Light reflection film and use method of light reflection film

A lightweight light-reflecting film with a transparent resin layer and reflective layer addresses the installation challenges of conventional materials by reflecting sunlight upward, reducing heat island effects and ground glare, and providing radiative cooling.

JP2024136078APending Publication Date: 2024-10-04OSAKA GAS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023047047
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional solar reflective civil engineering and construction materials are heavy and difficult to install on vertical walls, leading to poor workability and inefficiency in addressing the heat island phenomenon.

Method used

A lightweight light-reflecting film with a transparent resin material layer and a reflective layer featuring protrusions that refract and reflect sunlight upward, utilizing a structure with short and long sides intersecting at different lengths to enhance workability and reduce heat island effects.

Benefits of technology

The film effectively reflects sunlight upward, reducing ground glare and ambient temperature, while maintaining flexibility and ease of installation, and exhibits a radiative cooling function without absorbing light, thus alleviating the heat island phenomenon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136078000001_ABST
    Figure 2024136078000001_ABST
Patent Text Reader

Abstract

To provide a light reflection film which suppresses a heat island phenomenon with a constitution whose workability is excellent.SOLUTION: A light reflection film includes a translucent resin material layer J, and a light reflection layer B positioned on a rear surface side of the resin material layer J. On a surface of the resin material layer J, protrusion parts U including a short side S and a long side T which, in a cross-sectional view, cross with each other extending linearly toward the surface side of the resin material layer J from different positions in a crossing direction orthogonal to a thickness direction of the resin material layer J and have different lengths, are formed in a state of being arranged side by side in the crossing direction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a light-reflecting film that reflects sunlight and a method for using the light-reflecting film. [Background technology]

[0002] When sunlight is reflected by the walls of buildings and the like and irradiates the ground surface, the amount of heat stored on the ground surface, such as roads, increases, resulting in the so-called heat island phenomenon. One way to suppress this heat island effect is, for example, to reflect sunlight shining on the walls of a building upward (towards space).

[0003] For the purpose of such reflection, solar reflective civil engineering and construction materials (such as roofing tiles, tiles, etc.) have been proposed that have a solar reflective layer made of metallic aluminum with solar reflective properties on the outer surface of a base material (see, for example, Patent Document 1). Patent Document 1 describes attaching a sunlight reflective civil engineering and construction material to a vertical wall of a building or house with a gradient that reflects sunlight upward (towards space). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-192016 A Summary of the Invention [Problem to be solved by the invention]

[0005] Conventionally, heavy and difficult-to-install sunlight reflective civil engineering and construction materials have been attached to vertical walls of buildings and houses, making installation difficult and making improvements to the system desirable.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a light-reflecting film that has an excellent workability and suppresses the heat island phenomenon, and a method of using the light-reflecting film. [Means for solving the problem]

[0007] The light-reflecting film of the present invention has a characteristic configuration including a light-transmitting resin material layer and a light-reflecting layer located on a back surface side of the resin material layer, The present invention is characterized in that, when viewed in cross section, protrusion portions having short and long sides of different lengths that extend linearly from different positions in a cross direction perpendicular to the thickness direction of the resin material layer toward the surface side of the resin material layer and intersect are formed on the surface of the resin material layer so as to be aligned in the cross direction. The protrusion portion refers to a long and thin protrusion having a cross-sectional shape with short sides and long sides.

[0008] In other words, when the light reflecting film is installed in an upright position with the short side of one of the protrusions positioned above the long side, most of the sunlight coming from all directions and irradiating the surface of the resin material layer (sunlight irradiated from above) can be refracted from the long side to the short side of the protrusion due to the presence of the protrusion, and reflected (irradiated) upward. In other words, when sunlight is incident on a light-reflecting film having protrusions on its surface, the sunlight passes through the inside of the resin material layer and is reflected by the light-reflecting layer, and then passes through the inside of the resin material layer to be irradiated from the surface of the resin material layer.Since the refractive index of the resin material layer is greater than the refractive index of air, most of the reflection angle (reflection direction) of the sunlight shifts from the long side to the direction of the short side (see Figure 2).

[0009] In this way, by installing the light-reflecting film in an upright position with the short side positioned above the long side of one of the protrusions, most of the sunlight coming from all directions (sunlight irradiated from above) can be reflected (irradiated) upward, thereby mitigating the heat island effect.

[0010] Possible forms of installing a light-reflecting film on an object to which it is to be attached include, for example, forming the light-reflecting film into a thin film and connecting it to the object to which it is to be attached (connecting it with adhesive or pressure-sensitive adhesive). Light-reflecting films are lightweight and easy to handle, making them easy to install.

[0011] In addition to mitigating the above-mentioned heat island phenomenon, the light reflective film also provides the following operational effects. The light reflective film can reflect (irradiate) most of the sunlight coming from all directions (sunlight irradiated from above) upwards, so it can reduce the glare on the ground caused by the reflected (irradiated) light, especially when the light reflective film is applied to the side walls of a building (above the lower end). Incidentally, although it can be dazzling if it is within the angle of the reflected (irradiated) sunlight, outdoor work is usually performed at a lower position than the location where the light reflective film is installed, so it can reduce the glare on the ground.

[0012] In addition, since the light reflecting film is configured such that the resin material layer radiates infrared light from its surface and the light reflecting layer reflects light that has passed through the resin material layer, it functions as a radiative cooling film that exhibits a radiative cooling function. Furthermore, as described above, the light-reflecting film reduces the heat island effect, thereby lowering the surrounding air temperature and the temperatures of surrounding objects, and therefore the temperature of the light-reflecting film itself can be further reduced, thereby enabling the radiative cooling function to be effectively exerted.

[0013] Furthermore, sunlight that is incident on the protrusions of the light-reflecting film is reflected while being dispersed due to the dispersion of light (see FIG. 3). In other words, light-reflecting films can color objects without absorbing light. To explain further, the refractive index of light varies with wavelength. This wavelength dependency of the refractive index means that colors appear different depending on the observation angle, improving design. However, since light-reflecting films do not absorb sunlight, they can effectively exert a radiative cooling function.

[0014] In addition, the surface of the light-reflecting film is able to reflect (irradiate) most of the sunlight coming from all directions (sunlight irradiated from above) upwards due to reflection from the surface of the protrusions (see Figure 5). 10% to 15% of the sunlight that enters the light-reflecting film is reflected by the surface of the light-reflecting film, but this reflected light can be reflected (irradiated) upwards, which is also advantageous in terms of mitigating the heat island effect and reducing glare on the ground.

[0015] In short, the characteristic configuration of the light reflecting film of the present invention makes it possible to suppress the heat island phenomenon with a configuration that is easy to apply.

[0016] A further characteristic feature of the light reflecting film of the present invention is that a base end of the short side of each of the protrusions and a base end of the long side of each of the protrusions adjacent to each of the protrusions are at the same position in the intersecting direction.

[0017] In other words, the base end of the short side of the protrusion portion provided on the surface of the resin material layer and the base end of the long side of the adjacent protrusion portion are configured to be at the same position in the intersecting direction that intersects the thickness direction of the resin material layer; in other words, the short sides and long sides are arranged alternately in close contact with each other, so that the protrusion portions can be provided all over the surface of the resin material layer, and the entire surface of the resin material layer can be effectively used to reflect (irradiate) much of the sunlight upwards.

[0018] That is, when providing the protrusions on the surface of the resin material layer, it is possible to provide the protrusions in a form in which the base end of the short side of the protrusion and the base end of the long side of the protrusion adjacent to the protrusion are positioned apart in the intersecting direction, and a flat plane exists between the base end of the short side of the protrusion and the base end of the long side of the protrusion adjacent to the protrusion. Rather than this configuration, when the base end of the short side of the protrusion and the base end of the long side of the protrusion adjacent to the protrusion are in the same position in the intersecting direction, the entire surface of the resin material layer can be effectively used to reflect (irradiate) much of the sunlight upward.

[0019] A further characteristic feature of the light reflecting film of the present invention is that, in the cross-sectional view, for one of the protrusions, the base end of the short side and the base end of the long side are at the same position in the thickness direction of the resin material layer.

[0020] That is, since the base end of the short side and the base end of the long side of each protrusion are at the same position in the thickness direction of the resin material layer, the protrusion can be formed well.

[0021] A further characteristic feature of the light-reflecting film of the present invention is that, in the cross-sectional view, for one of the protrusion portions, the angle of the side of the long side of the short side relative to an imaginary plane passing through the base end of the short side along the intersecting direction is in the range of 80 degrees to 100 degrees.

[0022] That is, in a cross-sectional view, for one of the protrusions, the angle of the long side of the short side with respect to an imaginary plane passing through the base end of the short side along an intersecting direction intersecting with the thickness direction of the resin material layer is in the range of 80 degrees to 100 degrees. In other words, in a cross-sectional view, the short side of the protrusion stands at an angle of approximately 90 degrees with respect to an imaginary plane passing through the base end of the short side along an intersecting direction intersecting with the thickness direction of the resin material layer.

[0023] The presence of short sides in such a configuration makes it possible, for example, to make the length of the long sides sufficiently long, thereby enabling the function of reflecting (irradiating) most of the sunlight upward to be properly exhibited.

[0024] A further characteristic feature of the light-reflecting film of the present invention is that, in the cross-sectional view, for one of the protrusion portions, the angle of the side of the short side of the long side relative to an imaginary plane passing through the base end of the long side along the intersecting direction is greater than 0 degrees and less than 65 degrees.

[0025] That is, in a cross-sectional view, for one of the protrusion portions, the angle of the short side of the long side relative to an imaginary plane passing through the base end of the long side along a transverse direction that intersects with the thickness direction of the resin material layer is greater than 0 degrees and less than 65 degrees, so that, for example, light that is multiple-reflected inside the resin material layer and absorbed by the reflective layer or the resin material layer can be reduced.

[0026] In other words, if the amount of light absorbed by the reflective layer or the resin material layer increases, the temperature of the reflective layer or the resin material layer will rise, resulting in disadvantages such as a decrease in the radiative cooling function; however, by reducing the amount of light absorbed by the reflective layer or the resin material layer, the radiative cooling function can be effectively exerted.

[0027] Incidentally, in a cross-sectional view, the angle of the short side of the long side relative to an imaginary plane passing through the base end of the long side along a cross direction that intersects with the thickness direction of the resin material layer is preferably greater than 0 degrees and less than 55 degrees, and more preferably greater than 0 degrees and less than 45 degrees.

[0028] A further characteristic feature of the light reflecting film of the present invention is that the base end of the short side and the base end of the long side are located in the middle of the resin material layer in the thickness direction.

[0029] In other words, since the base ends of the short sides and the base ends of the long sides of the protrusion are located in the middle of the resin material layer in the thickness direction of the resin material layer, it is easy to form the protrusion in the resin material layer. That is, it becomes easy to form the protrusions in the resin material layer by, for example, embossing or cutting.

[0030] Incidentally, when the base end of the short side and the base end of the long side of the protrusion portion are located in the middle of the resin material layer in the thickness direction of the resin material layer, this means that the base end of the short side and the base end of the long side are located on the surface side of the resin material layer relative to the midpoint in the thickness direction of the resin material layer, at a location equivalent to the midpoint in the thickness direction of the resin material layer, or on the side where the light reflective layer is present relative to the midpoint in the thickness direction of the resin material layer.

[0031] A further characteristic feature of the light reflecting film of the present invention is that the base end of the short side and the base end of the long side are located at the end of the resin material layer on the side where the light reflecting layer is present in the thickness direction.

[0032] In other words, the base ends of the short sides and the long sides of the protrusion portion are located at the ends of the resin material layer on the side where the light-reflecting layer is present, in the thickness direction of the resin material layer. This makes it possible to effectively utilize the light-reflecting film, for example, by shortening the distance between the long side and the light-reflecting layer, so that sunlight incident from the surface of the long side can be irradiated to the outside from the surface of the same long side.

[0033] To explain further, when the light reflecting film is installed in an upright position with the short side positioned above the long side of one of the protrusions, for example, sunlight incident from the surface of the long side located at the lower end of the light reflecting film can be irradiated to the outside from the surface of the same long side, and the lower end portion of the light reflecting film can also be effectively used to reflect (irradiate) sunlight upwards.

[0034] A further characteristic configuration of the light reflecting film of the present invention is that a light-transmitting coating layer covering a surface of the resin material layer is provided in a form that fills spaces between adjacent protrusions to make an outer surface a flat surface, The refractive index of the resin material forming the coating layer is smaller than the refractive index of the resin material forming the resin material layer.

[0035] In other words, sunlight that enters the light-reflecting film from the air is refracted when it enters the coating layer, and then is refracted when it enters the resin material layer, and the sunlight reflected by the light-reflecting layer is refracted when it enters the coating layer, and then is refracted when it is irradiated into the air, making it possible to more effectively reflect (irradiate) sunlight upward.

[0036] A further characteristic feature of the light-reflecting film of the present invention is that the surface of the light-reflecting layer on the side where the resin material layer is present is formed, in the cross-sectional view, in plane symmetry with the surface of the resin material layer having the protrusion portion, with respect to a reference plane located along the intersecting direction and between the surface of the resin material layer and the light-reflecting layer.

[0037] In other words, the surface of the light reflecting layer on the side where the resin material layer is present is formed in plane symmetry with the surface of the resin material layer having the protrusion portion, so that sunlight that enters the resin material layer and is reflected by the light reflecting layer can be reflected toward the side where the short side is present when reflected by the light reflecting layer.

[0038] Therefore, when the light reflecting film is installed in an upright position with the short side positioned above the long side of one of the protrusion portions, sunlight that enters the resin material layer and is reflected by the light reflecting layer can be reflected upward, making it possible to more effectively reflect (irradiate) sunlight upward.

[0039] A further characteristic configuration of the light reflecting film of the present invention is that the resin material layer is an infrared emitting layer that emits infrared light from an emitting surface, The infrared radiation layer is made of an infrared radiation resin material whose thickness is adjusted to emit greater thermal radiation energy than absorbed solar energy in the wavelength band from 8 μm to 14 μm.

[0040] In other words, sunlight incident on the radiation surface (surface of the resin material layer) of the infrared radiation layer in the light reflecting film passes through the infrared radiation layer, is reflected by the light reflecting layer located opposite to the side where the radiation surface of the infrared radiation layer is present, and is then allowed to escape from the system through the radiation surface. In the description of this specification, when simply referring to light, the concept of light includes ultraviolet light (ultraviolet light), visible light, and infrared light. When these are described in terms of the wavelength of light as electromagnetic waves, they include electromagnetic waves with wavelengths of 10 nm to 20,000 nm (electromagnetic waves of 0.01 μm to 20 μm).

[0041] Moreover, the heat transferred (heat input) to the light reflecting film is converted into infrared rays by the infrared emitting layer, which serves as the infrared emitting layer, and is released to the outside of the system from the emitting surface. In this way, the light-reflecting film reflects the sunlight irradiated onto it, and can also radiate heat transferred to the light-reflecting film (e.g., heat transferred from the atmosphere or from an object to be cooled by the light-reflecting film) outside the system as infrared light.

[0042] The thickness of the infrared radiation layer is adjusted so that it emits greater thermal radiation energy in the 8 μm to 14 μm wavelength band than the absorbed solar energy, so that the light reflecting layer appropriately reflects solar light, while still providing a cooling function even in a daytime solar environment.

[0043] A further characteristic feature of the light-reflecting film of the present invention is that the light-reflecting layer comprises silver or a silver alloy.

[0044] In other words, the light-reflecting layer made of silver or a silver alloy can be provided with reflectance characteristics of 90% or more at wavelengths of 0.4 μm to 0.5 μm and 96% or more at wavelengths longer than 0.5 μm, thereby enabling the appropriate reflection of sunlight. That is, the solar spectrum exists from wavelength 0.295 μm to 4 μm, and the intensity increases as the wavelength increases from 0.4 μm, and the intensity is particularly high from wavelength 0.5 μm to wavelength 2.5 μm. A light-reflective layer made of silver or a silver alloy can be provided with reflective properties that show a reflectance of 90% or more from wavelengths of 0.4 μm to 0.5 μm, and a reflectance of 96% or more at wavelengths longer than 0.5 μm, so that the light-reflective layer absorbs only about 5% or less of the solar energy.

[0045] As a result, the solar energy absorbed by the light-reflecting layer at noon in summer was reduced to 50 W / m 2 Since the temperature can be kept at about 1000° C. or less, radiation cooling by the infrared radiative layer can be performed satisfactorily. In this specification, unless otherwise specified, the spectrum of sunlight is in accordance with the AM1.5G standard. As described above, the object to be cooled can be cooled by radiative cooling even in a daytime solar radiation environment.

[0046] A further characteristic configuration of the light reflecting film of the present invention is that the infrared radiation resin material is a vinyl chloride resin or vinylidene chloride resin mixed with a plasticizer, The plasticizer is one or more compounds selected from the group consisting of phthalic acid esters, aliphatic dibasic acid esters, and phosphate esters.

[0047] That is, vinyl chloride resins provide sufficient thermal radiation in window regions exposed to the atmosphere, and as a result, can provide appropriate radiative cooling outdoors even in a solar radiation environment. In other words, vinyl chloride resins have thermal radiation characteristics equivalent to those of fluororesins and silicone rubbers, which provide large thermal radiation in window regions exposed to the atmosphere, and are considerably cheaper than these resins, so they are effective in inexpensively constructing a light reflective film whose temperature drops below the ambient temperature under direct sunlight.

[0048] In addition, since a plasticizer is mixed into the polyvinyl chloride resin, for example, the light-reflecting layer made of silver or a silver alloy has elasticity, and in addition, the infrared radiation layer has sufficient elasticity (ease of stretching). As a result, the light-reflecting film has sufficient elasticity (ease of stretching), and the light-reflecting film can be attached to the object to be attached while being stretched, thereby improving workability.

[0049] By the way, vinyl chloride resins can be made soft by adding plasticizers, and when they come into contact with other objects, they can flexibly change shape to fit the object, avoiding damage, and can therefore be maintained in a beautiful condition for a long period of time.By the way, thin-film fluororesin is hard, so it cannot flexibly change shape when it comes into contact with other objects, is easily damaged, and is difficult to maintain in a beautiful condition.

[0050] Furthermore, since vinyl chloride resins are flame retardant and difficult to biodegrade, they are suitable as resin materials for forming the resin material layer of a light reflecting film that is used outdoors for a long period of time.

[0051] In addition, since the plasticizer is composed of one or more compounds selected from the group consisting of phthalate esters, aliphatic dibasic acid esters, and phosphate esters, deterioration of the plasticizer due to ultraviolet rays can be avoided and discoloration of the vinyl chloride resin can be suppressed.

[0052] In other words, since the plasticizer mixed into the polyvinyl chloride resin is one or more compounds selected from the group consisting of phthalate esters, aliphatic dibasic acid esters, and phosphate esters, the plasticizer is less likely to absorb the ultraviolet rays contained in sunlight (ultraviolet light with wavelengths of 295 nm to 400 nm), and the weather resistance of the polyvinyl chloride resin mixed with the plasticizer can be appropriately improved.

[0053] To explain further, when a plasticizer mixed into polyvinyl chloride resin absorbs ultraviolet light, hydrolysis of the plasticizer progresses, causing the polyvinyl chloride resin to undergo dechlorination, etc., and become discolored (brown), and there is a risk of a decrease in mechanical strength. However, because the plasticizer becomes less able to absorb the ultraviolet light contained in sunlight, the weather resistance of the polyvinyl chloride resin mixed with the plasticizer can be further improved.

[0054] A further characteristic configuration of the light reflecting film of the present invention is to further include an adjacent-side protective layer between the infrared emitting layer and the light reflecting layer, The adjacent-side protective layer is made of a polyolefin resin having a thickness of 300 nm or more and 40 μm or less, or an ethylene terephthalate resin having a thickness of 17 μm or more and 40 μm or less.

[0055] In other words, since the adjacent-side protective layer is made of a polyolefin resin with a thickness of 300 nm or more and 40 μm or less, or is made of an ethylene terephthalate resin with a thickness of 17 μm or more and 40 μm or less, discoloration of the silver or silver alloy in the light-reflecting layer can be adequately prevented even in a daytime solar radiation environment, so that the light-reflecting layer can appropriately reflect sunlight while adequately exerting its cooling function even in a daytime solar radiation environment.

[0056] In other words, if the adjacent-side protective layer were not present, radicals generated in the infrared radiation layer would reach the silver or silver alloy that forms the light-reflecting layer, or moisture that penetrates the infrared radiation layer would reach the silver or silver alloy that forms the light-reflecting layer, causing the silver or silver alloy of the light-reflecting layer to discolor in a short period of time and resulting in a state in which the light-reflecting function is not properly performed. However, the presence of the adjacent-side protective layer made of a polyolefin resin or an ethylene terephthalate resin can prevent the silver or silver alloy of the light-reflecting layer from discoloring in a short period of time.

[0057] An explanation will now be given of the fact that the adjacent protective layer prevents discoloration of the silver or silver alloy in the light reflective layer. When the adjacent-side protective layer is formed from a polyolefin-based resin to a thickness of 300 nm or more and 40 μm or less, the polyolefin-based resin is a synthetic resin whose ultraviolet light absorptance is 10% or less over the entire ultraviolet wavelength range from 0.295 μm to 0.4 μm, and therefore the adjacent-side protective layer is less likely to deteriorate due to absorption of ultraviolet light.

[0058] Furthermore, since the thickness of the polyolefin resin forming the adjacent-side protective layer is 300 nm or more, it effectively exhibits a blocking function of blocking radicals generated in the infrared-emitting layer from reaching the silver or silver alloy forming the light-reflecting layer, and also blocks moisture passing through the infrared-emitting layer from reaching the silver or silver alloy forming the light-reflecting layer, thereby making it possible to suppress discoloration of the silver or silver alloy forming the light-reflecting layer.

[0059] In other words, the adjacent side protective layer made of a polyolefin resin will deteriorate as it absorbs ultraviolet rays, forming radicals on the surface side away from the light reflecting layer. However, since the thickness is 300 nm or more, the formed radicals will not reach the light reflecting layer. Furthermore, even if the adjacent side protective layer deteriorates as radicals are formed, the rate of deterioration is slow due to the low absorption of ultraviolet rays, so the above-mentioned blocking function will be maintained for a long period of time.

[0060] When the adjacent-side protective layer is formed from ethylene terephthalate resin to a thickness of 17 μm or more and 40 μm or less, ethylene terephthalate resin is a resin material that has a higher ultraviolet light absorptance in the ultraviolet wavelength range of 0.295 μm to 0.4 μm than polyolefin-based resins. However, since the thickness is 17 μm or more, the layer can effectively perform blocking functions for a long period of time, such as blocking radicals generated in the infrared-emitting layer from reaching the silver or silver alloy that forms the light-reflecting layer and blocking moisture that penetrates the infrared-emitting layer from reaching the silver or silver alloy that forms the light-reflecting layer, and thus suppressing discoloration of the silver or silver alloy that forms the adjacent-side protective layer.

[0061] In other words, the adjacent-side protective layer made of ethylene terephthalate resin deteriorates as it absorbs ultraviolet rays, forming radicals on the surface side away from the light-reflecting layer. However, since the thickness is 17 μm or more, the formed radicals will not reach the light-reflecting layer. Furthermore, even if the adjacent-side protective layer deteriorates while forming radicals, the thickness is 17 μm or more, so the above-mentioned blocking function will be exhibited for a long period of time.

[0062] In addition, when the adjacent-side protective layer is formed of a polyolefin resin and an ethylene terephthalate resin, the upper limit of the thickness is set, so that it is possible to prevent the adjacent-side protective layer from exhibiting heat insulating properties that do not contribute to radiative cooling as much as possible. In other words, the thicker the adjacent-side protective layer is, the more heat insulating properties it exhibits that do not contribute to radiative cooling, so the upper limit of the thickness is set in order to prevent heat insulating properties that do not contribute to radiative cooling as much as possible while still exerting the function of protecting the light reflecting layer.

[0063] A further characteristic feature of the light reflecting film of the present invention is that a spacing-side protective layer is provided on the surface of the light reflecting layer facing away from the infrared emitting layer, and the spacing-side protective layer is made of an acrylic resin.

[0064] In other words, since a separation-side protective layer is provided on the surface of the light-reflecting layer facing away from the infrared radiation layer, and the resin material forming the separation-side protective layer is an acrylic resin, it is possible to appropriately prevent moisture and the like from penetrating from the back surface side of the light-reflecting layer opposite the side on which the infrared radiation layer is present and reaching the light-reflecting layer, thereby appropriately suppressing deterioration of the light-reflecting layer.

[0065] A further characteristic configuration of the light reflecting film of the present invention is that a connecting resin material layer is provided on a back surface portion of the separation-side protective layer that is away from the light reflecting layer, The connecting resin material layer is made of any one of ethylene terephthalate resin, polypropylene, polyethylene, and acrylic resin.

[0066] That is, since the back surface of the light reflecting film is provided with a connecting resin material layer for connecting to an attachment object, the light reflecting film can be easily attached to an attachment object, improving usability.

[0067] Furthermore, since the resin material forming the connecting resin material layer is any one of ethylene terephthalate resin, polypropylene, polyethylene, and acrylic resin, it can be appropriately connected to the mounting object using an adhesive or pressure sensitive adhesive.

[0068] A characteristic feature of the method of using a light-reflecting film of the present invention is that, in the method of using a light-reflecting film described above, the light-reflecting film is installed on a wall surface in an upright position with the short side positioned above the long side of one of the protrusion portions.

[0069] In other words, the light reflecting film is installed on the wall in an upright position with the short side positioned above the long side of one of the protrusions, so that the light reflecting film is in an upright position with the short side positioned above the long side of one of the protrusions. As described above, most of the sunlight coming from all directions and irradiating the surface of the resin material layer (sunlight irradiated from above) can be refracted from the long side to the short side of the protrusions and reflected (irradiated) upward, due to the presence of the protrusions.

[0070] In this way, by installing the light-reflecting film on a wall in an upright position with the short side positioned above the long side of one of the protrusions, most of the sunlight coming from all directions (sunlight irradiated from above) can be reflected (irradiated) upward, thereby mitigating the heat island effect. [Brief description of the drawings]

[0071] [Figure 1] FIG. 2 is a diagram illustrating a basic configuration of a light reflecting film. [Diagram 2] FIG. 2 is a diagram illustrating the solar light reflection form of a light-reflecting film. [Diagram 3] 11A and 11B are diagrams illustrating dispersion of light by protrusions. [Figure 4] 13A to 13C are diagrams illustrating another form of formation of the protrusions. [Diagram 5] 6A and 6B are diagrams illustrating reflection of light by the surface of a protrusion portion. [Figure 6] 13A and 13B are diagrams illustrating a configuration in which a resin material layer is covered with a coating layer. [Figure 7] 13 is a diagram illustrating a configuration in which a light reflecting layer side protrusion portion is formed on the light reflecting layer. FIG. [Figure 8] FIG. 2 is a diagram illustrating a form of light reflection. [Figure 9] FIG. 2 is a diagram showing the relationship between the angle of incidence and the angle of reflection with respect to a reflecting surface. [Figure 10] FIG. 2 is a diagram showing the relationship between the angle of incidence and the angle of reflection with respect to a reflecting surface. [Figure 11] FIG. 2 is a diagram showing the relationship between the angle of incidence and the angle of reflection with respect to a reflecting surface. [Figure 12] FIG. 1 is a diagram illustrating a conventional light reflection form. [Figure 13] FIG. 2 is a diagram comparing the light reflection form of the present invention with a conventional light reflection form. [Figure 14] FIG. 2 is a diagram illustrating a specific configuration of a light reflecting film. [Figure 15] FIG. 4 is a diagram showing the relationship between the light absorptance of a resin material and the wavelength. [Figure 16] FIG. 1 is a diagram showing the emissivity spectrum of polyvinyl chloride resin. [Figure 17] FIG. 2 is a diagram showing the emissivity spectrum of vinylidene chloride resin. [Figure 18] FIG. 2 shows the light reflectance spectrum of a silver-based light reflective layer. [Figure 19] FIG. 1 shows a specific configuration of a radiative cooling film. [Figure 20] FIG. 1 illustrates the fabrication procedure of a radiative cooling film. [Figure 21] FIG. 1 is a graph showing the relationship between light transmittance and wavelength of polyethylene. [Figure 22] FIG. 2 is a diagram showing the emissivity spectrum of polyethylene. [Figure 23] FIG. 1 is a diagram showing test results of a plasticizer mixed into a polyvinyl chloride resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0072] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. [Basic structure of light-reflecting film] As shown in FIG. 1, the light reflecting film M includes a light-transmitting resin material layer J and a light reflecting layer B located on the rear surface side of the resin material layer J. On the surface of the resin material layer J, in a cross-sectional view, protrusion portions U having short sides S and long sides T of different lengths that extend linearly from different positions in a cross direction perpendicular to the thickness direction of the resin material layer J to intersect with each other are formed so as to be aligned in the cross direction. In addition, in a cross-sectional view, for one of the protrusions U, the base end of the short side S and the base end of the long side T are at the same position in the thickness direction of the resin material layer J.

[0073] The protrusion U refers to a long and slender protrusion having a cross-sectional shape with a short side S and a long side T. The protrusion having a cross-sectional shape with a short side S and a long side T exists on the surface of the resin material layer J in a state of protruding outward. In the following description, the surface of the resin material layer J may be referred to as a reflective surface.

[0074] The resin material forming the resin material layer J is selected from resin materials having one or more of a carbon-fluorine bond, a siloxane bond, a carbon-chlorine bond, a carbon-oxygen bond, an ether bond, an ester bond, and a benzene ring. For example, vinyl chloride resin, fluororesin, siloxane, silicone rubber, etc. can be suitably used. The thickness of the resin material layer J is, for example, not less than 5 μm and not more than 200 μm.

[0075] The light reflecting layer B can be made of silver or a silver alloy, aluminum or an aluminum alloy, or indium, and further can have a laminated structure of silver or a silver alloy located on the side where the resin material layer J is present and aluminum or an aluminum alloy located on the side away from the resin material layer J. In other words, the light reflecting layer B is made of metal. The thickness of the light reflecting layer B is, for example, not less than 60 nm and not more than 500 nm.

[0076] As described below, the light reflecting film M has the function of reflecting sunlight. In addition, since the resin material layer J emits infrared light from its surface and the light reflecting layer B reflects the light that has passed through the resin material layer J, the light reflecting film M functions as a radiation cooling film that exhibits a radiation cooling function.

[0077] [Details of the protrusions] Regarding the protrusion portion U, as shown in Figures 1 and 2, the base end of the short side S of the protrusion portion U (the end of the short side S on the side where the light-reflecting layer B is present) and the base end of the long side T of the protrusion portion U adjacent to the protrusion portion U (the end of the long side T on the side where the light-reflecting layer B is present) are configured to be in the same position in the above-mentioned intersecting direction. Incidentally, although not shown in the illustration, the protrusion portion U may be formed in such a form that the base end of the short side S of the protrusion portion U and the base end of the long side T of the protrusion portion U adjacent to the protrusion portion U are positioned apart in the intersecting direction, and a flat plane exists between the base end of the short side S and the base end of the long side T.

[0078] In addition, in a cross-sectional view, a short side angle β (see FIG. 8), which is the angle of the short side S with respect to an imaginary plane Q that passes through the base end of the short side S along the intersecting direction, is in the range of 80 degrees to 100 degrees. Note that FIG. 8 illustrates an example in which the short side angle β is 90 degrees. In addition, in cross-sectional view, a long side angle δ (see FIG. 8) which is the angle of the long side T with respect to an imaginary plane Q passing through the base end of the long side T along the intersecting direction is greater than 0 degrees and less than 65 degrees. Preferably, it is greater than 0 degrees and less than 55 degrees, and more preferably, it is greater than 0 degrees and less than 45 degrees.

[0079] The protrusions U on the resin material layer J can be formed by a method such as transferring an embossing roll in a molding process such as roll-to-roll, but can also be formed in the following manner. That is, after the laminate of the resin material layer J and the light reflecting layer B is applied to the attachment target, a sawtooth mold in which mold portions for forming the protrusions U are arranged in crossing directions is pressed against the laminate to form it. Incidentally, as a form in which the laminate of the resin material layer J and the light reflecting layer B is applied to the attachment target, a form in which the laminate of the resin material layer J and the light reflecting layer B is prepared in advance and the prepared laminate is connected to the attachment target (a form in which the laminate is connected with an adhesive or a pressure sensitive adhesive) is conceivable, but there are also various other forms conceivable, such as a form in which a previously prepared light reflecting layer B is connected to the attachment target and a resin material that forms the resin material layer J is applied thereto.

[0080] After or before application of the laminate of the resin material layer J and the light reflecting layer B to the application target, the protrusions U are cut to have a sawtooth shape arranged in a cross direction. In the following description, the state in which the protrusions U are aligned in the intersecting direction in a cross-sectional view may be abbreviated as a sawtooth shape. Accordingly, the surface of the resin material layer J on which the protrusions U are aligned in the intersecting direction may be abbreviated as a sawtooth reflective surface.

[0081] 1 and 2, when forming the protrusion portion U on the surface of the resin material layer J, the base end of the short side S and the base end of the long side T may be configured to be located at a middle part of the resin material layer J in the thickness direction of the resin material layer J. For example, the base end of the short side S and the base end of the long side T may be located at a position on the surface side of the resin material layer J relative to the center point of the resin material layer J in the thickness direction, at a position equivalent to the center point of the resin material layer J in the thickness direction, or at a position on the side of the light reflecting layer B relative to the center point of the resin material layer J in the thickness direction. 4, the base end of the short side S and the base end of the long side T may be located at the end of the resin material layer J on the side where the light reflecting layer B is present in the thickness direction of the resin material layer J.

[0082] Incidentally, for example, when forming the protrusion portion U by transferring an embossing roll in a molding process such as roll-to-roll, if the base end of the short side S and the base end of the long side T are formed to be located at the end of the resin material layer J on the side where the light-reflecting layer B is present in the thickness direction of the resin material layer J, the height (thickness) of the protrusion portion U will be twice the height (thickness) of the resin material layer J having a flat surface before processing.

[0083] [How to use the light reflective film] A suitable method for using the light-reflecting film M is to install the light-reflecting film M on a wall surface in an upright position with the short side S positioned above the long side T of one of the protrusions U, as shown in Figure 2. In addition, examples of the wall surface in a standing position include the side walls of buildings such as houses and buildings, as well as various other surfaces such as the side walls of containers in container trucks.

[0084] Sunlight L irradiated toward a light-reflecting film M installed on a wall surface in a standing position passes through the resin material layer J and is reflected by the light-reflecting layer B, and then passes through the resin material layer J and is reflected by the light-reflecting film M in a form in which it is irradiated from the surface of the resin material layer J. As shown in Figure 2, since the refractive index of the resin material layer J is greater than the refractive index of air, much of the sunlight L is refracted in the direction from the long side T to the short side S of the protrusion portion U when it enters the resin material layer J, and is refracted in the direction from the long side T to the short side S of the protrusion portion U when it is irradiated from the surface of the resin material layer J.

[0085] In other words, when the light reflecting film M is installed in an upright position with the short side S positioned above the long side T of one of the protrusions U, as shown in Figure 2, most of the sunlight L coming from all directions (sunlight irradiated from above) can be refracted from the long side T of the sawtooth-shaped reflective surface in the direction of the short side S, and reflected (irradiated) upward (see dotted line in Figure 2). In other words, when sunlight L is incident on a light reflecting film M having a surface with ridges U having a sawtooth cross section, most of the reflection angle of the sunlight L shifts from the long side T in the direction of the short side S relative to the angle of incidence.

[0086] In this way, the light reflecting film M installed on the wall surface in a standing position can reflect (irradiate) most of the sunlight L coming from all directions upward, thereby helping to mitigate the heat island effect. In addition, the light reflective film M can reflect (irradiate) most of the sunlight L coming from all directions (sunlight irradiated from above) upwards, so it can reduce glare on the ground caused by the reflected (irradiated) light, especially when applied to the side walls of a building (parts above the lower end). Incidentally, although it can be dazzling if it is at the angle of the reflected (irradiated) sunlight L, outdoor work is usually performed at a lower position than the location where the light reflective film M is installed, so it is possible to reduce glare on the ground.

[0087] In addition, by mitigating the heat island effect, the temperature of the surrounding air and surrounding objects is reduced, which further reduces the temperature of the light-reflecting film M itself, thereby enabling the radiation cooling function to be effectively exerted.

[0088] As shown in Fig. 3, sunlight L incident on the protrusions U is reflected while being dispersed due to the dispersion of light. Note that Fig. 3 is a diagram showing a schematic diagram of the dispersion of light. In other words, the light reflecting film M can color an object without absorbing light. In other words, the refractive index of light varies depending on the wavelength. This wavelength dependency of the refractive index means that the color appears different depending on the observation angle, improving the design. And because the light reflecting film M does not absorb sunlight L, it can effectively exert a radiative cooling function.

[0089] 5, the surface (sawtooth-shaped reflective surface) of the light reflecting film M can reflect (irradiate) most of the sunlight L coming from all directions upward by reflection on the surface of the protrusions U. In other words, 10% to 15% of the sunlight L incident on the light reflecting film M is reflected by the surface of the light reflecting film M, but this reflected light can be reflected (irradiated) upward, which is also advantageous in terms of mitigating the heat island effect and reducing glare on the ground.

[0090] [Another configuration of the light reflecting film] As shown in FIG. 6, a light-transmitting covering layer R covering the surface of a resin material layer J is provided in a form that fills the spaces between adjacent protrusions U and makes the outer surface a flat surface. The refractive index N3 of the resin material forming the coating layer R is smaller than the refractive index N2 of the resin material forming the resin material layer J. The refractive index N3 of the resin material forming the coating layer R is larger than the refractive index N1 of air. With this configuration, it is possible to improve the function of refracting sunlight L in the direction from the long side T to the short side S of the sawtooth-shaped protrusions U and reflecting (irradiating) it upward.

[0091] As shown in FIG. 7, the surface B of the light reflecting layer B on the side where the resin material layer J is present Z In cross-sectional view, the protrusions U are formed symmetrically with respect to a reference plane that is located along the intersecting direction and between the surface of the resin material layer J and the light reflecting layer B. With this configuration, it is possible to improve the function of refracting sunlight L in the direction from the long side T to the short side S of the sawtooth-shaped protrusions U and irradiating (reflecting) it upward.

[0092] [Analysis of light reflection patterns] Making the surface of the resin material layer J into a sawtooth reflective surface with a row of protrusions U is, in terms of photonics, equivalent to making the cross-sectional shape of the light reflective film M into a right triangle as shown in Figure 8. To make the incident angle θ1 and the reflection angle θ3 different, it is necessary to have a structure including a prism and a light reflective layer B in the shape shown in Figure 8, but it is difficult to realize such a structure as a film. In Figure 8, θ2 is the refraction angle. Incidentally, the incident angle θ1, the refraction angle θ2, and the reflection angle θ3 are angles with respect to the normal line (the normal line of the long side T in Figure 8).

[0093] Incidentally, if one were to try to realize the above structure by thickening the resin material layer J of the light-reflecting film M, the amount of solar radiation absorbed would increase due to increased absorption of sunlight in the resin material layer J, which would reduce the radiative cooling function and make it impossible to cool under direct sunlight during the day. In the present invention, by forming the surface of the resin material layer J into a sawtooth reflective surface, much of the sunlight L is refracted in the direction from the long side T to the short side S of the sawtooth protrusion portion U, and reflected (irradiated) upward, while also suppressing an increase in the absorption of sunlight, thereby improving the radiative cooling function.

[0094] [Consideration of long side angle δ] FIG. 9 is a plot of the relationship between the incident side angle (θ1-δ) and the reflective side angle (θ3-δ) shown in FIG. 8 when the long side angle δ is changed in increments of 5 degrees. In other words, the horizontal axis (X) is the incident angle (θ1-δ) to the reflecting surface, and the vertical axis (Y) is the reflecting angle (θ3-δ) to the reflecting surface. The angle is defined as positive in the direction of the short side S (the side on which the short side S is located). Incidentally, the incident side angle (θ1-δ) is the angle obtained by subtracting the long side angle δ from the incident angle θ1, and the reflective side angle (θ3-δ) is the angle obtained by subtracting the long side angle δ from the reflective angle θ3. In addition, in FIG. 9, for example, 0 degrees is written as 0°, and "degrees" is written as "°", and the same is true in FIG. 10 and FIG.

[0095] Figure 9 shows the results of calculations where the refractive index N2 of the resin material layer J is set to 1.33, which is the refractive index of fluororesin, and the refractive index N1 of air is set to 1. Incidentally, fluororesin is used in the calculations here because it has a small refractive index among resin materials.

[0096] When δ = 0 degrees, the relationship is X = -Y, which is regular reflection. In contrast, when the long side angle δ is greater than 0, the plot of the reflection side angle (θ3-δ) is found to be above the line of regular reflection. This means that the reflection side angle (θ3-δ) is shifted toward the short side from the regular reflection angle. Angles where no lines are drawn are angles where the light that enters the resin material layer J is totally reflected inside the resin material layer J, and no reflected light is emitted. If the range of the long side angle δ is considered to be the condition where the angle at which the reflected light is emitted from the long side T exists even at a few degrees, then in the case of fluororesin, the range of the long side angle δ is greater than 0 degrees and less than 55 degrees. In addition, light with an incident angle (θ1-δ) that is totally reflected at the long side T is emitted from the short side S while being multiple-reflected inside the resin material layer J, or is absorbed by the light reflecting layer B or the resin material layer J.

[0097] Figure 10 plots the relationship between the incident side angle (θ1-δ) and the reflective side angle (θ3-δ) shown in Figure 8 when the refractive index N2 of the resin material layer J is 1.5, which is equivalent to the refractive index of polyvinyl chloride resin or acrylic resin, and the refractive index N1 of air is 1, as the long side angle δ is changed in increments of 5 degrees. That is, like Fig. 9, the horizontal axis (X) is the incident side angle (θ1-δ) to the reflecting surface, and the vertical axis (Y) is the reflecting side angle (θ3-δ) to the reflecting surface. The angle is defined as positive in the direction of the short side S (the side where the short side S is located). As described above, the calculation results are obtained by setting the refractive index N2 of the resin material layer J to 1.5, which is the refractive index corresponding to the refractive index of polyvinyl chloride resin or acrylic resin, and the refractive index N1 of air to 1. Incidentally, the refractive index of polyvinyl chloride resin or acrylic resin is larger than that of fluororesin, at about 1.5. As shown in FIG. 10, when the refractive index N2 of the resin material layer J is 1.5, the long side angle δ at which the reflected light is emitted from the long side T is greater than 0 degrees and less than 45 degrees.

[0098] Fig. 11 plots the relationship between the incident side angle (θ1-δ) and the reflective side angle (θ3-δ) when the long side angle δ is changed in increments of 5 degrees in a configuration including the coating layer R as shown in Fig. 6. In this case, the surface (reflective surface) of the light reflecting film M corresponds to the surface of the coating layer R, and the incident side angle (θ1-δ) and the reflective side angle (θ3-δ) are angles corresponding to the surface of the coating layer R.

[0099] That is, like Fig. 9, the horizontal axis (X) is the incident side angle (θ1-δ) to the reflecting surface, and the vertical axis (Y) is the reflecting side angle (θ3-δ) to the reflecting surface. The angle is defined as positive in the direction of the short side S (the side where the short side S is located).

[0100] The refractive index N3 of the cover layer R is 1.33, and the refractive index N2 of the resin material layer J is 1.5. In other words, the refractive index N3 of the coating layer R is greater than the refractive index N1 of air and is smaller than the refractive index N2 of the resin material layer J. As a result, as shown in FIG. 11, the long side angle δ at which the reflected light is emitted from the long side T is greater than 0 degrees and less than 65 degrees.

[0101] [Comparison between the present invention configuration and the comparative configuration] Conventionally, there are three types of comparative configurations for a configuration having a resin material layer J and a light-reflecting layer B: a structure in which the surface of the resin material layer J is a mirror surface, a structure in which the surface of the resin material layer J is embossed to scatter light, and a structure in which a filler such as titanium oxide is introduced into the resin material layer J to scatter light. When the surface of the resin material layer J has a mirror structure, the light is reflected at the same angle as the incident angle, as shown by the dashed line in FIG. 13, and therefore objects present on the ground side are heated.

[0102] In the case of a light scattering structure, although the glare at the reflection angle is somewhat reduced, the thinness of the material means that only light scattering can occur with a large amount of regular reflection remaining, and so objects on the ground will still be heated. Furthermore, in the case of a structure that scatters light, there is a problem that glare occurs even when not in the direction of regular reflection. The problem of glare occurs especially when the structure is applied to a wall surface in a standing position, and also occurs on objects below the wall surface in a standing position. The light reflecting film M of the present invention can reduce glare, especially when applied to a wall surface in a standing position.

[0103] 12 shows, as a comparative configuration, a configuration in which the surface of the resin material layer J is embossed, in other words, a configuration in which the light reflecting film M is provided with embossed protrusions Z having a pair of sides Y of the same length, in other words, a configuration in which the light reflecting film M is provided with embossed protrusions Z having an isosceles triangular cross section. In this comparative configuration, most of the incident sunlight L is reflected (irradiated) downward. Therefore, as shown in Figure 13, compared to the inventive configuration which improves the function of refracting most of the sunlight L irradiated from above in the direction from the long side T to the short side S of the sawtooth protrusion portion U, and irradiating (reflecting) it upward, in the comparative configuration, most of the irradiated sunlight L is reflected (irradiated) downward, making it impossible to reduce glare or mitigate the heat island effect.

[0104] [Specific configuration of light reflecting film M] Next, we will explain the specific configuration of the light reflecting film M. This specific configuration is a configuration that appropriately exhibits the radiative cooling function, and in the following, the light reflecting film M that appropriately exhibits the radiative cooling function will be described as a radiative cooling film CP. As shown in FIG. 14, the radiative cooling film CP includes a light-transmitting resin material layer J and a light reflecting layer B. That is, the resin material layer J functions as an infrared emitting layer A that radiates infrared light IR from an emitting surface H, and the light reflecting layer B is positioned on the opposite side of the infrared emitting layer A to the side where the emitting surface H exists. As is clear from the above description, the emitting surface H corresponds to the surface of the resin material layer J, that is, the sawtooth reflective surface.

[0105] As described above, the light-reflecting layer B can be constructed using silver or a silver alloy, aluminum or an aluminum alloy, or indium, and further, a laminated structure can be used in which silver or a silver alloy is positioned on the side where the resin material layer J is present and aluminum or an aluminum alloy is positioned on the side away from the resin material layer J. In the following description, it is assumed that the light reflecting layer B is made of silver or a silver alloy.

[0106] In addition, an adjacent-side protective layer Du is provided between the infrared radiation layer A and the light reflecting layer B, and is located on the side of the light reflecting layer B adjacent to the infrared radiation layer A, and a separating-side protective layer Ds is provided on the side of the light reflecting layer B away from the infrared radiation layer A. Therefore, the radiative cooling film CP is configured as a film body F including a resin material layer J (infrared radiative layer A), an adjacent-side protective layer Du, a light-reflecting layer B, and a distant-side protective layer Ds in a laminated state. A connecting resin material layer W is provided on the rear surface of the film body F to be connected to an attachment target (an object to be cooled E).

[0107] The light reflecting layer B reflects light such as sunlight L that has passed through the infrared emitting layer A and the adjacent-side protective layer Du. Its reflection characteristics are such that the reflectance at wavelengths of 0.4 μm to 0.5 μm is 90% or more, and the reflectance at wavelengths longer than 0.5 μm is 96% or more. The solar spectrum extends from wavelengths 0.295 μm (295 nm) to 4 μm (4000 nm), with the intensity increasing as the wavelength increases from 0.4 μm (400 nm), and the intensity is particularly high from wavelengths 0.5 μm (500 nm) to 1.8 μm (1800 nm).

[0108] In this embodiment, sunlight L includes ultraviolet light (ultraviolet light), visible light, and infrared light, and when described in terms of the wavelength of light as electromagnetic waves, includes electromagnetic waves with wavelengths of 10 nm to 20,000 nm (0.01 μm to 20 μm). In this specification, the wavelength range of ultraviolet light (ultraviolet light) is set to be 295 nm (0.295 μm) or more and 400 nm (0.4 μm) or less.

[0109] The light-reflecting layer B exhibits a reflectance of 90% or more from 0.4 μm to 0.5 μm wavelengths and a reflectance of 96% or more for wavelengths longer than 0.5 μm. This enables the solar energy absorbed by the light-reflecting layer B of the radiative cooling film CP to be reduced to 5% or less. In other words, the solar energy absorbed at noon in summer can be reduced to about 50 W.

[0110] The thickness of the infrared radiation layer A is adjusted so that it emits greater thermal radiation energy in the wavelength range from 8 μm to 14 μm than the absorbed solar energy. The resin material layer J constituting the infrared radiation layer A will be described in detail later, but in this embodiment, the resin material forming the resin material layer J is a vinyl chloride resin mixed with a plasticizer. That is, the resin material forming the resin material layer J is a vinyl chloride resin mixed with a plasticizer, or a vinylidene chloride resin mixed with a plasticizer. A vinyl chloride resin mixed with a plasticizer has excellent extensibility (ease of stretching).

[0111] The vinyl chloride resin used in the present invention is a homopolymer of vinyl chloride or vinylidene chloride or a copolymer of vinyl chloride or vinylidene chloride, and the production method thereof is carried out by a conventionally known polymerization method.

[0112] Therefore, the radiative cooling film CP is configured to reflect a part of the sunlight L incident on the radiative cooling film CP at the radiation surface H of the infrared radiation layer A, and to reflect the light (such as sunlight and light emitted by the infrared radiation layer A) that has passed through the resin material layer J and the adjacent-side protective layer Du out of the sunlight L incident on the radiative cooling film CP at the light reflecting layer B and to allow it to escape from the radiation surface H to the outside.

[0113] The heat input to the radiative cooling film CP from the object to be cooled E, which is located on the opposite side of the light reflecting layer B from the side where the resin material layer J is present (for example, heat input by thermal conduction from the object to be cooled E), is converted into infrared light IR by the resin material layer J (infrared radiation layer A) and radiated, thereby cooling the object to be cooled E.

[0114] In other words, the radiative cooling film CP is configured to reflect the sunlight L irradiated onto the radiative cooling film CP, and to radiate heat transferred to the radiative cooling film CP (e.g., heat transferred from the atmosphere or from the object to be cooled E) to the outside as infrared light IR. In addition, the resin material layer J, the adjacent-side protective layer Du, the light-reflecting layer B, the separating-side protective layer Ds and the connecting resin material layer W are flexible, so that the radiative cooling film CP is configured to be flexible.

[0115] In addition, the radiative cooling film CP is used to implement a radiative cooling method in which infrared light IR is radiated from a radiation surface H on the opposite side to the surface of the resin material layer J that is in contact with the light reflecting layer B. Specifically, the radiation surface H is directed toward the sky, and infrared light IR is radiated from the radiation surface H directed toward the sky.

[0116] [Outline of resin material layer] The light absorptivity and emissivity (light emissivity) of the resin material (vinyl chloride resin) forming the resin material layer (infrared radiation layer A) J change depending on the thickness. Therefore, it is necessary to adjust the thickness of the resin material layer J so that it absorbs as little sunlight as possible and emits large thermal radiation in the so-called atmospheric window wavelength band (wavelength band from 8 μm to 14 μm).

[0117] Specifically, in terms of the light absorptance of sunlight, the thickness of the resin material layer J needs to be adjusted to a thickness such that the wavelength average of the light absorptance from 0.4 μm to 0.5 μm is 13% or less, the wavelength average of the light absorptance from 0.5 μm to 0.8 μm is 4% or less, the wavelength average of the light absorptance from 0.8 μm to 1.5 μm is within 1%, the wavelength average of the light absorptance from 1.5 μm to 2.5 μm is 40% or less, and the wavelength average of the light absorptance from 2.5 μm to 4 μm is 100% or less. In the case of such an absorptance distribution, the light absorptance of sunlight is 10% or less, which corresponds to 100 W or less in terms of energy.

[0118] As described later, the light absorption rate of the resin material increases as the thickness of the resin material increases. When the resin material is made thick, the emissivity of the atmospheric window becomes almost 1, and the thermal radiation emitted into space is 125 W / m 2 from 160 W / m 2 The solar light absorption in the adjacent protective layer Du and the light reflecting layer B is 50 W / m 2 The sum of the solar light absorption in the resin material layer J, the adjacent side protective layer Du, and the light reflecting layer B is 150 W / m 2 The temperature is below 100° C., and cooling proceeds if the atmospheric conditions are good. As described above, it is preferable to use a resin material that has a small light absorptance near the peak value of the solar spectrum for the resin material layer J.

[0119] Moreover, from the viewpoint of infrared radiation (thermal radiation), the thickness of the resin material layer J needs to be adjusted to a thickness such that the wavelength average of the emissivity in the wavelength range from 8 μm to 14 μm is 40% or more. 50 W / m absorbed by the adjacent protective layer Du and light reflecting layer B 2 In order to release about that amount of thermal energy of sunlight from the resin material layer J into space through thermal radiation from the resin material layer J, the resin material layer J needs to emit more thermal radiation than that amount. For example, when the outside temperature is 30°C, the maximum thermal radiation of the 8μm to 14μm atmospheric window is 200W / m 2(Calculated with an emissivity of 1). This value can be obtained on a clear day in a dry environment with thin air, such as a high mountain. Since the atmosphere is thicker in lowlands than in high mountains, the wavelength band of the atmospheric window is narrower and the transmittance is lower. Incidentally, this is called the "atmospheric window becoming narrower."

[0120] In addition, the environment in which the radiative cooling film CP is actually used may be humid, and in that case the atmospheric window will be narrow. When used in low altitudes, the thermal radiation generated in the atmospheric window area is 160 W / m at 30°C under good conditions. 2 (calculated with emissivity of 1). When there is haze or smog in the sky, which is common in Japan, the atmospheric window becomes even narrower, and radiation into space is estimated at 125 W / m 2 It will be about that amount. In consideration of this situation, the wavelength average of the emissivity from 8 μm to 14 μm is set to 40% or more (thermal radiation intensity in the atmospheric window band is 50 W / m 2 ) it cannot be used in low altitude areas of the mid-latitudes.

[0121] Therefore, if the thickness of the resin material layer J is adjusted so as to fall within the optically specified range taking into consideration the above factors, the heat output at the atmospheric window will be greater than the heat input due to absorption of sunlight, and it will be possible to cool the temperature below the outside air temperature by radiative cooling even outdoors in a solar radiation environment. In this embodiment, the thickness of the resin material layer J made of vinyl chloride resin is 100 μm or less and 10 μm or more, preferably 100 μm or less and 50 μm or more.

[0122] [Details of resin material] According to Kirchhoff's law, emissivity (ε) and light absorptance (A) are equal. Light absorptance can be calculated from the absorption coefficient (α) using the following formula (1) (hereinafter sometimes referred to as the light absorptance relationship formula). A=1-exp(-αt) ---(1) where t is the film thickness. In other words, by adjusting the film thickness of the resin material layer J, a large thermal radiation can be obtained in a wavelength band with a large absorption coefficient. When performing radiative cooling outdoors, it is recommended to use a material with a large absorption coefficient in the wavelength band of the atmospheric window, that is, from 8 μm to 14 μm. In addition, to suppress the absorption of sunlight, it is advisable to use a material that has no or has a small absorption coefficient in the wavelength range of 0.3 μm to 4 μm, especially in the range of 0.4 μm to 2.5 μm. As can be seen from the relational equation between the absorption coefficient and the absorptance, the light absorptance (emissivity) changes depending on the film thickness of the resin material.

[0123] In order to lower the temperature below the surrounding atmosphere by radiative cooling in a solar radiation environment, if a material is selected that has a large absorption coefficient in the wavelength band of the atmospheric window and almost no absorption coefficient in the wavelength band of sunlight, then by adjusting the film thickness, it is possible to create a state in which almost no sunlight is absorbed but a lot of thermal radiation is emitted by the atmospheric window, in other words, a state in which the output by radiative cooling is greater than the input of sunlight.

[0124] The solar spectrum only contains wavelengths longer than 0.295 μm. Note that ultraviolet rays are defined as the range of wavelengths shorter than 0.4 μm, visible light is defined as the range of wavelengths from 0.4 μm to 0.8 μm, near infrared rays are defined as the range of wavelengths from 0.8 μm to 3 μm, mid infrared rays are defined as the range of wavelengths from 3 μm to 8 μm, and far infrared rays are defined as the range of wavelengths longer than 8 μm.

[0125] Regarding the carbon-chlorine bond (C-Cl), the bond energy between the carbon and chlorine in alkenes is 3.28 eV, and the wavelength is 0.378 μm, so it absorbs a lot of ultraviolet light in sunlight, but has almost no absorption in the visible range. FIG. 15 shows the absorption spectrum of a 100 μm thick polyvinyl chloride resin in the ultraviolet to visible range, and light absorption is large on the shorter wavelength side than 0.38 μm. FIG. 15 shows the absorptance spectrum of a 100 μm thick vinylidene chloride resin in the ultraviolet to visible region, and shows a slight increase in the absorptance spectrum on the shorter wavelength side than 0.4 μm.

[0126] Figure 16 shows the emissivity of polyvinyl chloride resin (PVC) with carbon-chlorine bonds at the atmospheric window, and Figure 17 shows the emissivity of polyvinylidene chloride resin (PVDC) with carbon-chlorine bonds at the atmospheric window. For carbon-chlorine bonds, the absorption coefficient due to the C-Cl stretching vibration appears in a broad band with a half-width of 1 μm or more centered at a wavelength of 12 μm. In the case of polyvinyl chloride resin, the absorption coefficient due to the bending vibration of CH of the alkene contained in the main chain appears at a wavelength of around 10 μm due to the electron-withdrawing effect of chlorine. The same is true for vinylidene chloride resin. Due to these effects, the wavelength average of the emissivity of a 10 μm thick film is 43% in the wavelength range from 8 μm to 14 μm, which falls within the regulation of a wavelength average of 40% or more. As shown in the figure, the emissivity in the atmospheric window region increases as the film thickness increases.

[0127] Thermal radiation from the atmospheric window of the resin material layer J occurs near the surface of the resin material. As shown in Figure 16, in the case of polyvinyl chloride resin, even if the thickness exceeds 100 μm, there is almost no increase in thermal radiation in the atmospheric window region. In other words, in the case of polyvinyl chloride resin, thermal radiation in the atmospheric window occurs within a depth of about 100 μm from the surface, and radiation from deeper parts does not escape to the outside. As shown in FIG. 17, vinylidene chloride resin is similar to polyvinyl chloride resin.

[0128] As described above, the thermal radiation from the atmospheric window region generated from the resin material surface occurs within a depth of approximately 100 μm from the surface. If the resin thickness increases beyond this, the cold generated by the radiative cooling film CP is insulated by the resin material that does not contribute to thermal radiation. Consider fabricating a resin material layer J that ideally does not absorb any sunlight on top of the light reflecting layer B. In this case, sunlight L is absorbed only by the light reflecting layer B of the radiative cooling film CP. The thermal conductivity of resin materials is generally about 0.2 W / m / K. When calculations are made taking this thermal conductivity into account, if the thickness of the resin material layer J exceeds 20 mm, the temperature of the cooling surface (the surface of the light-reflecting layer B opposite the side where the resin material layer J is present) will rise.

[0129] Even if an ideal resin material that does not absorb any sunlight exists, the thermal conductivity of the resin material is generally about 0.2 W / m / K, so if the thickness exceeds 20 mm, the light reflecting layer B will be heated by the sunlight, and the object to be cooled E placed on the light reflecting layer side will be heated. In other words, the thickness of the resin material of the radiative cooling film CP needs to be 20 mm or less.

[0130] [Thickness of resin material layer] From the viewpoint of practical use of the radiative cooling film CP, it is preferable that the thickness of the resin material layer (infrared resin material layer) J is thin. The thermal conductivity of resin materials is generally lower than that of metals and glass. To effectively cool the object to be cooled E, it is preferable that the thickness of the resin material layer J is the minimum necessary. The thicker the resin material layer J is, the greater the thermal radiation of the atmospheric window becomes, and above a certain thickness, the thermal radiation energy at the atmospheric window becomes saturated.

[0131] The film thickness at which the film saturates depends on the resin material, but in the case of resins containing carbon-chlorine bonds, the film is saturated even at a thickness of 100 μm, and sufficient heat radiation can be obtained in the atmospheric window region even at a thickness of 50 μm. The thinner the resin material, the higher the thermal conductivity and the more effectively the temperature of the object to be cooled can be lowered, so in the case of resins containing carbon-chlorine bonds, a thickness of 50 μm or less reduces the insulation and allows the object to be cooled E to be cooled effectively. In the case of carbon-chlorine bonds, a thickness of 100 μm or less allows the object to be cooled E to be cooled effectively.

[0132] The benefit of making the film thinner is not only that it reduces heat insulation and makes it easier to transfer cold. It also reduces the absorption of near-infrared light from CH, CH2, and CH3, which are caused by resins containing carbon-chlorine bonds. By making the film thinner, the amount of sunlight absorbed by these compounds can be reduced, which increases the cooling capacity of the radiative cooling film CP. From the above perspective, in the case of polyvinyl chloride resin, which is a resin containing carbon-chlorine bonds, a thickness of 50 μm or less can more effectively produce a radiative cooling effect under sunlight.

[0133] [Details of the light reflecting layer] In order to provide the light reflecting layer B with the above-mentioned reflectance characteristics, the reflective material on the side where the emitting surface H exists (the side where the resin material layer J exists) is preferably silver or a silver alloy. 18, if the light-reflecting layer B is formed based on silver, it is possible to obtain the desired reflectance of the light-reflecting layer B. Incidentally, since indium also exhibits the same reflective properties as silver or a silver alloy, indium may be used instead of silver or a silver alloy.

[0134] When reflecting sunlight using only silver or a silver alloy while maintaining the above-mentioned reflectance characteristics, a thickness of 50 nm or more is required. However, in order to provide flexibility to the light reflecting layer B, the thickness must be 100 μm or less. If it is thicker than this, it becomes difficult to bend. Incidentally, the "silver alloy" may be an alloy in which, for example, 0.4% to 4.5% by mass of any of copper, palladium, gold, zinc, tin, magnesium, nickel, and titanium is added to silver. A specific example is "APC-TR (made by Furuya Metal)," a silver alloy made by adding copper and palladium to silver.

[0135] Silver and silver alloys are vulnerable to rain and humidity and need to be protected from them and to prevent discoloration. For this reason, adjacent-side protective layer Du and distant-side protective layer Ds are required to protect the silver and silver alloy. The adjacent-side protective layer Du and the distant-side protective layer Ds will be described in detail later.

[0136] [Details of plasticizer] The plasticizer mixed into the vinyl chloride resin forming the resin material layer J is made of one or more compounds selected from the group consisting of phthalates, aliphatic dibasic acid esters, and phosphates. The plasticizer is mixed in an amount of 1 part by weight or more and 100 parts by weight or less per 100 parts by weight of the vinyl chloride resin.

[0137] The aliphatic dibasic acid ester of the plasticizer may be composed of adipic acid esters, adipic acid ester copolymers, azelaic acid esters, azelaic acid ester copolymers, sebacic acid esters, sebacic acid ester copolymers, succinic acid esters, and succinic acid ester copolymers, either alone or in combination.

[0138] The aliphatic dibasic acid ester of the plasticizer is preferably an aliphatic dibasic acid and two molecules of a saturated aliphatic alcohol bonded together via an ester bond. The phthalate ester of the plasticizer is preferably an ester bond between phthalic acid and two molecules of a saturated aliphatic alcohol. The phosphate ester of the plasticizer may be a phosphate triester or an aromatic phosphate ester.

[0139] <Details on phthalate esters> The list of phthalate esters is as follows: Dimethyl phthalate (DMP), diethyl phthalate (DEP), dibutyl phthalate (DBP), di-2-ethylhexyl phthalate (DOP), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), diundecyl phthalate (DUP), ditridecyl phthalate (DTDP), bis(2-ethylhexyl) terephthalate (DOTP), bis(2-ethylhexyl) isophthalate (DOIP), etc.

[0140] <Details of Aliphatic Dibasic Acid Esters> The aliphatic dibasic acid esters are listed below. Dibutyl adipate (DBA), diisobutyl adipate (DIBA), di-2-ethylhexyl adipate (DOA), diisononyl adipate (DINA), diisodecyl adipate (DIDA), bis-2-ethylhexyl azelaate (DOZ), dibutyl sebacate (DBS), di-2-ethylhexyl sebacate (DOS), diisononyl sebacate (DINS), diethyl succinate (DESU), and the like. Also, an aliphatic polyester having a molecular weight of 400 to 4000 synthesized by copolymerization (polyesterification) of a dibasic acid such as adipic acid with a diol (difunctional alcohol or glycol).

[0141] <Phosphate triester> The phosphoric acid triesters are listed as follows: Trimethyl phosphate (TMP), triethyl phosphate (TEP), tributyl phosphate (TBP), tris(2-ethylhexyl) phosphate (TOP).

[0142] <Aromatic phosphate ester> The aromatic phosphate esters are listed as follows: Triphenyl phosphate (TPP), tricresyl phosphate (TCP), trixylenyl phosphate (TXP), tresyl diphenyl phosphate (CDP), 2-ethylhexyl diphenyl phosphate.

[0143] <Appropriate evaluation of plasticizers> Plasticizers for vinyl chloride resins include phthalates, aliphatic dibasic acid esters, phosphate triesters, aromatic phosphate esters, trimellitic acid esters, and epoxidized fatty acid esters. The following compounds were selected from these plasticizers, and 43 parts by weight of each plasticizer was mixed with 100 parts by weight of vinyl chloride and evaluated using a xenon weather test. The vinyl chloride resin was mixed with 0.5 parts by weight of each of a triazine-based ultraviolet absorber and a hindered amine-based light stabilizer per 100 parts by weight of vinyl chloride.

[0144] Representative phthalate esters include di-2-ethylhexyl phthalate (DOP) and diisodecyl phthalate (DIDP). Representative aliphatic dibasic acid esters include di-2-ethylhexyl adipate (DOA), butanediol adipate copolymer (average molecular weight about 1000), and diisononyl adipate (DINA). A representative phosphate triester is tributyl phosphate (TBP). Tricresyl phosphate (TCP) is a representative aromatic phosphate ester. A representative trimellitic acid ester is tri-2-ethylhexyl trimellitate (TOTM). Epoxidized soybean oil is a representative example of an epoxidized fatty acid ester.

[0145] The durability test was conducted using a xenon weather test for 1920 hours (equivalent to 4 years of actual exposure), and the durability was judged based on the results. Note that 487 hours is equivalent to 1 year of UV exposure. The conditions for the xenon weather test are as follows: UV intensity 180W / m 2 (wavelength 295-400nm). <Conditions without watering> BPT89℃, humidity 50%, 1 hour 42 minutes. <Conditions with watering> Temperature inside the tank: 38°C, humidity: 90%, 18 minutes.

[0146] The test results for 1920 hours are shown in Figure 23. As a result of the above experiment, it became clear that durability was significantly reduced when trimellitic acid ester (TOTM) and epoxidized fatty acid ester (epoxidized soybean oil) were used as plasticizers. Note that epoxidized fatty acid turned brown after 1120 hours and the test could not be continued, so it is not shown in the figure.

[0147] In contrast, it was found that when phthalate esters, aliphatic dibasic acid esters, phosphate triesters, and aromatic phosphate esters were used as plasticizers to be mixed into polyvinyl chloride resin, the reflectance of the radiative cooling film CP did not decrease even after about four years, but when trimellitate esters and epoxidized fatty acid esters were used as plasticizers to be mixed into polyvinyl chloride resin, the reflectance of the radiative cooling film CP decreased significantly after about four years.

[0148] From the above test results, it is clear that, as plasticizers for polyvinyl chloride resin, phthalate esters, aliphatic dibasic acid esters, phosphate triesters, and aromatic phosphate esters have excellent durability, while trimellitate esters and epoxidized fatty acid esters have no durability. The same is true for vinylidene chloride resins, which have carbon-chlorine bonds.

[0149] [Consideration of plasticizers mixed into infrared radiation resin material layers] The plasticizer mixed into the vinyl chloride resin forming the resin material layer (infrared radiation resin material layer) J will be considered below. The deterioration of polyvinyl chloride resins due to sunlight is largely due to the deterioration of plasticizers caused by ultraviolet rays. PVC resins (mixed with plasticizers) that are normally used outdoors for long periods of time are protected from the ultraviolet rays contained in sunlight by coloring and additives. For example, they are often colored black or other colors to make them less susceptible to the effects of ultraviolet rays. On the other hand, in the case of radiative cooling films (CPs), it is necessary to minimize the absorption of sunlight in order to achieve radiative cooling performance. For this reason, it is not possible to add enough additives, dyes, or pigments to protect the plasticizers.

[0150] As shown in Fig. 19, the radiative cooling film CP has an adhesive layer N for the light reflecting layer, an adjacent-side protective layer Du under a resin material layer J made of a vinyl chloride resin, and a light reflecting layer B containing silver under the adhesive layer N. The resin material layer J is more susceptible to the influence of sunlight due to the influence of the light reflecting layer B. In other words, sunlight that has once entered the radiative cooling film CP is reflected by the light reflecting layer B and passes through the resin material layer J twice. In other words, the influence of sunlight on degradation is about twice as much as usual.

[0151] In addition, when comparing the resin material layer J formed on the light-reflecting layer B containing silver with the resin material layer J formed on aluminum, iron, or ceramics, which have low reflectivity, the radiative cooling film CP having the resin material layer J formed on the light-reflecting layer B containing silver is more affected by sunlight. These facts suggest that the polyvinyl chloride resin of the radiative cooling film CP, which has the resin material layer J on the light-reflecting layer B with silver, is more sensitive to ultraviolet light contained in sunlight than polyvinyl chloride resins for general use.

[0152] Deterioration of ester-based plasticizers due to ultraviolet light occurs mainly due to the plasticizer absorbing ultraviolet light energy. Ultraviolet light absorption occurs mainly due to the occurrence of electronic transitions that exceed the bond energy of the ester bonds in the plasticizer. The activation energy provided by ultraviolet light and water molecules promotes hydrolysis of the plasticizer mixed into the polyvinyl chloride resin. When the plasticizer bonds break, the broken bonds attack the surrounding vinyl chloride resin, causing dehydrochlorination, etc., resulting in coloration. This also reduces the mechanical strength. When the polyvinyl chloride resin becomes discolored, the radiative cooling film CP absorbs sunlight and is no longer able to cool during the day.

[0153] Therefore, as shown in the experimental results in Fig. 23, plasticizers (trimellitic acid esters, epoxidized fatty acid esters) used for outdoor applications exposed to direct sunlight cannot be used in the radiative cooling film CP, and phthalic acid esters, aliphatic dibasic acid esters, phosphate triesters, and aromatic phosphate esters can be used as plasticizers for the radiative cooling film CP.

[0154] [Other additives] The vinyl chloride resin forming the resin material layer J may contain flame retardants, stabilizers, stabilization aids, fillers, antioxidants, UV absorbers, and light stabilizers, the details of which are well known and therefore will not be described in detail in this document.

[0155] [Specific configuration of radiative cooling film] As shown in Fig. 19, the specific configuration of the radiative cooling film CP (film body F) is such that the adjacent-side protective layer Du in the laminated portion consisting of the adjacent-side protective layer Du, the light reflecting layer B, and the separating-side protective layer Ds is bonded to the resin material layer J with a light reflecting layer adhesive layer N, and the connecting resin material layer W and the separating-side protective layer Ds in the laminated portion consisting of the adjacent-side protective layer Du, the light reflecting layer B, and the separating-side protective layer Ds are bonded to each other with a connecting adhesive layer V.

[0156] The adhesive layer N for the light reflecting layer is, for example, a urethane resin adhesive (adhesive) or an acrylic resin adhesive (adhesive), and it is desirable for it to have high transparency to sunlight. The thickness of the adhesive layer N for the light reflecting layer is 5 μm or more and 30 μm or less. The connecting adhesive layer V is, for example, a urethane resin adhesive (adhesive) or an acrylic resin adhesive (adhesive).

[0157] The radiative cooling film CP can be installed on a wall in an upright position with the short side S of the protrusion U positioned above the long side T. As mentioned above, examples of the wall surface in the standing position include the wall surface of a building such as a house or a building, as well as various other surfaces such as the side wall of a container of a container truck.

[0158] In addition, the radiative cooling film CP can be easily attached to existing objects to provide radiative cooling, such as wrapping the exterior of a car, the exterior wall of a warehouse or building, or the exterior of a helmet. Other examples of objects to which the film-shaped radiative cooling film CP can be attached include the outer surfaces of various tents, the outer surfaces of boxes for storing electrical equipment, the outer surfaces of containers for transporting goods, the outer surfaces of milk tanks for storing milk, the outer surfaces of the milk storage parts of milk tanker trucks, and various other objects that require cooling.

[0159] [Procedure for creating a radiative cooling film with specific configuration] An example of the procedure for fabricating the radiative cooling film CP (film body F) is shown in Figure 20. First, a release layer G is formed on top of a film-like substrate K such as PET, then a separating-side protective layer Ds is applied or pasted on the release layer G, a light-reflecting layer B is formed on the separating-side protective layer Ds by deposition, sputtering, ion plating, silver mirror reaction, or the like, and an adjacent-side protective layer Du is applied or pasted on the light-reflecting layer B. Incidentally, the release layer G is formed from either silicone resin or fluororesin. That is, on the upper part of the base material K, a release layer G, a separating-side protective layer Ds, a light-reflecting layer B, and an adjacent-side protective layer Du are laminated in this order to form a light-reflecting layer-side laminate P. In addition, a resin material layer J and a connecting resin material layer W are separately formed in the form of a film.

[0160] Then, the resin material layer J fabricated in a film form and the adjacent protective layer Du in the light reflecting layer side laminate P are bonded with an adhesive layer N for the light reflecting layer. Thereafter, the release layer G is separated from the separating-side protective layer Ds, and then the separating-side protective layer Ds and the connecting resin material layer W are bonded together by the connecting adhesive layer V. When the release layer G is separated from the separating-side protective layer Ds, basically, the release layer G having the base material K is separated from the separating-side protective layer Ds.

[0161] Incidentally, when the adjacent-side protective layer Du is formed from ethylene terephthalate resin as described below, the adjacent-side protective layer Du may be used as a substrate, and a light-reflecting layer B may be formed on the adjacent-side protective layer Du by vapor deposition, sputtering, ion plating, silver mirror reaction, or the like, and a separating-side protective layer Ds may be applied or attached to the light-reflecting layer B to form the light-reflecting layer side laminate P. The resin material layer J fabricated in a film form and the adjacent side protective layer Du in the light-reflecting layer side laminate P may be bonded with a light-reflecting layer adhesive layer N, and the separating side protective layer Ds of the light-reflecting layer side laminate P and the connecting resin material layer W fabricated in a film form may be bonded with a connecting adhesive layer V.

[0162] [Details of adjacent protective layer] The adjacent-side protective layer Du is made of a polyolefin resin having a thickness of 300 nm or more and 40 μm or less, or an ethylene terephthalate resin having a thickness of 17 μm or more and 40 μm or less. Polyolefin resins include polyethylene and polypropylene.

[0163] FIG. 15 shows the ultraviolet light absorptance of polyethylene, vinylidene chloride resin, ethylene terephthalate resin, and vinyl chloride resin. FIG. 21 shows the light transmittance of polyethylene, which is suitable as the synthetic resin for forming the adjacent-side protective layer Du.

[0164] Since the radiative cooling film CP exerts a radiative cooling effect not only at night but also under a solar radiation environment, in order for the light reflecting layer B to maintain its light reflecting function, it is necessary to protect the light reflecting layer B with the adjacent protective layer Du so that the silver of the light reflecting layer B does not discolor under a solar radiation environment.

[0165] When the adjacent side protective layer Du is formed from a polyolefin-based resin with a thickness of 300 nm or more and 40 μm or less, the polyolefin-based resin is a synthetic resin with an ultraviolet light absorptance of 10% or less over the entire ultraviolet wavelength range of 0.3 μm to 0.4 μm, so that the adjacent side protective layer Du is less likely to deteriorate due to absorption of ultraviolet rays.

[0166] Furthermore, since the thickness of the polyolefin resin forming the adjacent side protective layer Du is 300 nm or more, it effectively performs the blocking function of blocking radicals generated in the resin material layer J from reaching the silver or silver alloy forming the light reflecting layer, and also blocks moisture penetrating the resin material layer J from reaching the silver or silver alloy forming the light reflecting layer B, thereby suppressing discoloration of the silver or silver alloy forming the light reflecting layer B.

[0167] Incidentally, the adjacent side protective layer Du made of a polyolefin resin will deteriorate as it absorbs ultraviolet rays, forming radicals on the surface side away from the light-reflecting layer B. However, since the thickness is 300 nm or more, the formed radicals will not reach the light-reflecting layer. Furthermore, even if the adjacent side protective layer Du deteriorates as radicals are formed, the rate of deterioration is slow due to the low absorption of ultraviolet rays, so the above-mentioned blocking function will be exerted for a long period of time.

[0168] When the adjacent side protective layer Du is formed from ethylene terephthalate resin to a thickness of 17 μm or more and 40 μm or less, ethylene terephthalate resin is a synthetic resin that has a higher ultraviolet light absorption rate in the ultraviolet wavelength range of 0.3 μm to 0.4 μm than polyolefin resins. However, since the thickness is 17 μm or more, it can effectively perform blocking functions for a long period of time, such as blocking radicals generated in the resin material layer J from reaching the silver or silver alloy that forms the light reflecting layer B, and blocking moisture that penetrates the resin material layer J from reaching the silver or silver alloy that forms the light reflecting layer B, thereby suppressing discoloration of the silver or silver alloy that forms the light reflecting layer B.

[0169] In other words, the adjacent-side protective layer Du made of ethylene terephthalate resin will deteriorate as it absorbs ultraviolet rays, forming radicals on the surface side away from the light-reflecting layer B. However, since the thickness is 17 μm or more, the formed radicals will not reach the reflective layer. Furthermore, even if the adjacent-side protective layer Du deteriorates while forming radicals, the thickness is 17 μm or more, so the above-mentioned blocking function will be maintained for a long period of time.

[0170] To explain further, the deterioration of ethylene terephthalate resin (PET) is caused by ultraviolet light cleaving the ester bonds between ethylene glycol and terephthalic acid to form radicals. This deterioration progresses from the surface of the ethylene terephthalate resin (PET) that is irradiated with ultraviolet light.

[0171] For example, when ethylene terephthalate resin (PET) is irradiated with ultraviolet rays with the strength in Osaka, the ester bonds of the ethylene terephthalate resin (PET) are cleaved by about 9 nm per day, starting from the irradiated surface. Because the ethylene terephthalate resin (PET) is sufficiently polymerized, the cleaved ethylene terephthalate resin (PET) on the surface does not attack the silver (silver alloy) of the light-reflecting layer B. However, when the cleaved end of the ethylene terephthalate resin (PET) reaches the silver (silver alloy) of the light-reflecting layer B, the silver (silver alloy) will discolor.

[0172] Therefore, in order for the adjacent-side protective layer Du to last for one year or more when used outdoors, a thickness of about 3 μm is required, calculated by multiplying 9 nm / day by 365 days. In order for the ethylene terephthalate resin (PET) of the adjacent-side protective layer Du to last for three years or more, a thickness of 10 μm or more is required. In order for it to last for five years or more, a thickness of 17 μm or more is required.

[0173] In addition, when the adjacent-side protective layer Du is formed of a polyolefin resin and an ethylene terephthalate resin, the reason for determining the upper limit of the thickness is to prevent the adjacent-side protective layer Du from exhibiting heat insulating properties that do not contribute to radiation cooling. In other words, the thicker the adjacent-side protective layer Du is, the more heat insulating properties it exhibits that do not contribute to radiation cooling. Therefore, the upper limit of the thickness is determined to prevent heat insulating properties that do not contribute to radiation cooling while still exerting the function of protecting the light reflecting layer B.

[0174] Incidentally, as shown in Figure 19, when an adhesive layer N for a light reflecting layer that bonds the resin material layer J and the adjacent side protective layer Du is located between them, radicals will also be generated from the adhesive layer N for a light reflecting layer. However, if the thickness of the polyolefin resin that forms the adjacent side protective layer Du is 300 nm or more and the thickness of the ethylene terephthalate resin that forms the adjacent side protective layer Du is 17 μm or more, the radicals generated in the adhesive layer N for a light reflecting layer can be prevented from reaching the light reflecting layer B for a long period of time.

[0175] As described above, if the adjacent-side protective layer Du becomes thick, there is no disadvantage in terms of preventing coloring of the silver (silver alloy) of the light-reflecting layer B, but a problem occurs in terms of radiative cooling. In other words, if the thickness is increased, the heat insulating property of the radiative cooling material increases. For example, a resin whose main component is polyethylene, which is an excellent synthetic resin for forming the adjacent side protective layer Du, has a low emissivity at the atmospheric window as shown in Figure 22, so even if it is formed thickly, it does not contribute to radiative cooling. On the contrary, making it thicker increases the thermal insulation of the radiative cooling material. Next, as the thickness increases, absorption of near-infrared light originating from the vibration of the main chain increases, increasing the effect of increasing solar light absorption. Due to these factors, a thick adjacent-side protective layer Du is disadvantageous for radiation cooling. From this viewpoint, the thickness of the adjacent-side protective layer Du made of a polyolefin resin is preferably 5 μm or less, and more preferably 1 μm or less.

[0176] [Details of the separation side protective layer] The separating-side protective layer Ds is made of an acrylic resin. More specifically, the resin material forming the separating-side protective layer Ds is an acrylic resin having a thickness of 100 nm or more and 2 μm or less.

[0177] [Details of the connecting resin material layer] The resin material forming the connecting resin material layer W is any one of ethylene terephthalate resin, polypropylene, polyethylene, and acrylic resin. The connecting resin material layer W has a thickness of 10 μm or more and 500 μm or less. In other words, since the resin material forming the connecting resin material layer W is ethylene terephthalate resin, polypropylene, polyethylene, or acrylic resin, the film body F can be properly attached to the installation object using an adhesive or pressure-sensitive adhesive, and the film body F can be properly thermally laminated to the installation object.

[0178] The resin material forming the connecting resin material layer W may be a vinyl chloride resin mixed with a plasticizer. That is, 5 parts by weight or more and 100 parts by weight or less of a plasticizer is mixed into 100 parts by weight of the vinyl chloride resin. The polyvinyl chloride resin mixed with a plasticizer has excellent ductility, and improves the ease of attachment (workability) to the attachment object (object E to be cooled).

[0179] Incidentally, since the connecting resin material layer W is not irradiated with a large amount of ultraviolet light, the plasticizers to be mixed into the resin material forming the connecting resin material layer W can be phthalate esters, aliphatic dibasic acid esters, phosphate triesters, aromatic phosphate esters, trimellitate esters, epoxidized fatty acid esters, as well as trimellitate esters and epoxidized fatty acid esters.

[0180] Furthermore, the resin material forming the connecting resin material layer W may contain a light-reflecting filler. Examples of fillers that can be used include silicon dioxide (SiO2), titanium oxide (TiO2), aluminum oxide (Al2O3), and magnesium oxide (MgO).

[0181] If a light-reflecting filler (not shown) is mixed into the resin material that forms the connecting resin material layer W, when the silver or silver alloy that constitutes the light-reflecting layer B breaks and cracks, causing the light-reflecting layer B to become unable to reflect light properly, the connecting resin material layer W will reflect the light that has passed through the light-reflecting layer B, thereby preventing a decrease in design and radiative cooling performance even when the silver or silver alloy that constitutes the light-reflecting layer B breaks.

[0182] In other words, even if the silver or silver alloy of the light reflecting layer B breaks and cracks when attaching the film body F, the light that passes through the cracked part of the light reflecting layer B is reflected by the connecting resin material layer W, and the entire film body F can be made to have a uniform state when viewed from the radiation surface side. Therefore, even if the silver or silver alloy of the light reflecting layer B breaks and cracks, deterioration of the design can be suppressed. Furthermore, since light that passes through the cracked parts of the light reflecting layer B can be reflected by the connecting resin material layer W, even if the silver or silver alloy of the light reflecting layer B breaks and cracks, the deterioration of the radiative cooling performance of the film body F can be suppressed.

[0183] [Another embodiment] Other embodiments are listed below. (1) In the above embodiment, an object that is in close contact with the back surface of the radiative cooling film CP is exemplified as the cooling target E, but various cooling targets such as a space to be cooled can be applied as the cooling target E. That is, the light reflecting film M of the present invention is installed on a wall surface in a standing position, but when the light reflecting film M is configured as a radiative cooling film CP, it can be installed and used in other places such as the roof of a house and the ceiling wall of a container car in addition to the wall surface in a standing position.

[0184] (2) In the above embodiment, the radiative cooling film CP has an exposed radiative surface H of the resin material layer J, but it may be provided with a hard coat to cover the radiative surface H. In other words, when the resin material layer J does not have a coating layer R on its surface, a thin-film hard coat may be provided to cover the surface of the resin material layer J, i.e., the sawtooth reflective surface. The hard coat may be any of the following: UV-curable acrylic, heat-curable acrylic, UV-curable silicone, heat-curable silicone, organic-inorganic hybrid, and vinyl chloride. An organic antistatic agent may be used as an additive. Among the UV-curable acrylics, urethane acrylates are particularly good.

[0185] The hard coat can be formed by a method such as gravure coating, bar coating, knife coating, roll coating, blade coating, or die coating. The thickness of the hard coat (coating film) is 1 to 50 μm, and preferably 2 to 20 μm.

[0186] (3) In the above embodiment, vinyl chloride resin is exemplified as the resin material of the resin material layer J. However, other resin materials, such as a resin material having one or more of a carbon-fluorine bond, a siloxane bond, a carbon-chlorine bond, a carbon-oxygen bond, an ether bond, an ester bond, and a benzene ring, may also be used.

[0187] (4) In the above embodiment of the radiative cooling film CP, the light reflecting layer B is formed using silver or a silver alloy. However, the light reflecting layer B can be formed using aluminum or an aluminum alloy, or indium, which has reflective properties equivalent to those of silver. Furthermore, a laminated structure of silver or a silver alloy located on the side where the resin material layer J is present and aluminum or an aluminum alloy located on the side away from the resin material layer J can be used.

[0188] (5) As a method for producing the film body F of the specific configuration of the radiative cooling film CP, instead of the method described in the above embodiment, other formation methods may be used, such as forming an adhesive layer N for a light reflecting layer on a resin material layer (a resin material layer for infrared radiation) J, forming an adjacent-side protective layer Du on the adhesive layer N for a light reflecting layer, directly depositing a light reflecting layer B on the adjacent-side protective layer Du, forming a separating-side protective layer Ds on the light reflecting layer B, and adhering the connecting resin material layer W to the separating-side protective layer Ds with a connecting adhesive layer V.

[0189] (6) The protrusion portion U means a long and slender protrusion having a cross-sectional shape with a short side S and a long side T. The long and slender protrusion shape includes a shape in which the divided parts, which are divided into appropriate lengths in the extension direction, are arranged at slightly different positions in the intersecting direction, and a shape in which the divided parts are arranged at intervals.

[0190] In addition, the configurations disclosed in the above embodiments (including other embodiments, the same applies below) can be applied in combination with configurations disclosed in other embodiments, provided no contradiction arises. Furthermore, the embodiments disclosed in this specification are illustrative, and the embodiments of the present invention are not limited thereto, and can be appropriately modified within the scope that does not deviate from the purpose of the present invention. [Explanation of symbols]

[0191] A Infrared radiation layer B Light reflective layer Du adjacent side protective layer Ds Separation side protective layer IR Infrared light J Resin material layer R coating layer S Short side T Long side U protrusion W Resin material layer for connection Y Plate adhesive layer Z Plate

Claims

1. a light-transmitting resin material layer and a light-reflecting layer located on a back surface side of the resin material layer; A light-reflecting film in which, when viewed in cross section, protrusions having short and long sides of different lengths that extend in a straight line from different positions in a cross direction perpendicular to the thickness direction of the resin material layer toward the surface side of the resin material layer and intersect with each other are formed on the surface of the resin material layer so that the protrusions are aligned in the cross direction.

2. The light reflecting film according to claim 1 , wherein a base end of the short side of each of the protrusions and a base end of the long side of each of the protrusions adjacent to each of the protrusions are located at the same position in the intersecting direction.

3. The light reflecting film according to claim 1 , wherein in the cross-sectional view, a base end of the short side and a base end of the long side of one of the protrusions are at the same position in a thickness direction of the resin material layer.

4. 4. The light reflecting film according to claim 1, wherein, in the cross-sectional view, for one of the protrusions, an angle of the side of the long side of the short side with respect to a virtual plane passing through a base end of the short side along the intersecting direction is in the range of 80 degrees to 100 degrees.

5. 4. The light reflecting film according to claim 1, wherein, in the cross-sectional view, for one of the protrusions, an angle of the side of the short side of the long side with respect to a virtual plane passing through a base end of the long side along the intersecting direction is greater than 0 degrees and less than 65 degrees.

6. 4. The light reflecting film according to claim 1, wherein a base end of the short side and a base end of the long side are located in a middle part of the resin material layer in the thickness direction.

7. A light-reflecting film according to any one of claims 1 to 3, wherein the base end of the short side and the base end of the long side are located at the end of the resin material layer on the side where the light-reflecting layer is present in the thickness direction.

8. a light-transmitting coating layer covering a surface of the resin material layer is provided in a form that fills spaces between adjacent protrusions and makes an outer surface a flat surface; 4. The light reflecting film according to claim 1, wherein the refractive index of the resin material forming the coating layer is smaller than the refractive index of the resin material forming the resin material layer.

9. The light-reflecting film according to any one of claims 1 to 3, wherein a surface of the light-reflecting layer on the side where the resin material layer is present is formed in plane symmetry with the surface of the resin material layer having the protrusion portion with respect to a reference plane located along the intersecting direction and between the surface of the resin material layer and the light-reflecting layer in the cross-sectional view.

10. the resin material layer is an infrared radiation layer that emits infrared light from an emission surface, The light-reflecting film according to any one of claims 1 to 3, wherein the infrared radiation layer is made of an infrared radiation resin material adjusted to a thickness such that the infrared radiation layer emits thermal radiation energy in a wavelength band from 8 μm to 14 μm that is greater than the absorbed solar light energy.

11. The light reflective film of claim 10 , wherein the light reflective layer comprises silver or a silver alloy.

12. the infrared radiation resin material is a vinyl chloride resin or vinylidene chloride resin mixed with a plasticizer, 11. The light-reflecting film according to claim 10, wherein the plasticizer comprises one or more compounds selected from the group consisting of phthalic acid esters, aliphatic dibasic acid esters, and phosphoric acid esters.

13. an adjacent-side protective layer between the infrared emitting layer and the light reflecting layer; 11. The light-reflecting film according to claim 10, wherein the adjacent-side protective layer is made of a polyolefin resin having a thickness of 300 nm or more and 40 μm or less, or an ethylene terephthalate resin having a thickness of 17 μm or more and 40 μm or less.

14. The light-reflecting film according to claim 13 , further comprising a spaced-side protective layer on a surface of the light-reflecting layer facing away from the infrared-emitting layer, the spaced-side protective layer being made of an acrylic resin.

15. The light-reflecting film according to claim 14, wherein a connecting resin material layer is provided on a back surface portion of the separating side protective layer that is away from the light-reflecting layer, and the connecting resin material layer is any one of ethylene terephthalate resin, polypropylene, polyethylene, and acrylic resin.

16. A method for using the light reflecting film according to any one of claims 1 to 3, comprising the steps of: A method of using a light reflecting film, comprising installing the light reflecting film on a wall surface in an upright position with the short side positioned above the long side with respect to one of the protrusions.

Citation Information

Patent Citations

  • Sunlight reflecting civil engineering building material, shading material, and method of restraining heat island phenomenon