By installing thermometers and using a heat-curing stamp material to measure temperature changes near the furnace surface, the method addresses inefficiencies in viscous layer thickness measurement, ensuring precise control and extending blast furnace life.
Patent Information
- Application Number
- JP2023047102
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing methods for measuring the thickness of the viscous layer in blast furnaces are inefficient and lack precision, leading to inaccurate detection of temperature changes over time, which can result in rapid wear of bricks and reduced furnace life.
The method involves installing a plurality of thermometers within 600 mm from the furnace surface, using sheathed thermocouples, and filling the installation openings with a heat-curing stamp material to measure temperature changes accurately, allowing for precise determination of viscous layer thickness.
Enables accurate and rapid measurement of viscous layer thickness, preventing rapid brick wear and extending the lifespan of the blast furnace by controlling the thickness effectively.
Smart Images

Figure 2024136117000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for measuring a viscous layer thickness, a method for operating a blast furnace, and a blast furnace. [Background technology]
[0002] Among blast furnaces, there are known those in which thermometers are embedded at intervals inside the bricks that form the vessel in the thickness direction of the bricks, and the embedded thermometers measure the temperature change of the bricks to determine the remaining thickness of the bricks (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 1-230711 Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, in this type of blast furnace, it is sometimes desirable to measure the thickness of the viscous layer.
[0005] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to make it possible to measure the thickness of a viscous layer with a short time constant. [Means for solving the problem]
[0006] <1> A method for measuring the thickness of a viscous layer according to one embodiment of the present invention comprises installing the temperature measuring parts of a plurality of thermometers within a range of 600 mm from the inner surface of a blast furnace brick in a direction perpendicular to the surface, and measuring the thickness of the viscous layer formed on the surface based on temperature information measured by the plurality of thermometers.
[0007] <2> the above <1> In the method for measuring the viscous layer thickness according to the above, the plurality of thermometers are arranged in installation openings that open to the outside in the bricks of the side wall of the blast furnace, and the installation openings are filled with a stamp material.
[0008] <3> the above <2> In the method for measuring a viscous layer thickness according to the above, the stamp material is a material that is thermally hardened within one hour under the environmental temperature inside the blast furnace.
[0009] <4> the above <3> In the method for measuring the thickness of the viscous layer according to the present invention, the bulk density of the stamp material is 1.8 g / cm 3 That's all.
[0010] <5> the above <2> In the method for measuring a viscous layer thickness according to the above, the plurality of thermometers are bundled together.
[0011] <6> the above <1> In the method for measuring a viscous layer thickness according to the above, the plurality of thermometers are installed in the joints of the bricks constituting the bottom wall of the blast furnace.
[0012] <7> A method for operating a blast furnace according to one aspect of the present invention includes: <1> from <7> The thickness of the viscous layer is controlled based on the thickness of the viscous layer measured by the method for measuring the thickness of the viscous layer described in any one of the above.
[0013] <8> the above <7> In the blast furnace operating method according to the above, during tapping, the temperature measuring portion of each of the plurality of thermometers is installed at the same height as a hearth tapping reference point at which molten metal is discharged from inside the blast furnace to the outside.
[0014] <9> In a blast furnace according to one embodiment of the present invention, the temperature measuring parts of a plurality of thermometers are installed within a range of 600 mm from the surface of the bricks on the inside of the furnace in a direction perpendicular to the surface.
[0015] The inventors of the present application found that the thickness of the viscous layer can be measured with high accuracy by detecting temperature changes at multiple positions (multiple positions close to the surface) within 600 mm from the surface of the brick inside the furnace in a direction perpendicular to the surface with a thermometer. In other words, if the position for detecting the temperature change is farther than 600 mm from the surface, it becomes impossible to detect the temperature change with high accuracy over a predetermined time period. When the thickness of the viscous layer attached to the surface approaches 0 mm, the bricks are rapidly worn away, whereas when the viscous layer recovers, the wear of the bricks stops. Therefore, by appropriately controlling the thickness of the viscous layer, for example, it is possible to avoid rapid wear of the bricks, etc. As a result, it is possible to extend the life of a blast furnace, etc. Effect of the Invention
[0016] According to the present invention, the viscous layer thickness can be measured with a short time constant. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a cross-sectional view showing a blast furnace according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a state in which molten iron is stored in the blast furnace shown in FIG. [Diagram 3] 2 is a cross-sectional view showing a state in which two first thermometers are installed in installation openings formed in a second brick of the blast furnace shown in FIG. 1. FIG. [Figure 4] 4 is an enlarged cross-sectional view showing a state in which a stamp material is tamped into the installation opening shown in FIG. 3. FIG. [Diagram 5] FIG. 11 is a cross-sectional view illustrating the process of placing the stamp material to be pressed into the installation opening on the chute jig. [Figure 6] A cross-sectional view illustrating the construction of pushing the stamp material up to the tip of the installation opening. [Figure 7] A cross-sectional view illustrating the construction of tamping a stamp material into an installation opening. [Figure 8] 11 is a cross-sectional view illustrating an example in which the stamp material is repeatedly tamped into the installation opening multiple times. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, a method for measuring a viscous layer thickness, a method for operating a blast furnace, and a blast furnace according to one embodiment of the present invention will be described with reference to Figs.
[0019] [First embodiment] (blast furnace) As shown in Figures 1 and 2, molten iron 12 is produced on the bottom side of a blast furnace 10. The blast furnace 10 includes a blast furnace body 20, a plurality of first thermometers 22, a plurality of second thermometers 26, and a plurality of third thermometers 55.
[0020] (Blast furnace body) The blast furnace body 20 includes a bottom wall 31, a side wall 32, an inner stamping member 33, a stave 34, an outer stamping member 35, and a shell 36.
[0021] The bottom wall 31 constitutes the hearth of the blast furnace 10. In the bottom wall 31, a plurality of first bricks (bricks) 41 are arranged vertically with their longitudinal direction facing vertically. The first bricks 41 are made of, for example, carbon bricks. In the bottom wall 31, a plurality of first bricks 41 are provided continuously in the horizontal direction, and joints 42 are formed between adjacent first bricks 41. Gaps in the joints 42 are filled with, for example, a joint material.
[0022] The side wall 32 constitutes the furnace wall of the blast furnace 10. The bottom 32a of the side wall 32 is formed in a cylindrical shape so as to cover the outer peripheral surface 31a of the bottom wall 31 from the outside in the radial direction. The side wall 32 is formed in a cylindrical shape extending upward from the bottom 32a. In the side wall 32, a plurality of second bricks (bricks) 45 are arranged sideways with their longitudinal direction directed horizontally. For the second bricks 45, for example, carbon bricks are used. The second bricks 45 are stacked in a plurality of layers. A joint 46 is formed between the second bricks 45 adjacent to each other in the vertical direction. The gaps in the joints 46 are filled with a joint material.
[0023] A space 48 is formed in the furnace by the bottom wall 31 and the side wall 32. Filler bricks 49 are arranged at the bottom of the space 48. The filler bricks 49 are stacked, for example, in two stages on the bottom wall 31. The filler bricks 49 are consumed by the molten iron 12 in the furnace.
[0024] The inner stamped member 33 is a refractory material formed in a cylindrical shape along the outer circumferential surface of the side wall 32. The inner stamped member 33 is applied by, for example, tamping. The stave 34 is, for example, a water-cooled metal member provided with a coolant water passage. The stave 34 cools the iron shell 36 and the like to protect the iron shell 36 and the like from high heat in the furnace. The outer stamped member 35 is a refractory material formed in a cylindrical shape along the outer circumferential surface of the stave 34. The outer stamped member 35 is applied by tamping in the same manner as the inner stamped member 33. The shell 36 is a member made of a steel plate and formed into a cylindrical shape along the outer peripheral surface of the outer stamp member 35. The shell 36 covers the outer stamp member 35 to form the exterior of the blast furnace.
[0025] When the blast furnace 10 is in operation, molten iron 12 is produced in the furnace, and part or all of the filler bricks 49 and part of the second bricks 45 on the furnace inner side are lost due to the molten iron 12. A viscous layer 50 is formed on the surface (brick surface) 31b of the bottom wall 31 and the surface (brick surface) 32b of the side wall 32. The surface 31b of the bottom wall 31 is formed by the inner surface of the first brick 41 facing the furnace inner side. The surface 32b of the side wall 32 is formed by the inner surface of the second brick 45 facing the furnace inner side. The positions of the surfaces 31b, 32b can be estimated from the temperature measurement results of the bricks 41, 45, such as the measurement results of the third thermometer 44, as described later.
[0026] The viscous layer 50 is attached to the surface 31b of the bottom wall 31 and the surface 32b of the side wall 32. The viscous layer 50 is a semi-molten layer that is interposed between the surface 31b and the molten pig iron 12 and further between the surface 32b and the molten pig iron 12. The viscous layer 50 is interposed between the surface 31b and the molten pig iron 12, thereby protecting the first brick 41 of the bottom wall 31. The viscous layer 50 is interposed between the surface 32b and the molten pig iron 12, thereby protecting the second brick 45 of the side wall 32. In other words, the viscous layer 50 is a brick protection layer that is attached to the surface 31b and the surface 32b to protect the first brick 41 and the second brick 45.
[0027] The third thermometers 55 are existing thermometers that are installed before the operation of the blast furnace 10. The third thermometers 55 are arranged on the outer peripheral surface side of the side wall 32 at intervals in the circumferential direction of the side wall 32. The third thermometers 55 are arranged as a pair of third thermometers 55. For example, one of the pair of third thermometers 55 is installed at a position 50 mm from the outer peripheral surface of the side wall 32 toward the inside of the furnace. The other third thermometer 55 is installed at a position 150 mm from the outer peripheral surface of the side wall 32 toward the inside of the furnace. The third thermometers 55 are installed, for example, at each tier of stacked second bricks 45. The third thermometers 55 are used, for example, to estimate (manage) the remaining thickness of the second bricks 45. That is, by measuring the temperature with the third thermometers 55 from the time when the blast furnace 10 is operated, the remaining pressure of the second bricks 45 can be estimated according to changes in the measurement results. Furthermore, the third thermometer 55 is also used to check the cooling state of the shell 36 and the like, for example.
[0028] As shown in FIG. 2 to FIG. 4, the blast furnace body 20 has an installation opening 58. The installation opening 58 is provided in the side wall 32c (hereinafter, also referred to as the hearth side wall) of the side wall 32 closer to the bottom wall 31. The installation opening 58 is provided, for example, in the second brick 45 of the fourth row from the bottom in the hearth side wall 32c. The installation opening 58 is formed in a direction perpendicular to the surface 32b of the side wall 32 from the outside of the blast furnace body 20 toward the inside of the furnace. In this embodiment, the installation opening 58 opens to the outside in the second brick 45 of the fourth row from the bottom. The hole diameter of the installation opening 58 can be selected arbitrarily, and is, for example, 20 mm. The tip portion 58a of the installation opening 58 is located within a range of 600 mm from the surface 32b of the side wall 32 in a direction perpendicular to the surface 32b (radial direction).
[0029] A single pipe 61 is inserted into the installation opening 58 from the outside of the blast furnace body 20. The single pipe 61 is inserted into the installation opening 58 from the tip. In the illustrated example, the single pipe 61 is inserted into the installation opening 58 in a portion located at the stave 34, the outer stamping material 35, and the steel shell 36. The tip of the single pipe 61 is not inserted into the inner stamping material 33. The base end 61a of the single pipe 61 protrudes from the outer peripheral surface of the blast furnace body 20 to the outside. A flange 62 is fixed to the base end 61a of the single pipe 61. An insertion hole 63 is formed in the flange 62 coaxially with the single pipe 61. A flange 65 is detachably attached to the flange 62. A through hole 66 is formed in the flange 65 coaxially with the insertion hole 63 of the flange 62.
[0030] (1st thermometer) A plurality of first thermometers 22 are installed in the installation opening 58 through the through-hole 66 of the flange 65, the insertion hole 63 of the flange 62, and the single pipe 61. In this embodiment, two first thermometers 22 will be described as an example of the plurality of first thermometers 22. The two first thermometers 22 are installed in the installation opening 58, and thereby installed in the fourth row of second bricks 45 (see FIG. 1) in the hearth side wall 32c on the hearth side.
[0031] The two first thermometers 22 are installed at a height position between 1500 mm and 5500 mm from the first brick 41 at the hearth bottom (the third to tenth rows of the second bricks 45). The locations of the two first thermometers 22 may be determined after the blast furnace 10 is put into operation, for example, based on temperature information measured by a plurality of third thermometers 55. For example, the two first thermometers 22 are installed at locations of the second bricks 45 that require temperature management. Examples of the second bricks 45 that require temperature management include locations where the remaining thickness of the second bricks 45 is thin and locations where the temperature measured by the first thermometers 22 is high. The number of first thermometers 22 is not limited to two and may be three or more. In the present embodiment, an example in which two first thermometers 22 are installed at one location on the hearth side wall 32c is described, but the two first thermometers 22 may be installed at multiple locations on the hearth side wall 32c (multiple locations in the vertical direction, multiple locations in the circumferential direction), for example.
[0032] For example, a commonly known sheathed thermocouple is used as the two first thermometers 22. The sheathed thermocouple has a thermocouple wire (not shown) enclosed inside a sheath. The two first thermometers 22 include a first thermometer 23 and a first thermometer 24. One of the first thermometers 23 has a sheath (sheath of the thermometer) 23a with a diameter of 3.2 mm, for example, and is installed in a state of contact with the first bottom 58c. The diameter of the sheath 23a can be selected arbitrarily. The tip 23b of one of the first thermometers 23 is in contact with the tip 58a of the installation opening 58. Thus, the tip 23b of one of the first thermometers 23 is installed so as to be located within a range of 600 mm from the surface 32b of the sidewall 32 on the hearth side of the blast furnace 10 in a direction perpendicular to the surface 32b.
[0033] The other first thermometer 24 has, for example, a sheath (sheath of the thermometer) 24a with a diameter of 1.6 mm, and is installed in a state of contact with the second bottom 58d. The diameter of the sheath 24a can be selected arbitrarily. The tip 24b of the other first thermometer 24 is in contact with the tip 58e of the second bottom 58d. Therefore, the tip 24b of the other first thermometer 24 is installed at a position a predetermined distance away from the tip 23b of the one first thermometer 23 on the outside of the blast furnace body 20. The tip 24b of the other first thermometer 24 is installed so as to be located within a range of 600 mm from the surface 32b of the sidewall 32 on the hearth side of the blast furnace 10 in a direction perpendicular to the surface 32b.
[0034] That is, the tip 23b and the tip 24b of each of the two first thermometers 22 are located within a range of 600 mm from the surface 32b of the sidewall 32 at the hearth side of the blast furnace 10 in a direction perpendicular to the surface 32b. In other words, the distance from the tip 24b, which is the farthest from the surface 32b among the tips 23b and 24b of each of the multiple first thermometers 22, to the surface 32b is within 600 mm. Here, the tip 23b and the tip 24b of each of the multiple first thermometers 22 are the temperature measuring parts of each first thermometer 22. In addition, the tip 23b and the tip 24b of each of the multiple first thermometers 22 are located within the range of 600 as described above from the surface 32b of the sidewall 32 at the same height position. In the first embodiment, an example is described in which the tip 23b of one first thermometer 23 and the tip 24b of the other first thermometer 24 are installed 500 mm apart, but the distance between the tip 23b and the tip 24b can be selected arbitrarily.
[0035] The two first thermometers 22 are bundled at multiple points with, for example, cable ties 25, etc., with the sheath 23a of one first thermometer 23 and the sheath 24a of the other first thermometer 24 spaced apart in the longitudinal direction of the sheaths. This increases the strength of the two first thermometers 22. This makes it easier to install the two first thermometers 22 straight along the first bottom 58c and the second bottom 58d of the installation opening 58.
[0036] With the two first thermometers 22 disposed in the installation opening 58, the installation opening 58 is filled with the stamping material 68. In other words, the installation opening 58 is filled with the stamping material 68. The stamping material 68 is a material based on, for example, the inner stamping material 33 or the outer stamping material 35. The stamping material 68 has thermosetting properties such that it is thermally hardened within one hour under the furnace environment temperature of the blast furnace 10. In addition, the stamping material 68 has thermal conductivity equivalent to that of, for example, the second brick 45. The stamping material 68 has a bulk density of 1.8 g / cm3 inside the installation opening 58. 3In the illustrated example, the stamp material 68 is filled not in the entire installation opening 58 but in a part of the installation opening 58 on the inner side of the furnace.
[0037] (Second thermometer) As shown in FIG. 1, the plurality of second thermometers 26 are installed in the joints 42 between the first bricks 41 that constitute the bottom wall 31. In this embodiment, two second thermometers 26 are used as the plurality of second thermometers 26. By installing the two second thermometers 26 in the joints 42 between the first bricks 41, for example, it is not necessary to form an installation opening in the first brick 41 to install the two second thermometers 26. This ensures the strength of the first brick 41. For the two second thermometers 26, for example, a sheathed thermocouple that is generally known in the same way as the first thermometer 22 is used. The two second thermometers 26 include a second thermometer 27 on one side and a second thermometer 28 on the other side.
[0038] One tip 27a of the second thermometer 27 is installed so as to be located within a range of 600 mm from a surface 31b of the bottom wall 31 on the hearth side of the blast furnace 10 in a direction perpendicular to the surface 31b (up and down direction). The other second thermometer 28 has a tip 28a installed at a position a predetermined distance away from the tip 27a of the one second thermometer 27 on the outside of the bottom wall 31. The tip 28a of the other second thermometer 28 is installed so as to be located within a range of 600 mm from the surface 31b of the bottom wall 31 on the hearth side of the blast furnace 10 in a direction perpendicular to the surface 31b.
[0039] Thus, the tips 27a and 28a of the two second thermometers 26 are installed so as to be located within a range of 600 mm in a direction perpendicular to the surface 31b of the bottom wall 31 at the hearth side of the blast furnace 10. The distance between the tips 27a and 28a can be selected arbitrarily.
[0040] The number of second thermometers 26 is not limited to two and may be three or more. In the embodiment, an example in which two second thermometers 26 are installed at one location on the bottom wall 31 is described, but the two second thermometers 26 may be installed at multiple locations on the bottom wall 31, for example.
[0041] (Example of installation where stamping material is filled into the installation opening) Next, an example of installation in which two first thermometers 22 are installed in the installation opening 58 and the installation opening 58 is filled with a stamping material 68 will be described with reference to Figs. 3 to 8. The two first thermometers 22 can be installed, for example, when it becomes necessary to control the temperature of the second bricks 45 after the blast furnace 10 starts operating. As shown in Figures 3 and 4, with the two first thermometers 22 bundled together, the two first thermometers 22 are installed straight along the first bottom 58c and the second bottom 58d of the installation opening 58. After the two first thermometers 22 are installed in the installation opening 58, the cap 65 is removed from the flange 62. Markings are made on the sheaths 23a and 24a of the two first thermometers 22 in accordance with the position of the flange 62. Thus, any misalignment of the two first thermometers 22 can be confirmed during application of the stamp material 68.
[0042] The temperature inside the installation opening 58 is measured with a radiation thermometer. It is checked whether the temperature inside the installation opening 58 is high, taking into consideration the hot pot life of the stamp material 68. It is preferable to prepare an air pipe for air cooling in case the temperature inside the installation opening 58 is high. In addition, the length from the tip 58a of the installation opening 58 to the flange 62 is measured with a convex (not shown). The measured length is used as the basis for calculating the bulk density of the stamp material 68. Here, it is preferable to individually divide and package the stamp material 68 into 33 g portions as the amount to be applied at one time, and wrap them in paper in a long and narrow shape to fit the chute jig 71 (see FIG. 5), which will be described later. This allows the stamp material 68 to be placed on the chute jig 71 in a short time.
[0043] As shown in FIG. 5, 33 g of stamp material 68 individually wrapped and wrapped in elongated paper is removed from the packaging and placed on the chute jig 71. The chute jig 71 has a part 71a protruding outward from the flange 62 formed as a half pipe. The half pipe part 71a is formed in a shape that makes it easy to place the stamp material 68 on it and prevents the stamp material 68 from spilling out. The chute jig 71 also has a part (not shown) that is inserted from the flange 62 into the single pipe 61 formed in a pipe shape. The pipe-shaped part is formed with a smaller diameter than the hole diameter of the single pipe 61. Therefore, the pipe-shaped part can be inserted from the flange 62 into the single pipe 61. The hole diameter of the installation opening 58 is, for example, 20 mm.
[0044] 33 g of stamp material 68 is placed on the chute jig 71 as the amount of material to be applied at one time, and the stamp material 68 placed on the chute jig 71 is pushed from the chute jig 71 into the installation opening 58 with a sponge brush (not shown). The sponge brush (not shown) is an elastically deformable brush. 6, the stamp material 68 around the sheaths 23a and 24a of the two first thermometers 22 is pushed into the installation opening 58 together with other portions of the stamp material 68 to the tip 58a of the installation opening 58 with a sponge brush. It is preferable to use a sponge brush as a tool for pushing the stamp material 68 into the tip 58a of the installation opening 58.
[0045] 7, the stamp material 68 is pushed into the installation opening 58 up to the tip 58a with a sponge brush, and then the stamp material 68 is tamped down for 30 seconds with a stamp stick 75. This makes it possible to prevent the stamp material 68 from having any voids. The stamped stick 75 has a disk-shaped veneer 75b at the tip of the stamped stick 75a. It is preferable that the gap between the veneer 75b and the installation opening 58 is as narrow as possible. Specifically, the veneer 75b is formed to have a diameter of 18 mm while the installation opening 58 has a hole diameter of 20 mm. In addition, the veneer 75b has a recess 75c formed in the lower part corresponding to the sheaths 23a and 24a of the two first thermometers 22. The recess 75c is a cutout. This prevents the veneer 75b from interfering with the sheaths 23a and 24a of the two first thermometers 22, the cable tie 25 that binds the sheaths 23a and 24a, and the like. Furthermore, the attachment rod 75a is formed as an extension type because the external space of the blast furnace 10 is narrow. In addition, it is preferable to prepare a spare attachment rod having a veneer 75b with a diameter of 16 mm, which is smaller than 18 mm.
[0046] Here, the two first thermometers 22 are installed straight along the bottom of the installation opening 58. This makes it difficult for the two first thermometers 22 to interfere with the construction of forcing the stamp material 68 into the installation opening 58 and tamping it down. Also, in the two first thermometers 22, it is preferable that the sheaths 23a and 24a are bound together so as not to interfere with the veneer 75b that presses the stamp material 68 into the installation opening 58 and tamps it down.
[0047] After the stamp material 68 is compacted with the stamp rod 75, the length from the surface of the compacted stamp material 68 to the flange 62 is measured with a convex (not shown). The bulk density of the compacted stamp material 68 is calculated based on the measured length from the surface of the stamp material 68 to the flange 62 and the previously measured length from the tip 58a of the installation opening 58 to the flange 62. If the bulk density of the stamp material 68 is 1.8 g / cm 3 Verify that this is the case. It is checked whether the markings on the sheaths 23a and 24a of the two first thermometers 22 are misaligned with the flange 62. For example, if the markings are misaligned from the flange 62 to the outside of the furnace, the two first thermometers 22 are pushed in so that the markings are aligned with the flange 62.
[0048] As shown in FIG. 8, the stamp material 68 is divided into small pieces and pushed into the installation opening 58 to be tamped down. This is repeated several times. In this case, as an example, the length L of the stamp material 68 filled into the installation opening 58 is set to 600 mm. Here, the two first thermometers 22 are, for example, such that the tip 23b of one first thermometer 23 and the tip 24b of the other first thermometer 24 are spaced apart by 500 mm. Therefore, by setting the length of the stamp material 68 to 600 mm, the stamp material 68 can be extended to a position 100 mm away from the tip 24b of the other first thermometer 24 to the outside of the furnace. This allows the two first thermometers 22 to accurately measure the temperature of the second brick 45 (i.e., the furnace environment temperature).
[0049] Here, in order to make the length of the stamp material 68 600 mm, it is necessary to repeat the process of tamping the divided stamp material 68 to about 30 mm in one operation about 20 times. If one operation takes about 5 minutes, the operation time to make the length of the stamp material 68 600 mm is about 100 minutes. If the environmental temperature inside the furnace (i.e., the expected temperature on the surface side of the installation opening) is 300°C, the usable time of the stamp material 68 is within 1 hour (specifically, 30 to 60 minutes).
[0050] As an example, assuming that the pot life of the stamp material 68 is 30 minutes, the stamp material 68 applied the first time starts to harden during, for example, the seventh application. Meanwhile, the stamp material 68 applied from the third to sixth times has not hardened. Therefore, the stamp material 68 applied the seventh time can be hardened integrally with the stamp material 68 applied the sixth time. From the above, by using a material that hardens thermally within one hour at the furnace environmental temperature as the stamp material 68, the bulk density of the stamp material 68 can be set to 1.8 g / cm 3 With the above secured, the installation opening 58 can be filled with the stamp material 68.
[0051] During the construction of filling the stamping material 68 into the installation opening 58, it is considered that the inner stamping material 33 and the outer stamping material 35 (see FIG. 1 ) of the blast furnace body 20 may slightly crumble and mix with the stamping material 68 inside the installation opening 58. However, if the inner stamping material 33 and the outer stamping material 35 are made of the same type of material as the stamping material 68, even if the inner stamping material 33 and the outer stamping material 35 crumble and mix with the stamping material 68, problems are unlikely to occur. The distance between the tip 23b of one first thermometer 23 and the tip 24b of the other first thermometer 24 is not limited to 500 mm and can be selected arbitrarily. The length of the stamp member 68 is not limited to 600 mm and can be selected arbitrarily.
[0052] (Method of measuring viscosity layer thickness and method of operating blast furnace) Next, a method for measuring the thickness of the viscous layer 50 (the position of the working surface) using the two first thermometers 22 and a method for operating the blast furnace 10 will be described with reference to Fig. 2 and Fig. 4. Hereinafter, the thickness of the viscous layer 50 may be referred to as the "viscous layer thickness". The method of measuring the viscous layer thickness using the two second thermometers 26 and the method of operating the blast furnace 10 are similar to the method of measuring the viscous layer thickness using the two first thermometers 22 and the method of operating the blast furnace 10. Therefore, the description of the method of measuring the viscous layer thickness using the two second thermometers 26 and the method of operating the blast furnace 10 will be omitted.
[0053] The inventors of the present application found that the thickness of the viscous layer can be measured with high accuracy by detecting temperature changes at multiple positions (multiple positions close to the surface 32b) within 600 mm from the surface 32b of the second brick 45 in a direction perpendicular to the surface 32b with the first thermometer 22. That is, if the position for detecting the temperature change is farther than 600 mm from the surface 32b, it becomes impossible to detect the temperature change with high accuracy after a predetermined time has elapsed.
[0054] Therefore, as shown in FIG. 2, the two first thermometers 22 were installed so that the tips 23b and 24b (temperature measuring parts) were located within a range of 600 mm in a direction (radial direction) perpendicular to the surface 32b of the sidewall 32 at the bottom side of the blast furnace 10 from the surface 32b (the position of the working surface when the viscous layer thickness is assumed to be 0 mm). By continuously measuring the temperature at regular time intervals using these two first thermometers 22, it is possible to measure a temperature change with a short time constant (i.e., a non-steady temperature change in the furnace). This makes it possible to accurately measure and understand the phenomenon inside the furnace (specifically, the thickness of the viscous layer 50 formed on the surface 32b of the sidewall 32).
[0055] The viscous layer thickness can be calculated using factors such as the temperature difference (ΔT) between the temperatures measured by the two first thermometers 22, the distance (ΔX) between the two first thermometers 22, the brick physical property value (λ) of the second brick 45, and the like. Specifically, the temperature (hereinafter also referred to as the estimated temperature) of the part located radially inside the first thermometer 22 at the height position of the first thermometer 22 is estimated using the above-mentioned factors. Here, assuming that the melting temperature of pig iron is 1150°C, the viscous layer thickness is set to the surface (inner surface) of the viscous layer 50 at a position where the water bottom temperature is 1150°C or less. Therefore, the viscous layer thickness can be calculated by subtracting the remaining thickness of the second brick 45 from the surface position of the viscous layer 50. The remaining pressure of the second brick 45 can be estimated, for example, from the measurement result of the third thermometer 55. The viscous layer thickness is controlled based on the viscous layer thickness calculated as above, and the blast furnace 10 is operated so as to ensure an appropriate viscous layer thickness. For example, when the viscous layer thickness becomes small and the temperature inside the furnace rises, a means for quickly lowering the temperature of the surrounding area where the temperature has risen (specifically, adjusting the amount of air blown to that location and adjusting the amount of tapping by blocking a nearby tap hole) can be implemented. Here, controlling the viscous layer thickness based on the measurement result of the viscous layer thickness includes the following cases. (1) The measurement result of the viscous layer thickness is compared with a target value set for the viscous layer thickness. If there is a difference between the measurement result and the target value, the operating conditions of the blast furnace 10 are adjusted so that the measurement result approaches the target value. (2) The measurement result of the viscous layer thickness is compared with the minimum value set for the viscous layer thickness. If the measurement result is below the minimum value, the operating conditions of the blast furnace 10 are adjusted so that the viscous layer becomes thicker.
[0056] In this manner, in the method for operating the blast furnace 10, the thickness of the viscous layer 50 is controlled based on the viscous layer thickness measured by the method for measuring the viscous layer thickness. Therefore, the viscous layer 50 can be controlled to an appropriate thickness without losing the viscous layer 50 adhering to the surface 32b of the side wall 32. Here, for example, when the thickness of the viscous layer attached to the surface 32b approaches 0 mm, the second brick 45 is rapidly worn away, whereas when the viscous layer 50 is restored, the wear of the second brick 45 stops. Therefore, by appropriately controlling the thickness of the viscous layer, it is possible to avoid, for example, rapid wear of the second bricks 45. As a result, it is possible to extend the life of the blast furnace 10, for example.
[0057] 2 and 4, the installation opening 58 in which the two first thermometers 22 are arranged is filled with a stamp material 68. Furthermore, the bulk density of the stamp material 68 is set to 1.8 g / cm 3 As described above, the stamping material 68 can be made dense, and volatilization (bumping and voids caused by bumping) during thermal hardening due to heat in the furnace can be prevented. As a result, by filling the installation opening 58 with the stamping material 68, it is possible to prevent the molten iron and slag in the furnace from penetrating into the installation opening 58. Therefore, the risk of trouble due to leakage of the molten iron and slag can be avoided. Furthermore, the two first thermometers 22 can continuously measure the temperature indication value stably over a long period of time. As a result, the two first thermometers 22 can continue stable temperature management until the end of the blast furnace 10.
[0058] [Second embodiment] Next, an example of utilizing the method for measuring the viscous layer thickness of the first embodiment when tapping molten iron 12 from inside the blast furnace 10 will be described with reference to FIG. As shown in Fig. 2, for example, when refurbishing a blast furnace 10, it is necessary to tap molten iron 12 from the inside of the blast furnace 10 (i.e., inside the furnace). In this case, it is preferable to reduce the amount of molten iron 12 remaining in the furnace as much as possible. When taking out the molten iron 12 from inside the furnace to the outside, a molten iron tapping hole 82 is opened with a drill or the like on the outside of the blast furnace 10 from the hearth tapping hole position P1 toward the inside of the furnace in the side wall 32 on the hearth side. Here, for example, equipment related to the blast furnace 10 is provided around the blast furnace 10. Therefore, the space around the blast furnace 10 is narrow. Therefore, the space around the blast furnace 10 for installing a drill is limited.
[0059] Under these conditions, in order to minimize the amount of molten iron 12 remaining in the furnace, the hearth tapping hole position P1 and the inclination angle of the molten iron removal hole 82 on the outside of the blast furnace 10 are limited. Therefore, by taking into consideration the location of the drill, the hearth tapping hole position P1, the inclination angle of the molten iron removal hole 82, the viscous layer thickness, etc., it is possible to predict in advance the position P2 where the molten iron removal hole 82 opens onto the surface of the viscous layer 50. Hereinafter, the position P2 where the molten iron removal hole 82 opens onto the surface of the viscous layer 50 may be referred to as the hearth tapping reference point P2.
[0060] In this embodiment, the two first thermometers 22 are installed at the same height as the hearth tapping reference point P2. Therefore, by controlling the temperatures measured by the two first thermometers 22, the viscous layer thickness at the hearth tapping reference point P2 can be controlled accurately in accordance with the revamping of the blast furnace 10. This allows the molten iron discharge hole 82 to be appropriately drilled from the hearth tapping opening position P1 to the hearth tapping reference point P2 on the surface of the viscous layer 50 when the blast furnace 10 is revamped. Therefore, the molten iron 12 in the furnace can be discharged to the outside from the opening of the molten iron discharge hole 82 (i.e., the hearth tapping reference point P2). This allows the blast furnace 10 to be revamped appropriately.
[0061] The technical scope of the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention.
[0062] For example, the single pipe 61 and the flange 62 may be omitted.
[0063] In addition, within the scope of the invention, the components in the above-described embodiments may be replaced with well-known components, and the above-described modified examples may be combined as appropriate. [Explanation of symbols]
[0064] 10 blast furnace 12 Molten iron 22 2 primary thermometers (multiple thermometers) 23 First thermometer on one side 23a Sheath of one of the first thermometers (thermometer sheath) 24 The other first thermometer 24a The sheath of the other first thermometer (thermometer sheath) 26 2 secondary thermometers (multiple thermometers) 27 Second thermometer on one side 28 The other second thermometer 31 Bottom wall 31b Bottom wall surface (brick surface) 32 Side wall 32b Side wall surface (brick surface) 41 1st brick (brick) 42 Joint 45 Second brick (brick) 50 viscous layer 58 Installation opening 68 Stamp material P2 Hearth tap reference point
Claims
1. A temperature measuring portion of each of a plurality of thermometers is disposed within a range of 600 mm from a surface of the blast furnace inner side of the brick in a direction perpendicular to the surface, A method for measuring a thickness of a viscous layer, comprising measuring a thickness of a viscous layer formed on the surface based on temperature information measured by the plurality of thermometers.
2. The plurality of thermometers are arranged in installation openings that open to the outside in the bricks of the side wall of the blast furnace, The method for measuring a thickness of a viscous layer according to claim 1 , wherein the installation opening is filled with a stamp material.
3. The method for measuring a viscous layer thickness according to claim 2, wherein the stamp material is a material that is thermally hardened within one hour under an environmental temperature inside the blast furnace.
4. The bulk density of the stamp material is 1.8 g / cm 3 The method for measuring a viscous layer thickness according to claim 3, wherein the thickness of the viscous layer is measured by the above method.
5. The method for measuring a viscous layer thickness according to claim 2 , wherein the plurality of thermometers are bundled together.
6. The method for measuring a viscous layer thickness according to claim 1 , wherein the plurality of thermometers are installed in joints between bricks constituting the bottom wall of the blast furnace.
7. A method for operating a blast furnace, comprising controlling a viscous layer thickness based on a viscous layer thickness measured by the method for measuring a viscous layer thickness according to any one of claims 1 to 6.
8. 8. The method for operating a blast furnace according to claim 7, wherein, during tapping, the temperature measuring parts of the respective thermometers are installed at the same height as a hearth tapping reference point at which molten iron is taken out from inside the blast furnace to the outside.
9. A blast furnace in which the temperature measuring parts of a plurality of thermometers are installed within a range of 600 mm from the surface of the bricks inside the furnace in a direction perpendicular to said surface.
Citation Information
Patent Citations
Method for measuring residual thickness of brick in steelmaking furnace
JP1989230711A