing is performed using 9-point smoothing, and horizontal axis correction is performed using Nb 5 / 2 The peak is 207.1 eV (Nb 3+ ) and correction is performed. This makes it possible to obtain an XPS spectrum for the electrode surface.
[0186] If the obtained XPS spectrum has a peak that exists in the XPS spectrum of the electrode surface containing a fluororesin described above, it can be determined that the electrode contains a fluororesin.
[0187] From the obtained XPS spectrum, it is possible to identify whether the electrode contains a coating and the type of material contained in the coating. For example, if the obtained XPS spectrum has the same characteristics as the XPS spectrum of the electrode surface containing a coating containing cyanates described above, it is possible to identify whether the electrode contains a coating containing cyanates. In the same manner, it is possible to identify whether the electrode contains a coating containing sulfates. It is also possible to identify whether the electrode contains a coating containing at least one selected from the group consisting of metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide.
[0188] (XPS analysis of the first binder) The XPS analysis of the first binder can be carried out as follows.
[0189] The active material-containing layer is peeled off from the measurement electrode and dispersed in a solvent such as N-methylpyrrolidone to dissolve the first binder in the solvent. This is filtered to obtain a liquid fraction. The obtained liquid fraction is dried to remove the solvent to obtain a film-like first binder (binder film). The obtained binder film is subjected to XPS analysis.
[0190] The XPS device used may be a Quantera SXM manufactured by ULVAC-PHI, Inc., or a device with equivalent functions. Single crystal spectroscopic Al-Kα radiation (1486.6 eV) is used as the excitation X-ray source. The X-ray output is 4 kW (13 kV x 310 mA), the photoelectron detection angle is 45°, and the analysis area is approximately 4 mm x 0.2 mm. Scanning is performed at 0.10 eV / step.
[0191] In the spectrum obtained by XPS analysis of the binder film, a peak appearing in the range of 680 eV to 691 eV is the F1s peak. From the integrated intensity of the F1s peak, the atomic weight ratio of fluorine atoms (mol / mol) can be calculated using the internal calibration curve of the measurement device. The atomic weight ratio of fluorine atoms is expressed as the amount A of fluorine atoms. F It is.
[0192] The peak appearing in the range of 528 eV to 538 eV is the O1s peak. In the same manner as above, the amount of oxygen atoms A is calculated from the integrated intensity of the O1s peak. O The peak appearing in the range of 392 eV to 408 eV is the N1s peak. In the same manner as above, the amount of nitrogen atoms A can be calculated from the integrated intensity of the N1s peak. N can be calculated.
[0193] When the ratio of the acrylic resin in the first binder is 5% or more and 70% or less, A F , A O and A N However, 0.01≦A F / (A F +A O +2A N )≦0.95.
[0194] (Raman spectroscopy) The inclusion of at least one compound selected from the group consisting of amide compounds and organic sulfur compounds in the aqueous electrolyte can be confirmed by subjecting the aqueous electrolyte to Raman spectroscopy.
[0195] When the battery contains an aqueous electrolyte, the battery can be disassembled, the electrodes can be removed, and the electrodes can be subjected to Raman spectroscopy as samples without being washed. In this way, the aqueous electrolyte attached to the electrodes can be measured. Alternatively, the aqueous electrolyte can be extracted and subjected to Raman spectroscopy as a sample.
[0196] The Raman spectrometer may be a JASCO NRS-7500 or a device with equivalent functions. The above sample is sealed in a sample container such as a glass tube, and the measurement can be performed through the sample container. The measurement can be performed, for example, using a laser beam with a wavelength of 532 nm.
[0197] The secondary battery according to the first embodiment includes an aqueous electrolyte, a positive electrode, and a negative electrode. At least one of the positive electrode and the negative electrode includes a first binder. The first binder includes a fluorine-based resin and an acrylic resin. Therefore, the secondary battery has excellent cycle life performance.
[0198] Second embodiment According to a second embodiment, there is provided a battery pack including a plurality of secondary batteries according to the first embodiment.
[0199] In such a battery pack, the individual cells may be electrically connected in series or parallel, or may be arranged in a combination of series and parallel connections.
[0200] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0201] Fig. 5 is a perspective view showing an example of a battery pack. The battery pack 200 shown in Fig. 5 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the first embodiment.
[0202] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 5 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, so that the plurality of cells are electrically connected to each other.
[0203] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.
[0204] The battery pack according to the second embodiment includes the secondary battery according to the first embodiment, and therefore can achieve excellent cycle life performance.
[0205] (Third embodiment) According to a third embodiment, a battery pack is provided. The battery pack includes the battery pack according to the second embodiment. The battery pack may include a single secondary battery according to the first embodiment instead of the battery pack according to the second embodiment.
[0206] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0207] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, a current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0208] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0209] Fig. 6 is an exploded perspective view showing an example of a battery pack, and Fig. 7 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 6.
[0210] The battery pack 300 shown in Figs. 6 and 7 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0211] 6 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0212] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.
[0213] At least one of the plurality of unit cells 100 is the secondary battery according to the first embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 7. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0214] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0215] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.
[0216] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0217] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.
[0218] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.
[0219] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0220] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0221] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0222] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0223] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0224] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0225] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0226] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal 352 and a negative terminal 353, respectively, of the external terminal 350 for current supply.
[0227] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0228] The battery pack according to the third embodiment includes the secondary battery according to the first embodiment or the battery pack according to the second embodiment, and therefore can achieve excellent cycle life performance.
[0229] (Fourth embodiment) According to a fourth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the third embodiment.
[0230] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0231] Examples of vehicles include, for example, two to four wheel hybrid electric vehicles, two to four wheel electric vehicles, power assisted bicycles, and rail vehicles.
[0232] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0233] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.
[0234] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0235] FIG. 8 is a partially see-through view that illustrates a schematic example of a vehicle.
[0236] A vehicle 400 shown in Fig. 8 includes a vehicle body 40 and a battery pack 300 according to the third embodiment. In the example shown in Fig. 8, the vehicle 400 is a four-wheeled automobile.
[0237] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0238] 8 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0239] Next, an embodiment of a vehicle according to the present embodiment will be described with reference to FIG.
[0240] Fig. 9 is a diagram illustrating an example of a control system for an electrical system in a vehicle. The vehicle 400 illustrated in Fig. 9 is an electric vehicle.
[0241] The vehicle 400 shown in FIG. 9 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.
[0242] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 9, the mounting location of the vehicle power supply 41 is shown diagrammatically.
[0243] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.
[0244] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (for example, VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a to 300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a to 200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.
[0245] Each of the assembled batteries 200a to 200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the first embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive terminal 413 and a negative terminal 414.
[0246] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c, and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a to 200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.
[0247] The battery management unit 411 and the assembled battery monitoring units 301a to 301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a to 301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.
[0248] The battery pack monitoring devices 301a to 301c measure the voltage and temperature of each of the cells constituting the battery packs 200a to 200c based on commands communicated from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.
[0249] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 9) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a-200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a-200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed in the vicinity of the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.
[0250] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.
[0251] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.
[0252] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.
[0253] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.
[0254] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.
[0255] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.
[0256] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.
[0257] The vehicle according to the fourth embodiment is equipped with the battery pack according to the third embodiment, and therefore the cycle life performance of the battery pack is high, and the reliability of the vehicle is therefore high. EXAMPLES
[0258] Examples will be described below, but the embodiments are not limited to the examples described below.
[0259] <Example 1> (Preparation of negative electrode) The negative electrode active material is lithium titanate (Li4Ti5O 12 :TLO) particles were used. 12 The average particle diameter of the particles was 1 μm. Acetylene black was used as the conductive agent. A first binder made by mixing an acrylic resin and a fluororesin was used as the negative electrode binder. The mixing ratio of the acrylic resin and the fluororesin was set so that the ratio of the acrylic resin to the first binder was 20% by mass. An acrylic acid ester polymer was used as the acrylic resin. PVDF was used as the fluororesin. The negative electrode active material, conductive agent, and negative electrode binder were mixed in ratios of 90% by mass, 5% by mass, and 5% by mass, respectively, and dispersed in NMP to prepare a slurry.
[0260] The obtained slurry was applied to a nickel foil having a thickness of 10 μm as a negative electrode current collector, and the coating was dried and subjected to a hot pressing process to prepare a negative electrode.
[0261] (Preparation of positive electrode) Lithium manganese composite oxide (LiMn2O4:LMO) particles having a spinel structure were used as the positive electrode active material. The average particle diameter of the LiMn2O4 particles was 2 μm. Acetylene black was used as the conductive agent. PVDF was used as the positive electrode binder. The positive electrode active material, conductive agent, and positive electrode binder were mixed in proportions of 90 mass%, 5 mass%, and 5 mass%, respectively, and dispersed in NMP to prepare a slurry.
[0262] The obtained slurry was applied to both sides of a titanium foil having a thickness of 10 μm as a positive electrode current collector, dried, and subjected to a pressing process to prepare a positive electrode.
[0263] (Preparation of aqueous electrolyte) 1.2 mol of lithium chloride (LiCl) was mixed as an electrolyte salt with 1 mol of water as an aqueous solvent. Urea was prepared as an additive. The mixture of water and lithium chloride was mixed with urea in a weight ratio of 1:3. Thus, an aqueous electrolyte was prepared.
[0264] (Secondary battery assembly) A secondary battery was fabricated as follows using the prepared negative electrode, positive electrode, and aqueous electrolyte.
[0265] A polyethylene nonwoven fabric having a thickness of 20 μm was prepared as a separator. The surface of the positive electrode was covered with the separator, and the negative electrode was stacked and spirally wound so that the negative electrode active material-containing layer faced the positive electrode active material-containing layer via the separator to prepare an electrode group. This electrode group was pressed to form a flat shape. The electrode group was stored in a thin metal can container made of stainless steel having a thickness of 0.25 mm.
[0266] The aqueous electrolyte was poured into the electrode group in the container to prepare a secondary battery.
[0267] <Example 2> In the preparation of the negative electrode, PVDF was used as a negative electrode binder.
[0268] In the preparation of the positive electrode, a first binder made by mixing an acrylic resin and a fluororesin was used as a positive electrode binder. The mixing ratio of the acrylic resin and the fluororesin was set so that the ratio of the acrylic resin to the first binder was 20 mass%. An acrylic acid ester polymer was used as the acrylic resin. PVDF was used as the fluororesin.
[0269] Except for the above, a secondary battery was fabricated in the same manner as in Example 1.
[0270] <Example 3> A secondary battery was produced in the same manner as in Example 1, except that a negative electrode was produced in the same manner as in Example 1, and a positive electrode was produced in the same manner as in Example 2 and used.
[0271] <Example 4> In the preparation of the positive electrode, lithium phosphate oxide (LiMn 0.8 Fe 0.2PO4:LMFP) particles were used. The average particle diameter of the LMFP particles was 0.8 μm. As the positive electrode binder, a first binder was used in which an acrylic resin and a fluorine-based resin were mixed so that the ratio of the acrylic resin to the first binder was 35 mass%.
[0272] In the preparation of the aqueous electrolyte, the electrolyte salt was changed to LiTFSI. Other than the above, a secondary battery was fabricated in the same manner as in Example 2.
[0273] <Example 5> In the preparation of the positive electrode, lithium nickel cobalt manganese composite oxide (LiNi 0.5 Co 0.2 Mn 0.3 O2:NCM) particles were used. The average particle size of the NCM particles was 5 μm.
[0274] In the preparation of the aqueous electrolyte, the electrolyte salt was changed to LiTFSI. Other than the above, a secondary battery was fabricated in the same manner as in Example 3.
[0275] <Example 6> A secondary battery was produced in the same manner as in Example 5, except that in the production of the negative electrode and the positive electrode, a methacrylic acid ester polymer was used as the acrylic resin.
[0276] <Example 7> A secondary battery was produced in the same manner as in Example 5, except that in the production of the negative electrode and the positive electrode, an acrylonitrile polymer was used as the acrylic resin.
[0277] <Example 8> In the preparation of the negative electrode, monoclinic niobium titanium oxide (TiNb2O7:TNO) particles were used as the negative electrode active material. The average particle diameter of the TNO particles was 1.5 μm. As the acrylic resin, an acrylic acid / acrylonitrile mixed polymer (a copolymer containing acrylic acid and acrylonitrile as monomers) was used.
[0278] In the preparation of the positive electrode, a mixed polymer of acrylic acid and acrylonitrile was used as the acrylic resin. A secondary battery was prepared in the same manner as in Example 5 except for the above.
[0279] <Example 9> In producing the negative electrode, a first binder was used as the negative electrode binder, which was a mixture of an acrylic resin and a fluorine-based resin such that the ratio of the acrylic resin to the first binder was 5% by mass.
[0280] In the preparation of the positive electrode, the LMO particles described in Example 1 were used as the positive electrode active material. As the positive electrode binder, a first binder was used in which an acrylic resin and a fluorine-based resin were mixed so that the ratio of the acrylic resin to the first binder was 5 mass%. As the acrylic resin, an acrylic acid / acrylonitrile mixed polymer was used. A secondary battery was prepared in the same manner as in Example 8 except for the above.
[0281] <Example 10> In the preparation of the negative electrode and the positive electrode, a first binder was used as the negative electrode binder and the positive electrode binder, in which an acrylic resin and a fluorine-based resin were mixed so that the ratio of the acrylic resin to the first binder was 70 mass %. Except for the above, a secondary battery was prepared in the same manner as in Example 9.
[0282] <Example 11> In the preparation of the negative electrode and the positive electrode, a first binder was used as the negative electrode binder and the positive electrode binder, in which an acrylic resin and a fluorine-based resin were mixed so that the ratio of the acrylic resin to the first binder was 2.5 mass%. Except for the above, a secondary battery was prepared in the same manner as in Example 9.
[0283] <Example 12> In the preparation of the negative electrode and the positive electrode, a first binder was used as the negative electrode binder and the positive electrode binder, in which an acrylic resin and a fluorine-based resin were mixed so that the ratio of the acrylic resin to the first binder was 95 mass %. Except for the above, a secondary battery was prepared in the same manner as in Example 9.
[0284] <Example 13> A secondary battery was produced in the same manner as in Example 5, except that in the production of the negative electrode and the positive electrode, an acrylic acid / acrylonitrile mixed polymer was used as the acrylic resin.
[0285] <Example 14> In the preparation of the aqueous electrolyte, the electrolyte salt was changed to LiCl. Dimethyl sulfone was prepared as an additive. A mixture of water and lithium chloride and dimethyl sulfone were mixed in a weight ratio of 1:3. A secondary battery was prepared in the same manner as in Example 13 except for the above.
[0286] <Example 15> In the preparation of the aqueous electrolyte, the electrolyte salt was changed to LiCl. The mixing ratio of water and electrolyte salt was changed to 3 mol of water to 1 mol of electrolyte salt. In addition, the addition of additives was omitted. A secondary battery was prepared in the same manner as in Example 13 except for the above.
[0287] <Example 16> In the preparation of the aqueous electrolyte, the electrolyte salt was changed to LiCl. Urea and ZnCl2 were prepared as additives. A mixture of water and lithium chloride was mixed with urea in a weight ratio of 1:3. ZnCl2 was added to this mixture at a ratio of 0.5 mass% and dissolved. A secondary battery was prepared in the same manner as in Example 8 except for the above.
[0288] <Example 17> A secondary battery was fabricated in the same manner as in Example 16, except that in the preparation of the aqueous electrolyte, ZnCl2 was changed to SnCl2.
[0289] <Example 18> In the preparation of the aqueous electrolyte, PbCl2 was added instead of ZnCl2. PbCl2 was suspended in the aqueous solvent. Except for the above, a secondary battery was fabricated in the same manner as in Example 16.
[0290] <Example 19> In the preparation of the aqueous electrolyte, the mixing ratio of water and electrolyte salt was changed to 3 mol of water and 1 mol of electrolyte salt. In addition, no additive was added. A secondary battery was prepared in the same manner as in Example 16 except for the above.
[0291] <Comparative Example 1> In the preparation of the negative electrode and the positive electrode, PVDF was used as the negative electrode binder and the positive electrode binder. Except for the above, a secondary battery was prepared in the same manner as in Example 8.
[0292] <Comparative Example 2> In the preparation of the negative electrode and the positive electrode, an acrylic acid / acrylonitrile mixed polymer was used as the negative electrode binder and the positive electrode binder. A secondary battery was prepared in the same manner as in Example 8 except for the above.
[0293] <Comparative Example 3> In producing the positive electrode, the positive electrode active material used was the LMFP particles described in Example 4. A secondary battery was produced in the same manner as in Comparative Example 1 except for the above.
[0294] The secondary batteries produced in each of the Examples and Comparative Examples were initially charged at a constant current of 0.1 C at 45° C.
[0295] For each of the Examples and Comparative Examples, the negative electrode designs are shown in Tables 1 and 2, the positive electrode designs are shown in Tables 3 and 4, and the aqueous electrolyte compositions are shown in Table 5, respectively.
[0296] [Table 1]
[0297] [Table 2]
[0298] [Table 3]
[0299] [Table 4]
[0300] [Table 5]
[0301] <Identifying the type of coating> The positive and negative electrodes of the batteries of each of the Examples and Comparative Examples after the first charge were subjected to FT-IR analysis and XPS analysis by the above-mentioned methods.
[0302] From the results of XPS analysis of the electrodes included in each of the Examples and Comparative Examples, O , A F , A N and A F / (A F +A O +2A N The values obtained for the negative electrode are shown in Table 6. The values obtained for the positive electrode are shown in Table 7.
[0303] [Table 6]
[0304] [Table 7]
[0305] From the FT-IR and XPS analysis results of the electrodes in each Example and Comparative Example after the first charge, the components contained in the coating formed on the electrodes were identified by the above-mentioned method. The types of coating formed on the negative and positive electrodes in each Example and Comparative Example are shown in Tables 8 and 9.
[0306] [Table 8]
[0307] [Table 9]
[0308] <Performance evaluation> The performance evaluation of the secondary batteries according to the respective examples and comparative examples was carried out as follows.
[0309] (1C cycle average efficiency) The 1C cycle average efficiency was measured as follows. After constant current charging at 1C, constant current discharging at 1C was performed. This charging and discharging was regarded as one cycle. The charge capacity and discharge capacity were measured during charging and discharging, respectively. The discharge capacity was divided by the charge capacity and multiplied by 100 to obtain the coulombic efficiency. The above charging and discharging was repeated for a total of 100 cycles, and the coulombic efficiency was measured for each of the 100 cycles. The average value of the coulombic efficiency for the 100 cycles was regarded as the 1C cycle average efficiency (%).
[0310] (Rate of resistance increase) The resistance increase rate was measured as follows. 100 cycles of charging and discharging were performed in the same manner as in the above 1C cycle average efficiency measurement. The average discharge voltage was measured during the first cycle discharge and the 100th cycle discharge. In addition, a constant current discharge was performed at 0.05C using another cell of the same configuration, and the average discharge voltage Va at 0.05C was measured. Va, the average discharge voltage V1 at the first cycle, and the average discharge voltage V at the 100th cycle were measured. 100 The rate of change in resistance was calculated using the following formula, and this was taken as the rate of increase in resistance (%).
[0311]
number
[0312] Table 10 shows the measurement results of the 1C cycle average efficiency and the resistance increase rate for each of the examples and comparative examples.
[0313] <Result>
[0314] [Table 10]
[0315] The secondary batteries according to the examples all had high 1C cycle average efficiency and low resistance increase rates, which revealed that they were excellent in cycle life performance.
[0316] In Example 1, only the negative electrode contains the first binder containing a fluorine-based resin and an acrylic resin. In Example 2, only the positive electrode contains the first binder. In Example 3, both the negative electrode and the positive electrode contain the first binder. Comparing these Examples, Example 3 had a higher 1C cycle average efficiency and a lower resistance increase rate than Examples 1 and 2. Therefore, it was revealed that the cycle life performance can be further improved when both the negative electrode and the positive electrode contain the first binder.
[0317] Comparative Example 1 is a comparative example containing NCM as a positive electrode active material and only PVDF as a positive electrode binder. Comparative Example 3 is similar to Comparative Example 1 except that it contains LMFP as a positive electrode active material. Comparative Example 3 has a lower 1C cycle average efficiency and a higher resistance increase rate than Comparative Example 1. This is believed to be due to the fact that LMFP is a positive electrode active material that is more prone to side reactions than NCM.
[0318] Example 4 is a secondary battery using a positive electrode containing LMFP as a positive electrode active material, similar to Comparative Example 3. Example 4, which contains a first binder containing a fluorine-based resin and an acrylic resin, had a higher 1C cycle average efficiency and a lower resistance increase rate than Comparative Example 3. Therefore, it was revealed that the cycle life performance can be improved even when a secondary battery is produced by combining a first binder containing a fluorine-based resin and an acrylic resin with a positive electrode active material that tends to easily cause side reactions.
[0319] Examples 5 to 7 and Example 13 are secondary batteries produced under similar conditions, except that the type of acrylic resin contained in the first binder is different. All of these secondary batteries had higher 1C cycle average efficiency and lower resistance increase rate than the comparative example. Therefore, it was revealed that the cycle life performance of the secondary battery can be improved regardless of whether the acrylic resin contains any of acrylic acid ester polymer, methacrylic acid ester polymer, acrylonitrile polymer, and acrylic acid / acrylonitrile mixed polymer.
[0320] The secondary batteries in Examples 8 and 13 were fabricated under similar conditions, except that the negative electrode active materials were TNO and TLO, respectively. These secondary batteries all had higher 1C cycle average efficiency and lower resistance increase rates than the comparative example. Therefore, it was revealed that the cycle life performance of the secondary battery can be improved regardless of whether it contains TNO or TLO as the negative electrode active material.
[0321] Examples 9 to 12 are secondary batteries produced under similar conditions, except that the ratio of the acrylic resin to the first binder is different. Examples 9 and 10, in which the ratio of the acrylic resin to the first binder is in the range of 5% by mass or more and 70% by mass or less, tended to have higher 1C cycle average efficiency than Example 11, in which the ratio of the acrylic resin to the first binder is less than 5% by mass. Also, compared to Example 12, in which the ratio of the acrylic resin to the first binder is higher than 70% by mass, the resistance increase rate tended to be lower. Therefore, it was revealed that the secondary battery in which the ratio of the acrylic resin to the first binder is in the range of 5% by mass or more and 70% by mass or less is particularly excellent in cycle life performance.
[0322] In addition, when comparing Examples 9 to 12, which have different ratios of acrylic resin to the first binder, Comparative Example 1, which does not contain acrylic resin, and Comparative Example 2, which does not contain fluororesin, it is found that as the ratio of acrylic resin to the total of fluororesin and acrylic resin increases, F / (A F +A O +2AN A tendency for the value of A to become smaller was evident. F , A O and A N However, 0.01≦A F / (A F +A O +2A N In Examples 9 to 12, A satisfies 0.95. F / (A F +A O +2A N In comparison with Comparative Example 1, in which A was larger than 0.95, the average efficiency of 1C cycle was higher in both cases. F / (A F +A O +2A N In comparison with Comparative Example 2, in which A) was less than 0.01, the resistance increase rate was lower in both cases. F , A O and A N However, 0.01≦A F / (A F +A O +2A N It has become clear that a secondary battery satisfying the condition (a) of 0.95 or less has particularly excellent cycle life performance.
[0323] Also, A F , A O and A N is 0.5≦A F / (A F +A O +2A N In Examples 1 to 8 and 13 to 19, which include electrodes that satisfy the condition A ≦0.8, F / (A F +A O +2A N ) was larger than 0.8, the 1C cycle average efficiency tended to be higher than in Examples 9 and 11 and Comparative Examples 1 and 3. F / (A F +A O +2A N The resistance increase rate tended to be smaller than that in Examples 10 and 12 and Comparative Example 2, in which A was smaller than 0.5. F , A O and A N is 0.5≦A F / (A F +A O +2A N It has become clear that secondary batteries that satisfy the condition 0.8≦1.0 are particularly excellent in cycle life performance.
[0324] Example 15 is a secondary battery similar to Example 13, except that an aqueous electrolyte not containing urea as an additive was used as the aqueous electrolyte. Although the addition of an additive was omitted in Example 15, the 1C cycle average efficiency was high and the resistance increase rate was low. This is believed to be because in Example 15, LiTFSI contained in the aqueous electrolyte was decomposed, forming a coating containing lithium fluoride, lithium oxide, lithium sulfite, and lithium sulfate.
[0325] Examples 16 to 18 are secondary batteries fabricated in the same manner except that different types of additives were added to the aqueous electrolyte. Example 19 is a secondary battery fabricated in the same manner as Examples 16 to 18 except that an aqueous electrolyte not containing urea as an additive was used as the aqueous electrolyte.
[0326] A coating containing the metal element contained in the additive was formed on the surface of the negative electrode in Examples 16 to 18. The coating further contained lithium isocyanate. The surface of the negative electrode in Example 16 contained metallic zinc, zinc oxide, and zinc hydroxide. The surface of the negative electrode in Example 17 contained metallic tin. The surface of the negative electrode in Example 18 contained metallic lead.
[0327] The electrode of Example 19 was not coated.
[0328] Compared with Example 19, Examples 16 to 18 tended to have a lower resistance increase rate.
[0329] In addition, when Example 8 and Example 19, which were prepared in the same manner except for using an aqueous electrolyte with a different composition, were compared, Example 8 tended to have a higher 1C cycle average efficiency and a lower resistance increase rate. A coating containing lithium isocyanate, lithium fluoride, lithium oxide, lithium sulfite, and lithium sulfate was formed on the surface of the electrode in Example 8.
[0330] From a comparison of the above Examples 8, 16 to 18 with Example 19, it has become clear that a secondary battery in which the negative electrode contains a first binder and the surface of the negative electrode contains at least one selected from the group consisting of cyanates, sulfates, metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide has a particularly excellent effect of suppressing an increase in resistance.
[0331] Examples 1 to 3, 14, 16 to 18, and Example 19, in which the aqueous electrolyte contains LiCl as an electrolyte salt, are compared. Examples 1 to 3 further contain urea, an amide compound, as an additive. Example 14 further contains dimethylsulfone, an organic sulfur compound, as an additive. Example 16 further contains ZnCl2, a salt containing Zn, as an additive. Example 17 further contains SnCl2, a salt containing Sn, as an additive. Example 18 further contains PbCl2, a salt containing Pb, as an additive. Example 19 does not contain any additive.
[0332] Comparing these Examples, Examples 1 to 3, 14, and 16 to 18 tended to have higher 1C cycle average efficiency than Example 19. Therefore, it was revealed that particularly excellent cycle life performance can be achieved when the aqueous electrolyte contains at least one selected from the group consisting of a salt containing at least one element selected from the group consisting of Zn, Sn, and Pb, an amide compound, and an organic sulfur compound.
[0333] According to at least one of the embodiments described above, a secondary battery is provided. The secondary battery includes an aqueous electrolyte, a positive electrode, and a negative electrode. At least one of the positive electrode and the negative electrode includes a first binder. The first binder includes a fluorine-based resin and an acrylic resin. Therefore, the secondary battery can achieve excellent cycle life performance.
[0334] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims.
[0335] The invention according to the embodiment will be described below.
[0336] <1> The battery includes an aqueous electrolyte, a positive electrode, and a negative electrode, At least one of the positive electrode and the negative electrode contains a first binder; The first binder comprises a fluorine-based resin and an acrylic resin.
[0337] <2> The first binder satisfies the following formula (1): 0.01≦A F / (A F +A O +2A N )≦0.95 (1) However, the above A O is the amount of oxygen atoms, F is the amount of fluorine atoms, N is the amount of nitrogen atoms, and A O +A N >0, A F >0, <1> The secondary battery described herein.
[0338] <3> The acrylic resin is a polymer containing at least one selected from the group consisting of acrylic acid esters, methacrylic acid esters, and acrylonitrile. <1> or <2> The secondary battery described herein.
[0339] <4> The X-ray photoelectron spectroscopy spectrum of the surface of the electrode has a peak in the range of 292 eV to 294 eV. <1> ~ <3> 13. The secondary battery according to claim 12 .
[0340] <5> The fluororesin is a polymer containing vinylidene fluoride. <1> ~ <4> 13. The secondary battery according to claim 12 .
[0341] <6> The X-ray photoelectron spectroscopy spectrum of the surface of the electrode has a peak in the range of 398 eV to 402 eV. <1> ~ <5> 13. The secondary battery according to claim 12 .
[0342] <7> The X-ray photoelectron spectroscopy spectrum of the surface of the electrode has a peak in the range of 168 eV to 173 eV. <1> ~ <6> 13. The secondary battery according to claim 12 .
[0343] <8> The aqueous electrolyte contains at least one selected from the group consisting of a salt containing at least one element selected from the group consisting of Zn, Sn, and Pb, an amide compound, and an organic sulfur compound. <1> ~ <7> 13. The secondary battery according to claim 12 .
[0344] <9> the negative electrode contains the first binder as a negative electrode binder, The surface of the negative electrode contains at least one selected from the group consisting of cyanates, sulfates, metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide; <1> ~ <8> 13. The secondary battery according to claim 12 .
[0345] <10> The positive electrode is At least one positive electrode active material selected from the group consisting of lithium manganese composite oxides, lithium phosphates having an olivine structure, and lithium nickel cobalt manganese composite oxides; The positive electrode binder includes the first binder, <1> ~ <9> 13. The secondary battery according to claim 12 .
[0346] <11> The negative electrode is At least one negative electrode active material selected from the group consisting of lithium titanate having a spinel structure and monoclinic niobium titanium oxide; The negative electrode binder includes the first binder, <1> ~ <10> 13. The secondary battery according to claim 12 .
[0347] <12> <1> ~ <11> 13. A battery pack comprising the secondary battery according to claim 12.
[0348] <13> An external terminal for supplying electricity; Protection circuit and Further includes <12> The battery pack according to claim 1 .
[0349] <14> A plurality of the secondary batteries are included, The secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel. <12> or <13> The battery pack according to claim 1 .
[0350] <15> <12> ~ <14> 2. A vehicle equipped with the battery pack according to claim 1.
[0351] <16> A mechanism for converting the kinetic energy of the vehicle into regenerative energy is included. <15> A vehicle as described in. [Explanation of symbols]
[0352] 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode active material-containing layer, 3c...negative electrode current collector tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 21...bus bar, 22...positive electrode side lead, 22a...other end, 23...negative electrode side lead, 23a...other end, 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 200...battery pack, 200a...battery pack, 200b...battery pack, 200c...battery pack, 300...battery pack, 30 0a...battery pack, 300b...battery pack, 300c...battery pack, 301a...assembled battery monitoring device, 301b...assembled battery monitoring device, 301c...assembled battery monitoring device, 342...positive connector, 343...negative connector, 345...thermistor, 346...protection circuit, 342a...wiring, 343a...wiring, 350...external terminal for energization, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.
Claims
1. The battery includes an aqueous electrolyte, a positive electrode, and a negative electrode, At least one of the positive electrode and the negative electrode contains a first binder, The first binder comprises a fluorine-based resin and an acrylic resin.
2. The first binder satisfies the following formula (1): 0.01≦A F / (A F +A O +2A N )≦0.95 (1) However, the above A O is the amount of oxygen atoms, F is the amount of fluorine atoms, N is the amount of nitrogen atoms, and A O +A N >0, A F The secondary battery according to claim 1 , wherein
3. 2. The secondary battery in accordance with claim 1, wherein the acrylic resin is a polymer containing at least one selected from the group consisting of acrylic acid esters, methacrylic acid esters, and acrylonitrile.
4. 2. The secondary battery according to claim 1, wherein an X-ray photoelectron spectroscopy spectrum of the surface of the electrode has a peak in a range of 292 eV to 294 eV.
5. 2. The secondary battery according to claim 1, wherein the fluorine-based resin is a polymer containing vinylidene fluoride.
6. 2. The secondary battery according to claim 1, wherein an X-ray photoelectron spectroscopy spectrum of the surface of the electrode has a peak in a range of 398 eV to 402 eV.
7. 2. The secondary battery according to claim 1, wherein an X-ray photoelectron spectroscopy spectrum of the surface of the electrode has a peak in a range of 168 eV to 173 eV.
8. 2. The secondary battery according to claim 1, wherein the aqueous electrolyte contains at least one selected from the group consisting of a salt containing at least one element selected from the group consisting of Zn, Sn, and Pb, an amide compound, and an organic sulfur compound.
9. the negative electrode contains the first binder as a negative electrode binder, 2. The secondary battery in accordance with claim 1, wherein the surface of the negative electrode comprises at least one selected from the group consisting of cyanates, sulfates, metallic zinc, metallic tin, metallic lead, lithium fluoride, lithium oxide, zinc oxide, and zinc hydroxide.
10. The positive electrode is At least one positive electrode active material selected from the group consisting of lithium manganese composite oxide, lithium phosphate having an olivine structure, and lithium nickel cobalt manganese composite oxide; The secondary battery in accordance with claim 1 , further comprising the first binder as a positive electrode binder.
11. The negative electrode is At least one negative electrode active material selected from the group consisting of lithium titanate having a spinel structure and monoclinic niobium titanium oxide; The secondary battery in accordance with claim 1 , further comprising the first binder as a negative electrode binder.
12. A battery pack comprising the secondary battery according to claim 1.
13. An external terminal for supplying electricity; Protection circuit and The battery pack of claim 12 further comprising:
14. A plurality of the secondary batteries are included, The battery pack according to claim 12 , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
15. A vehicle equipped with the battery pack according to claim 12.
16. 16. The vehicle of claim 15, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.
Citation Information
Patent Citations
Aqueous electrolyte battery pole piece, battery and pole piece preparation method
CN114678488A
Ni-h secondary battery
JP1992179052A
Hydrogen storage electrode and its manufacture
JP1994044964A
Lithium secondary battery negative electrode, its manufacture, and secondary battery using negative electrode
JP1998172573A
Secondary battery, battery pack and vehicle
JP2018156837A
Cited By
Positive electrode for nonaqueous electrolyte secondary battery and battery using same
WO2026121231A1
Positive electrode composition, positive electrode composition slurry, positive electrode composition layer, positive electrode, and secondary battery
WO2026192006A1