Rubber composition and tire

A rubber composition with styrene-butadiene rubber, C5C9 resin, and silica filler addresses the challenge of balancing fuel efficiency and wet grip performance, resulting in a tire with enhanced fuel efficiency and wet grip.

JP2024135989APending Publication Date: 2024-10-04MARUZEN PETROCHEMICAL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023046930
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing rubber compositions struggle to balance low fuel consumption with wet grip performance, as reducing rolling resistance typically deteriorates wet grip.

Method used

A rubber composition containing styrene-butadiene rubber, C5C9 resin, and silica filler, with specific ratios and properties, is used to enhance both fuel efficiency and wet grip performance.

Benefits of technology

The composition achieves a well-balanced tire performance with improved fuel efficiency and wet grip performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135989000001
    Figure 2024135989000001
  • Figure 2024135989000002
    Figure 2024135989000002
  • Figure 2024135989000003
    Figure 2024135989000003
Patent Text Reader

Abstract

To provide a rubber composition which achieves both fuel economy and wet grip performance.SOLUTION: The rubber composition contains: a rubber component (A) containing a styrene-butadiene rubber; a C5 / C9 resin (B); and a filler (C) containing silica. The content of the styrene-butadiene rubber in the rubber component (A) is 20-90 mass%. The content of the silica in the filler (C) is 50-100 mass%. The rubber composition contains 1-30 pts.mass of the C5 / C9 resin (B) and 20-130 pts.mass of the filler (C) based on 100 pts.mass of the rubber component (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition and a tire using the same. [Background technology]

[0002] In recent years, interest in environmental issues has increased, and there is a strong demand for automobiles with low fuel consumption. One method for reducing fuel consumption is to use tire rubber with low rolling resistance. However, it is known that using rubber with low rolling resistance reduces wet grip performance, and it is generally considered difficult to achieve both low fuel consumption and wet grip performance.

[0003] Various technologies for achieving both low fuel consumption and wet grip performance in tires have been studied. For example, a rubber composition using a styrene-butadiene rubber and butadiene rubber having a specific average molecular weight and average vinyl content (Patent Document 1), a rubber composition to which a copolymer resin of a C5 fraction of petroleum and dicyclopentadiene has been added (Patent Document 2), a rubber composition to which a certain amount of styrene-based resin has been added relative to the styrene amount of styrene-butadiene rubber (Patent Document 3), and a rubber composition using a specific aromatic resin and liquid polymer (Patent Document 4) have been disclosed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-145271 A [Patent Document 2] Patent Publication No. 2022-55449 [Patent Document 3] JP 2019-183009 A [Patent Document 4] JP 2019-112598 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a rubber composition which achieves both low fuel consumption and wet grip performance. [Means for solving the problem]

[0006] As a result of intensive research conducted by the inventors to solve the above problems, they discovered that by using a filler containing silica in a rubber composition and blending a C5C9 resin, it is possible to improve wet grip performance without reducing fuel economy, and thus completed the present invention.

[0007] That is, the present invention is as follows. (1) A rubber composition comprising a rubber component (A) containing styrene-butadiene rubber, a C5C9 resin (B) and a filler (C) containing silica, the content of the styrene-butadiene rubber in the rubber component (A) being 20 to 90% by mass, the content of the silica in the filler (C) being 50% by mass to 100% by mass, and containing 1 to 30 parts by mass of the C5C9 resin (B) and 20 to 130 parts by mass of the filler (C) per 100 parts by mass of the rubber component (A).

[0008] (2) The rubber composition according to (1), wherein the C5C9 resin (B) has a hydrogen peak ratio in the aromatic region of the total peak area in the proton nuclear magnetic resonance spectrum of 2 to 35%.

[0009] (3) The rubber composition according to (2), wherein the hydrogen peak ratio in the aromatic region of the total peak area in the proton nuclear magnetic resonance spectrum of the C5C9 resin (B) is 5 to 20%.

[0010] (4) A rubber composition according to any one of claims (1) to (3), wherein the C5C9 resin (B) has a softening point of 60°C to 95°C.

[0011] (5) A tire using the rubber composition according to any one of (1) to (4). Effect of the Invention

[0012] By using the rubber composition of the present invention, a tire having a good balance between low fuel consumption and wet grip performance can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The rubber composition of the present invention contains styrene-butadiene rubber (SBR) as the rubber component (A). The styrene-butadiene rubber is not particularly limited, and for example, emulsion-polymerized styrene-butadiene rubber, solution-polymerized styrene-butadiene rubber, etc. can be used.

[0014] The content of the styrene-butadiene rubber in the rubber component (A) is 20 to 90% by mass, preferably 35 to 85% by mass, from the viewpoints of fuel economy and wet grip performance. In this specification, when a numerical range is expressed using "to", the numerical range includes both ends of the range.

[0015] Other rubbers such as butadiene rubber (BR), isoprene rubber, and natural rubber can be used as the rubber component (A) in addition to styrene-butadiene rubber, and among these, butadiene rubber is preferably used. When butadiene rubber is blended, the content of butadiene rubber in the rubber component (A) is preferably 0 to 40 mass%, more preferably 5 to 35 mass%, from the viewpoints of fuel economy and wet grip performance.

[0016] The rubber composition of the present invention contains a C5C9 resin. The C5C9 resin is a copolymer resin made from petroleum-derived C5 fraction and C9 fraction. The C5C9 resin is not particularly limited, but preferably contains at least one selected from trans-1,3-pentadiene, cis-1,3-pentadiene, isoprene, 2-methyl-2-butene, cyclopentene, cyclopentadiene, trans-2-pentene and cis-2-pentene as the C5 fraction, and more preferably contains at least one selected from trans-1,3-pentadiene, cis-1,3-pentadiene, 2-methyl-2-butene and cyclopentene. A preferred embodiment of the C5 resin is one containing 15 to 40 mass% of trans-1,3-pentadiene, 5 to 30 mass% of cis-1,3-pentadiene, 2 to 25 mass% of 2-methyl-2-butene and 5 to 30 mass% of cyclopentene. The C9 fraction preferably contains at least one selected from styrene, vinyltoluene, α-methylstyrene, and β-methylstyrene, and more preferably contains styrene. The C5 fraction or C9 fraction also includes fractions separated into one or more of the above components.

[0017] From the viewpoints of fuel economy and wet grip performance, the hydrogen peak ratio in the aromatic region of the total peak area of ​​the proton nuclear magnetic resonance spectrum of the C5C9 resin is preferably 2 to 35%, more preferably 5 to 20%. In this specification, the hydrogen peak ratio in the aromatic region of the total peak area of ​​the proton nuclear magnetic resonance spectrum of the C5C9 resin means a value determined by the method described in the Examples.

[0018] From the viewpoints of fuel economy and wet grip performance, the softening point of the C5C9 resin is preferably 60 to 95° C., and more preferably 65 to 91° C. In this specification, the softening point of the C5C9 resin means a value measured by the method described in the examples.

[0019] Furthermore, (1) the hydrogen peak ratio in the aromatic region of the total peak area of ​​the proton nuclear magnetic resonance spectrum of the C5C9 resin is 6 to 10%, and the softening point is 65 to 95 ° C., more preferably in the range of 65 to 80 ° C., (2) the hydrogen peak ratio in the aromatic region of the total peak area of ​​the proton nuclear magnetic resonance spectrum is 10 to 15%, more preferably 11 to 14%, and the softening point is 65 to 95 ° C., more preferably in the range of 75 to 95 ° C., or (3) the hydrogen peak ratio in the aromatic region of the total peak area of ​​the proton nuclear magnetic resonance spectrum is 15 to 25%, more preferably 18 to 20%, and the softening point is 60 to 95 ° C., more preferably in the range of 65 to 80 ° C., thereby obtaining a product that is particularly excellent in fuel economy and wet grip performance.

[0020] The molecular weight of the C5C9 resin is not particularly limited, but from the viewpoint of fuel economy and wet grip performance, the number average molecular weight (Mn) is preferably 300 to 3500, more preferably 500 to 2000. The molecular weight distribution (Mw / Mn) is preferably 1.0 to 3.5, more preferably 1.0 to 2.5. The number average molecular weight and molecular weight distribution of the C5C9 resin are values ​​measured by the method described in the examples.

[0021] The method for producing the C5C9 resin is not particularly limited, and for example, it can be produced by using hexane, toluene, etc. as a solvent, mixing the solvent with the C5 fraction and the C9 fraction, and carrying out a polymerization reaction using a polymerization catalyst. The charging ratio of the C5 fraction and the C9 fraction is not particularly limited, and for example, 30 to 95 mass% of the C5 fraction and 5 to 70 mass% of the C9 fraction are preferable, and 40 to 90 mass% of the C5 fraction and 10 to 60 mass% of the C9 fraction are more preferable. As the polymerization catalyst, aluminum chloride, ethylaluminum dichloride, ethylaluminum sesquichloride, aluminum bromide, gallium chloride, triphenylmethylium tetrakis(pentafluorophenyl)borate, etc. can be used. The polymerization temperature is not particularly limited, but 50 to 110°C is preferable, and 65 to 90°C is more preferable.

[0022] The content of the C5C9 resin in the rubber composition is preferably 1 to 30 parts by mass, and more preferably 3 to 25 parts by mass, per 100 parts by mass of the rubber component (A) from the viewpoints of fuel economy and wet grip performance.

[0023] The rubber composition of the present invention contains silica as a filler (C). The silica is not particularly limited, and examples thereof include dry-type white carbon, wet-type white carbon, colloidal silica, precipitated silica, etc., among which precipitated silica is preferably used. The physical properties such as specific surface area are also not particularly limited. Silica is preferably used in combination with a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include sulfide-based, mercapto-based, vinyl-based, amino-based, glycidoxy-based, nitro-based, and chloro-based agents, among which sulfide-based agents are preferably used.

[0024] The filler (C) may contain carbon black. The manufacturing method of the carbon black is not limited, and any of furnace black, acetylene black, channel black, etc. may be used. The particle size, specific surface area, and other physical properties are not particularly limited, and GPF, FEF, HAF, ISAF, SAF, etc. may be used.

[0025] The content of silica in the filler (C) is 50% by mass to 100% by mass, and more preferably 75% to 100% by mass, from the viewpoints of fuel economy and wet grip performance. When the filler (C) contains carbon black, the content is preferably 50% by mass or less, and more preferably 25% by mass or less.

[0026] The content of component (C) in the rubber composition of the present invention is preferably 20 to 130 parts by mass, and more preferably 50 to 80 parts by mass, per 100 parts by mass of rubber component (A) from the viewpoints of fuel economy and wet grip performance.

[0027] The rubber composition of the present invention may contain various additives that are generally used in rubber compositions, such as vulcanizing agents, vulcanization accelerators, antioxidants, reinforcing materials, and colorants, within the range that does not impair the object of the present invention.

[0028] The rubber composition of the present invention can be suitably used in the tread portion of a pneumatic tire. By using the rubber composition of the present invention, a tire having both excellent fuel economy and wet performance can be obtained.

[0029] The tire of the present invention can be manufactured by a conventional method using the above-mentioned rubber composition. For example, the rubber composition of the present invention is extruded into a shape of a tread while still unvulcanized, and molded together with other tire components in a tire building machine by a conventional method to form an unvulcanized tire, which is then heated and pressurized to obtain a tire. EXAMPLES

[0030] The present invention will be described below with reference to examples, but the present invention is not limited to these examples in any way.

[0031] Manufacturing Example 1 60g of hexane, 20g of toluene, and 1080mg of aluminum chloride powder were put into an autoclave, heated with a heater set at 90°C, and the C5 fraction and the C9 fraction mixed in advance in the ratio shown in Table 1 were added and polymerized for 3 hours. As the C5 fraction, one containing 28% by mass of trans-1,3-pentadiene, 17% by mass of cis-1,3-pentadiene, 12% by mass of 2-methyl-2-butene, and 16% by mass of cyclopentene was used, and styrene was used as the C9 fraction. Then, 10mL of a terminator (isopropanol / ammonia = 1 / 1 (v / v)) was added, and the catalyst residue was filtered. After further purification by liquid separation, light fractions were removed with an evaporator to obtain resin A1. For the obtained resin A1, the hydrogen peak ratio in the aromatic region of the total peak area of ​​the proton nuclear magnetic resonance spectrum, the number average molecular weight (Mn), the molecular weight distribution (Mw / Mn), and the softening point were measured by the following method. The results are shown in Table 1.

[0032] (Proton nuclear magnetic resonance spectrum ( 1 H NMR) and measurement method for hydrogen peak ratio in aromatic region) 1 H NMR was performed using a JEOL JNM AL-400. The resin was dissolved in deuterated chloroform and measured. The hydrogen peak ratio in the aromatic region was calculated by dividing the area of ​​the peak at 6.0-7.5 ppm derived from aromatics in the obtained spectrum by the total peak area. Note that the peaks derived from water and chloroform were removed in advance before the calculation.

[0033] (Method of measuring number average molecular weight (Mn) and molecular weight distribution (Mw / Mn)) The number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) of the obtained resin were analyzed by gel permeation chromatography (GPC) (HLC-8320, manufactured by Tosoh Corporation). <Condition> Columns: G4000HXL, G3000HXL, G2000HXL (2 columns used) (Tosoh Corporation) Solvent: Tetrahydrofuran Measurement temperature: 40℃ Flow rate: 1.0 mL / min Calibration standard: Polystyrene

[0034] (Method of measuring softening point) The softening point of the obtained resin was measured by the ring and ball method in accordance with JIS K-2207 (1991).

[0035] Production Examples 2 to 8, Production Comparative Examples 1 to 3 The experimental conditions were changed as shown in Table 1 or Table 2, and resins A2 to A8 and resins B1 to B3 were obtained in the same manner as in Production Example 1. The hydrogen peak ratio in the aromatic region of the total peak area of ​​the proton nuclear magnetic resonance spectrum, the number average molecular weight (Mn), the molecular weight distribution (Mw / Mn), and the softening point of the obtained resins were measured in the same manner as in Production Example 1. The results are also shown in Table 1 or Table 2.

[0036] [Table 1]

[0037] [Table 2]

[0038] Example 1 In a Banbury mixer (capacity 600 ml), 100 parts by mass of a rubber component containing 80 parts by mass of HPR355 (styrene butadiene rubber, ENEOS Materials Corporation) and 20 parts by mass of BR01 (butadiene rubber, ENEOS Materials Corporation) were mixed with 70 parts by mass of silica (Nipsil AQ, Tosoh Silica Corporation), 7 parts by mass of a silane coupling agent (Si69, Evonik Corporation), 2 parts by mass of a rubber antioxidant (Ozonone 6C, Seiko Chemical Co., Ltd.), 3 parts by mass of zinc oxide (Seido Chemical Industry Co., Ltd.), 2 parts by mass of stearic acid (Tsubaki, Nippon Oil & Fats Corporation), 5 parts by mass of TDAE (Aromax 3, ENEOS Corporation), and 10 parts by mass of the C5C9 resin A1 obtained in Production Example 1. Then, 2.316 parts by mass of 5% sulfur, 1.8 parts by mass of vulcanization accelerators Sancerer CM-G and 0.5 parts by mass of Sancerer D were added, and the mixture was kneaded with a roll machine for 5 minutes. This was placed in a mold (100 mm x 200 mm x 2 mm) and heated at 170°C for 10 minutes to obtain a rubber sheet with a thickness of 2 mm. The obtained rubber sheet was evaluated for wet grip performance and fuel economy (rolling resistance) by the viscoelasticity measurement test described below. The results are shown in Table 1.

[0039] Examples 2 to 8, Comparative Examples 1 to 3 Except for replacing Resin A1 with Resins A2 to A8 or B1 to B3 obtained in Production Examples 2 to 8 or Comparative Production Examples 1 to 3, rubber sheets were prepared in the same manner as in Example 1, and the wet grip performance and fuel economy were evaluated in the same manner as in Example 1. The results are shown in Tables 3 and 4.

[0040] (Measuring conditions for viscoelasticity tester) Start temperature: -40℃ End temperature: 100℃ Temperature step: 1℃ Frequency: 10Hz Distortion (below -1°C): 0.1% Distortion (above -1℃): 2%

[0041] (Wet grip performance) The loss tangent (tan δ) value at a temperature of 0° C. was used as an index of wet grip performance. The larger this value, the shorter the braking distance and the better the wet grip performance. If the relative value, taking the value of Comparative Example 1 as 100, was 98 or more, the wet grip performance was evaluated as good.

[0042] (Fuel efficiency (rolling resistance)) The loss tangent (tan δ) value at a temperature of 60°C was used as an index of fuel economy. The smaller this value, the better the low heat build-up, the smaller the rolling resistance of the rubber composition, and the better the fuel economy. If the relative value, with the value of Comparative Example 1 taken as 100, was less than 100, the fuel economy was evaluated as good.

[0043] [Table 3]

[0044] [Table 4]

[0045] The rubbers of Examples 1 to 8 obtained from the rubber compositions containing the C5C9 resin were excellent in rolling resistance and wet grip properties. [Industrial Applicability]

[0046] The rubber composition of the present invention is capable of achieving both low fuel consumption and wet grip performance, and is useful as a rubber composition for tires such as summer tires.

Claims

1. A rubber composition comprising a rubber component (A) containing styrene-butadiene rubber, a C5C9 resin (B) and a filler (C) containing silica, the rubber component (A) having a content of styrene-butadiene rubber of 20 to 90 mass%, the filler (C) having a content of silica of 50 mass% to 100 mass%, and containing 1 to 30 parts by mass of C5C9 resin (B) and 20 to 130 parts by mass of filler (C) per 100 parts by mass of rubber component (A).

2. 2. The rubber composition according to claim 1, wherein the ratio of hydrogen peaks in the aromatic region to the total peak area in the proton nuclear magnetic resonance spectrum of the C5C9 resin (B) is 2 to 35%.

3. 3. The rubber composition according to claim 2, wherein the ratio of hydrogen peaks in the aromatic region to the total peak area in the proton nuclear magnetic resonance spectrum of the C5C9 resin (B) is 5 to 20%.

4. 2. The rubber composition according to claim 1, wherein the softening point of the C5C9 resin (B) is 60°C to 95°C.

5. A tire using the rubber composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Pneumatic tire

    JP2017190364A

  • Pneumatic tire

    JP2019026712A

  • Rubber composition for tire and pneumatic tire

    JP2019112599A

  • Pneumatic tire

    JP2020169313A

  • Rubber composition for tires, and pneumatic tire

    JP2020186322A