Method for manufacturing glass oscillator and fusion molding device

The method addresses asymmetrical glass resonator shapes by using a melt molding mold with a support column and controlled negative pressures to uniformly heat and deform the workpiece, resulting in highly symmetrical and reproducible glass resonators for gyro sensors.

JP2024136146APending Publication Date: 2024-10-04KK TOYOTA CHUO KENKYUSHO +3
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023047141
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Fluctuations in heat input distribution cause variations in the temperature rise distribution of the workpiece material, leading to asymmetrical glass resonator shapes due to localized start of melt molding.

Method used

A method involving a melt molding mold with a support column, first and second negative pressures, and temperature detection to uniformly heat and deform the workpiece, ensuring symmetrical glass resonator production.

Benefits of technology

The method enables the production of highly symmetrical glass resonators with high reproducibility and accuracy, suitable for gyro sensors, by uniformly heating and deforming the workpiece material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136146000001_ABST
    Figure 2024136146000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a glass oscillator.SOLUTION: A fusion molding die comprises a flat surface, a hole part formed at one part of the surface, and a column extending upward from a bottom face of the hole part. A method for manufacturing a glass oscillator includes: an arrangement step for arranging a plate-like processed material on a surface of the fusion molding die so that it covers the hole part and is separated from an upper face of the column; a first negative pressure generation step for generating first negative pressure at the hole part; a heating step for heating an upper face of the processed material by heating means after the first negative pressure generation step; a detection step for detecting instantaneous temperature rise on the upper face of the column due to deformation of the processed material and contact with the upper face of the column in the heating step; and a second negative pressure generation step for making the negative pressure of the hole part larger than the first negative pressure toward a negative side according to the detection of the temperature rise.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present specification relates to a manufacturing method and a melt forming apparatus for a glass vibrator. [Background technology]

[0002] Patent Document 1 discloses a Bird-bath Resonator Gyroscope (BRG) using a fused silica vibrator as a gyro capable of achieving high accuracy. Specifically, a fusion molding die is prepared with a hole formed in a part of the upper surface. Inside the hole, a support is provided extending upward from the bottom surface of the hole. A material to be processed (e.g., a quartz plate) is placed so as to close the hole, and while reducing the pressure inside the hole, the upper surface of the material to be processed is heated by a heating means. The softened material to be processed can be melted and deformed by a distributed load due to the pressure difference between the negative pressure and atmospheric pressure so as to enter the inside of the hole. This makes it possible to produce a hemispherical glass vibrator with the support as the central axis. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] US Patent Application Publication No. 2018 / 079129 Summary of the Invention [Problem to be solved by the invention]

[0004] Fluctuations in the heat input distribution from the heating means may cause variations in the temperature rise distribution of the processed material. In this case, melt forming begins at a point where the material reaches the softening temperature locally. As a result, the shape of the glass vibrator becomes asymmetric. [Means for solving the problem]

[0005] The manufacturing method of the glass vibrator disclosed in this specification is a manufacturing method of the glass vibrator using a fusion molding die. The fusion molding die has a flat surface, a hole formed in a part of the surface, and a support extending upward from the bottom surface of the hole. The upper surface of the support is located at a lower position than the surface of the fusion molding die. The manufacturing method of the glass vibrator includes an arrangement step of arranging a plate-shaped workpiece material on the surface of the fusion molding die so as to cover the hole and to be spaced apart from the upper surface of the support. The manufacturing method of the glass vibrator includes a first negative pressure generation step of generating a first negative pressure in the hole. The manufacturing method of the glass vibrator includes a heating step of heating the upper surface of the workpiece material by a heating means after the first negative pressure generation step. The manufacturing method of the glass vibrator includes a detection step of detecting an instantaneous temperature rise on the upper surface of the support caused by the workpiece material being deformed by the heating step and coming into contact with the upper surface of the support. The manufacturing method of the glass vibrator includes a second negative pressure generation step of increasing the negative pressure in the hole from the first negative pressure to a more negative side in response to the detection of the temperature rise.

[0006] According to the above configuration, the workpiece material can be adsorbed and fixed to the surface of the melt forming mold by the first negative pressure. Then, the workpiece material is deformed by the heating process and contacts the upper surface of the support, and this can be detected by the instantaneous temperature rise of the upper surface of the support. At this time, since a relatively small first negative pressure is used, even if a portion locally reaches the softening temperature, the start of melt deformation can be suppressed. This makes it possible to heat the entire processing area without starting deformation. Then, after the entire processing area reaches the softening temperature, the first negative pressure is made even more negative, so that the entire processing area can start to melt and deform uniformly. This makes it possible to manufacture a glass vibrator with high symmetry. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view of a melt-molding apparatus 1 of Example 1. FIG. [Diagram 2] FIG. 1 is a top view of a melt-molding apparatus 1 according to a first embodiment. [Diagram 3]FIG. 2 is a flow diagram illustrating a manufacturing process of the glass vibrator of the first embodiment. [Figure 4] 4 is a timing chart illustrating a manufacturing process of the glass vibrator according to the first embodiment. [Diagram 5] 1 is a schematic diagram showing a state in which the center of a quartz plate 30 is in contact with an upper surface TS of a support column. [Figure 6] FIG. 2 is a schematic diagram showing a state after melt deformation. [Figure 7] 11 is a timing chart of a first modified example. [Figure 8] 13 is a timing chart of a second modified example. [Figure 9] 13 is a timing chart of a third modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS EXAMPLES

[0008] Fig. 1 shows a schematic cross-sectional view of the melt-molding apparatus 1. Fig. 2 shows a top view of the melt-molding apparatus 1. Fig. 1 corresponds to the cross-sectional view taken along line II in Fig. 2. Note that Fig. 2 omits the illustration of the burner 50, radiation thermometer 60, and motorized stage 45. The melt-molding apparatus 1 mainly includes a plate 10, a molding die 20, a quartz plate 30, a heat sink 40, a motorized stage 45, a burner 50, a radiation thermometer 60, a control unit 70, and a hole negative pressure generating means 81.

[0009] The mold 20 is a mold for melting and deforming the quartz plate 30 to mold a hemispherical vibrator. The material of the mold 20 is graphite. In this embodiment, the mold 20 is a disk shape with a central axis CA. The mold 20 has a lower surface 20r, a surface 20s, a hole 20h, a support 20p, and a through hole 20e. The lower surface 20r and the surface 20s are flat surfaces perpendicular to the central axis CA. The surface 20s is parallel to the lower surface 20r. A hole 20h is formed in a part of the surface 20s. The hole 20h is a deformation space for the quartz plate 30 to melt and deform. In this embodiment, the hole 20h has a cylindrical hollowed-out shape centered on the central axis CA. The hole 20h has a bottom surface 20b. A plurality of through holes 20e penetrating the lower surface 20r are formed in the bottom surface 20b. The through hole 20e communicates with the first communication hole 10c1.

[0010] A support 20p extending vertically upward from the bottom surface 20b is disposed in the center of the hole 20h. The support 20p is a cylinder having a central axis CA as a center axis, and has a shape that is rotationally symmetrical about the central axis CA. The support 20p has a support upper surface TS. The support upper surface TS is located at the upper end of the support 20p and is a surface perpendicular to the central axis CA. The support upper surface TS is located at a position lower than the surface 20s of the forming die 20. As a result, a gap GA1 is formed between the lower surface of the quartz plate 30 and the support upper surface TS (see FIG. 1). The gap GA1 may be any value, for example, 100 to 500 μm.

[0011] The plate 10 is a stainless steel base for placing the forming die 20. The plate 10 has a function of cooling the forming die 20. A first communication hole 10c1 is formed in the surface 10s of the plate 10. The first communication hole 10c1 is disposed at a position corresponding to the through hole 20e and is connected to the through hole 20e. The first communication hole 10c1 is connected to a hole negative pressure generating means 81 via a first communication path 10p1. The hole negative pressure generating means 81 is a means capable of generating a negative pressure in the hole 20h. The hole negative pressure generating means 81 may be, for example, a vacuum pump.

[0012] The heat sink 40 is in contact with the lower surface 10r of the plate 10. A circulation pipe 41 is arranged inside the heat sink 40. The circulation pipe 41 is connected to a chiller device 42. A refrigerant that is kept at a constant temperature above room temperature by the chiller device 42 circulates through the circulation pipe 41. This allows the heat sink 40 to maintain a constant temperature during the process. The fluctuation in heat dissipation performance from the mold 20 to the plate 10 during processing of the quartz plate 30 can be suppressed. That is, the heat sink 40 is configured to be able to adjust the temperature of the mold 20 through the plate 10. This allows the reproducibility of heat transfer (exhaust heat) from the mold 20 heated by a flame to the plate 10 to be improved. Therefore, it is possible to improve the processing reproducibility of the glass vibrator regardless of environmental changes such as seasonal variations.

[0013] The heat sink 40, the plate 10, and the molding die 20 are placed on the motorized stage 45. The motorized stage 45 is configured to be movable in the x and y directions (horizontal directions).

[0014] A quartz plate 30 is disposed on the surface 20s of the mold 20 so as to cover the hole 20h. The quartz plate 30 is a material to be processed for forming a glass vibrator. The thickness of the quartz plate 30 is, for example, 100 μm or less. In this embodiment, the quartz plate 30 is circular, but it may be square, regular hexagonal, or regular octagonal.

[0015] The burner 50 is a means for heating the quartz plate 30 by a flame. The burner 50 is fixed to a movable mechanism 53 that moves in the vertical direction (±z direction). This allows the burner 50 to move up and down along the central axis CA. The burner 50 is equipped with a premixing chamber 50c. Fuel gas G1 and oxygen gas G2 are supplied to the premixing chamber 50c from a gas supply facility 51 via a gas flow regulator 52. The premixing chamber 50c allows the fuel gas G1 and oxygen gas G2 to be mixed in advance before burning, making it possible to generate a stable flame.

[0016] Radiation thermometer 60 is a non-contact thermometer. Radiation thermometer 60 is disposed above molding die 20 by a fixture (not shown). By focusing radiation thermometer 60 on support upper surface TS of support 20p, the surface temperature of support upper surface TS can be measured in a non-contact manner.

[0017] The partition 11 is disposed on the surface 10s of the plate 10 so as to surround the outer periphery of the mold 20. The partition 11 is a cylindrical wall made of stainless steel. The upper end 11u of the partition 11 is located above the surface 20s of the mold 20 (on the +z direction side). This makes it possible to block disturbances in the airflow, thereby making it possible to suppress fluctuations in the flame. The temperature distribution of the quartz plate 30 heated by the flame can be made point-symmetrical with respect to the central axis CA, making it possible to manufacture a highly symmetrical glass vibrator with good reproducibility. In addition, the partition 11 is not in contact with the mold 20. This prevents the partition 11 from functioning as a fin for cooling the mold 20.

[0018] The control unit 70 is connected to the hole negative pressure generating means 81, the movable mechanism 53, the gas flow regulator 52, the radiation thermometer 60, and the chiller equipment 42, and acquires various information from these devices and controls these devices. The control unit 70 may be, for example, a PC.

[0019] (Glass vibrator manufacturing process) The manufacturing process of the glass vibrator will be described using the flow diagram of Fig. 3. A timing chart is shown in Fig. 4. The vertical axis of Fig. 4(A) is the pressure in the hole 20h. The vertical axis of Fig. 4(B) is the distance between the tip 50s of the burner 50 and the surface of the quartz plate 30. The vertical axis of Fig. 4(C) is the surface temperature of the support upper surface TS.

[0020] In step S10, the control unit 70 supplies and circulates a refrigerant, whose temperature is controlled to 40° C. by the chiller equipment 42, to the circulation pipes 41 of the heat sink 40. In step S20, the forming die 20 is placed on the front surface 10s of the plate 10.

[0021] In step S30, quartz plate 30 is placed on surface 20s of mold 20. At this time, it is positioned so that central axis CA coincides with the center of quartz plate 30. A gap GA1 exists between the lower surface of quartz plate 30 and upper surface TS of the support. In step S35, partition 11 is placed on surface 10s of plate 10.

[0022] In step S40, the control unit 70 operates the hole negative pressure generating means 81 (see time t1 in FIG. 4). This causes the hole 20h to be subjected to a first negative pressure NP1 via the first communication hole 10c1 and the through hole 20e. In this embodiment, the first negative pressure NP1 is set to a negative pressure of 10 kPa. In step S50, the control unit 70 starts measuring the temperature of the pillar upper surface TS of the pillar 20p using the radiation thermometer 60.

[0023] In step S60, the control unit 70 ignites the burner 50 (see FIG. 4, time t2). Specifically, the flow rates of the fuel gas G1 and oxygen gas G2 provided from the gas supply equipment 51 are controlled by the gas flow regulator 52. Then, the process waits until the flame stabilizes. In this embodiment, after ignition, the propane fuel gas G1 is adjusted to a flow rate of 1000 sccm, and the oxygen gas G2 is adjusted to a flow rate of 5000 sccm. This results in the state shown in FIG. 1. At time t2, the burner 50 is located at the initial position. The distance between the tip 50s of the burner 50 and the surface of the quartz plate 30 in the initial position is the initial distance L0 (see FIG. 1).

[0024] In step S70, the control unit 70 controls the movable mechanism 53 to lower the burner 50 at a constant speed (see time t2-t4 in FIG. 4). This causes the flame to heat the quartz plate 30. In this embodiment, the burner 50 is lowered at a speed of 50 mm / sec.

[0025] In step S80, the control unit 70 judges whether or not an instantaneous temperature rise of the support upper surface TS is detected by the radiation thermometer 60. The instantaneous temperature rise will be described. In the initial heating state, a gap GA1 is formed between the upper surface of the support 20p and the lower surface of the quartz plate 30, and they are not in contact. Therefore, no heat conduction path is formed from the quartz plate 30 to the support 20p. Therefore, the temperature distribution of the quartz plate 30 is highest in the vicinity of the support 20p at the center, and decreases as it moves away from the support 20p toward the outer periphery. Then, the center of the quartz plate 30 reaches the softening temperature first, and melting deformation begins. Therefore, as shown in FIG. 5, the center of the quartz plate 30 comes into contact with the support upper surface TS. The heat accumulated in the center of the quartz plate 30 is discharged to the support 20p by contact, so the temperature of the support upper surface TS rises instantaneously (see FIG. 4(C), region A1). Furthermore, the temperature at the center of the quartz plate 30 drops rapidly, and deformation stops near the center of the quartz plate 30. As described above, by detecting the instantaneous temperature rise on the support upper surface TS, it is possible to detect that the quartz plate 30 has started to deform.

[0026] When the start of deformation of the quartz plate 30 is detected at time t3 (S80: YES), the process proceeds to step S85. In step S85, the control unit 70 stops the descent of the burner 50 after the second predetermined time PT2 has elapsed since the start of deformation of the quartz plate 30 was detected (see FIG. 4, time t4, arrow Y1). This allows the distance between the burner 50 and the quartz plate 30 to be set to distance L2, which is closer to the deformation start distance L1 by a predetermined distance PL (see FIG. 4(B)). In this embodiment, the second predetermined time PT2 is set to 3 seconds, and the predetermined distance PL is set to 150 mm.

[0027] In step S90, the control unit 70 increases the negative pressure in the hole 20h from the first negative pressure NP1 to a more negative side after the first predetermined time PT1 has elapsed since the start of deformation of the quartz plate 30 was detected (see FIG. 4, time t5, arrow Y2). Specifically, evacuation is performed at a constant speed until the second negative pressure NP2 is reached. In this embodiment, the first predetermined time PT1 is set to 10 seconds, the second negative pressure NP2 is set to a negative pressure of 75 kPa, and evacuation is performed at a speed of 10 kPa / sec. This allows the quartz plate 30 to melt and deform so as to enter the hole 20h due to the heat input from the flame and the distributed load due to the pressure difference between the negative pressure generated in the hole 20h and the atmospheric pressure. This allows the quartz plate 30 to melt and deform into a desired shape as shown in FIG. 6.

[0028] In step S100, the control unit 70 determines whether the negative pressure in the hole 20h has reached the second negative pressure NP2 (75 kPa). If it is detected at time t6 that the negative pressure has reached the second negative pressure NP2 (S100: YES), the process proceeds to step S110.

[0029] In step S110, the control unit 70 starts to raise the burner 50 after the third predetermined time PT3 has elapsed since the second negative pressure NP2 was reached (see FIG. 4, time t7). In this embodiment, the third predetermined time PT3 is set to 10 seconds, and the rising speed of the burner 50 is set to 200 mm / sec. When the burner 50 rises to the initial position at time t8, the movement of the burner 50 is stopped and the flame is extinguished.

[0030] In step S120, the control unit 70 stops the vacuuming by the hole negative pressure generating means 81 after the fourth predetermined time PT4 has elapsed since the flame was extinguished (see FIG. 4, time t9). This causes the hole 20h to be open to the atmosphere. In this embodiment, the fourth predetermined time PT4 is set to 3 seconds. In step S130, the fused and molded quartz plate 30 is removed from the mold 20. This completes the glass vibrator.

[0031] (effect) Fluctuations in the heat input distribution caused by the burner 50 may cause variations in the temperature rise distribution of the quartz plate 30. In this case, melting and forming will start from the part where the softening temperature is locally reached. As a result, the shape of the glass vibrator will become asymmetric. According to the technology of this embodiment, the quartz plate 30 can be adsorbed and fixed to the surface 20s of the mold 20 by the first negative pressure NP1 (step S40). Then, the quartz plate 30 is deformed by the heating process and comes into contact with the upper surface TS of the support, and this can be detected by the instantaneous temperature rise of the upper surface TS of the support (step S80). At this time, since the first negative pressure NP1, which is smaller than the second negative pressure NP2, is used, even if a part where the softening temperature is locally reached occurs, the start of melting and deformation can be suppressed. This makes it possible to heat the entire processing area of ​​the quartz plate 30 without starting deformation. Then, by uniformly heating the quartz plate 30 to the softening temperature in a concentric circle centered on the support 20p, the second negative pressure NP2 can be applied to start melting and deformation uniformly over the entire processing area. Melting deformation can be started simultaneously at any location of the quartz plate 30 above the hole 20h. Therefore, a glass vibrator having a highly symmetric shape with respect to the central axis CA can be processed with high reproducibility. The glass vibrator having a highly symmetric shape manufactured by this technology has a high Q value with little vibration loss, making it possible to manufacture a high-precision gyro sensor.

[0032] In the fusion molding of glass vibrators, there are variations in various manufacturing parameters. For example, there are variations in the amount of heat input due to the fluctuation of the flame, variations in the thickness of the quartz plate 30 within the surface and between lots, and environmental variations (temperature, humidity). Due to the influence of these manufacturing parameter variations, the temperature distribution and temperature rise gradient of the quartz plate 30 also vary, which causes a problem of low reproducibility of the processed shape of the glass vibrator. In the technology of this embodiment, the deformation start time of the quartz plate 30 can be detected by detecting the instantaneous temperature rise of the support upper surface TS (step S80). That is, even if the manufacturing parameters vary, the time when a certain state, namely the start of deformation, occurs can be detected. And, since the heating time and the amount of heat input can be controlled based on the deformation start time, the influence of the variation of the manufacturing parameters can be suppressed. It is possible to improve the reproducibility of the processed shape of the glass vibrator.

[0033] The pressure in the hole 20h can be maintained at the first negative pressure NP1 until the first predetermined time PT1 (10 seconds) has elapsed since the start of deformation of the quartz plate 30 was detected (step S90). This allows the quartz plate 30 to be heated without being deformed during the first predetermined time PT1. This allows the quartz plate 30 to be uniformly heated in a concentric circle around the support 20p.

[0034] The lowered state of the burner 50 can be maintained until the second predetermined time PT2 (3 seconds) has elapsed since the start of deformation of the quartz plate 30 was detected (step S85). The longer the second predetermined time PT2 is, the smaller the distance between the burner 50 and the quartz plate 30 can be, and therefore the greater the amount of heat input to the quartz plate 30 can be. As a result, the amount of downward deformation of the quartz plate 30 can be increased, and therefore the height of the completed glass vibrator can be increased. EXAMPLES

[0035] In the second embodiment, various modifications of the timing at which the lowering of the burner 50 is stopped (step S85) and the timing at which the first negative pressure NP1 is made further negative (step S90) will be described.

[0036] FIG. 7 shows a timing chart of the first modified example. The contents of FIG. 7 are the same as those of FIG. 4 of the first embodiment. The same parts are given the same reference numerals and the explanation is omitted. In the first modified example, immediately after detecting an instantaneous temperature rise of the support upper surface TS (S80), the descent of the burner 50 is stopped (S85) (see arrow Y11). At the same time, the negative pressure in the hole 20h is increased from the first negative pressure NP1 to a more negative side (S90) (see arrow Y12). This also makes it possible to improve the reproducibility of the processed shape of the glass vibrator.

[0037] 8 shows a timing chart of the second modified example. In the second modified example, immediately after detecting an instantaneous temperature rise on the support upper surface TS (S80), the descent of the burner 50 is stopped (S85) (see arrow Y21). Then, after a first predetermined time PT1 has elapsed since detecting the temperature rise (S80), the negative pressure in the hole 20h is increased from the first negative pressure NP1 to a more negative pressure (S90) (see arrow Y22). This allows the quartz plate 30 to be heated without being deformed during the first predetermined time PT1.

[0038] 9 shows a timing chart of the third modified example. In the third modified example, immediately after detecting an instantaneous temperature rise on the support upper surface TS (S80), the negative pressure in the hole 20h is increased from the first negative pressure NP1 to a more negative pressure (S90) (see arrow Y32). Then, after a second predetermined time PT2 has elapsed since the temperature rise was detected (S80), the descent of the burner 50 is stopped (S85) (see arrow Y31). This allows the amount of heat input to the quartz plate 30 to be increased. EXAMPLES

[0039] When the start of deformation of the quartz plate 30 is detected in step S80 (S80: YES), the control unit 70 controls the gas flow regulator 52. This makes it possible to change the flow rates of the fuel gas G1 and the oxygen gas G2.

[0040] When the flow rate of the fuel gas G1 or the oxygen gas G2 is reduced, the heating power can be reduced. Since the amount of heat input can be reduced, the deformation speed of the quartz plate 30 can be reduced. Therefore, the processing symmetry of the glass vibrator can be improved.

[0041] In addition, when the flow rate of the fuel gas G1 or the oxygen gas G2 is increased, the heating power can be increased. Since the amount of heat input can be increased, it is possible to increase the deformation speed of the quartz plate 30. Therefore, it is possible to improve the reproducibility of the processed shape of the glass vibrator.

[0042] Although specific examples of the present invention have been described above in detail, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and variations of the specific examples exemplified above. Furthermore, the technical elements described in this specification or drawings exhibit technical utility alone or in various combinations, and are not limited to the combinations described in the claims at the time of filing. Furthermore, the technology exemplified in this specification or drawings can achieve multiple objectives simultaneously, and achieving one of these objectives is itself technically useful.

[0043] (Modification) The material of the vibrator is not limited to the quartz plate 30. It may be borosilicate glass, which is quartz mixed with sodium or the like, or other glass materials.

[0044] Aspects of the present technology are listed below. [Aspect 1] A method for manufacturing a glass vibrator using a fusion molding mold, comprising the steps of: The melt molding die includes a flat surface, a hole formed in a part of the surface, and a support extending upward from a bottom surface of the hole, The upper surface of the support is located lower than the surface of the melt-molding mold, The manufacturing method of the glass vibrator is as follows: a placement step of placing a plate-shaped workpiece material on the surface of the melt-molding mold so as to cover the hole and be spaced apart from the upper surface of the support; a first negative pressure generating step of generating a first negative pressure in the hole; a heating step of heating the upper surface of the workpiece by a heating means after the first negative pressure generating step; a detection step of detecting an instantaneous temperature rise on the upper surface of the support caused by the workpiece being deformed by the heating step and coming into contact with the upper surface of the support; a second negative pressure generating step of increasing the negative pressure in the hole from the first negative pressure to a further negative pressure in response to the detection of the temperature increase; A method for manufacturing a glass vibrator comprising the steps of: [Aspect 2] 2. The method for manufacturing a glass vibrator according to claim 1, wherein the second negative pressure generating step is performed immediately after the temperature increase is detected or after a first predetermined time has elapsed since the temperature increase is detected. [Aspect 3] In the heating step, the heating means is brought closer to the support at a predetermined speed, 3. The method for manufacturing a glass vibrator according to aspect 1 or 2, further comprising the step of stopping the movement of the heating means immediately after the temperature increase is detected or after a second predetermined time has elapsed since the temperature increase was detected. [Aspect 4] The heating means is a device that generates a flame using a fuel gas, The method for manufacturing a glass vibrator according to any one of aspects 1 to 3, further comprising the step of changing an amount of the fuel gas supplied in response to detection of the temperature increase. [Aspect 5] A melt-molding mold including a flat surface, a hole formed in a part of the surface, and a support extending upward from a bottom surface of the hole, the support upper surface of the support being located at a position lower than the surface, and a plate-shaped workpiece material being able to be placed on the surface so as to cover the hole and be spaced apart from the support upper surface; A thermometer configured to be able to measure the temperature of the upper surface of the support; a heating means configured to be capable of heating the hole portion in a state in which the workpiece is placed; and a hole negative pressure generating means configured to generate a negative pressure in the hole when the workpiece is placed therein; A melt molding apparatus comprising: the thermometer is configured to be capable of detecting an instantaneous temperature rise on the upper surface of the support caused by the workpiece being deformed by the heating means and coming into contact with the upper surface of the support; The hole negative pressure generating means is configured to be able to further increase the negative pressure in the hole in response to the temperature rise being detected by the thermometer. Melt molding equipment. [Aspect 6] The melt molding apparatus of aspect 5, wherein the hole negative pressure generating means is configured to be able to further increase the negative pressure in the hole to the negative side immediately after the temperature rise is detected by the thermometer or after a first predetermined time has elapsed since the temperature rise was detected by the thermometer. [Aspect 7] The heating means is configured to be movable at a predetermined speed in a direction approaching the support, The melt molding apparatus according to aspect 5 or 6, wherein the heating means is configured to be capable of stopping movement immediately after the temperature increase is detected by the thermometer or after a second predetermined time has elapsed since the temperature increase was detected by the thermometer. [Aspect 8] The heating means is a device that generates a flame using a fuel gas, The melt molding apparatus according to any one of aspects 5 to 7, wherein the heating means is configured to be capable of changing the supply amount of the fuel gas in response to a temperature increase detected by the thermometer. [Aspect 9] Further comprising a wall portion surrounding the outer periphery of the melt molding mold; A melt-molding apparatus according to any one of aspects 5-8, wherein an upper end of the wall portion is located above the surface of the melt-molding mold. [Aspect 10] The melt-molding apparatus according to any one of aspects 5 to 9, further comprising a heat sink arranged on the back side of the melt-molding mold and configured to be capable of maintaining a constant temperature. [Explanation of symbols]

[0045] 1: Melt forming device 10: Plate 20: Mold 20h: Hole 20p: Support 30: Quartz plate 50: Burner 60: Radiation thermometer 70: Control unit 81: Hole negative pressure generating means TS Support upper surface

Claims

1. A method for manufacturing a glass vibrator using a fusion molding mold, comprising the steps of: The melt molding die includes a flat surface, a hole formed in a part of the surface, and a support extending upward from a bottom surface of the hole, The upper surface of the support is located lower than the surface of the melt-molding mold, The manufacturing method of the glass vibrator is as follows: a placement step of placing a plate-shaped workpiece material on the surface of the melt-molding mold so as to cover the hole and be spaced apart from the upper surface of the support; a first negative pressure generating step of generating a first negative pressure in the hole; a heating step of heating an upper surface of the workpiece by a heating means after the first negative pressure generating step; a detection step of detecting an instantaneous temperature rise on the upper surface of the support caused by the workpiece being deformed by the heating step and coming into contact with the upper surface of the support; a second negative pressure generating step of increasing the negative pressure in the hole from the first negative pressure to a further negative pressure in response to the detection of the temperature increase; A method for manufacturing a glass vibrator comprising the steps of:

2. 2. The method for manufacturing a glass vibrator according to claim 1, wherein the second negative pressure generating step is performed immediately after the temperature increase is detected or after a first predetermined time has elapsed since the temperature increase is detected.

3. In the heating step, the heating means is brought closer to the support at a predetermined speed, 2. The method for manufacturing a glass vibrator according to claim 1, further comprising the step of stopping the movement of the heating means immediately after the temperature increase is detected or after a second predetermined time has elapsed since the temperature increase was detected.

4. The heating means is a device that generates a flame using a fuel gas, The method for manufacturing a glass vibrator according to claim 1 , further comprising the step of changing an amount of the fuel gas supplied in response to the detection of the temperature increase.

5. A melt-molding mold including a flat surface, a hole formed in a part of the surface, and a support extending upward from a bottom surface of the hole, the support upper surface of the support being located at a position lower than the surface, and a plate-shaped workpiece material being able to be placed on the surface so as to cover the hole and be spaced apart from the support upper surface; A thermometer configured to be able to measure the temperature of the upper surface of the support; a heating means configured to be capable of heating the hole portion in a state in which the workpiece is placed; and a hole negative pressure generating means configured to generate a negative pressure in the hole when the workpiece is placed therein; A melt molding apparatus comprising: the thermometer is configured to be capable of detecting an instantaneous temperature rise on the upper surface of the support caused by the workpiece being deformed by the heating means and coming into contact with the upper surface of the support; The hole negative pressure generating means is configured to be able to further increase the negative pressure in the hole in response to the temperature rise being detected by the thermometer. Melt molding equipment.

6. The melt molding device of claim 5, wherein the hole negative pressure generating means is configured to be able to further increase the negative pressure in the hole to the negative side immediately after the temperature rise is detected by the thermometer or after a first predetermined time has elapsed since the temperature rise was detected by the thermometer.

7. The heating means is configured to be movable at a predetermined speed in a direction approaching the support, The melt molding device according to claim 5, wherein the heating means is configured to be capable of stopping movement immediately after the temperature increase is detected by the thermometer or after a second predetermined time has elapsed since the temperature increase is detected by the thermometer.

8. The heating means is a device that generates a flame using a fuel gas, 6. The melt molding apparatus according to claim 5, wherein the heating means is configured to be able to change the supply amount of the fuel gas in response to a temperature rise detected by the thermometer.

9. Further comprising a wall portion surrounding the outer periphery of the melt molding mold; The melt-molding apparatus according to claim 5 , wherein an upper end of the wall portion is located above the surface of the melt-molding mold.

10. The melt-molding apparatus according to claim 5 , further comprising a heat sink arranged on a rear side of the melt-molding mold and configured to be capable of maintaining a constant temperature.

Citation Information

Patent Citations

  • Thermal Control Mold For Making Three-Dimensional Microstructures

    US20180079129A1