Non-aqueous inkjet ink and cured product formation method
The non-aqueous inkjet ink with silicone resin particles addresses sedimentation issues by enhancing redispersibility and stability, ensuring stable ejection and circulation of inorganic particles.
Patent Information
- Application Number
- JP2023046946
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing inkjet inks containing inorganic particles face issues with sedimentation during storage or standby, and once settled, these particles are difficult to redisperse, especially when larger particles are used.
A non-aqueous inkjet ink formulation incorporating silicone resin particles with a specific size range and silsesquioxane structure, which are smaller than the inorganic particles, enhances redispersibility and stability by allowing the silicone resin particles to penetrate between inorganic particles, preventing nozzle damage and maintaining ink circulation.
The formulation ensures stable ejection and circulation of inks with improved redispersibility of settled inorganic particles, reducing nozzle damage and maintaining consistent ink properties.
Smart Images

Figure 2024136001000001 
Figure 2024136001000002 
Figure 2024136001000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-aqueous ink-jet ink and a method for forming a cured product. [Background technology]
[0002] Ink-jet inks containing inorganic particles such as titanium oxide as a white pigment and conductive particles are known. The inorganic particles have a problem that they tend to settle in the ink during storage or while waiting before ejection.
[0003] To solve this problem, in the white inkjet ink composition described in Patent Document 1, fine barium sulfate particles are blended in the ink together with titanium oxide, and the barium sulfate particles suppress the precipitation of titanium oxide.
[0004] Furthermore, the inkjet ink described in Patent Document 2 uses titanium oxide, which has an average particle size of less than 100 nm and is therefore less prone to settling, and hollow particles, which have an average particle size of 100 nm or more and are therefore made hollow to make them less prone to settling, thereby sufficiently increasing the whiteness of the printed matter.
[0005] In addition, the anisotropic conductive adhesive inkjet ink described in Patent Document 3 uses an acrylic polymer, silica particles with a particle size of 0.001 to 0.5 μm, and silicone resin powder with a particle size of 0.5 to 10 μm to suppress settling of each component, including the conductive particles. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-256726 A [Patent Document 2] Patent Publication No. 2021-155502 [Patent Document 3] JP 2001-135141 A Summary of the Invention [Problem to be solved by the invention]
[0007] As described in Patent Documents 1 to 3, various methods for suppressing the settling of inorganic particles in inkjet inks have been investigated. However, according to the knowledge of the present inventors, even the methods described in these documents cannot completely suppress the settling of inorganic particles. Once the inorganic particles have settled, it is not easy to redisperse them. In addition, in recent years, it has been investigated to blend large inorganic particles, such as those having a particle size of 1 μm or more, into inkjet inks, but such large inorganic particles tend to settle and are not easy to redisperse after settling.
[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a non-aqueous ink-jet ink that has excellent re-dispersibility of settled inorganic particles, and a method for forming a cured product using the non-aqueous ink-jet ink. [Means for solving the problem]
[0009] One aspect of the present invention for solving the above problems relates to the following non-aqueous ink-jet inks [1] to
[10] . [1] A composition comprising inorganic particles and silicone resin particles, The average particle size of the silicone resin particles is 0.3 μm or more and 10 μm or less, The average particle size of the silicone resin particles is smaller than the median particle size of the inorganic particles. Non-aqueous inkjet ink. [2] The silicone resin particles have a silicone resin having a silsesquioxane structure. The non-aqueous inkjet ink according to [1]. [3] The average particle size of the silicone resin particles is 0.3 μm or more and 5 μm or less. The non-aqueous inkjet ink according to [1] or [2]. [4] The viscosity of the non-aqueous ink-jet ink at 25°C is 20 mPa s or more and 500 mPa s or less. The non-aqueous ink-jet ink according to any one of [1] to [3]. [5] Having a polymerizable compound that polymerizes when irradiated with active energy rays, The non-aqueous ink-jet ink according to any one of [1] to [4]. [6] The polymerizable compound includes a compound having an aromatic ring. [5] The non-aqueous inkjet ink according to [5]. [7] Volume resistivity is 10 11 It is possible to form a hardened product with a strength of Ω·m or higher. The non-aqueous ink-jet ink according to any one of [1] to [6]. [8] The median diameter of the inorganic particles is 0.5 μm or more and 5 μm or less. The non-aqueous ink-jet ink according to any one of [1] to [7]. [9] The inorganic particles are particles selected from the group consisting of glittering pigment particles, zinc oxide particles, and phosphorescent pigment particles; The non-aqueous ink-jet ink according to any one of [1] to [8].
[10] The inorganic particles are phosphorescent pigment particles. The non-aqueous ink-jet ink according to any one of [1] to [9].
[0010] Another aspect of the present invention for solving the above-mentioned problems relates to the following methods for forming a cured product
[11] to
[13] .
[11] A step of applying the non-aqueous inkjet ink according to any one of [1] to
[10] to a substrate; forming a film from the applied non-aqueous ink-jet ink; The method for forming a cured product comprising the steps of:
[12] The step of applying the ink-jet ink to the substrate is carried out while circulating the ink-jet ink. The method for forming a cured product according to
[11] .
[13] The method for forming a cured product according to
[11] or
[12] , wherein X in the following general formula is 0.30 or more and 95.0 or less, where X is a median diameter of the inorganic particles, A μm, an average particle diameter of the silicone resin particles, and a flow rate of the non-aqueous inkjet ink is C mL / s: X = (A / B) × C Effect of the Invention
[0011] According to the present invention, there are provided a non-aqueous ink-jet ink having excellent re-dispersibility of settled inorganic particles, and a method for forming a cured product using the non-aqueous ink-jet ink. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] 1. Non-aqueous inkjet ink One embodiment of the present invention relates to a non-aqueous ink-jet ink (hereinafter, simply referred to as "ink") containing inorganic particles and silicone resin particles. Each component will be described below.
[0013] 1-1.Inorganic particles The type of inorganic particles is not particularly limited. The inorganic particles may be pigment particles that impart characteristics such as color tone, electrical conductivity, insulating properties, heat dissipation properties, and a negative thermal expansion coefficient to a cured product formed from the ink, or may be particles that are added separately from the pigment to adjust the physical properties of the cured product.
[0014] The inorganic particles may be particles containing atoms other than carbon as a main component, where "containing atoms other than carbon" means that 50 mass % or more of the total mass of the inorganic particles is an atom other than carbon.
[0015] Examples of inorganic particles include: Silica particles, Metal oxide particles such as titanium oxide particles, alumina particles, zirconia particles, zinc oxide particles, and iron oxide particles Metal hydroxide particles, such as magnesium hydroxide particles, aluminum hydroxide particles, and calcium hydroxide particles Nitride particles such as silicon nitride particles, titanium nitride particles, and aluminum nitride particles Luster pigment particles such as silver particles (or conductive particles), Glass particles such as glass beads and glass flakes; silicate particles, such as magnesium silicate particles; Kaolin particles, calcined kaolin particles, ceramic particles such as clay, talc, zeolite, etc., Luminous pigment particles that can absorb light of a specific wavelength, store the light energy, and release the stored light energy for a long period of time as light of a different wavelength than the absorbed light. etc.
[0016] Examples of phosphorescent pigments include those in which the host crystal of a metal compound has been subjected to an activation treatment.
[0017] Examples of the above-mentioned parent crystal include sulfides such as zinc sulfide, calcium sulfide, germanium sulfide, strontium sulfide, and yttrium sulfide; metal oxides such as calcium oxide, strontium oxide, barium oxide, alumina, and cerium oxide; and aluminates such as calcium aluminate, strontium aluminate, and barium aluminate. Of these, strontium aluminate (SrAl 2 O 4 :Eu, Dy) are preferred.
[0018] Examples of the activator for activating the mother crystal include europium, terbium, yttrium, zirconium, dysprosium, barium, etc. Among these, europium and dysprosium are preferred.
[0019] The peak wavelength of the excitation spectrum of the phosphorescent pigment is preferably 300 nm or more and 400 nm or less. When the peak wavelength of the excitation spectrum of the phosphorescent pigment is in the above range, the phosphorescent pigment can be sufficiently excited by sunlight, and the cured product can be easily adapted for outdoor use.
[0020] The peak wavelength of the emission spectrum of the phosphorescent pigment may be, for example, from 400 nm to 700 nm, and from the viewpoint of further improving the visibility of the cured product, it is preferably from 450 nm to 600 nm.
[0021] Of these inorganic particles, preferred are glittering pigment particles, zinc oxide particles, and phosphorescent pigment particles, and from the viewpoint of facilitating diffusion of the silicone resin particles in the ink, more preferred are zinc oxide particles and phosphorescent pigment particles, and even more preferred are phosphorescent pigment particles.
[0022] The inorganic particles may be hollow particles or solid particles.
[0023] The shape of inorganic particles is not particularly limited, and may be spherical or non-spherical such as flat plate or whisker. Among these, spherical is preferred because it is easy to enhance the effect of improving redispersibility after settling by silicone resin particles. For example, the aspect ratio of inorganic particles, which is the ratio of major axis to minor axis, is preferably 1.0 or more and 1.5 or less, more preferably 1.0 or more and 1.2 or less.
[0024] The long axis and short axis of the inorganic particles can be the average of the long axis and the average of the short axis in an image of 1,000 inorganic particles arbitrarily selected from the inorganic particles in the ink captured in an image taken with a transmission electron microscope (TEM) or a scanning electron microscope (SEM), respectively.
[0025] The median diameter of the inorganic particles in the ink is not particularly limited, and can be 0.2 μm or more and 20 μm or less, preferably 0.3 μm or more and 10 μm or less, more preferably 0.5 μm or more and 5 μm or less, and even more preferably 0.5 μm or more and 3 μm or less. The larger the median diameter, the easier the inorganic particles will settle in the ink, and the silicone resin particles will have a significant effect of improving the redispersibility after settling. The smaller the median diameter, the easier the particles will be redispersed after settling, and the better the ejection properties from the inkjet head will be.
[0026] The median diameter of inorganic particles is the particle size at which the cumulative value in the volume-based particle size distribution reaches 50% (d 50 ) can be used.
[0027] The specific gravity of the inorganic particles can be from 2 to 6, preferably from 2.5 to 5, and more preferably from 3 to 4.5. The higher the specific gravity, the easier the inorganic particles will settle in the ink, and the silicone resin particles will have a significant effect of improving redispersibility after settling.
[0028] The inorganic particles may be dispersed by a dispersant. The inorganic particles may be dispersed by only one type of dispersant, or may be dispersed by two or more types of dispersants.
[0029] Examples of dispersants include carboxylates having a hydroxyl group, salts of long-chain polyaminoamides and high molecular weight acid esters, salts of high molecular weight polycarboxylic acids, salts of long-chain polyaminoamides and polar acid esters, high molecular weight unsaturated acid esters, polymer copolymers, modified polyurethanes, modified polyacrylates, polyether ester-type anionic surfactants, naphthalenesulfonic acid formalin condensate salts, aromatic sulfonic acid formalin condensate salts, polyoxyethylene alkyl phosphate esters, polyoxyethylene nonylphenyl ether, and stearylamine acetate. Commercially available examples of pigment dispersants include the Solsperse series (manufactured by Avecia, "Solsperse" is a registered trademark of the company), the PB series (manufactured by Ajinomoto Fine-Techno Co., Ltd.), and the EFKA series (manufactured by BASF, "EFKA" is a registered trademark of the company).
[0030] The content of the dispersant is preferably 0.01% by mass or more and 20% by mass or less with respect to the total mass of the inorganic particles.
[0031] The content of inorganic particles may be set according to the application of the inorganic particles. For example, the content of inorganic particles may be 1% by mass or more and 40% by mass or less, preferably 2% by mass or more and 35% by mass or less, and more preferably 3% by mass or more and 30% by mass or less, based on the total mass of the ink. The lower the content of inorganic particles, the higher the redispersibility of the precipitated inorganic particles.
[0032] 1-2. Silicone resin particles The silicone resin particles have an average particle size smaller than the median size of the inorganic particles. Such silicone resin particles penetrate between the inorganic particles to increase the fluidity of the inorganic particles. This is believed to make it easier to redisperse the settled inorganic particles.
[0033] If the settled inorganic particles cannot be redispersed, the concentration of the inorganic particles in the ejected inkjet ink is likely to fluctuate, or the viscosity of the inkjet ink may fluctuate, making the ejection unstable. In addition, when the inkjet ink before ejection is circulated in the ink flow path or the inkjet head, the circulation of the inkjet ink is likely to become unstable. In this embodiment, the silicone resin particles make it easy to redisperse the settled inorganic particles, making these problems less likely to occur.
[0034] In addition, inorganic particles often have a high hardness and are prone to damaging the nozzle surface of an inkjet head; however, it is thought that the silicone resin particles that get between the inorganic particles increase the fluidity of the inorganic particles, making it difficult for the inorganic particles to stick to the nozzle surface and thereby suppressing damage to the nozzle surface caused by the inorganic particles.
[0035] The average particle size of the silicone resin particles is preferably 0.2 μm or more and 7 μm or less, more preferably 0.3 μm or more and 5 μm or less, and even more preferably 0.5 μm or more and 3 μm or less. The smaller the average particle size of the silicone resin particles, the higher the redispersibility of the inorganic particles that have settled due to the above-mentioned action, the less likely they are to damage the nozzle surface, and the higher the circulation stability and storage stability. If the average particle size of the silicone resin particles is increased to a certain extent, the specific surface area of the inorganic particles to which the silicone resin particles are attached can be reduced, making it less likely that the inorganic particles will damage the nozzle surface.
[0036] The average particle diameter of silicone resin particles can be the value published by the manufacturer. It can also be measured as the volume average diameter using a particle size distribution analyzer (LUMiSizer, manufactured by LUM Japan Co., Ltd.) that uses the Stokes sedimentation method.
[0037] From the above viewpoint, the ratio of the median diameter of the inorganic particles to the average particle diameter of the silicone resin particles (median diameter of the inorganic particles / average particle diameter of the silicone resin particles) is preferably 1.2 or more and 15 or less, more preferably 1.3 or more and 10 or less, and even more preferably 1.5 or more and 6 or less.
[0038] The silicone resin constituting the silicone resin particles has a silsesquioxane structure ((RSiO 1.5 ) n and R is any organic group.) The type of R in the silsesquioxane structure is not limited, and may be an alkyl group or a halogen-substituted alkyl group, and is preferably a methyl group.
[0039] The silicone resin particles may be particles made of only silicone resin having a silsesquioxane structure, or may be particles formed of a blend structure or a core-shell structure by silicone resin having a silsesquioxane structure and other resin. As the other resin, vinyl resin or the like can be used, and acrylic resin is preferable. When having a core-shell structure, it is preferable that the shell contains silicone resin. From the viewpoint of increasing the redispersibility and circulation stability of the precipitated inorganic particles, it is preferable that the silicone resin particles are particles made of only silicone resin.
[0040] Specific examples of silicone resin particles include TOSPEARL 2000B, TOSPEARL 145, TOSPEARL 130, and XC-99-A8808 manufactured by MOMENTIVE Corporation.
[0041] The shape of silicone resin particles is preferably spherical.For example, the aspect ratio of silicone resin particles, which is the ratio of major axis to minor axis, is preferably 1.0 or more and 1.5 or less, more preferably 1.0 or more and 1.2 or less.The major axis and minor axis of silicone resin particles can be measured in the same manner as the major axis and minor axis of inorganic particles described above.
[0042] The content of the silicone resin particles can be 0.01% by mass or more and 5% by mass or less, preferably 0.1% by mass or more and 3% by mass or less, and more preferably 0.3% by mass or more and 2% by mass or less, based on the total mass of the ink. If the content of the silicone resin particles is 0.01% by mass or more, the redispersibility of the settled inorganic particles is improved. If the content of the silicone resin particles is 5% by mass or less, the decrease in circulation stability caused by the silicone resin particles that do not enter between the inorganic particles is suppressed.
[0043] In addition, the ratio of the silicone resin particle content to the inorganic particle content (silicone resin particle content (mass basis) / inorganic particle content (mass basis)) is preferably 0.0004 or more and 0.3 or less, more preferably 0.004 or more and 0.2 or less, and even more preferably 0.01 or more and 0.1 or less.
[0044] 1-3.Liquid component The ink according to the present embodiment is a non-aqueous ink. Specifically, the ink according to the present embodiment may be a polymerizable ink, a solvent-based ink, an oil ink, or the like. The non-aqueous ink preferably contains water in an amount of 0% by mass or more and less than 50% by mass, more preferably 0% by mass or more and less than 30% by mass, even more preferably 0% by mass or more and less than 10% by mass, even more preferably 0% by mass or more and less than 5% by mass, and particularly preferably does not contain water substantially. Note that "substantially does not contain water" means that the water content in the ink is 0% by mass or more and less than 1% by mass.
[0045] Non-aqueous inks have a small amount of water in the liquid components (or no water). In other words, non-aqueous inks have a small amount of polar water molecules. Therefore, in non-aqueous inks, the silicone resin particles are easily wetted due to the small amount of polar components, and are easily inserted between inorganic particles. This is thought to effectively achieve the above-mentioned effects, such as improved redispersibility of settled inorganic particles, improved abrasion resistance of the nozzle surface, and improved circulation stability and storage stability.
[0046] The polymerizable ink may be an ink in which the content of a polymerizable compound that polymerizes upon irradiation with active energy rays is 50% by mass or more relative to the total mass of the ink. The solvent-based ink may be an ink in which the content of an organic solvent is 50% by mass or more relative to the total mass of the ink. The polymerizable ink may be an ink in which the content of a polymerizable compound is 50% by mass or more relative to the total mass of the ink. The polymerizable ink may contain a photopolymerization initiator for initiating polymerization and crosslinking of the polymerizable compound. The oil ink may be an ink in which the content of oil is 50% by mass or more relative to the total mass of the ink.
[0047] 1-3-1. Polymerizable compounds and photopolymerization initiators 1-3-1-1.Polymerizable compound The polymerizable compound may be a radically polymerizable compound or a cationic polymerizable compound, and the polymerizable compound may be a combination of a radically polymerizable compound and a cationic polymerizable compound.
[0048] The radically polymerizable compound is a compound (monomer, oligomer, polymer, or a mixture thereof) having an ethylenically unsaturated bond capable of radical polymerization.
[0049] Examples of the compound having a radically polymerizable ethylenically unsaturated bond include unsaturated carboxylic acids and their salts, unsaturated carboxylic acid ester compounds, unsaturated carboxylic acid urethane compounds, unsaturated carboxylic acid amide compounds and their anhydrides, acrylonitrile, styrene, unsaturated polyesters, unsaturated polyethers, unsaturated polyamides, and unsaturated urethanes, etc. Examples of unsaturated carboxylic acids include (meth)acrylic acid, itaconic acid, crotonic acid, isocrotonic acid, maleic acid, etc.
[0050] Among them, the radical polymerizable compound is preferably an unsaturated carboxylic acid ester compound, more preferably a (meth)acrylate. The (meth)acrylate may be not only a monomer described below, but also an oligomer, a mixture of a monomer and an oligomer, a modified product, an oligomer having a polymerizable functional group, or the like.
[0051] Examples of monofunctional (meth)acrylates include isoamyl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, isomylstyryl (meth)acrylate, isostearyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 2-ethylhexyl-diglycol (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-(meth)acryloyloxyethylhexahydrophthalic acid, butoxyethyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, o-phenylenediamine (meth)acrylate, methyl meth ... arylphenoxyethyl (meth)acrylate, m-phenoxybenzyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, ethoxylated phenoxy (meth)acrylate, alkoxylated phenol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-hydroxy-o-phenylphenolpropyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl-phthalate, and t-butylcyclohexyl (meth)acrylate.
[0052] Examples of polyfunctional (meth)acrylates include triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol diacrylate, dimethylol-tricyclodecane di(meth)acrylate, bisphenol A type di(meth)acrylate, and hydroxypivalin. Examples of the (meth)acrylates include difunctional (meth)acrylates such as acid neopentyl glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, polyethylene glycol diacrylate, dipropylene glycol diacrylate, and tripropylene glycol diacrylate, as well as trifunctional or higher (meth)acrylates such as trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerin propoxy tri(meth)acrylate, and pentaerythritol ethoxy tetra(meth)acrylate.
[0053] The (meth)acrylate may be a modified product. Examples of modified (meth)acrylates include ethylene oxide modified (meth)acrylates including ethylene oxide modified trimethylolpropane tri(meth)acrylate and ethylene oxide modified pentaerythritol tetraacrylate, caprolactone modified (meth)acrylates including caprolactone modified trimethylolpropane tri(meth)acrylate, and caprolactam modified (meth)acrylates including caprolactam modified dipentaerythritol hexa(meth)acrylate.
[0054] The (meth)acrylate may be a polymerizable oligomer. Examples of the (meth)acrylate that is a polymerizable oligomer include an epoxy (meth)acrylate oligomer, an aliphatic urethane (meth)acrylate oligomer, an aromatic urethane (meth)acrylate oligomer, a polyester (meth)acrylate oligomer, and a linear (meth)acrylic oligomer.
[0055] Examples of the cationically polymerizable compound include an epoxy compound, a vinyl ether compound, and an oxetane compound.
[0056] Examples of the epoxy compounds include cycloaliphatic epoxy resins such as 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, bis(3,4-epoxycyclohexylmethyl)adipate, vinylcyclohexene monoepoxide, ε-caprolactone-modified 3,4-epoxycyclohexylmethyl 3',4'-epoxycyclohexanecarboxylate, 1-methyl-4-(2-methyloxiranyl)-7-oxabicyclo[4,1,0]heptane, 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexanone-meta-dioxane and bis(2,3-epoxycyclopentyl)ether, diglycidyl ether of 1,4-butanediol, diglycidyl ether of 1,6-hexanediol, triglyceride of glycerin, and the like. Examples of the epoxy compounds include aliphatic epoxy compounds including polyglycidyl ethers of polyether polyols obtained by adding one or more alkylene oxides (such as ethylene oxide and propylene oxide) to aliphatic polyhydric alcohols such as ethylene glycol, propylene glycol, and glycerin, as well as di- or polyglycidyl ethers of bisphenol A or its alkylene oxide adducts, di- or polyglycidyl ethers of hydrogenated bisphenol A or its alkylene oxide adducts, and novolac-type epoxy resins.
[0057] Examples of the vinyl ether compound include monovinyl ether compounds including ethyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, octadecyl vinyl ether, cyclohexyl vinyl ether, hydroxybutyl vinyl ether, 2-ethylhexyl vinyl ether, cyclohexanedimethanol monovinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, isopropenyl ether-o-propylene carbonate, dodecyl vinyl ether, diethylene glycol monovinyl ether, and octadecyl vinyl ether, as well as di- or trivinyl ether compounds including ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, propylene glycol divinyl ether, dipropylene glycol divinyl ether, butanediol divinyl ether, hexanediol divinyl ether, cyclohexanedimethanol divinyl ether, and trimethylolpropane trivinyl ether.
[0058] Examples of the oxetane compound include 3-hydroxymethyl-3-methyloxetane, 3-hydroxymethyl-3-ethyloxetane, 3-hydroxymethyl-3-propyloxetane, 3-hydroxymethyl-3-n-butyloxetane, 3-hydroxymethyl-3-phenyloxetane, 3-hydroxymethyl-3-benzyloxetane, 3-hydroxyethyl-3-methyloxetane, 3-hydroxyethyl-3-ethyloxetane, 3-hydroxyethyl-3-propyloxetane, 3-hydroxyethyl -3-phenyloxetane, 3-hydroxypropyl-3-methyloxetane, 3-hydroxypropyl-3-ethyloxetane, 3-hydroxypropyl-3-propyloxetane, 3-hydroxypropyl-3-phenyloxetane, 3-hydroxybutyl-3-methyloxetane, 1,4 bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane and di[1-ethyl(3-oxetanyl)]methyl ether.
[0059] The polymerizable compound preferably contains a compound having an aromatic ring in the molecule. The polymerizable compound having an aromatic ring in the molecule has an aromatic ring with low polarity, which makes it easier to wet the silicone resin particles and to easily penetrate between the inorganic particles, thereby more effectively achieving the effects of the silicone resin particles.
[0060] The content of the polymerizable compound having an aromatic ring is preferably from 20% by mass to 80% by mass, and more preferably from 30% by mass to 70% by mass, based on the total mass of the ink.
[0061] Examples of the polymerizable compound having an aromatic ring include phenol 4EO modified acrylate, 2-phenoxyethyl acrylate, m-phenoxybenzyl acrylate, EO modified o-phenylphenol acrylate, bisphenol fluorene diacrylate (A-BPEF), bisphenol A type 10EO modified diacrylate, bisphenol A type diacrylate, bisphenol A type PO modified diacrylate, bisphenol A type EO modified diacrylate, benzyl acrylate, cumylphenoxyethyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-o-phenylphenolpropyl acrylate, and the like.
[0062] The content of the polymerizable compound is preferably from 50% by mass to 97% by mass, and more preferably from 60% by mass to 95% by mass, based on the total mass of the polymerizable ink.
[0063] 1-3-1-2. Photopolymerization initiator The photopolymerization initiator can be a radical initiator when the polymerizable ink contains a radical polymerizable compound, and can be a cationic initiator (photoacid generator) when the polymerizable ink contains a cationic polymerizable compound. Note that when the polymerization is initiated by irradiation with an electron beam, the polymerizable ink does not need to contain a photopolymerization initiator.
[0064] Examples of the radical polymerization initiator include a hydrogen abstraction type photopolymerization initiator, an intramolecular cleavage type photopolymerization initiator, etc. The hydrogen abstraction type photopolymerization initiator includes an intramolecular hydrogen abstraction type photopolymerization initiator, an intermolecular hydrogen abstraction type photopolymerization initiator, etc.
[0065] The intramolecular hydrogen abstraction type photopolymerization initiator is a photopolymerization initiator that is excited by irradiation with active energy rays and generates a hydrogen abstraction reaction in the molecule to generate radicals. Examples of the intramolecular hydrogen abstraction type photopolymerization initiator include benzoyl formate-based photopolymerization initiators such as methyl phenylglyoxylate, and oxyphenyl-based photopolymerization initiators such as a mixture of oxyphenylacetic acid-2-[2-oxo-2-phenylacetoxy-ethoxy]ethyl ester and oxyphenylacetic acid 2-[2-hydroxy-ethoxy]ethyl ester. Among these, compounds having a glyoxylic acid structure such as benzoyl formate-based photopolymerization initiators are preferred because they are less likely to cause hydrogen abstraction from the molecular chain of the polymerizable compound during polymerization.
[0066] Examples of commercially available intramolecular hydrogen abstraction type photopolymerization initiators include Omnirad MBF and Omnirad 754 (both manufactured by IGM Resins, "Omnirad" being a registered trademark of the company).
[0067] The intermolecular hydrogen abstraction type photopolymerization initiator is a photopolymerization initiator that is excited by irradiation with active energy rays such as ultraviolet rays and abstracts hydrogen from other molecules to generate radicals. Examples of the intermolecular hydrogen abstraction type photopolymerization initiator include benzophenone-based initiators including benzophenone, o-benzoyl methyl benzoate, 4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, acrylated benzophenone, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, and 3,3'-dimethyl-4-methoxybenzophenone, and thioxanthone-based initiators such as 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone.
[0068] Examples of commercially available intermolecular hydrogen abstraction type photopolymerization initiators include Omnirad 500 (manufactured by IGM Resins) and Speedcure ITX (manufactured by Sartomer, "Speedcure" is a registered trademark of Arkema France).
[0069] Examples of the intramolecular cleavage type photopolymerization initiator include acetophenone-based initiators such as 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl-phenyl ketone, 2-methyl-2-morpholino(4-methylthiophenyl)propan-1-one, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone; benzoin-based initiators such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; and acylphosphine oxide-based initiators such as 2,4,6-trimethylbenzoin diphenylphosphine oxide and bis(2,4,6-trimethylbenzoin)phenylphosphine oxide.
[0070] Commercially available examples of intramolecular cleavage type photopolymerization initiators include Omnirad 127, Omnirad 184, Omnirad 651, Omnirad 2959, Omnirad 819, and Esacure One (all manufactured by IGM Resins).
[0071] The content of the photopolymerization initiator is preferably 3% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less, even more preferably 3% by mass or more and 10% by mass or less, and particularly preferably 5% by mass or more and 10% by mass or less, based on the total mass of the polymerizable ink. By making the content 3% by mass or more, the curability and adhesion of the polymerizable ink can be further improved.
[0072] 1-3-2. Organic solvents Examples of organic solvents include aliphatic alcohols, aromatic alcohols, diols, triols, glycol ethers, poly(glycol) ethers, lactams, formamides, acetamides, long chain alcohols, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, glycerin, dipropylene glycol, glycol butyl ethers, polyethylene glycol, polypropylene glycol, amides, amines, ethers, carboxylic acids, esters, organosulfides, organosulfoxides, sulfones, alcohol derivatives, carbitol, butyl carbitol, cellosolves, ether derivatives, amino alcohols, and ketones.
[0073] Of these, glycol ethers and fatty acid esters are preferred from the viewpoint of enhancing the dispersibility of inorganic particles.
[0074] Examples of glycol ethers include diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, dipropylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, other polyethylene glycols, other polypropylene glycols, and the like.
[0075] Examples of fatty acid esters include methyl oleate, methyl caprylate, methyl caprate, methyl laurate, methyl myristate, methyl palmitate, methyl stearate, methyl oleate, methyl tallowate, methyl rice branate, methyl rapeseedate, methyl soyate, n-butyl palmitate, n-butyl stearate, n-butyl rapeseedate, n-butyl soyate, i-butyl rice branate, i-butyl rapeseedate, octyl palmitate, octyl oleate, octyl rapeseedate, octyl vegetable acid, isopropyl myristate, and isopropyl palmitate.
[0076] The content of the organic solvent is preferably from 50% by mass to 97% by mass, and more preferably from 60% by mass to 95% by mass, based on the total mass of the solvent-based ink.
[0077] 1-3-3.Oil Examples of oils include aliphatic hydrocarbons including octane, nonane, decane, dodecane, isooctane, and isodecane, alicyclic hydrocarbons including cyclohexane, cyclooctane, and cyclodecane, and higher alcohols including octanol, decanol, and octadecenol.
[0078] The oil ink may further contain higher fatty acid esters and silicone oils as solvents, and may further contain vegetable oils. Examples of the vegetable oils include semi-drying oils such as soybean oil, cottonseed oil, rapeseed oil, sesame oil, and corn oil, non-drying oils such as olive oil, peanut oil, and camellia oil, and drying oils such as linseed oil and safflower oil.
[0079] The oil content is preferably from 50% by mass to 97% by mass, and more preferably from 60% by mass to 95% by mass, relative to the total mass of the oil ink.
[0080] 1-4.Other ingredients The ink may further contain other ingredients such as organic pigments, dyes, surfactants, optical brighteners, gelling agents, and polymerization inhibitors.
[0081] Examples of organic pigments include red pigments, yellow pigments, blue pigments, white pigments, etc., which are used in inks for forming images. Known pigments can be used for these pigments. Examples of dyes include red dyes, yellow dyes, blue dyes, etc., which are used in inks for forming images. Known dyes can be used for these dyes.
[0082] Examples of surfactants include anionic surfactants such as dialkyl sulfosuccinates, alkyl naphthalene sulfonates, and fatty acid salts; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, acetylene glycols, and polyoxyethylene-polyoxypropylene block copolymers; cationic surfactants such as alkylamine salts and quaternary ammonium salts; and silicone-based and fluorine-based surfactants.
[0083] The content of the surfactant is not particularly limited, but can be, for example, from 0.001% by mass to less than 1.0% by mass relative to the total mass of the ink.
[0084] The gelling agent is a compound that causes the ink to be in a gel state at room temperature (25°C) and in a sol state when heated (e.g., 80°C). For example, the gelling agent is preferably a compound that dissolves in the liquid components (polymerizable compounds and organic solvents, etc.) contained in the ink at a temperature higher than the gelling temperature of the ink and crystallizes at a temperature lower than the gelling temperature of the ink. The gelling temperature means the temperature at which the ink undergoes a phase transition from sol to gel and the viscosity of the ink suddenly changes when the ink that has been solated or liquefied by heating is cooled. Specifically, the temperature at which the viscosity of the ink suddenly increases when the ink that has been solated or liquefied by heating is cooled while the viscosity is measured with a rheometer (e.g., MCR300, manufactured by Anton Paar) can be regarded as the gelling temperature of the ink.
[0085] Examples of gelling agents include ketone waxes, ester waxes, petroleum waxes, vegetable waxes, animal waxes, mineral waxes, hydrogenated castor oil, modified waxes, higher fatty acids, higher alcohols, hydroxystearic acid, fatty acid amides including N-substituted fatty acid amides and special fatty acid amides, higher amines, esters of sucrose fatty acids, synthetic waxes, dibenzylidene sorbitol, dimer acid and dimer diol.
[0086] The content of the gelling agent is preferably from 1.0% to 10.0% by mass, more preferably from 2.0% to 7.5% by mass, and even more preferably from 2.0% to 3.5% by mass, relative to the total mass of the ink.
[0087] Examples of the polymerization inhibitor include N-oxyl-based polymerization inhibitors, phenol-based polymerization inhibitors, quinone-based polymerization inhibitors, amine-based polymerization inhibitors, copper dithiocarbamate-based polymerization inhibitors, etc. The polymerization inhibitor may be contained in the ink alone or in combination of two or more types.
[0088] Examples of N-oxyl polymerization inhibitors include 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl (TEMPO), 4-hydroxy-2,2,6,6-tetramethyl-piperidine-N-oxyl, 4-oxo-2,2,6,6-tetramethyl-piperidine-N-oxyl, 4-methoxy-2,2,6,6-tetramethyl-piperidine-N-oxyl, 4-acetoxy-2,2,6,6-tetramethyl-piperidine-N-oxyl, etc. Examples of commercially available N-oxyl polymerization inhibitors include Irgastab UV10 (manufactured by BASF ("Irgastab" is a registered trademark of the company)).
[0089] Examples of the phenol-based polymerization inhibitor include 2,6-di-tert-butylphenol, 2,4-di-tert-butylphenol, 2-tert-butyl-4,6-dimethylphenol, 2,6-di-tert-butyl-4-methylphenol, 2,4,6-tri-tert-butylphenol, 2,6-di-t-butyl-p-cresol (butylated hydroxytoluene: BHT), 4-methoxyphenol, 2-methoxy-4-methylphenol, and the like.
[0090] Examples of the quinone polymerization inhibitor include hydroquinone, methoxyhydroquinone, benzoquinone, 1,4-naphthoquinone, and p-tert-butylcatechol.
[0091] Examples of amine-based polymerization inhibitors include alkylated diphenylamines, N,N'-diphenyl-p-phenylenediamine, phenothiazine, and the like.
[0092] Examples of the copper dithiocarbamate polymerization inhibitor include copper dimethyldithiocarbamate, copper diethyldithiocarbamate, copper dibutyldithiocarbamate, and the like.
[0093] The content of the polymerization inhibitor is not particularly limited, but can be, for example, from 0.01% by mass to 0.5% by mass relative to the total mass of the ink.
[0094] 1-5. Ink properties The viscosity of the ink is not particularly limited, but the viscosity at 25°C is preferably 5 mPa·s or more and 1000 mPa·s or less, and more preferably 20 mPa·s or more and 500 mPa·s or less. Ink is often stored or on standby at about 25°C. The lower the viscosity at 25°C, the easier it is for the silicone resin particles to flow and for the inorganic pigment that has settled to be redispersed. On the other hand, by appropriately increasing the viscosity at 25°C, it is possible to suppress the settling of the inorganic pigment.
[0095] The viscosity of the composition at 25°C can be determined using a rheometer at a shear rate of 1000 / sec. The rheometer can be a stress-controlled rheometer from the Physica MCR series manufactured by Anton Paar. The diameter of the cone plate can be 75 mm, and the cone angle can be 1.0°.
[0096] The ink has a volume resistivity of 10 11 It is preferable that the cured film can have a resistivity of Ω·m or more. The surface resistivity of the cured film can be measured using a Hiresta UX (MCP-HT800, manufactured by Nitto Seiko Analytech Co., Ltd.).
[0097] 1-6. Ink preparation method The ink can be prepared by mixing the above-mentioned components. In this case, the components other than the inorganic particles may be mixed first, and the inorganic particles may be added to the resulting mixture later.
[0098] In addition, when dispersing inorganic particles with a dispersant, a dispersion liquid containing inorganic particles, a dispersant, and a liquid component may be prepared in advance, and the remaining components may be added and mixed thereto. In this case, in order to increase the solubility of the dispersant, etc., it is preferable to prepare the dispersion liquid by mixing the inorganic particles and the dispersant while heating them.
[0099] Furthermore, when inorganic particles are dispersed with a dispersant, silicone resin particles may be added in advance and dispersed. From the viewpoint of wetting the silicone resin particles with the ink and allowing them to penetrate between the inorganic particles, it is preferable to add the silicone resin particles in advance at the time of dispersion.
[0100] 2. Method for forming the cured product The ink described above can be applied to a substrate by an inkjet method to form a film, and can be used to form a cured product.
[0101] The application of the ink to the substrate may be performed by ejecting the ink from an inkjet head and allowing the ink to land on the substrate.
[0102] The ejection method from the inkjet head may be either an on-demand method or a continuous method. The on-demand inkjet head may be any of electro-mechanical conversion methods such as single cavity type, double cavity type, bender type, piston type, shear mode type, and shared wall type, and electro-thermal conversion methods such as thermal inkjet type and bubble jet type ("Bubble Jet" is a registered trademark of Canon Inc.).
[0103] These inkjet heads or image forming apparatuses having inkjet heads may have a configuration in which the ink is circulated inside or outside the inkjet head. When the ink is circulated while being ejected, if inorganic particles settle in the ink circulation flow path, the ejectability of the ink may be reduced. In contrast, in the present embodiment, the redispersibility of the settled inorganic particles is good, so that good ejectability can be maintained even when the ink is circulated.
[0104] In addition, the flow of ink in an inkjet head or an image forming apparatus preferably satisfies the following general formula, X, in the range of 0.30 to 95.0, where A μm is the median diameter of the inorganic particles, B μm is the average particle diameter of the silicone resin particles, and C mL / s is the flow rate of the ink. X = (A / B) × C
[0105] In addition to the median diameter of the inorganic particles and the average particle diameter of the silicone resin particles, the ink delivery flow rate can also be optimized to improve the redispersibility of the settled inorganic particles. From the above viewpoint, X is more preferably 0.30 or more and 95.0 or less, even more preferably 1.0 or more and 60 or less, particularly preferably 1.4 or more and 40 or less, and particularly preferably 1.5 or more and 40 or less. When the above X is satisfied, the flow stability of the ink can be improved. The effect of improving the flow stability is particularly noticeable in polymerizable inks.
[0106] The type of the substrate is not particularly limited, and may be, for example, paper, a resin film, an ABS resin plate, an acrylic resin plate, an aluminum plate, a glass plate, a polycarbonate plate, a cloth, etc. The shape of the substrate is not particularly limited, and may be a plate, a film, a sheet, or various three-dimensional shapes. The composition may be applied to the space formed inside the substrate by various methods.
[0107] The ink film may be formed by a method according to the type of ink. For example, when the ink is a polymerizable ink, the polymerizable compound is polymerized and crosslinked by irradiation with active energy rays to form a film of a cured product. Alternatively, when the ink is a solvent-based ink, the organic solvent is evaporated by heating to form a film of a cured product of the solid components in the ink.
[0108] Examples of active energy rays include electron beams, ultraviolet rays, α rays, γ rays, and X-rays. Of these, ultraviolet rays and electron beams are preferred. The ultraviolet rays are preferably light having a peak wavelength of 360 nm or more and 410 nm or less. The ultraviolet rays are preferably irradiated from an LED light source. LEDs emit less radiant heat than conventional light sources (e.g., metal halide lamps), so when LEDs are used, the ink is less likely to melt when irradiated with active energy rays, and uneven gloss is less likely to occur.
[0109] When ultraviolet rays are used as the active energy rays, the light intensity per irradiation is 500 mJ / cm 2 More than 4000mJ / cm 2 It is preferable that the intensity is 500 mJ / cm or less. 2 When the intensity is 4000 mJ / cm or more, the curability of the polymerizable compound can be improved. 2 When the content is equal to or less than this, discoloration of the cured product can be suppressed.
[0110] When forming a cured product with a large thickness, the application of the ink and the formation of a film may be repeated.
[0111] After the cured product is produced in this manner, a protective film for covering the cured product may be formed using a varnish, a laminate film, an ink, or the like, or the cured product may be post-processed into a desired shape. EXAMPLES
[0112] The present invention will be specifically described below with reference to examples, but the scope of the present invention is not limited to the description of the examples.
[0113] [Experiment 1] 1. Preparation of materials An inkjet ink was prepared using the following materials:
[0114] 1-1. Organic solvents Organic solvent 1: Polypropylene glycol Organic solvent 2: Methyl myristate
[0115] 1-2.Polymerizable compound Monomer 1: Dipropylene glycol diacrylate Monomer 2: Isobornyl acrylate Monomer 3: Phenol 4EO modified acrylate Monomer 4: 2-phenoxyethyl acrylate Monomer 5: Bisphenol A type 10EO modified diacrylate Monomer 6: Benzyl acrylate
[0116] 1-3. Photopolymerization initiator Initiator 1: Omnirad MBF, manufactured by IGM RESINS BV Initiator 2: Omnirad 754, manufactured by IGM RESINS BV Initiator 3: Omnirad 819, manufactured by IGM RESINS BV
[0117] 1-4.Inorganic particles Inorganic particle 1: Barium sulfate (Sakai Chemical Industry Co., Ltd., H-LFM) Inorganic particle 2: Glass flakes coated with iron oxide (GlassFlake, Moonshine Bronze Ultra Shimmer; "Moonshine" is a registered trademark of the company) Inorganic particle 3: Luminescent pigment (manufactured by Nemoto Specialty Chemical Co., Ltd., Luminova G-300F ("Luminova" is a registered trademark of the company) Inorganic particle 4: Zinc oxide (manufactured by Sakai Chemical Industry Co., Ltd., Candy Zinc 1000 ("Candy Zinz" is a registered trademark of the company) Inorganic particle 5: Luminescent pigment (manufactured by Nemoto Specialty Chemical Co., Ltd., Luminova G-300FF ("Luminova" is a registered trademark of the company) Inorganic particles 6: Conductive particles (manufactured by Ishihara Sangyo Kaisha, Ltd., ET-500W)
[0118] 1-5. Silicone resin particles Silicone 1: Particles of silicone resin having silsesquioxane bonds (manufactured by Nippon Shokubai Sangyo Co., Ltd., Tospearl 145 ("Tospearl" is a registered trademark of the company), average particle size: 4.5 μm) Silicone 2: Particles of silicone resin having silsesquioxane bonds (Tospearl 130, manufactured by Nippon Shokubai Sangyo Co., Ltd., average particle size: 2.0 μm) Silicone 3: Particles of silicone resin with silsesquioxane bonds (Momentive Performance Materials, Inc., XC-99-A8808, average particle size: 0.7 μm) Silicone 4: Particles of silicone resin having silsesquioxane bonds (Tospearl 2000B, manufactured by Nippon Shokubai Sangyo Co., Ltd., average particle size: 6.0 μm)
[0119] 1-6.Other particles Glass beads (Unitika Ltd., UBS-K0005MF, average particle size: 2.8 μm)
[0120] 1-7.Other ingredients Polymerization inhibitor: BASF, Irgastab UV-10
[0121] 2. Preparation of inkjet ink-1 (solvent-based ink) 2-1. Preparation of dispersion 20 parts by weight of inorganic particles 1 and 80 parts by weight of organic solvent 2 were placed in a polypropylene container together with 50 parts by weight of zirconia beads having an average particle size of 0.3 mm, and a dispersion treatment was carried out for 30 minutes using a paint shaker. The zirconia beads were then removed to prepare dispersion liquid 1A.
[0122] Dispersion liquid 1B to Dispersion liquid 1E were prepared in the same manner as Dispersion liquid 1A, except that inorganic particles were changed to Inorganic Particles 2 to 5, respectively.
[0123] Thereafter, the median diameter of the inorganic particles in the dispersion was measured using a particle size distribution analyzer (LUMiSizer, manufactured by LUM Japan Co., Ltd.) that utilizes the Stokes sedimentation method.
[0124] The organic solvent, dispersion, and silicone resin were mixed in the ratios shown in Table 1 and filtered through a 30 μm polypropylene pleated filter (manufactured by ROKI TECHNO Co., Ltd.) to obtain Inks 1 to 6. The values in parentheses in the "Inorganic particles" and "Silicone resin particles" columns in Table 1 are the median diameter and average particle diameter of each particle in the dispersion.
[0125] [Table 1]
[0126] 3. Preparation of Inkjet Ink-2 (Polymerizable Ink) 3-1. Preparation of dispersion 20 parts by weight of inorganic particles 1 and 80 parts by weight of monomer 1 were placed in a polypropylene container together with 50 parts by weight of zirconia beads having an average particle size of 0.3 mm, and the mixture was dispersed for 30 minutes using a paint shaker. The zirconia beads were then removed to prepare dispersion 2A.
[0127] Dispersions 2B to 2D and Dispersion 2F were prepared in the same manner as Dispersion 2A, except that the inorganic particles were changed to Inorganic Particles 2 to 5, respectively.
[0128] Dispersion liquid 2E was prepared in the same manner as in the preparation of dispersion liquid 2A, except that the inorganic particles were changed to inorganic particles 3 and the dispersion time was changed to 4 hours.
[0129] Dispersion liquid 2G was prepared in the same manner as in the preparation of dispersion liquid 2A, except that the inorganic particles were changed to inorganic particles 5 and the dispersion time was changed to 4 hours.
[0130] 50 parts by mass of inorganic particles 5 and 50 parts by mass of monomer 1 were placed in a polypropylene container together with 50 parts by mass of zirconia beads having an average particle size of 0.3 mm, and a dispersion treatment was carried out for 30 minutes using a paint shaker. The zirconia beads were then removed to prepare dispersion 2H.
[0131] 50 parts by mass of inorganic particles 5, 50 parts by mass of monomer 1, and 2 parts by mass of silicone 3 were placed in a polypropylene container together with 50 parts by mass of zirconia beads having an average particle size of 0.3 mm, and a dispersion treatment was carried out for 30 minutes using a paint shaker. The zirconia beads were then removed to prepare dispersion liquid 2I.
[0132] 20 parts by mass of inorganic particles 6 and 80 parts by mass of monomer 1 were placed in a polypropylene container together with 50 parts by mass of zirconia beads having an average particle size of 0.3 mm, and a dispersion treatment was carried out for 30 minutes using a paint shaker. The zirconia beads were then removed to prepare dispersion 2J.
[0133] Thereafter, the median diameter of the inorganic particles in the dispersion was measured using a particle size distribution analyzer (LUMiSizer, manufactured by LUM Japan Co., Ltd.) that utilizes the Stokes sedimentation method.
[0134] Monomer, photopolymerization initiator, dispersion, silicone resin, and polymerization inhibitor were mixed in the ratios shown in Tables 2 to 5 and filtered through a 30 μm polypropylene pleated filter (manufactured by ROKI TECHNO Co., Ltd.) to obtain Inks 7 to 35. The numerical values shown in parentheses in the columns "Inorganic particles" and "Silicone resin particles" in Tables 2 to 5 are the median diameter and average particle diameter of each particle in the dispersion.
[0135] [Table 2]
[0136] [Table 3]
[0137] [Table 4]
[0138] [Table 5]
[0139] 4. Evaluation The inks 1 to 35 prepared above were evaluated as follows.
[0140] 4-1. Viscosity at 25°C Using a rheometer (Anton Paar's stress-controlled rheometer Physica MCR, cone plate diameter 75 mm, cone angle 1.0°), the viscosity of each ink heated to 25° C. was measured at a shear rate of 1000 / sec.
[0141] Based on the measured viscosity, the viscosity of each ink was evaluated according to the following criteria. The ink viscosity is between 20mPa·s and 500mPa·s. △ Ink viscosity is greater than 500 mPa·s
[0142] 4-2. Settling recovery 10 g of the sample was placed in a 20 mL glass sample tube and left to stand at 25°C for 3 days to allow the solid matter to accumulate at the bottom of the sample tube. The sediment was shaken up and down vigorously by hand to measure the number of shakes required to loosen the sediment. ◎ After 1 to 10 times, most of the deposits will come off from the bottom of the sample tube. After 11 to 30 times, most of the deposits come off from the bottom of the sample tube. △ After 31 to 60 times, the deposits were almost completely peeled off from the bottom of the sample tube. × The sample does not come off from the bottom of the sediment sample tube within 60 tries.
[0143] 4-3.Abrasion resistance of nozzle surface A maintenance cloth (Savina CK: manufactured by KB Seiren) with each ink attached was pressed against the nozzle face of a Konica Minolta KM1024iLHE and rubbed 100 times, after which the surface of the nozzle face was observed. ○ Almost no scratches △ Slightly damaged × Large scratches are visible
[0144] 4-4. Circulatory stability The ink was circulated in a transparent tube with an inner diameter of 4 mm at 1.0 mL / s for 1 hour, and then the ink flow was stopped for 30 minutes. The ink was then circulated again at the same flow rate for 30 minutes, and the state of deposits formed in the tube and the state of circulation were observed. ◎ There was no change in the state of the liquid before and after the liquid supply was stopped, and it circulated smoothly. ○ Circulation was successful, but when the inside of the tank was checked after the experiment, a small amount of deposit was found. △ Although circulation was possible without any problems, a relatively large amount of deposits was found when the inside was checked after the experiment. × Deposits formed inside the tubes, causing blockages and preventing circulation.
[0145] 4-5.Storage stability Each ink was allowed to stand at a high temperature of 70° C. for one week, and then the circulation stability was evaluated. ○ The circulation stability was almost the same as that of the ink before being left to stand at high temperature, and there was almost no change. △: The circulation stability was slightly deteriorated compared to the ink before being left standing at high temperature.
[0146] The evaluation results of each ink are shown in Tables 6 to 10. Tables 6 to 10 also show the particle size ratio of each ink (median diameter of inorganic particles / average particle diameter of silicone resin particles), the ink flow rate, and parameter X (X = (A / B) x C).
[0147] [Table 6]
[0148] [Table 7]
[0149] [Table 8]
[0150] [Table 9]
[0151] [Table 10]
[0152] As is apparent from Tables 1 to 10, when the non-aqueous inkjet ink contained inorganic particles and silicone resin particles, the average particle diameter of the silicone resin particles was 0.3 μm or more and 10 μm or less, and the average particle diameter of the silicone resin particles was larger than the median diameter of the inorganic particles, the redispersibility of the settled inorganic particles was good.
[0153] [Experiment 2] Inks 9, 10, 11, and 13 prepared in Experiment 1 were used, and the flow rate was changed and circulated for 1 hour. After that, the ink flow was stopped for 30 minutes, and then the ink was circulated again at the same flow rate for 30 minutes. The appearance of deposits in the tube and the circulation status were observed to evaluate the circulation stability. ◎ There was no change in the state of the liquid before and after the liquid supply was stopped, and it circulated smoothly. ○ Circulation was successful, but when the inside of the tank was checked after the experiment, a small amount of deposit was found. △ Deposits formed and the tubes were prone to clogging. × Deposits formed inside the tubes, causing blockages and preventing circulation.
[0154] The evaluation results are shown in Table 11. Table 11 also shows the particle size ratio of each ink (median diameter of inorganic particles / average particle diameter of silicone resin particles), the ink flow rate, and parameter X (X = (A / B) x C).
[0155] [Table 11]
[0156] As is clear from Table 11, the circulation stability could be improved by setting the ink flow rate according to the particle size ratio of the inorganic particles to the silicone resin particles. [Industrial Applicability]
[0157] According to the present invention, it is possible to make it easier to use non-aqueous ink-jet inks containing inorganic particles. Therefore, the present invention is expected to broaden the applications to which non-aqueous ink-jet inks can be applied, and contribute to further development of this field.
Claims
1. The composition includes inorganic particles and silicone resin particles, The average particle size of the silicone resin particles is 0.3 μm or more and 10 μm or less, The average particle size of the silicone resin particles is smaller than the median particle size of the inorganic particles. Non-aqueous inkjet ink.
2. The silicone resin particles have a silicone resin having a silsesquioxane structure. The non-aqueous ink-jet ink according to claim 1 .
3. The average particle diameter of the silicone resin particles is 0.3 μm or more and 5 μm or less. The non-aqueous ink-jet ink according to claim 1 .
4. The viscosity of the non-aqueous ink-jet ink at 25° C. is 20 mPa·s or more and 500 mPa·s or less. The non-aqueous ink-jet ink according to claim 1 .
5. The composition has a polymerizable compound that polymerizes when irradiated with active energy rays. The non-aqueous ink-jet ink according to claim 1 .
6. The polymerizable compound includes a compound having an aromatic ring. The non-aqueous ink-jet ink according to claim 5 .
7. Volume resistivity is 10 11 It is possible to form a cured product with a hardness of Ω·m or more. The non-aqueous ink-jet ink according to claim 1 .
8. The median diameter of the inorganic particles is 0.5 μm or more and 5 μm or less. The non-aqueous ink-jet ink according to claim 1 .
9. The inorganic particles are particles selected from the group consisting of glittering pigment particles, zinc oxide particles, and phosphorescent pigment particles. The non-aqueous ink-jet ink according to claim 1 .
10. The inorganic particles are phosphorescent pigment particles. The non-aqueous ink-jet ink according to claim 1 .
11. applying the non-aqueous inkjet ink according to any one of claims 1 to 10 to a substrate; forming a film from the applied non-aqueous ink-jet ink; The method for forming a cured product comprising the steps of:
12. the step of applying the non-aqueous ink-jet ink to a substrate is performed while circulating the non-aqueous ink-jet ink; A method for forming a cured product according to claim 11.
13. 12. The method for forming a cured product according to claim 11, wherein X in the following general formula is 0.30 or more and 95.0 or less, where X is a median diameter of the inorganic particles, A μm, an average particle diameter of the silicone resin particles, B μm, and a flow rate of the non-aqueous ink-jet ink is C mL / s: X = (A / B) x C
Citation Information
Patent Citations
Anisotropic conductive bonding ink, liquid crystal display device and method of producing liquid crystal display device
JP2001135141A
Ink composition of white pigment
JP2004256726A
White pigment composition and recorded matter
JP2021155502A