Method for manufacturing semiconductor device
By forming a porous silicon layer within an insulating film using anodization, the method stabilizes the manufacturing process of semiconductor devices, addressing positional and electrolyte flow issues to enhance bonding and separation consistency.
Patent Information
- Application Number
- JP2023046865
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The challenge in manufacturing semiconductor devices is to achieve a stable manufacturing process when bonding two substrates together, particularly in the context of three-dimensional NAND flash memory production, where the formation of a porous silicon layer can lead to instability due to variations in position and electrolyte flow, causing dust generation and process inconsistencies.
The method involves forming an insulating film on the outer periphery of a substrate, followed by creating a porous silicon layer using an anodization process, which is contained within the insulating film to stabilize the position of the porous layer, thereby ensuring consistent bonding and separation of substrates.
This approach stabilizes the manufacturing process by controlling the position of the porous silicon layer, reducing dust generation and process variability, leading to more reliable bonding and separation of substrates in semiconductor devices.
Smart Images

Figure 2024135945000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to a method for manufacturing a semiconductor device. [Background technology]
[0002] For example, a highly functional or highly integrated semiconductor device can be realized by bonding a support substrate on which a first electronic circuit is formed and a semiconductor substrate on which a second electronic circuit is formed. After bonding the support substrate and the semiconductor substrate, for example, the support substrate is separated and reused in order to reduce the manufacturing cost of the semiconductor device. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-112880 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of one embodiment of the present invention is to realize a stable manufacturing process when manufacturing a semiconductor device by bonding two substrates together. [Means for solving the problem]
[0005] In a method for manufacturing a semiconductor device according to an embodiment, an insulating film is formed on the outer periphery of a surface of a first substrate, and after forming the insulating film, a silicon layer is formed in contact with the surface inside the insulating film, and the silicon layer inside the insulating film is made porous using an anodization method to form a porous silicon layer. [Brief description of the drawings]
[0006] [Figure 1] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Diagram 2] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Diagram 3] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 4] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Diagram 5] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 6] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 7] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 8] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 9] 2A to 2C are explanatory views of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 10] 5A to 5C are explanatory diagrams of a manufacturing method of a semiconductor device according to a comparative example. [Figure 11] 5A to 5C are explanatory diagrams of a manufacturing method of a semiconductor device according to a comparative example. [Figure 12] 5A to 5C are explanatory views for the operation and effect of the manufacturing method according to the first embodiment. [Figure 13] 5A to 5C are explanatory views of a method for manufacturing a semiconductor device according to a first modified example of the first embodiment. [Figure 14] 6A to 6C are explanatory views of a method for manufacturing a semiconductor device according to a second modified example of the first embodiment. [Figure 15] 5A to 5C are explanatory views of a method for manufacturing a semiconductor device according to a second embodiment. [Figure 16] 5A to 5C are explanatory views of a method for manufacturing a semiconductor device according to a second embodiment. [Figure 17] 10A to 10C are explanatory diagrams of a manufacturing method of a semiconductor device according to a modified example of the second embodiment. [Figure 18] 10A to 10C are explanatory diagrams of a manufacturing method of a semiconductor device according to a third embodiment. [Figure 19] 10A to 10C are explanatory diagrams of a manufacturing method of a semiconductor device according to a third embodiment. [Figure 20] 10A to 10C are explanatory diagrams of a manufacturing method of a semiconductor device according to a third embodiment. [Figure 21] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a first modified example of the third embodiment. [Figure 22] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a first modified example of the third embodiment. [Figure 23] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a first modified example of the third embodiment. [Figure 24] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a first modified example of the semiconductor device of the third embodiment. [Diagram 25] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a second modified example of the third embodiment. [Figure 26] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a second modified example of the third embodiment. [Figure 27] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a second modified example of the third embodiment. [Figure 28] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a fourth embodiment. [Figure 29] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a fourth embodiment. [Diagram 30] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a fourth embodiment. [Diagram 31] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a fourth embodiment. [Diagram 32] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a fifth embodiment. [Diagram 33] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a fifth embodiment. [Diagram 34] 13A to 13C are explanatory views of a method for manufacturing a semiconductor device according to a fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, the same reference numerals will be used to designate the same or similar components, and the description of components that have already been described will be omitted as appropriate.
[0008] In addition, the terms "upper" and "lower" may be used for convenience in this specification. "Upper" and "lower" are terms that indicate, for example, a relative positional relationship in a drawing. The terms "upper" and "lower" do not necessarily specify a positional relationship with respect to gravity.
[0009] The qualitative and quantitative analysis of the chemical composition of the members constituting the semiconductor device in this specification can be performed by, for example, secondary ion mass spectrometry (SIMS) or energy dispersive X-ray spectroscopy (EDX). In addition, the thickness of the members constituting the semiconductor device, the distance between the members, etc. can be measured by, for example, a scanning electron microscope (SEM).
[0010] (First embodiment) The method for manufacturing a semiconductor device of the first embodiment includes forming an insulating film on the outer periphery of the surface of a first substrate, forming a silicon layer in contact with the inner surface of the insulating film after the insulating film is formed, and making the silicon layer on the inner side of the insulating film porous using an anodization method to form a porous silicon layer.
[0011] The method for manufacturing a semiconductor device according to the first embodiment is a method for manufacturing a semiconductor device by bonding two substrates together. The semiconductor device is, for example, a semiconductor memory. The semiconductor memory is, for example, a three-dimensional NAND flash memory in which memory cells are arranged three-dimensionally.
[0012] Figures 1(a), 1(b), 1(c), 1(d), 2(a), 2(b), 3(a), 3(b), 3(c), 4, 5(a), 5(b), 6(a), 6(b), 7(a), 7(b), 8, and 9 are explanatory diagrams of a manufacturing method of a semiconductor device according to the first embodiment.
[0013] Figures 1(a), 1(b), 1(c), 1(d), 2(a), 3(a), 3(b), 3(c), 5(a), 5(b), 6(a), 6(b), 7(a), 7(b), 8, and 9 are schematic cross-sectional views. Figure 2(b) is a schematic top view. Figure 4 is a schematic view of an example of an anodizing apparatus.
[0014] First, a support substrate 10 is prepared (FIG. 1(a)). The support substrate 10 is an example of a first substrate.
[0015] The support substrate 10 is a conductor. The support substrate 10 is, for example, a semiconductor. The support substrate 10 is, for example, single crystal silicon. The support substrate 10 is, for example, a silicon substrate. The support substrate 10 is, for example, a p-type silicon substrate containing boron (B) as a p-type impurity. The support substrate 10 is, for example, a silicon wafer. The support substrate 10 is, for example, a p-type silicon wafer containing boron (B) as a p-type impurity. The support substrate 10 may be, for example, an insulating substrate such as a quartz substrate.
[0016] The diameter of the support substrate 10 is, for example, not less than 150 mm and not more than 300 mm.
[0017] Next, an insulating film 12 is formed on the surface of the support substrate 10 (FIG. 1(b)). The insulating film 12 is formed by using, for example, a chemical vapor deposition method (CVD method).
[0018] The insulating film 12 is, for example, an oxide, a nitride, an oxynitride, or a carbide, and is, for example, a silicon oxide, a silicon nitride, or a nitrogen-added silicon carbide.
[0019] The thickness of the insulating film 12 is, for example, not less than 100 nm and not more than 10 μm.
[0020] Next, a photoresist film 14 is formed so as to cover the insulating film 12 on the outer periphery of the support substrate 10 (FIG. 1(c)). The photoresist film 14 is formed by patterning using, for example, a photolithography method.
[0021] For example, when a positive resist is used as the photoresist film 14, the photoresist film 14 is applied to the surface of the support substrate 10, and then the central portion of the support substrate 10 is exposed to light to expose the photoresist film 14, thereby removing the photoresist film 14 from the central portion of the support substrate 10.
[0022] Furthermore, for example, when a negative resist is used as the photoresist film 14, the photoresist film 14 is applied to the surface of the support substrate 10, and then the outer periphery of the support substrate 10 is exposed to light to expose the photoresist film 14, thereby removing the photoresist film 14 from the central portion of the support substrate 10.
[0023] Next, the insulating film 12 in the center of the support substrate 10 is removed using the patterned photoresist film 14 as a mask (FIG. 1(d)). The insulating film 12 is removed by using, for example, a wet etching method.
[0024] Next, the photoresist film 14 is removed (FIG. 2(a)). As shown in FIGS. 2(a) and 2(b), a ring-shaped insulating film 12 is formed on the outer periphery of the support substrate 10.
[0025] The distance from the outer edge of the support substrate 10 to the inner edge of the annular insulating film 12 (d in FIG. 2(b)) is, for example, 1 mm or more and 10 mm or less. In FIG. 2(b), the outer edge of the insulating film 12 may coincide with the outer edge of the support substrate 10.
[0026] Next, a polycrystalline silicon layer 16 is formed on the surface of the support substrate 10 (FIG. 3(a)). The polycrystalline silicon layer 16 is an example of a silicon layer. The polycrystalline silicon layer 16 is formed inside the insulating film 12 so as to contact the surface of the support substrate 10.
[0027] The polycrystalline silicon layer 16 is formed by, for example, a CVD method. The thickness of the polycrystalline silicon layer 16 is, for example, not less than 100 nm and not more than 10 μm.
[0028] Next, the polycrystalline silicon layer 16 formed on the insulating film 12 is removed (FIG. 3(b)). The polycrystalline silicon layer 16 is removed by using, for example, a chemical mechanical polishing method (CMP method).
[0029] Next, the polycrystalline silicon layer 16 inside the insulating film 12 is made porous by anodization (FIG. 3(c)). By making the polycrystalline silicon layer 16 porous, a porous silicon layer 18 is formed inside the insulating film 12. The porous silicon layer 18 has a void inside.
[0030] Fig. 4 is a schematic diagram of an example of an anodizing apparatus 20 used to make the polycrystalline silicon layer 16 porous. Fig. 4 illustrates a state in which the support substrate 10 is being processed.
[0031] 4, the anodizing apparatus 20 includes a treatment tank 21, a substrate holder 22, a first electrode 23, and a second electrode 24. The anodizing apparatus 20 is, for example, a batch-type apparatus capable of simultaneously treating a plurality of substrates.
[0032] The treatment tank 21 is, for example, a container made of a fluororesin. An electrolytic solution 25 is stored in the treatment tank 21. The electrolytic solution 25 contains, for example, hydrofluoric acid.
[0033] The substrate holder 22 holds the support substrate 10. The substrate holder 22 has a support portion 22a and a seal portion 22b. The seal portion 22b has a function of blocking a flow path of the electrolyte from one surface side to the other surface side of the support substrate 10. The seal portion 22b is, for example, an O-ring.
[0034] A voltage is applied between the first electrode 23 and the second electrode 24. For example, a positive voltage is applied to the first electrode 23, and a negative voltage is applied to the second electrode 24. In this case, the first electrode 23 is a positive electrode, and the second electrode 24 is a negative electrode. As shown by the arrow in FIG. 4, a current flows through the support substrate 10 to the electrolyte 25 between the first electrode 23 and the second electrode.
[0035] The silicon layer on the cathode side of the support substrate 10, i.e., on the side of the second electrode 24 of the support substrate 10 held in the electrolytic solution 25, is made porous by anodization to form a porous silicon layer 18. The insulating film 12 has a higher resistance than the polycrystalline silicon layer 16, and is therefore less likely to be made porous.
[0036] After the polycrystalline silicon layer 16 is made porous to form the porous silicon layer 18, the memory layer 30 is formed on the porous silicon layer 18 (FIG. 5(a)). The memory layer 30 is formed using a known process technology.
[0037] Fig. 5(b) is an enlarged view of a region R1 surrounded by a dashed line in Fig. 5(a). As shown in Fig. 5(b), the memory layer 30 includes a memory cell array 30x having a plurality of memory cells. The plurality of memory cells are, for example, three-dimensionally arranged in the memory cell array 30x. The memory cells included in the memory cell array 30x are, for example, three-terminal nonvolatile memory cells.
[0038] The memory cell array 30x is an example of a first electronic circuit.
[0039] Next, a semiconductor substrate 40 is prepared (FIG. 6(a)). The semiconductor substrate 40 is an example of a second substrate.
[0040] Figures 6(a) and 6(b) are schematic cross-sectional views of a semiconductor substrate 40. Figure 6(b) is an enlarged schematic cross-sectional view of a portion of the semiconductor substrate. Figure 6(b) is an enlarged view of a region R2 surrounded by a dashed line in Figure 6(a).
[0041] As shown in FIG. 6(b), the semiconductor substrate 40 includes, for example, a semiconductor layer 40a and a wiring layer 40b. The semiconductor layer 40a is, for example, single crystal silicon. The semiconductor substrate 40 includes, for example, a silicon substrate. The semiconductor substrate 40 is, for example, a silicon wafer. The semiconductor substrate 40 is, for example, a p-type silicon wafer containing boron (B) as a p-type impurity.
[0042] The semiconductor substrate 40 includes a control circuit 40x. The control circuit 40x is an example of a second electronic circuit.
[0043] The control circuit 40x is formed of a semiconductor layer 40a and a wiring layer 40b. The control circuit 40x is formed of, for example, transistors and multi-layer wiring that connects between the transistors. The control circuit 40x is, for example, a CMOS circuit including n-type transistors and p-type transistors.
[0044] Next, as shown in FIG. 7(a), the wiring layer 40b of the semiconductor substrate 40 and the memory layer 30 are made to face each other.
[0045] 7(b), the support substrate 10 and the semiconductor substrate 40 are bonded together. The memory layer 30 formed on the support substrate 10 and the wiring layer 40b of the semiconductor substrate 40 are bonded together so that they come into contact with each other. The support substrate 10 and the semiconductor substrate 40 are bonded together so that the memory cell array 30x of the memory layer 30 and the control circuit 40x of the semiconductor substrate 40 are physically and electrically connected to each other.
[0046] For example, mechanical pressure is applied between the support substrate 10 and the semiconductor substrate 40. For example, by applying heat treatment while applying mechanical pressure, the memory layer 30 and the wiring layer 40b are bonded together. The temperature of the heat treatment is, for example, 300° C. or higher and 500° C. or lower. By applying heat treatment while applying mechanical pressure between the support substrate 10 and the semiconductor substrate 40, the strength of the bonding surface between the support substrate 10 and the semiconductor substrate 40 is increased.
[0047] Fig. 8 is an enlarged view of a region R3 surrounded by a dashed line in Fig. 7(b). The memory layer 30 and the wiring layer 40b are joined together to electrically connect the memory cell array 30x and the control circuit 40x. The control circuit 40x has, for example, a function of controlling the operation of the memory cell array 30x.
[0048] 9, the support substrate 10 and the semiconductor substrate 40 are separated with the porous silicon layer 18 as a boundary. That is, the support substrate 10 and the memory layer 30 are separated with the porous silicon layer 18 as a boundary. That is, the support substrate 10 and the memory cell array 30x are separated with the porous silicon layer 18 as a boundary.
[0049] For example, by pressing a wedge-shaped tool from the side toward the boundary between the memory layer 30 and the wiring layer 40b and / or spraying a water jet, the porous silicon layer 18 is mechanically divided starting from the boundary between the memory layer 30 and the wiring layer 40b, and the support substrate 10 and the semiconductor substrate 40 are separated.
[0050] The porous silicon layer 18 remaining on the separated semiconductor substrate 40 is removed by, for example, the CMP method.
[0051] Thereafter, the bonded semiconductor substrate 40 and memory layer 30 are divided into a plurality of semiconductor memory chips using, for example, a blade dicing method.
[0052] The porous silicon layer 18 or the insulating film 12 remaining on the separated support substrate 10 is removed by, for example, a CMP method. The support substrate 10 can then be reused and used in the manufacture of a semiconductor device.
[0053] By the above manufacturing method, the support substrate 10 and the semiconductor substrate 40 are bonded together to manufacture the 3D NAND flash memory of the first embodiment.
[0054] Next, the operation and effects of the method for manufacturing the semiconductor device according to the first embodiment will be described.
[0055] 10(a), 10(b), 10(c), and 11 are explanatory diagrams of a method for manufacturing a semiconductor device of a comparative example.
[0056] Figures 10(a), 10(b), and 10(c) are schematic cross-sectional views. Figure 11 is a schematic view of an example of an anodizing apparatus.
[0057] The method for manufacturing a semiconductor device of the comparative example differs from the method for manufacturing a semiconductor device of the first embodiment in that the annular insulating film 12 is not formed on the outer periphery of the support substrate 10.
[0058] First, a support substrate 10 is prepared (FIG. 10(a)). The support substrate 10 is, for example, a silicon substrate.
[0059] Next, a polycrystalline silicon layer 16 is formed on the surface of the support substrate 10 (FIG. 10(b)). The polycrystalline silicon layer 16 is formed by using, for example, a CVD method.
[0060] Next, the polycrystalline silicon layer 16 is made porous by anodization (FIG. 10(c)). By making the polycrystalline silicon layer 16 porous, a porous silicon layer 18 is formed. The porous silicon layer 18 has a hollow portion therein. The outermost periphery of the polycrystalline silicon layer 16 remains without being made porous.
[0061] 11 is a schematic diagram of an example of an anodizing apparatus 20 used to make the polycrystalline silicon layer 16 porous. The anodizing apparatus 20 has the same configuration as the apparatus used in the manufacturing method of the first embodiment.
[0062] As in the first embodiment, the silicon layer on the cathode side of the support substrate 10, i.e., the side of the second electrode 24 of the support substrate 10 held in the electrolyte, is made porous by anodization, and a porous silicon layer 18 is formed.
[0063] Figures 12(a) and 12(b) are explanatory views of the operation and effect of the manufacturing method of the first embodiment. Figures 12(a) and 12(b) are enlarged views of the substrate holder 22 of the anodizing apparatus 20. Figure 12(a) is a view showing the case where a support substrate 10 of a comparative example is processed, and Figure 12(b) is a view showing the case where a support substrate 10 of the first embodiment is processed.
[0064] The substrate holder 22 has a support portion 22a and a seal portion 22b. The seal portion 22b has a function of blocking a flow path of the electrolyte from one surface side to the other surface side of the support substrate 10. By blocking the flow path of the electrolyte with the seal portion 22b, the current is prevented from flowing along the outer edge of the support substrate 10, and the current flows through the support substrate 10.
[0065] 12(a), in the comparative example, the flow path of the electrolyte is blocked by the seal portion 22b, so that the polycrystalline silicon layer 16 on the outer periphery side of the support substrate 10 from the seal portion 22b does not become porous, and the outermost periphery of the polycrystalline silicon layer 16 remains without being made porous. On the other hand, a current flows in the polycrystalline silicon layer 16 on the inner side of the seal portion 22b, making it porous and forming the porous silicon layer 18. In other words, in the comparative example, the position of the outer periphery side end of the porous silicon layer 18 is determined by the position where the seal portion 22b comes into contact.
[0066] A memory layer 30 is formed on the support substrate 10 on which the porous silicon layer 18 is formed. The support substrate 10 is processed in various semiconductor manufacturing equipment to form the memory layer 30. When the support substrate 10 is processed, the outermost periphery of the support substrate 10 may come into contact with, for example, a transport jig or carrier of the semiconductor manufacturing equipment.
[0067] For example, when the mechanically fragile porous silicon layer 18 comes into contact with a transport jig, carrier, or the like, dust may be generated. If dust is generated, for example, the manufacturing yield of semiconductor devices may decrease, which causes a problem. Therefore, it is preferable that the porous silicon layer 18 is not formed in a predetermined range on the outer periphery of the support substrate 10.
[0068] As described above, in the comparative example, the position of the outer peripheral end of the porous silicon layer 18 is determined by the position where the seal portion 22b contacts. For example, when the support substrate 10 is held by the substrate holder 22, if the support substrate 10 is misaligned with respect to the substrate holder 22, the position where the seal portion 22b contacts the support substrate 10 changes. Therefore, there is a risk that the porous silicon layer 18 will be formed in an area beyond a predetermined range on the outer peripheral portion of the support substrate 10.
[0069] Furthermore, in the case of the comparative example, for example, sealing of the flow path of the electrolyte by the seal portion 22b is insufficient, and the electrolyte may penetrate between the seal portion 22b and the support substrate 10. If the electrolyte penetrates, a current may flow through the polycrystalline silicon layer 16 on the outer periphery of the support substrate 10 rather than through the seal portion 22b, and a porous silicon layer 18 may be formed in an area beyond a predetermined range on the outer periphery of the support substrate 10.
[0070] As described above, in the case of the comparative example, the position of the outer peripheral end of the porous silicon layer 18 varies, and therefore the porous silicon layer 18 may become a cause of dust generation.
[0071] In the case of the first embodiment, the position of the outer peripheral end of the porous silicon layer 18 is determined by the inner peripheral end of the insulating film 12 provided in an annular shape on the outer peripheral part of the support substrate 10. Therefore, even if the support substrate 10 is misaligned with respect to the substrate holder 22 or the electrolytic solution penetrates between the seal portion 22b and the support substrate 10, the position of the outer peripheral end of the porous silicon layer 18 does not change. Therefore, the position of the outer peripheral end of the porous silicon layer 18 is stable, and the porous silicon layer 18 can be prevented from becoming a cause of dust generation.
[0072] According to the method for manufacturing a semiconductor device of the first embodiment, the position of the outer peripheral end of the porous silicon layer 18 is stabilized. Therefore, according to the method for manufacturing a semiconductor device of the first embodiment, it is possible to stabilize the manufacturing process of the semiconductor device manufactured by bonding the support substrate 10 and the semiconductor substrate 40 together.
[0073] (First Modification)
[0074] 13(a) and 13(b) are schematic cross-sectional views illustrating a method for manufacturing a semiconductor device according to a first modified example of the first embodiment.
[0075] The method for manufacturing a semiconductor device according to the first modification of the first embodiment differs from the method for manufacturing a semiconductor device according to the first embodiment in that the silicon layer formed on the insulating film is not removed.
[0076] The process is the same as the method for manufacturing the semiconductor device of the first embodiment up to the formation of the polycrystalline silicon layer 16 on the surface of the support substrate 10 (FIG. 13(a)).
[0077] Next, without removing the polycrystalline silicon layer 16 formed on the insulating film 12, the polycrystalline silicon layer 16 inside the insulating film 12 is made porous by using anodization (FIG. 13(b)). By making the polycrystalline silicon layer 16 porous, a porous silicon layer 18 is formed inside the insulating film 12.
[0078] During anodization, no current flows through the polycrystalline silicon layer 16 on the insulating film 12 due to the presence of the insulating film 12, and the polycrystalline silicon layer 16 is not made porous.
[0079] Thereafter, a 3D NAND flash memory is manufactured by the same method as the manufacturing method of the semiconductor device of the first embodiment. After the anodization and before the formation of the memory layer 30, the surface may be planarized by, for example, a CMP method.
[0080] (Second Modification)
[0081] 14(a), 14(b), and 14(c) are schematic cross-sectional views illustrating a method for manufacturing a semiconductor device according to a second modified example of the first embodiment.
[0082] The method for manufacturing a semiconductor device according to the second modification of the first embodiment differs from the method for manufacturing a semiconductor device according to the first embodiment in that the silicon layer is a single crystal silicon layer formed by epitaxial growth.
[0083] The manufacturing method for the semiconductor device according to the first embodiment is the same as that for forming the annular insulating film 12 on the outer periphery of the support substrate 10 (FIG. 14(a)).
[0084] Next, a single crystal silicon layer 17 is formed on the surface of the support substrate 10 (FIG. 14(b)). The single crystal silicon layer 17 is an example of a silicon layer. The single crystal silicon layer 17 is formed inside the insulating film 12 so as to be in contact with the surface of the support substrate 10.
[0085] The single crystal silicon layer 17 is formed by epitaxial growth and has a thickness of, for example, 100 nm to 10 μm.
[0086] Next, the single crystal silicon layer 17 on the inner side of the insulating film 12 is made porous by anodization (FIG. 14(c)). By making the single crystal silicon layer 17 porous, a porous silicon layer 18 is formed on the inner side of the insulating film 12.
[0087] Thereafter, a 3D NAND flash memory is manufactured by a method similar to the method for manufacturing the semiconductor device of the first embodiment.
[0088] In the embodiment, an example has been described in which the insulating film 12 is patterned using a photoresist. However, it is also possible to form the insulating film 12 using, for example, a film forming device that selectively forms an insulating film only on the outer periphery of the support substrate 10.
[0089] As described above, according to the method for manufacturing a semiconductor device of the first embodiment and the modified example, the position of the outer peripheral edge of the porous silicon layer is stabilized, and therefore, a stable manufacturing process can be realized when manufacturing a semiconductor device by bonding two substrates together.
[0090] Second Embodiment The method for manufacturing a semiconductor device according to the second embodiment includes preparing a first substrate having an insulating film on the outer periphery and a silicon layer on the inner side of the outer periphery, and forming a porous silicon layer by making the silicon layer on the inner side of the insulating film porous using an anodization method. The method for manufacturing a semiconductor device according to the second embodiment differs from the method for manufacturing a semiconductor device according to the first embodiment in that the silicon layer is not formed after the insulating film is formed on the outer periphery of the surface of the first substrate. Hereinafter, some of the details common to the method for manufacturing the first embodiment may be omitted.
[0091] The method for manufacturing a semiconductor device according to the second embodiment is a method for manufacturing a semiconductor device by bonding two substrates together. The semiconductor device is, for example, a semiconductor memory. The semiconductor memory is, for example, a three-dimensional NAND flash memory in which memory cells are arranged three-dimensionally.
[0092] 15(a), 15(b), 15(c), 15(d), 16(a) and 16(b) are explanatory views of a method for manufacturing a semiconductor device according to the second embodiment.
[0093] 15(a), 15(b), 15(c), 15(d), 16(a) and 16(b) are schematic cross-sectional views.
[0094] First, a support substrate 10 is prepared (FIG. 15(a)).
[0095] The support substrate 10 is a conductor. The support substrate 10 is, for example, a semiconductor. For example, the support substrate 10 is, for example, single crystal silicon. The support substrate 10 is, for example, a silicon substrate. The support substrate 10 is, for example, a silicon wafer. The support substrate 10 contains, for example, boron (B) as a p-type impurity. It is a p-type silicon wafer.
[0096] The diameter of the support substrate 10 is, for example, not less than 150 mm and not more than 300 mm.
[0097] Next, a polycrystalline silicon layer 16 is formed on the surface of the support substrate 10 (FIG. 15(b)). The polycrystalline silicon layer 16 is an example of a silicon layer. The support substrate 10 with the polycrystalline silicon layer 16 formed on its surface is an example of a first substrate.
[0098] The polycrystalline silicon layer 16 is formed by, for example, a CVD method. The thickness of the polycrystalline silicon layer 16 is, for example, not less than 100 nm and not more than 10 μm.
[0099] Next, the insulating film 12 is formed on the surface of the polycrystalline silicon layer 16 (FIG. 15(c)). The insulating film 12 is formed by using, for example, a chemical vapor deposition method (CVD method).
[0100] The insulating film 12 is, for example, an oxide, a nitride, an oxynitride, or a carbide. The insulating film 12 is, for example, silicon oxide, silicon nitride, or nitrogen-added silicon carbide.
[0101] The thickness of the insulating film 12 is, for example, not less than 100 nm and not more than 10 μm.
[0102] Next, a photoresist film 14 is formed so as to cover the insulating film 12 on the outer periphery of the support substrate 10 (FIG. 15(d)). The photoresist film 14 is formed by patterning using, for example, a photolithography method.
[0103] For example, when a positive resist is used as the photoresist film 14, the photoresist film 14 is applied to the surface of the support substrate 10, and then the central portion of the support substrate 10 is exposed to light to expose the photoresist film 14, thereby removing the photoresist film 14 from the central portion of the support substrate 10.
[0104] Furthermore, for example, when a negative resist is used as the photoresist film 14, the photoresist film 14 is applied to the surface of the support substrate 10, and then the outer periphery of the support substrate 10 is exposed to light to expose the photoresist film 14, thereby removing the photoresist film 14 from the central portion of the support substrate 10.
[0105] Next, the patterned photoresist film 14 is used as a mask to remove the insulating film 12 from the central portion of the support substrate 10. The insulating film 12 is removed by using, for example, a wet etching method.
[0106] Next, the photoresist film 14 is removed (FIG. 16(a)). A ring-shaped insulating film 12 is formed on the outer periphery of the support substrate 10. The surface of the outer periphery of the support substrate 10 is the insulating film 12, and the surface located inside the outer periphery is the polycrystalline silicon layer 16.
[0107] Next, the polycrystalline silicon layer 16 inside the insulating film 12 is made porous by anodization (FIG. 16(b)). By making the polycrystalline silicon layer 16 porous, a porous silicon layer 18 is formed inside the insulating film 12. The porous silicon layer 18 has a hollow portion inside.
[0108] The polycrystalline silicon layer 16 below the insulating film 12 does not become porous because no current flows therethrough during anodization due to the insulating film 12 being present thereon.
[0109] Next, the insulating film 12 on the polycrystalline silicon layer 16 is removed (FIG. 16(c)). The insulating film 12 is removed by, for example, wet etching.
[0110] Thereafter, a 3D NAND flash memory is manufactured by a method similar to the method for manufacturing the semiconductor device of the first embodiment.
[0111] According to the method for manufacturing a semiconductor device of the second embodiment, as in the first embodiment, the position of the outer peripheral end of the porous silicon layer 18 is stabilized, thereby stabilizing the manufacturing process of the semiconductor device manufactured by bonding the support substrate 10 and the semiconductor substrate 40 together.
[0112] (Modification)
[0113] 17(a), 17(b), 17(c), and 17(d) are schematic cross-sectional views illustrating a method for manufacturing a semiconductor device according to a modified example of the second embodiment.
[0114] The manufacturing method of the semiconductor device according to the modified example of the second embodiment differs from the manufacturing method of the second embodiment in that the silicon layer is a surface layer portion of a silicon substrate.
[0115] An insulating film 12 is formed on the surface of a support substrate 10 (FIG. 17(a)). The insulating film 12 is formed by, for example, chemical vapor deposition (CVD). The support substrate 10 is a silicon substrate. The support substrate 10 is an example of a first substrate. A surface layer portion of the silicon substrate is an example of a silicon layer.
[0116] The insulating film 12 is, for example, an oxide, a nitride, an oxynitride, or a carbide. The insulating film 12 is, for example, silicon oxide, silicon nitride, or nitrogen-added silicon carbide.
[0117] The thickness of the insulating film 12 is, for example, not less than 100 nm and not more than 10 μm.
[0118] Next, a photoresist film 14 is formed so as to cover the insulating film 12 on the outer periphery of the support substrate 10 (FIG. 17(b)). The photoresist film 14 is formed by patterning using, for example, a photolithography method.
[0119] Next, the patterned photoresist film 14 is used as a mask to remove the insulating film 12 from the central portion of the support substrate 10. The insulating film 12 is removed by using, for example, a wet etching method.
[0120] Next, the photoresist film 14 is removed (FIG. 17(c)). A ring-shaped insulating film 12 is formed on the outer periphery of the support substrate 10.
[0121] Next, the silicon layer on the surface portion of the silicon substrate inside the insulating film 12 is made porous by anodization (FIG. 17(d)). By making the silicon substrate porous, a porous silicon layer 18 is formed inside the insulating film 12. The porous silicon layer 18 has a hollow portion inside.
[0122] The silicon substrate below the insulating film 12 is not made porous because no current flows therethrough during anodization due to the presence of the insulating film 12 thereon.
[0123] Next, the insulating film 12 on the support substrate 10, which is a silicon substrate, is removed. The insulating film 12 is removed by, for example, a wet etching method.
[0124] Thereafter, a 3D NAND flash memory is manufactured by a method similar to the method for manufacturing the semiconductor device of the first embodiment.
[0125] According to the method for manufacturing a semiconductor device of the second embodiment and the modified example, the position of the outer peripheral edge of the porous silicon layer is stabilized, and therefore, a stable manufacturing process can be realized when manufacturing a semiconductor device by bonding two substrates together.
[0126] (Third embodiment) The manufacturing method of the semiconductor layer device of the third embodiment includes preparing a first substrate having at least a surface of a silicon layer, making the silicon layer porous using an anodization method, and forming a porous silicon layer having a first porous region having a first porosity and a second porous region having a second porosity higher than the first porosity, which is provided in a direction along the surface relative to the first porous region. Also, in the manufacturing method of the semiconductor layer device of the third embodiment, before forming the porous silicon layer, impurities are injected into the silicon layer using an ion implantation method to form a first region and a second region having an impurity concentration higher than that of the first region, and when making the silicon layer porous, the first region becomes the first porous region and the second region becomes the second porous region.
[0127] The method for manufacturing a semiconductor device according to the third embodiment differs from the method for manufacturing a semiconductor device according to the first embodiment in that the process for forming a porous silicon layer on a first substrate is different. Hereinafter, the description of the contents that overlap with the method for manufacturing a semiconductor device according to the first embodiment may be omitted.
[0128] The method for manufacturing a semiconductor device according to the third embodiment is a method for manufacturing a semiconductor device by bonding two substrates together. The semiconductor device is, for example, a semiconductor memory. The semiconductor memory is, for example, a three-dimensional NAND flash memory in which memory cells are arranged three-dimensionally.
[0129] 18(a), 18(b), 18(c), 18(d), 19(a), 19(b), 20(a), and 20(b) are explanatory diagrams of a manufacturing method of a semiconductor device according to the third embodiment.
[0130] Figures 18(a), 18(b), 18(c), 18(d), 19(a) and 20(a) are schematic cross-sectional views, and Figures 19(b) and 20(b) are schematic top views.
[0131] First, a support substrate 10 is prepared (FIG. 18(a)).
[0132] The support substrate 10 is a conductor. The support substrate 10 is, for example, a semiconductor. For example, the support substrate 10 is, for example, single crystal silicon. The support substrate 10 is, for example, a silicon substrate. The support substrate 10 is, for example, a p-type silicon substrate containing boron (B) as a p-type impurity.
[0133] The diameter of the support substrate 10 is, for example, not less than 150 mm and not more than 300 mm.
[0134] Next, a polycrystalline silicon layer 16 is formed on the surface of the support substrate 10 (FIG. 18(b)). The polycrystalline silicon layer 16 is an example of a silicon layer. The support substrate 10 with the polycrystalline silicon layer 16 formed on its surface is an example of a first substrate.
[0135] The polycrystalline silicon layer 16 is formed by, for example, a CVD method. The thickness of the polycrystalline silicon layer 16 is, for example, not less than 100 nm and not more than 10 μm.
[0136] Next, a photoresist film 14 is formed so as to cover the central portion of the support substrate 10 (FIG. 18(c)). The photoresist film 14 is formed by patterning using, for example, a photolithography method.
[0137] Next, using the patterned photoresist film 14 as a mask, boron (B) is ion-implanted into the outer periphery of the support substrate 10 by ion implantation (FIG. 18(d)). Boron (B) is an example of an impurity.
[0138] Next, the photoresist film 14 is removed (FIG. 19(a)). As shown in FIG. 19(a) and FIG. 19(b), a low impurity concentration region 16x is formed in the center of the polycrystalline silicon layer 16, and a high impurity concentration region 16y is formed in the outer periphery of the polycrystalline silicon layer 16. The low impurity concentration region 16x is an example of a first region. The high impurity concentration region 16y is an example of a second region.
[0139] The impurity concentration of the conductive impurity in the high impurity concentration region 16y is higher than the impurity concentration of the conductive impurity in the low impurity concentration region 16x. For example, the concentration of boron (B) in the high impurity concentration region 16y is higher than the concentration of boron (B) in the low impurity concentration region 16x.
[0140] The resistivity of the high impurity concentration region 16y is lower than the resistivity of the low impurity concentration region 16x. The resistivity of the high impurity concentration region 16y is between 1 / 1000 and 1 / 5 of the resistivity of the low impurity concentration region 16x. The resistivity of the high impurity concentration region 16y is between 0.001 Ω·cm and 0.09 Ω·cm, for example. The resistivity of the low impurity concentration region 16x is between 0.01 Ω·cm and 0.1 Ω·cm, for example.
[0141] In addition, if the concentration of boron (B) in the low impurity concentration region 16x is not as high as desired, for example, after removing the photoresist film 14, ion implantation may be performed again in the central and peripheral portions of the polycrystalline silicon layer 16.
[0142] Next, the polycrystalline silicon layer 16 is made porous by anodization (FIGS. 20(a) and 20(b)). The anodization used is the same as that used in the manufacturing method of the first embodiment.
[0143] The polycrystalline silicon layer 16 is made porous to form a porous silicon layer 18. The porous silicon layer 18 has a cavity portion therein.
[0144] The center of the porous silicon layer 18 is a low-porosity region 18x. The outer periphery of the porous silicon layer 18 is a high-porosity region 18y. The low-porosity region 18x is an example of a first porous region. The high-porosity region 18y is an example of a second porous region.
[0145] The highly porous region 18y surrounds the less porous region 18x. The highly porous region 18y is provided in a direction along the surface of the polycrystalline silicon layer 16 with respect to the less porous region 18x.
[0146] When the porous silicon layer 18 is formed by anodization, the low impurity concentration regions 16x become low porous regions 18x, and the high impurity concentration regions 16y become high porous regions 18y.
[0147] The highly porous region 18y has a first porosity, and the less porous region 18x has a second porosity, the first porosity being greater than the second porosity.
[0148] It should be noted that "porosity" refers to the ratio of the volume of voids in the porous silicon layer 18 to the total volume. For example, as the "porosity" of the porous silicon layer 18 increases, the volume ratio of silicon in the porous silicon layer 18 decreases. For example, the relationship between the magnitude of porosity can be determined by obtaining images of the cross sections of the porous silicon layer 18 by SEM and comparing the area ratios of the voids in the images.
[0149] When the porous silicon layer 18 is formed by anodization, a larger current flows through the high impurity concentration region 16y having a lower resistance than through the low impurity concentration region 16x having a higher resistance, and thus the high impurity concentration region 16y becomes more porous, becoming a highly porous region 18y having a higher porosity.
[0150] After the porous silicon layer 18 is formed, a three-dimensional NAND flash memory is manufactured in the same manner as the manufacturing method of the semiconductor device of the first embodiment.
[0151] Next, the operation and effects of the method for manufacturing the semiconductor device according to the third embodiment will be described.
[0152] 9 in the manufacturing method of the semiconductor device of the first embodiment, also in the manufacturing method of the semiconductor device of the third embodiment, the support substrate 10 and the semiconductor substrate 40 are separated at the boundary of the porous silicon layer 18. For example, a wedge-shaped tool is pressed from the side toward the boundary between the memory layer 30 and the wiring layer 40b and / or a water jet is sprayed, thereby mechanically dividing the porous silicon layer 18 starting from the boundary between the memory layer 30 and the wiring layer 40b, and the support substrate 10 and the semiconductor substrate 40 are separated.
[0153] In order to divide the porous silicon layer 18 when separating the support substrate 10 and the semiconductor substrate 40, the mechanical strength of the porous silicon layer 18 is required to be lower than that of other portions. For example, the mechanical strength of the porous silicon layer 18 is required to be lower than the mechanical strength of the bonding surface between the support substrate 10 and the semiconductor substrate 40.
[0154] On the other hand, after the porous silicon layer 18 is formed on the support substrate 10, the memory layer 30 is formed on the porous silicon layer 18. When forming the memory layer 30, film formation and heat treatment are performed. During the film formation and heat treatment, stress is applied to the porous silicon layer 18. Therefore, the porous silicon layer 18 is required to have a mechanical strength sufficient to prevent it from being destroyed by the stress applied when forming the memory layer 30.
[0155] If the mechanical strength of the porous silicon layer 18 is too high, for example, peeling occurs at the bonding surface between the support substrate 10 and the semiconductor substrate 40 when the support substrate 10 and the semiconductor substrate 40 are separated, making it impossible to continue manufacturing the product. If the mechanical strength of the porous silicon layer 18 is too low, the porous silicon layer 18 is destroyed during the formation of the memory layer 30, making it impossible to continue manufacturing the product.
[0156] In the manufacturing method of the semiconductor device of the third embodiment, a low porous region 18x is provided in the center of the support substrate 10, and a high porous region 18y is provided in the outer periphery of the support substrate 10. The porosity of the high porous region 18y is higher than that of the low porous region 18x. The mechanical strength of the high porous region 18y with high porosity is lower than that of the low porous region 18x with low porosity.
[0157] For example, consider a case where, when separating the support substrate 10 and the semiconductor substrate 40, a wedge-shaped jig is pressed from the side against the porous silicon layer 18 to separate the porous silicon layer 18. In the manufacturing method of the semiconductor device according to the third embodiment, the support substrate 10 has a highly porous region 18y with low mechanical strength at its outer periphery, which makes it easy to separate the support substrate 10 and the semiconductor substrate 40.
[0158] On the other hand, the presence of the low-porosity region 18x having high mechanical strength in the central part of the support substrate 10 maintains the mechanical strength of the porous silicon layer 18, and prevents the porous silicon layer 18 from being destroyed during the formation of the memory layer 30.
[0159] According to the manufacturing method of the semiconductor device of the third embodiment, the in-plane distribution of the porosity in the porous silicon layer 18 is controlled, thereby optimizing the in-plane distribution of the mechanical strength of the porous silicon layer 18. Therefore, according to the manufacturing method of the semiconductor device of the third embodiment, it is possible to stabilize the manufacturing process of the semiconductor device manufactured by bonding the support substrate 10 and the semiconductor substrate 40 together.
[0160] (First Modification)
[0161] Figures 21(a), 21(b), 21(c), 21(d), 22(a), 22(b), 23(a), and 23(b) are explanatory diagrams of a manufacturing method of a semiconductor device according to a first modified example of the third embodiment.
[0162] Figures 21(a), 21(b), 21(c), 21(d), 22(a) and 23(a) are schematic cross-sectional views, and Figures 22(b) and 23(b) are schematic top views.
[0163] The manufacturing method of the semiconductor device according to the first modification of the third embodiment differs from that of the third embodiment in that the first porous region surrounds the second porous region, for example, the low porous region 18x surrounds the high porous region 18y.
[0164] First, a support substrate 10 is prepared (FIG. 21(a)).
[0165] Next, a polycrystalline silicon layer 16 is formed on the surface of the support substrate 10 (FIG. 21(b)). The polycrystalline silicon layer 16 is an example of a silicon layer. The support substrate 10 with the polycrystalline silicon layer 16 formed on its surface is an example of a first substrate.
[0166] Next, a photoresist film 14 is formed so as to cover the outer periphery of the support substrate 10 (FIG. 21(c)). The photoresist film 14 is formed by patterning using, for example, a photolithography method.
[0167] Next, using the patterned photoresist film 14 as a mask, boron (B) is ion-implanted into the center of the support substrate 10 by ion implantation (FIG. 21(d)). Boron (B) is an example of an impurity.
[0168] Next, the photoresist film 14 is removed (FIG. 22(a)). As shown in FIG. 22(a) and FIG. 22(b), a low impurity concentration region 16x is formed in the outer periphery of the polycrystalline silicon layer 16, and a high impurity concentration region 16y is formed in the center of the polycrystalline silicon layer 16. The low impurity concentration region 16x is an example of a first region. The high impurity concentration region 16y is an example of a second region.
[0169] In addition, if the concentration of boron (B) in the low impurity concentration region 16x is not as high as desired, for example, after removing the photoresist film 14, ion implantation may be performed again in the central and peripheral portions of the polycrystalline silicon layer 16.
[0170] The impurity concentration of the conductive impurity in the high impurity concentration region 16y is higher than the impurity concentration of the conductive impurity in the low impurity concentration region 16x. For example, the concentration of boron (B) in the high impurity concentration region 16y is higher than the concentration of boron (B) in the low impurity concentration region 16x.
[0171] The resistivity of the high impurity concentration region 16y is lower than the resistivity of the low impurity concentration region 16x.
[0172] Next, the polycrystalline silicon layer 16 is made porous by anodization (FIGS. 23(a) and 23(b)).
[0173] The polycrystalline silicon layer 16 is made porous to form a porous silicon layer 18. The porous silicon layer 18 has a cavity portion therein.
[0174] The center of the porous silicon layer 18 is a high-porosity region 18y. The outer periphery of the porous silicon layer 18 is a low-porosity region 18x. The low-porosity region 18x is an example of a first porous region. The high-porosity region 18y is an example of a second porous region. The low-porosity region 18x surrounds the high-porosity region 18y. The high-porosity region 18y is provided in a direction along the surface of the polycrystalline silicon layer 16 relative to the low-porosity region 18x.
[0175] When the porous silicon layer 18 is formed by anodization, the low impurity concentration regions 16x become low porous regions 18x, and the high impurity concentration regions 16y become high porous regions 18y.
[0176] The highly porous region 18y has a first porosity, and the less porous region 18x has a second porosity, the first porosity being greater than the second porosity.
[0177] After the porous silicon layer 18 is formed, a three-dimensional NAND flash memory is manufactured in the same manner as the manufacturing method of the semiconductor device of the first embodiment.
[0178] In the manufacturing method of a semiconductor device according to the first modified example of the third embodiment, a high porous region 18y is provided in the center of the support substrate 10, and a low porous region 18x is provided in the outer periphery of the support substrate 10. The porosity of the high porous region 18y is higher than that of the low porous region 18x. The mechanical strength of the high porous region 18y with high porosity is lower than that of the low porous region 18x with low porosity.
[0179] 24(a) and 24(b) are explanatory diagrams of a method for manufacturing a semiconductor device according to a first modified example of the semiconductor device of the third embodiment. FIG 24 shows an example of a method for separating the support substrate 10 and the semiconductor substrate 40.
[0180] 24(a), when separating the support substrate 10 and the semiconductor substrate 40, the semiconductor substrate 40 is fixed to a first support member 61. For example, the semiconductor substrate 40 is fixed to the first support member 61 by vacuum suction. In addition, the support substrate 10 is fixed to a second support member 62. For example, the support substrate 10 is fixed to the second support member 62 by vacuum suction.
[0181] Thereafter, as shown in FIG. 24(a), the second support member 62 is rotated relative to the first support member 61 to apply a shear stress to the porous silicon layer 18, thereby dividing the porous silicon layer 18.
[0182] Fig. 24(b) is a schematic diagram showing the in-plane distribution of the magnitude of the shear stress applied to the porous silicon layer 18. As shown in Fig. 24(b), the shear stress applied to the porous silicon layer 18 is large at the outer periphery of the porous silicon layer 18. In other words, the shear stress applied to the porous silicon layer 18 is small at the center of the porous silicon layer 18.
[0183] In the manufacturing method of a semiconductor device according to the first modified example of the third embodiment, since a highly porous region 18y having low mechanical strength is present in the central portion of the support substrate 10, even if the shear stress applied to the porous silicon layer 18 in the central portion of the support substrate 10 is small, the support substrate 10 and the semiconductor substrate 40 can be easily separated from each other.
[0184] On the other hand, the presence of the low-porosity region 18x having high mechanical strength in the outer periphery of the support substrate 10 maintains the mechanical strength of the porous silicon layer 18, and prevents the porous silicon layer 18 from being destroyed during the formation of the memory layer 30.
[0185] (Second Modification)
[0186] Figures 25(a), 25(b), 25(c), 25(d), 26(a), 26(b), 27(a), and 27(b) are explanatory diagrams of a manufacturing method of a semiconductor device according to a second variant of the third embodiment.
[0187] Figures 25(a), 25(b), 25(c), 25(d), 26(a) and 27(a) are schematic cross-sectional views, and Figures 26(b) and 27(b) are schematic top views.
[0188] The manufacturing method of the semiconductor device according to the second modification of the third embodiment differs from that according to the third embodiment in that the first and second porous regions have a checkerboard pattern, for example, the low porous region 18x and the high porous region 18y have a checkerboard pattern.
[0189] First, a support substrate 10 is prepared (FIG. 25(a)).
[0190] Next, a polycrystalline silicon layer 16 is formed on the surface of the support substrate 10 (FIG. 25(b)). The polycrystalline silicon layer 16 is an example of a silicon layer. The support substrate 10 with the polycrystalline silicon layer 16 formed on its surface is an example of a first substrate.
[0191] Next, a photoresist film 14 is formed on the support substrate 10 (FIG. 25(c)). The photoresist film 14 is formed by patterning using, for example, a photolithography method. The photoresist film 14 has a checkerboard pattern.
[0192] Next, using the patterned photoresist film 14 as a mask, boron (B) is ion-implanted into the support substrate 10 by ion implantation (FIG. 25(d)). Boron (B) is an example of an impurity.
[0193] Next, the photoresist film 14 is removed (FIG. 26(a)). As shown in FIG. 26(a) and FIG. 26(b), a low impurity concentration region 16x and a high impurity concentration region 16y are formed in the polycrystalline silicon layer 16. The low impurity concentration region 16x and the high impurity concentration region 16y have a checkerboard pattern. The low impurity concentration region 16x is an example of a first region. The high impurity concentration region 16y is an example of a second region.
[0194] In addition, if the concentration of boron (B) in the low impurity concentration region 16x is not as high as desired, for example, after removing the photoresist film 14, ion implantation may be performed again in the central and peripheral portions of the polycrystalline silicon layer 16.
[0195] The impurity concentration of the conductive impurity in the high impurity concentration region 16y is higher than the impurity concentration of the conductive impurity in the low impurity concentration region 16x. For example, the concentration of boron (B) in the high impurity concentration region 16y is higher than the concentration of boron (B) in the low impurity concentration region 16x.
[0196] The resistivity of the high impurity concentration region 16y is lower than the resistivity of the low impurity concentration region 16x.
[0197] Next, the polycrystalline silicon layer 16 is made porous by anodization (FIGS. 27(a) and 27(b)).
[0198] The polycrystalline silicon layer 16 is made porous to form a porous silicon layer 18. The porous silicon layer 18 has a cavity portion therein.
[0199] In the porous silicon layer 18, a low porous region 18x and a high porous region 18y having a checkerboard pattern are formed. The low porous region 18x is an example of a first porous region. The high porous region 18y is an example of a second porous region. The low porous region 18x surrounds the high porous region 18y. The high porous region 18y is provided in a direction along the surface of the porous silicon layer 18 relative to the low porous region 18x.
[0200] When the porous silicon layer 18 is formed by anodization, the low impurity concentration regions 16x become low porous regions 18x, and the high impurity concentration regions 16y become high porous regions 18y.
[0201] The highly porous region 18y has a first porosity, and the less porous region 18x has a second porosity, the first porosity being greater than the second porosity.
[0202] After the porous silicon layer 18 is formed, a three-dimensional NAND flash memory is manufactured in the same manner as the manufacturing method of the semiconductor device of the first embodiment.
[0203] In the manufacturing method of the semiconductor device according to the second modification of the third embodiment, a low porous region 18x and a high porous region 18y having a checkerboard pattern are provided in the porous silicon layer 18 of the support substrate 10. The porosity of the high porous region 18y is higher than that of the low porous region 18x. The mechanical strength of the high porous region 18y having a higher porosity is lower than that of the low porous region 18x having a lower porosity.
[0204] In the manufacturing method of the semiconductor device according to the second modified example of the third embodiment, the highly porous regions 18y having low mechanical strength and the low porous regions 18x having low mechanical strength are evenly arranged in the porous silicon layer 18 of the support substrate 10. Therefore, for example, it becomes easy to separate the support substrate 10 and the semiconductor substrate 40, and the porous silicon layer 18 can be prevented from being destroyed during the formation of the memory layer 30.
[0205] Furthermore, compared to the manufacturing method of a semiconductor device of the third embodiment and the manufacturing method of a semiconductor device of the first variant of the third embodiment, the low porous regions 18x and the high porous regions 18y, which have different physical properties, are evenly arranged, thereby making it possible to suppress, for example, warping of the support substrate 10.
[0206] In the embodiment and the modified example, boron (B) is used as an example of the conductive impurity ion-implanted into the silicon layer, but the conductive impurity is not limited to boron (B). For example, phosphorus (P) or arsenic (As) can also be used as the conductive impurity.
[0207] For example, when the support substrate 10 is a p-type silicon substrate, the conductive impurity ion-implanted into the silicon layer is preferably boron (B), which is a p-type conductive impurity. Also, when the support substrate 10 is an n-type silicon substrate, the conductive impurity ion-implanted into the silicon layer is preferably phosphorus (P) or arsenic (As), which is an n-type conductive impurity.
[0208] In the embodiment and modified examples, a method for making the polycrystalline silicon layer 16 on the surface of the support substrate 10 porous has been described as an example, but the support substrate 10 may be a silicon substrate and the method may be for making the monocrystalline silicon layer on the surface portion of the support substrate 10 porous.
[0209] In the embodiment and the modified example, a method of performing one ion implantation has been described as an example, but a method of performing multiple ion implantations with different doses in different regions may also be used.
[0210] As described above, according to the manufacturing method of the semiconductor device of the third embodiment and the modified example, the in-plane distribution of the mechanical strength of the porous silicon layer is optimized by controlling the in-plane distribution of the porosity in the porous silicon layer, and therefore, a stable manufacturing process can be realized when manufacturing a semiconductor device by bonding two substrates together.
[0211] (Fourth embodiment) The manufacturing method of the semiconductor device of the fourth embodiment differs from the manufacturing method of the semiconductor device of the third embodiment in that, when forming a porous silicon layer, it has a first step and a second step, in which a first substrate holder is used in the first step to limit the portion of the silicon layer that comes into contact with the electrolyte to a first region, and in the second step, a second substrate holder is used to limit the portion of the silicon layer that comes into contact with the electrolyte to a second region inside the first region, so that the second region becomes the second porous region and the first region outside the second region becomes the first porous region.
[0212] The method for manufacturing a semiconductor layer device of the fourth embodiment differs from the methods for manufacturing semiconductor devices of the first and third embodiments in that the process for forming a porous silicon layer on a first substrate is different. Hereinafter, description of contents that overlap with the methods for manufacturing semiconductor devices of the first and third embodiments may be omitted.
[0213] The method for manufacturing a semiconductor device according to the fourth embodiment is a method for manufacturing a semiconductor device by bonding two substrates together. The semiconductor device is, for example, a semiconductor memory. The semiconductor memory is, for example, a three-dimensional NAND flash memory in which memory cells are arranged three-dimensionally.
[0214] Figures 28(a), 28(b), 28(c), 28(d), 28(e), 29(a), 29(b), 29(c), 30(a), 30(b), 30(c), 31(a) and 31(b) are explanatory diagrams of a manufacturing method of a semiconductor device of the fourth embodiment.
[0215] Fig. 28(a), Fig. 28(b), Fig. 28(c), Fig. 28(d), Fig. 28(e), and Fig. 31(a) are schematic cross-sectional views. Fig. 31(b) is a schematic top view. Fig. 29(a), Fig. 29(b), Fig. 29(c), Fig. 30(a), Fig. 30(b), and Fig. 30(c) are explanatory views of the anodization method of the manufacturing method of the semiconductor device of the fourth embodiment.
[0216] First, a support substrate 10 is prepared (FIG. 28(a)).
[0217] The support substrate 10 is a conductor. The support substrate 10 is, for example, a semiconductor. For example, the support substrate 10 is, for example, single crystal silicon. The support substrate 10 is, for example, a silicon substrate.
[0218] The diameter of the support substrate 10 is, for example, not less than 150 mm and not more than 300 mm.
[0219] Next, a polycrystalline silicon layer 16 is formed on the surface of the support substrate 10 (FIG. 28(b)). The polycrystalline silicon layer 16 is an example of a silicon layer. The support substrate 10 with the polycrystalline silicon layer 16 formed on its surface is an example of a first substrate.
[0220] The polycrystalline silicon layer 16 is formed by, for example, a CVD method. The thickness of the polycrystalline silicon layer 16 is, for example, not less than 100 nm and not more than 10 μm.
[0221] Next, the polycrystalline silicon layer 16 is made porous by anodizing. For example, the polycrystalline silicon layer 16 is made porous by using an apparatus similar to the anodizing apparatus 20 shown in FIG. 4 of the first embodiment. By making the polycrystalline silicon layer 16 porous, a porous silicon layer 18 is formed.
[0222] When the polycrystalline silicon layer 16 is made porous by anodization, a first step, a second step, and a third step are performed.
[0223] In the first step, a peripheral porous region 18a is formed in the polycrystalline silicon layer 16 (FIG. 28(c)). In the first step, a first substrate holder 22x is used when forming the polycrystalline silicon layer 16 by anodization. The peripheral porous region 18a is an example of a first porous region.
[0224] In the second step, an intermediate porous region 18b is formed in the polycrystalline silicon layer 16 (FIG. 28(d)). In the second step, a second substrate holder 22y is used when forming the polycrystalline silicon layer 16 by anodization. The intermediate porous region 18b is an example of a second porous region.
[0225] The intermediate porous region 18b is formed inside the outer periphery porous region 18a. The intermediate porous region 18b is provided in a direction along the surface of the polycrystalline silicon layer 16 with respect to the outer periphery porous region 18a.
[0226] The porosity of the intermediate porous region 18b is greater than the porosity of the peripheral porous region 18a.
[0227] In the third step, a central porous region 18c is formed in the polycrystalline silicon layer 16 (FIG. 28(e)). In the third step, a third substrate holder 22z is used when forming the polycrystalline silicon layer 16 by anodization.
[0228] The central porous region 18c is formed inside the intermediate porous region 18b. The central porous region 18c is provided in a direction along the surface of the polycrystalline silicon layer 16 with respect to the intermediate porous region 18b.
[0229] The porosity of the central porous region 18c is greater than the porosity of the intermediate porous region 18b.
[0230] Between each of the first step, the second step, and the third step, for example, the substrate is once removed from the processing bath 21, and the substrate holder 22 is replaced before proceeding to the next step.
[0231] Fig. 29(a) shows the first substrate holder 22x used in the first step, Fig. 29(b) shows the second substrate holder 22y used in the second step, and Fig. 29(c) shows the third substrate holder 22z used in the third step. Fig. 29(a), Fig. 29(b), and Fig. 29(c) are diagrams showing the state before the support substrate 10 is carried into the anodizing apparatus 20 and the process of making the polycrystalline silicon layer 16 porous is started. That is, these diagrams are diagrams showing the state before a voltage is applied between the first electrode 23 and the second electrode 24.
[0232] The first substrate holder 22x is an example of a first substrate holder, and the second substrate holder 22y is an example of a second substrate holder.
[0233] When the support substrate 10 is held by the first substrate holder 22x, the portion of the polycrystalline silicon layer 16 in contact with the electrolytic solution 25 is limited to a first region by the seal portion 22b as shown in Fig. 29(a). When the first substrate holder 22x is used, for example, the portion of the polycrystalline silicon layer 16 in contact with the electrolytic solution 25 on the second electrode 24 (Fig. 4) side is limited to the first region. Also, for example, the portion of the polycrystalline silicon layer 16 in contact with the electrolytic solution 25 on the cathode side is limited to the first region.
[0234] When the second substrate holder 22y holds the support substrate 10, as shown in Fig. 29(b), the portion of the polycrystalline silicon layer 16 that is in contact with the electrolyte 25 is limited to the second region by the seal portion 22b. The second region is located inside the first region.
[0235] When the second substrate holder 22y is used, for example, the portion of the polycrystalline silicon layer 16 that contacts the electrolytic solution 25 on the second electrode 24 (FIG. 4) side is limited to the second region. Also, for example, the portion of the polycrystalline silicon layer 16 that contacts the electrolytic solution 25 on the cathode side is limited to the second region.
[0236] When the support substrate 10 is held by the third substrate holder 22z, as shown in Fig. 29(c), the portion of the polycrystalline silicon layer 16 that is in contact with the electrolyte 25 is limited to a third region by the seal portion 22b. The third region is located inside the second region.
[0237] When the third substrate holder 22z is used, for example, the portion of the polycrystalline silicon layer 16 in contact with the electrolytic solution 25 on the second electrode 24 (FIG. 4) side is limited to the third region. Also, for example, the portion of the polycrystalline silicon layer 16 in contact with the electrolytic solution 25 on the cathode side is limited to the third region.
[0238] Figures 30(a), 30(b), and 30(c) are explanatory diagrams of making the polycrystalline silicon layer 16 porous. Figure 30(a) shows the first step, Figure 30(b) shows the second step, and Figure 30(c) shows the third step. Figures 29(a), 29(b), and 29(c) are diagrams after the support substrate 10 is carried into the anodizing apparatus 20 and the polycrystalline silicon layer 16 has been made porous in each step.
[0239] In the first step, as shown in Fig. 30(a), the polysilicon layer 16 in the first region inside the seal portion 22b is made porous to form the outer periphery porous region 18a. In the second step, as shown in Fig. 30(b), the polysilicon layer 16 in the second region inside the seal portion 22b is made more porous to form the middle porous region 18b. In the third step, as shown in Fig. 30(c), the polysilicon layer 16 in the third region inside the seal portion 22b is made more porous to form the central porous region 18c.
[0240] Figures 31(a) and 31(b) are schematic diagrams immediately after the porous silicon layer 18 is formed by anodization. As shown in Figures 31(a) and 31(b), the intermediate porous region 18b is surrounded by the peripheral porous region 18a, and the central porous region 18c is surrounded by the intermediate porous region 18b. The porosity of the porous silicon layer 18 increases from the outside to the inside of the porous silicon layer 18.
[0241] In the method for manufacturing a semiconductor device according to the fourth embodiment, the position of the seal portion 22b of the substrate holder 22 of the anodizing apparatus 20 is changed for each step, thereby changing the region to be made porous.
[0242] After the porous silicon layer 18 is formed, a three-dimensional NAND flash memory is manufactured in the same manner as the manufacturing method of the semiconductor device of the first embodiment.
[0243] For example, consider a case where, when separating the support substrate 10 and the semiconductor substrate 40, the second support member 62 is rotated relative to the first support member 61 to apply shear stress to the porous silicon layer 18 and divide the porous silicon layer 18, as described in the third embodiment. In the manufacturing method for a semiconductor device of the fourth embodiment, since the central porous region 18c having low mechanical strength is present in the central portion of the support substrate 10, the support substrate 10 and the semiconductor substrate 40 can be easily divided even if the shear stress applied to the porous silicon layer 18 in the central portion of the support substrate 10 is small.
[0244] On the other hand, the presence of a peripheral porous region 18a with high mechanical strength at the outer periphery of the support substrate 10 maintains the mechanical strength of the porous silicon layer 18, thereby preventing the porous silicon layer 18 from being destroyed during the formation of the memory layer 30.
[0245] Furthermore, the intermediate porous region 18b, which has a moderate mechanical strength, is present in the intermediate portion of the support substrate 10, thereby suppressing abrupt changes in the in-plane physical properties of the porous silicon layer 18. Therefore, for example, warping of the support substrate 10 is mitigated.
[0246] In making the polycrystalline silicon layer 16 porous, the order of the first step, the second step, and the third step can be reversed to obtain the same action and effect.
[0247] In the manufacturing method of the semiconductor device according to the fourth embodiment, the configurations of the substrate holder 22 and the sealing portion 22b are not limited to those shown in Fig. 29(a), Fig. 29(b), and Fig. 29(c). Any configuration may be used as long as the area where the polycrystalline silicon layer 16 is made porous can be changed for each step.
[0248] In the embodiment, a method for making the polycrystalline silicon layer 16 formed on the surface of the support substrate 10 porous has been described as an example, but the support substrate 10 may be a silicon substrate and the method may be such that the monocrystalline silicon layer on the surface portion of the support substrate 10 is made porous.
[0249] As described above, according to the method for manufacturing a semiconductor device of the fourth embodiment, the in-plane distribution of the mechanical strength of the porous silicon layer is optimized by controlling the in-plane distribution of the porosity in the porous silicon layer, and therefore a stable manufacturing process can be realized when manufacturing a semiconductor device by bonding two substrates together.
[0250] Fifth embodiment The manufacturing method of the semiconductor device of the fifth embodiment differs from the manufacturing method of the semiconductor device of the third embodiment in that, before forming the porous silicon layer, a first region having a first insulating film and a second region having either a second insulating film thinner than the first insulating film or no insulating film are formed on the surface of the silicon layer, and when the silicon layer is made porous, the first region becomes a first porous region and the second region becomes a second porous region.
[0251] The method for manufacturing the semiconductor layer device of the fifth embodiment differs from the methods for manufacturing the semiconductor device of the first and third embodiments in that the process for forming a porous silicon layer on the first substrate is different. Hereinafter, the description of the contents that overlap with the methods for manufacturing the semiconductor device of the first and third embodiments may be omitted.
[0252] The method for manufacturing a semiconductor device according to the fifth embodiment is a method for manufacturing a semiconductor device by bonding two substrates together. The semiconductor device is, for example, a semiconductor memory. The semiconductor memory is, for example, a three-dimensional NAND flash memory in which memory cells are arranged three-dimensionally.
[0253] 32(a), 32(b), 32(c), 32(d), 33(a), 33(b), 34(a), and 34(b) are explanatory diagrams of a manufacturing method of a semiconductor device according to the fifth embodiment.
[0254] Figures 32(a), 32(b), 32(c), 32(d), 33(a), 33(b) and 345(a) are schematic cross-sectional views. Figure 34(b) is a schematic top view.
[0255] First, a support substrate 10 is prepared (FIG. 32(a)).
[0256] The support substrate 10 is a conductor. The support substrate 10 is, for example, a semiconductor. For example, the support substrate 10 is, for example, single crystal silicon. The support substrate 10 is, for example, a silicon substrate.
[0257] The diameter of the support substrate 10 is, for example, not less than 150 mm and not more than 300 mm.
[0258] Next, a polycrystalline silicon layer 16 is formed on the surface of the support substrate 10 (FIG. 32(b)). The polycrystalline silicon layer 16 is an example of a silicon layer. The support substrate 10 with the polycrystalline silicon layer 16 formed on its surface is an example of a first substrate.
[0259] The polycrystalline silicon layer 16 is formed by, for example, a CVD method. The thickness of the polycrystalline silicon layer 16 is, for example, not less than 100 nm and not more than 10 μm.
[0260] Next, an insulating film 71 is formed on the surface of the polycrystalline silicon layer 16 (FIG. 32(c)). The insulating film 71 is formed by using, for example, a CVD method.
[0261] The insulating film 71 is, for example, an oxide, a nitride, an oxynitride, or a carbide. The insulating film 12 is, for example, a silicon oxide, a silicon nitride, or a nitrogen-added silicon carbide.
[0262] The thickness of the insulating film 71 is, for example, not less than 1 nm and not more than 100 nm.
[0263] Next, a photoresist film 14 is formed (FIG. 32(d)) so as to cover the central portion of the polycrystalline silicon layer 16. The photoresist film 14 is formed by patterning using, for example, a photolithography method.
[0264] Next, the insulating film 71 on the outer periphery of the support substrate 10 is removed using the patterned photoresist film 14 as a mask (FIG. 33(a)). The insulating film 71 is removed by, for example, wet etching.
[0265] Next, the photoresist film 14 is removed (FIG. 33(b)).
[0266] Next, an insulating film 72 is formed on the surfaces of the polycrystalline silicon layer 16 and the insulating film 71 (FIG. 33(c)). The insulating film 72 is formed by using, for example, a CVD method.
[0267] The thickness of the insulating film 72 is, for example, not less than 1 nm and not more than 100 nm.
[0268] A region on the surface of polycrystalline silicon layer 16 where insulating film 71 and insulating film 72 are stacked is an example of a first region. A laminated film 73 where insulating film 71 and insulating film 72 are stacked is an example of a first insulating film. A region on the surface of polycrystalline silicon layer 16 where only insulating film 72 is stacked is an example of a second region. Insulating film 72 formed on the second region is an example of a second insulating film.
[0269] The insulating film 72 is thinner than the laminated film 73 in which the insulating films 71 and 72 are laminated.
[0270] Next, the polycrystalline silicon layer 16 is made porous by anodization (FIG. 33(d)). The anodization used is the same as that used in the manufacturing method of the first embodiment.
[0271] The polycrystalline silicon layer 16 is made porous to form a porous silicon layer 18. The porous silicon layer 18 has a cavity portion therein.
[0272] Next, the insulating films 71 and 72 are removed (FIGS. 34(a) and 34(b)).
[0273] The center of the porous silicon layer 18 is a low porous region 18x. The outer periphery of the porous silicon layer 18 is a high porous region 18y. The low porous region 18x is an example of a first porous region. The high porous region 18y is an example of a second porous region. The high porous region 18y surrounds the low porous region 18x. The high porous region 18y is provided in a direction along the surface of the polycrystalline silicon layer 16 with respect to the low porous region 18x.
[0274] When the porous silicon layer 18 is formed by anodization, the region where the laminated film 73 is laminated becomes the low-porosity region 18x, and the region where only the insulating film 72 is formed becomes the high-porosity region 18y.
[0275] The highly porous region 18y has a first porosity, and the less porous region 18x has a second porosity, the first porosity being greater than the second porosity.
[0276] When the porous silicon layer 18 is formed by anodization, a larger current flows through the region where the insulating film is thin than through the region where the insulating film is thick. Therefore, the region where the laminated film 73 is formed becomes the low-porosity region 18x. Meanwhile, the region where only the insulating film 72 is laminated becomes the high-porosity region 18y.
[0277] After the porous silicon layer 18 is formed, a three-dimensional NAND flash memory is manufactured in the same manner as the manufacturing method of the semiconductor device of the first embodiment.
[0278] In the manufacturing method of the semiconductor device of the fifth embodiment, a low porous region 18x is provided in the center of the support substrate 10, and a high porous region 18y is provided in the outer periphery of the support substrate 10. The porosity of the high porous region 18y is higher than that of the low porous region 18x. The mechanical strength of the high porous region 18y with high porosity is lower than that of the low porous region 18x with low porosity.
[0279] For example, consider a case where, when separating the support substrate 10 and the semiconductor substrate 40, a wedge-shaped jig is pressed from the side toward the porous silicon layer 18 to separate the porous silicon layer 18. In the manufacturing method of the semiconductor device according to the fifth embodiment, the support substrate 10 has a highly porous region 18y with low mechanical strength at its outer periphery, which makes it easy to separate the support substrate 10 and the semiconductor substrate 40.
[0280] On the other hand, the presence of the low-porosity region 18x having high mechanical strength in the central part of the support substrate 10 maintains the mechanical strength of the porous silicon layer 18, and prevents the porous silicon layer 18 from being destroyed during the formation of the memory layer 30.
[0281] In the embodiment, a method for making the polycrystalline silicon layer 16 on the surface of the support substrate 10 porous has been described as an example, but the support substrate 10 may be a silicon substrate and the method may involve making the monocrystalline silicon layer on the surface of the support substrate 10 porous.
[0282] In the embodiment, a method in which an insulating film is formed in both the first region and the second region has been described as an example, but it is also possible to use a method in which, for example, no insulating film is provided in the second region.
[0283] Furthermore, in the embodiment, an example has been described in which two regions having insulating films with different thicknesses are provided, but a method in which three or more regions having insulating films with different thicknesses are provided may also be used.
[0284] Furthermore, in the embodiment, a pattern in which the highly porous region 18y surrounds the less porous region 18x has been described as an example, but other patterns can also be formed.
[0285] As described above, according to the method for manufacturing a semiconductor device of the fifth embodiment, the in-plane distribution of the mechanical strength of the porous silicon layer is optimized by controlling the in-plane distribution of the porosity in the porous silicon layer, and therefore a stable manufacturing process can be realized when manufacturing a semiconductor device by bonding two substrates together.
[0286] In the first to fifth embodiments, a three-dimensional NAND flash memory is shown as an example of a semiconductor device to be manufactured, a memory cell array is shown as an example of a first electronic circuit, and a control circuit for controlling the operation of the memory cell array is shown as an example of a second electronic circuit. However, the semiconductor device, the first electronic circuit, and the second semiconductor circuit to be manufactured are not limited to the above examples. For example, the semiconductor device to be manufactured may be an optical sensor, the electronic circuit may be a light receiving unit, and the semiconductor circuit may be a control circuit for the light receiving unit.
[0287] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. For example, components of one embodiment may be replaced or changed with components of another embodiment. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0288] 10 Support substrate (first substrate, silicon layer) 12 Insulating film 16 Polycrystalline silicon layer (silicon layer) 16x low impurity concentration region (first region) 16y High impurity concentration region (second region) 17 Single crystal silicon layer (silicon layer) 18 Porous silicon layer 18a: Peripheral porous region (first porous region) 18b Intermediate porous region (second porous region) 18x low porosity area (first porosity area) 18y Highly porous region (second porous region) 22x 1st PCB holder 22y Second Board Holder 30x memory cell array (first electronic circuit) 40 Semiconductor substrate (second substrate) 40x Control circuit (second electronic circuit) 72 Insulating film (second insulating film) 73 Laminated film (first insulating film)
Claims
1. forming an insulating film on a peripheral portion of a surface of a first substrate; forming a silicon layer in contact with the surface of the insulating film on the inside of the insulating film after forming the insulating film; a porous silicon layer is formed by making the silicon layer inside the insulating film porous using an anodization method.
2. 2. The method for manufacturing a semiconductor device according to claim 1, wherein said silicon layer is made of polycrystalline silicon.
3. 3. The method for manufacturing a semiconductor device according to claim 2, further comprising removing said silicon layer formed on said insulating film.
4. 2. The method for manufacturing a semiconductor device according to claim 1, wherein said first substrate is a silicon substrate.
5. 2. The method for manufacturing a semiconductor device according to claim 1, wherein said silicon layer is a single crystal silicon layer formed by epitaxial growth.
6. 2. The method for manufacturing a semiconductor device according to claim 1, wherein the insulating film is made of silicon oxide, silicon nitride, or nitrogen-added silicon carbide.
7. forming a first electronic circuit on the porous silicon layer after forming the porous silicon layer; providing a second substrate having a second electronic circuit; bonding the first substrate and the second substrate together so that the first electronic circuit and the second electronic circuit are connected; 2. The method for manufacturing a semiconductor device according to claim 1, wherein said first electronic circuit and said first substrate are separated by said porous silicon layer as a boundary.
8. 8. The method for manufacturing a semiconductor device according to claim 7, wherein said first electronic circuit includes a memory cell array, and said second electronic circuit includes a control circuit for controlling an operation of said memory cell array.
9. preparing a first substrate having an insulating film as a surface of an outer periphery and a silicon layer as a surface located inside the outer periphery; A method for manufacturing a semiconductor device, comprising the steps of: making the silicon layer inside the insulating film porous by anodization to form a porous silicon layer.
10. 10. The method for manufacturing a semiconductor device according to claim 9, wherein the first substrate is a silicon substrate, and the silicon layer is a surface layer portion of the silicon substrate.
11. 10. The method for manufacturing a semiconductor device according to claim 9, wherein the silicon layer is a silicon layer formed by chemical vapor deposition.
12. 10. The method for manufacturing a semiconductor device according to claim 9, wherein the insulating film is made of silicon oxide, silicon nitride, or nitrogen-added silicon carbide.
13. forming a first electronic circuit on the porous silicon layer after forming the porous silicon layer; providing a second substrate having a second electronic circuit; bonding the first substrate and the second substrate together so that the first electronic circuit and the second electronic circuit are connected; 10. The method for manufacturing a semiconductor device according to claim 9, wherein the first electronic circuit and the first substrate are separated by the porous silicon layer as a boundary.
14. 14. The method for manufacturing a semiconductor device according to claim 13, wherein the first electronic circuit includes a memory cell array, and the second electronic circuit includes a control circuit for controlling an operation of the memory cell array.
15. A first substrate having at least a surface layer of silicon is provided; 1. A method for manufacturing a semiconductor device, comprising: making the silicon layer porous by anodizing to form a porous silicon layer having a first porous region having a first porosity, and a second porous region provided in a direction along the surface relative to the first porous region, the second porous region having a second porosity higher than the first porosity.
16. The method for manufacturing a semiconductor device according to claim 15 , wherein the second porous region surrounds the first porous region.
17. 16. The method of claim 15, wherein the first porous region surrounds the second porous region.
18. before forming the porous silicon layer, an impurity is implanted into the silicon layer by an ion implantation method to form a first region and a second region having an impurity concentration higher than that of the first region; 16. The method for manufacturing a semiconductor device according to claim 15, wherein, when the silicon layer is made porous, the first region becomes the first porous region and the second region becomes the second porous region.
19. The method includes a first step and a second step in forming the porous silicon layer, In the first step, a first substrate holder is used to limit a portion of the silicon layer that is in contact with an electrolyte to a first region; In the second step, a second substrate holder is used to limit a portion of the silicon layer that is in contact with the electrolyte to a second region inside the first region; 16. The method for manufacturing a semiconductor device according to claim 15, wherein the second region becomes the second porous region, and the first region outside the second region becomes the first porous region.
20. Before forming the porous silicon layer, a first region having a first insulating film on the surface of the silicon layer and a second region having a second insulating film having a thickness smaller than that of the first insulating film or having no insulating film are formed; 16. The method for manufacturing a semiconductor device according to claim 15, wherein, when the silicon layer is made porous, the first region becomes the first porous region and the second region becomes the second porous region.
21. forming a first electronic circuit on the porous silicon layer after forming the porous silicon layer; providing a second substrate having a second electronic circuit; bonding the first substrate and the second substrate together so that the first electronic circuit and the second electronic circuit are connected; 16. The method for manufacturing a semiconductor device according to claim 15, wherein the first electronic circuit and the first substrate are separated by the porous silicon layer as a boundary.
22. 22. The method for manufacturing a semiconductor device according to claim 21, wherein the first electronic circuit includes a memory cell array, and the second electronic circuit includes a control circuit that controls an operation of the memory cell array.
Citation Information
Patent Citations
Anodization apparatus, anodization system including the same, and semiconductor wafer
JP2013112880A