Workpiece processing method

By applying an adhesive tape to the outer periphery of a workpiece with height differences, the method ensures uniform contact during back grinding, reducing TTV and preventing cracking.

JP2024136169APending Publication Date: 2024-10-04LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023047181
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

The height difference between the outer and inner peripheries of a workpiece due to protruding bump electrodes or chips causes suction errors during back grinding, leading to increased Total Thickness Variation (TTV) and potential cracking or processing issues.

Method used

A method involving the use of a surface protection sheet with an adhesive tape attached to suppress the height difference by ensuring uniform contact with the grinding table, comprising a base material and adhesive layer, with the adhesive tape applied to the outer periphery where the height is lower.

Benefits of technology

Reduces TTV of the workpiece by maintaining uniform thickness post-grinding, minimizing cracking and processing issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136169000001_ABST
    Figure 2024136169000001_ABST
Patent Text Reader

Abstract

To provide a workpiece processing method capable of reducing a TTV of a workpiece such as a wafer.SOLUTION: In a workpiece including a front surface having height difference and a rear surface opposite to the front surface and on which an adhesive tape for suppressing an influence of the height difference of the front surface is stuck, a workpiece processing method includes the steps of: sticking a surface protective sheet to the front surface of the workpiece; and grinding the rear surface of the workpiece to which the surface protective sheet is stuck.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for machining a workpiece, and more particularly to a method for machining a workpiece that can reduce the TTV of the workpiece after back surface grinding, even if the workpiece has a surface with height differences. [Background technology]

[0002] A known method for mounting chips with circuits, such as semiconductor chips, at a high density is to bond the chip to electrodes on a substrate via bump electrodes formed on the circuit surface of the chip. The bump electrodes are convex electrodes that protrude in the thickness direction of the chip.

[0003] Such chips are obtained as workpieces by dividing a workpiece such as a wafer on which a circuit is formed. With the rapid progress of miniaturization and multi-functionalization of electronic devices on which such chips are mounted, there is a demand for chips to be smaller, thinner, and more dense. In order to reduce the size and height of a chip, it is common to form a circuit on the front surface of a wafer, and then grind the back surface of the wafer to reduce the thickness of the chip.

[0004] Another known method for mounting chips at high density is the use of chip-on-wafer (CoW), in which multiple chips smaller than the wafer are arranged on the circuit surface of a wafer to obtain a chip-on-wafer, and then the chip-on-wafer is diced to obtain stacked chips.

[0005] Even in the method using chip-on-wafer, in order to reduce the size and height of the stacked chips, it is common to grind the back surface of the wafer as a workpiece to reduce the thickness of the wafer (workpiece), and then place the chip on the wafer (workpiece).

[0006] When grinding the back surface of a workpiece, a surface protection sheet called a backgrind tape is applied to the surface of the workpiece to protect the circuits and chips arranged on the surface of the workpiece and to hold the workpiece.

[0007] Patent Document 1 discloses an adhesive tape for processing semiconductor wafers that has good conformability to the surface of semiconductor wafers having steps and protrusions and can be peeled off without damaging the semiconductor wafer or leaving any adhesive residue. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2017-171896 A Summary of the Invention [Problem to be solved by the invention]

[0009] The bump electrodes are formed to protrude from the surface of the workpiece. Also, in a chip-on-wafer, the chips arranged on the surface of the workpiece protrude from the surface of the wafer (workpiece). Therefore, on the surface of the workpiece, there is a difference in height between the area where the bump electrodes are formed or the area where the chips are arranged and the other areas.

[0010] The height difference between the outer periphery and the inner periphery of the workpiece on the surface of the workpiece is reflected as a height difference in the surface protection sheet by attaching the surface protection sheet. That is, in the thickness direction of the workpiece, the height of the surface protection sheet is low in the area corresponding to the outer periphery of the workpiece, and the height of the surface protection sheet is high in the area corresponding to the inner periphery of the workpiece.

[0011] When grinding the backside of a workpiece with a surface protection sheet attached, the surface (front side) of the workpiece to which the surface protection sheet is attached is usually placed on a grinding table such as a chuck table and fixed by suction, etc. When the workpiece is placed on the table, the height of the surface protection sheet in the area corresponding to the outer periphery of the workpiece is lower than the height of the area corresponding to the inner periphery of the workpiece, so when the workpiece is placed on the grinding table, the outer periphery of the workpiece and the grinding table are not in sufficient contact with each other, resulting in a gap or the like, which may cause a suction error.

[0012] Also, if the workpiece can be adsorbed, when the workpiece is adsorbed in this state, the outer periphery of the workpiece drops toward the grinding table together with the surface protection sheet and is fixed there. Then, the back surface grinding is performed. When the adsorption is released after the back surface grinding is completed, the outer periphery of the workpiece is released and floats up from the grinding table. In the back surface grinding, the back surface of the workpiece is ground to approximately the same height, but when the outer periphery of the workpiece floats up, the thickness of the outer periphery of the workpiece becomes thicker than the thickness of the inner periphery of the workpiece by the amount of the drop during adsorption. The difference between the thickness of the outer periphery of the workpiece and the thickness of the inner periphery of the workpiece is reflected in the TTV (Total Thickness Variation) of the workpiece, and the TTV of the workpiece tends to be large. If the TTV of the workpiece is large, there are problems such as the workpiece being more likely to crack and problems occurring when the workpiece is divided into individual pieces, so it is preferable that the TTV of the workpiece is small.

[0013] In Patent Document 1, bumps are taken into consideration as steps or protrusions, and the problem of the height difference between the outer and inner peripheries of the wafer is not taken into consideration, so when the adhesive tape for semiconductor wafer processing described in Patent Document 1 is applied to a wafer, a height difference occurs between the inner and outer peripheries of the wafer. As a result, there is a problem that cracks are likely to occur during backgrinding, or even if no cracks occur, the TTV of the semiconductor wafer after backgrinding becomes large.

[0014] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for machining a workpiece that can reduce the TTV of the workpiece, such as a wafer. [Means for solving the problem]

[0015] The aspects of the present invention are as follows.

[0016] [1] A workpiece having a surface having a height difference and a back surface opposite to the surface, and an adhesive tape for suppressing the effect of the height difference on the surface, comprising: a step of attaching a surface protective sheet to the surface; and grinding the back surface of the workpiece to which the surface protection sheet is attached.

[0017] [2] A method for processing a workpiece according to [1], wherein the adhesive tape has a substrate and an adhesive layer.

[0018] [3] A method for processing a workpiece according to [2], in which the adhesive layer is formed on only one of the main surfaces of the substrate.

[0019] [4] A method for processing a workpiece described in any of [1] to [3], wherein the surface has an inner circumference and an outer circumference surrounding the inner circumference, the height of the outer circumference is lower than the height of the inner circumference, and an adhesive tape is attached onto the outer circumference.

[0020] [5] A method for machining a workpiece according to any one of [1] to [4], wherein the workpiece has a convex electrode formed on its surface.

[0021] [6] A method for processing a workpiece according to any one of [1] to [5], wherein the surface protection sheet has a substrate and an adhesive layer.

[0022] [7] A process for forming a groove on the surface of the workpiece before the process for attaching a surface protective sheet to the surface of the workpiece, A method for processing a workpiece according to any one of [1] to [6], wherein in a process of grinding the back surface of the workpiece, the workpiece is diced into a plurality of workpiece pieces starting from the grooves.

[0023] [8] A process for forming a modified region inside the workpiece before the process for grinding the back surface of the workpiece, A method for processing a workpiece according to any one of [1] to [7], wherein in a step of grinding the back surface of the workpiece, the workpiece is diced into a plurality of workpiece pieces starting from the modified region. Effect of the Invention

[0024] According to the present invention, it is possible to provide a method for processing a workpiece, which can reduce the TTV of the workpiece, such as a wafer. [Brief description of the drawings]

[0025] [Figure 1A] FIG. 1A is a schematic cross-sectional view of a workpiece having a height difference on its surface, in which a convex electrode is formed on the surface of the workpiece. [Figure 1B] FIG. 1B is a schematic cross-sectional view of a chip-on-wafer as a workpiece having height differences on its surface. [Figure 1C] FIG. 1C is a schematic cross-sectional view of a half-trim wafer as a workpiece having height differences on its surface. [Diagram 2] 2(A) to 2(E) are schematic cross-sectional views for explaining that the TTV of a workpiece increases when the workpiece is machined by a conventional method. [Figure 3A] FIG. 3A is a schematic plan view of a workpiece having a convex electrode with an adhesive tape attached to its outer periphery in the method for machining the workpiece according to the present embodiment. [Figure 3B] FIG. 3B is a schematic cross-sectional view taken along line IIIB-IIIB in FIG. 3A. [Figure 3C] FIG. 3C is a schematic cross-sectional view of an adhesive tape that is preferably used in the method for processing a workpiece according to this embodiment. [Figure 4A] FIG. 4A is a schematic cross-sectional view of a surface protection sheet that is preferably used in the workpiece processing method according to this embodiment. [Figure 4B] FIG. 4B is a schematic cross-sectional view showing another example of a surface protection sheet that is preferably used in the workpiece processing method according to this embodiment. [Figure 4C] FIG. 4C is a schematic cross-sectional view showing another example of a surface protection sheet that is preferably used in the workpiece processing method according to this embodiment. [Diagram 5] 5(A) to (C) are schematic cross-sectional views for explaining that the TTV of a workpiece is reduced when the workpiece is machined by the method according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings based on specific embodiments. First, the main terms used in this specification will be explained.

[0027] The work refers to a plate-like body to which a surface protection sheet is attached and then cut into individual pieces. Examples of the work include a circular wafer (including a case having an orientation flat), a rectangular panel level package, and a strip (rectangular substrate) sealed with molded resin. Among them, a wafer is preferable from the viewpoint of easily obtaining the effect of the present invention. The wafer may be, for example, a semiconductor wafer such as a silicon wafer, a gallium arsenide wafer, a silicon carbide wafer, a gallium nitride wafer, or an indium phosphide wafer, or an insulating wafer such as a glass wafer, a lithium tantalate wafer, or a lithium niobate wafer, or may be a reconstructed wafer made of a resin and a semiconductor used for producing a fan-out package or the like. From the viewpoint of easily obtaining the effect of the present invention, a semiconductor wafer or an insulating wafer is preferable, and a semiconductor wafer is more preferable.

[0028] Singulation of a work refers to dividing the work into individual circuits to obtain individual work pieces. For example, if the work is a wafer, the individual work pieces are chips, and if the work is a panel level package or a strip (rectangular substrate) sealed with molded resin, the individual work pieces are semiconductor packages.

[0029] The "front surface" of a workpiece refers to the side on which a circuit or the like is formed or on which the formation of a circuit or the like is planned, and the "back surface" of a workpiece refers to the side on which a circuit or the like is not formed or on which the formation of a circuit or the like is not planned.

[0030] DBG is a method in which a groove of a specified depth is formed on the front side of a workpiece, and then the workpiece is ground from the back side to separate the workpiece by grinding. The grooves formed on the front side of the workpiece are formed by methods such as blade dicing, laser dicing, and plasma dicing.

[0031] LDBG is a modified version of DBG, in which a modified region is created inside the workpiece using a laser, and the workpiece is divided into individual pieces by the stress generated when grinding the back surface of the workpiece.

[0032] The term "group of individual workpieces" refers to a plurality of individual workpieces held on the surface protection sheet of the present invention after the workpiece is singulated. These individual workpieces, as a whole, form a shape similar to that of the workpiece. The term "group of chips" refers to a plurality of chips held on the surface protection sheet of the present invention after the wafer as the workpiece is singulated. These chips, as a whole, form a shape similar to that of the wafer.

[0033] "(Meth)acrylate" is used as the term to refer to both "acrylate" and "methacrylate," and similar terms.

[0034] The term "energy rays" refers to ultraviolet rays, electron beams, etc., and is preferably ultraviolet rays.

[0035] Unless otherwise specified, the "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC). Measurements by such a method are performed, for example, using a high-speed GPC device "HLC-8120GPC" manufactured by Tosoh Corporation with a high-speed column "TSK guard column H XL -H", "TSK Gel GMH XL", "TSK Gel G2000 H XL (All of the above are manufactured by Tosoh Corporation) connected in the above order, the column temperature was 40° C., the liquid flow rate was 1.0 mL / min, and the detector was a differential refractometer.

[0036] The release sheet is a sheet that supports the pressure-sensitive adhesive layer in a releasable manner. The term "sheet" is not limited to a specific thickness, and is used to include a film.

[0037] The mass ratios in the explanations of compositions such as the pressure-sensitive adhesive layer composition are based on the active ingredient (solid content), and do not include the solvent unless otherwise specified.

[0038] (1. Workpiece machining method) The workpiece machined by the method according to the present embodiment is a workpiece having height differences on its surface. Examples of such workpieces include a workpiece having a convex electrode (such as a bump electrode or a pillar electrode) formed on its surface, a chip-on-wafer (CoW) having a chip disposed on its surface, and a half-trim wafer having a part of the edge of the workpiece removed.

[0039] As shown in Fig. 1A, the workpiece with a convex electrode is a workpiece with a convex electrode 2a formed on its surface for electrically connecting a circuit formed on the surface 1a of the workpiece 1 to a substrate or the like. The convex electrode 2a is formed to protrude in the thickness direction of the workpiece. Therefore, there is a height difference D between the tip of the convex electrode and an area on the workpiece where the convex electrode is not formed.

[0040] Chip-on-wafer is used to improve the performance and density of electronic devices. As shown in FIG. 1B, chip-on-wafer is a wafer in which a plurality of chips 2b, smaller in size than the wafer 1, are arranged on the inner periphery of a plate-like body such as a wafer 1. The chip-on-wafer is then diced to form a plurality of high-density stacked packages. The chips 2b are stacked on the surface 1a of the work. Therefore, there is a height difference D between the top surface of the chip and the area on the wafer where the chip is not arranged.

[0041] Half-trim wafers are used to prevent damage to the wafer. Specifically, a half-trim wafer is a wafer in which a part of the front side of the edge of the wafer is removed by trimming in order to prevent chipping, which may cause damage to the wafer, from occurring at the edge of the wafer during back grinding. Therefore, as shown in FIG. 1C, there is a height difference D between the removed area (edge) and the unremoved area of ​​the wafer 1.

[0042] 1A to 1C, the height difference D of the surface 1a corresponds to the height difference between the inner peripheral part and the outer peripheral part of the work (wafer) 1, and the inner peripheral part is surrounded by the outer peripheral part. Therefore, in this embodiment, the height difference of the surface is formed by the inner peripheral part and the outer peripheral part surrounding the inner peripheral part, and it is preferable that the height of the outer peripheral part is lower than the height of the inner peripheral part.

[0043] In the case of a workpiece having a convex electrode, the convex electrodes are formed at a predetermined interval. Therefore, even in the inner peripheral portion, there is a region between the convex electrodes that is approximately the same height as the region (outer peripheral portion) where no convex electrode is formed. However, the height of this region is not the height of the inner peripheral portion, but the height to the tip of the convex electrode is the height of the inner peripheral portion.

[0044] Also, in the case of chip-on-wafer, the chips are usually arranged at a predetermined interval. Therefore, even in the inner periphery, there are areas (usually lattice-shaped areas) between the chips where no chips are arranged, and the height of this area is almost the same as the height of the outer periphery. However, the height of this area is not the height of the inner periphery, but the height of the chip becomes the height of the inner periphery.

[0045] In the case of a half-trim wafer, the outer periphery is the area that has been removed by trimming, and the inner periphery is the area that has not been removed by trimming. Usually, the inner periphery has a uniform height, so that height is the height of the inner periphery.

[0046] As one example of processing a workpiece having circuits or the like formed on one surface (front surface) and no circuits or the like formed on the other surface (back surface), back grinding of the workpiece is exemplified. Back grinding of the workpiece can realize thinning of the individual workpieces obtained by dividing the workpiece. In back grinding of the workpiece, contamination of the circuits or the like due to infiltration of abrasives, cooling water, etc. into the workpiece surface, and damage to the circuits or the like due to the force applied during back grinding may occur, so it is useful to attach a surface protection sheet to protect the workpiece surface.

[0047] However, when a surface protection sheet is attached to the surface of a workpiece having a height difference, for example, the surface of a workpiece on which a convex electrode is formed, as shown in Figure 2 (A), the surface protection sheet 20 follows the shape of the surface 1a and the convex electrode 2a, so that the height difference D is reflected in the surface protection sheet 20, and a height difference occurs in the surface protection sheet 20.

[0048] 2B, when the wafer is subjected to back grinding in a state where a height difference occurs in the surface protection sheet, the front side of the wafer, i.e., the surface protection sheet 20, is placed so as to be in contact with the chuck table 100, and the wafer 1 and the surface protection sheet 20 are fixed to the chuck table 100, for example, by suction. At this time, the surface protection sheet 20 present on the convex electrode 2a is in contact with the chuck table 100 when placed on the chuck table 100, but the surface protection sheet 20 present on the area where the convex electrode 2a is not formed, i.e., on the outer periphery of the wafer 1, may not be in sufficient contact with the chuck table 100 or a gap C may be generated between the chuck table 100 and the surface protection sheet 20 when placed on the chuck table 100 due to the height difference.

[0049] When suction is performed in this state, as shown in Fig. 2(C), the surface protection sheet 20 present on the outer periphery of the wafer 1 is deformed by suction and drops toward the chuck table 100 and is fixed there, as shown in Fig. 2(C). Since the outer periphery of the wafer 1 is in close contact with the surface protection sheet 20, the outer periphery of the wafer 1 also deforms as the surface protection sheet 20 deforms. In other words, the outer periphery of the wafer 1 is fixed at a position closer to the chuck table 100 than the inner periphery of the wafer 1 (the region where the convex electrode 2a is formed).

[0050] After the wafer 1 and the surface protection sheet 20 are fixed to the chuck table 100, the back surface 1b of the wafer 1 is ground. The wafer after grinding is shown in FIG. 2(D). Since the back surface of the wafer is ground to approximately the same height, as shown in FIG. 2(D), the thickness of the outer peripheral portion of the wafer 1 is thicker than the thickness of the inner peripheral portion of the wafer 1 by the amount that the outer peripheral portion of the wafer 1 was fixed at a position closer to the chuck table 100. As a result, when the suction is released, the deformation of the surface protection sheet 10 is released as shown in FIG. 2(E), and the height difference between the inner peripheral portion of the wafer 1 and the outer peripheral portion of the wafer 1 becomes apparent. Therefore, in this case, the thickness of the outer peripheral portion of the wafer 1 tends to be the maximum value of the thickness of the wafer 1, and the thickness of the inner peripheral portion of the wafer 1 tends to be the minimum value of the thickness of the wafer 1.

[0051] The difference between the maximum thickness of the wafer and the minimum thickness of the wafer is called TTV (Total Thickness Variation), and the TTV becomes large due to the above-mentioned height difference. If the TTV becomes large, problems such as the wafer being easily cracked and defects occurring during wafer dicing may occur. In other words, the height difference D on the wafer surface that exists when the surface protection sheet is attached may affect the TTV of the wafer after back grinding.

[0052] The inventors have found that by adopting the following method, the above-mentioned height difference can be reduced, and as a result, a workpiece with a small TTV can be obtained. The method for machining a workpiece according to this embodiment will be described in detail below.

[0053] The method for machining a workpiece according to this embodiment includes at least the following steps 1 and 2. Step 1: A step of attaching a surface protection sheet to a workpiece having a surface with a height difference and a back surface opposite the surface, the workpiece having an adhesive tape attached to the surface to suppress the effect of the height difference on the surface. Process 2: Grinding the back surface of the workpiece with the surface protection sheet attached

[0054] In the following, in the workpiece machining method including the above-mentioned steps 1 and 2, a case will be described in which the workpiece is a wafer on which convex electrodes are formed, and the workpiece singulated objects are chips.

[0055] (1.1.Process 1) In step 1, a surface protection sheet is attached to the surface of the wafer. In this embodiment, as shown in Figures 3A and 3B, before the surface protection sheet is attached to the surface, an adhesive tape 3 is attached onto the surface 1a (step A). ​​That is, step A is performed before step 1.

[0056] (1.2. Adhesive tape) The adhesive tape 3 is not particularly limited as long as it is configured to exert adhesiveness and be fixed on the surface 1a of the wafer 1. As a method for suppressing the influence of the height difference, it is possible to form components having a predetermined height on the surface. Such components need to be formed according to the height difference. For example, when a fluid substance is applied to the surface and cured to form the components, the height, shape, etc. of the components can be changed according to the height difference, but there is a problem that the application process and the curing process are required, and the number of required processes increases. In addition, there is a risk that the applied substance will flow out from the predetermined application position and cause contamination of the circuits, etc. formed on the surface.

[0057] In contrast, when adhesive tape is used as a component for suppressing the effect of height difference as in the present embodiment, the tape is simply applied to a predetermined position on the surface, and the time required for application can be shortened. Furthermore, after application, the tape is fixed in place, so contamination of circuits, etc. can be suppressed.

[0058] In this embodiment, as shown in Figures 3A and 3B, the adhesive tape 3 is applied to an area where the convex electrodes 2a are not formed. That is, the adhesive tape 3 is applied to an area (outer periphery) that is lower in height than the inner periphery (area where the convex electrodes 2a are formed) of the wafer. In addition, the adhesive tape 3 is preferably applied to the front surface 1a of the wafer 1 such that the shortest distance between the adhesive tape 3 and the circuit surface (shown as L in Figure 3A) is 0.5 mm or more.

[0059] Since such adhesive tape 3 is formed on the outer periphery, the adhesive tape 3 can have a predetermined height on the surface 1a. Therefore, when the surface protection sheet 10 is attached to the surface 1a of the wafer 1, in addition to the portion corresponding to the region where the convex electrode 2a is formed, the portion corresponding to the adhesive tape 3 will also be elevated. As a result, the height difference between the region where the convex electrode 2a is formed (the inner periphery of the wafer) and the region where it is not formed (the outer periphery of the wafer) is suppressed. Therefore, the height difference on the surface of the wafer that exists when the surface protection sheet is attached is suppressed, and problems caused by the height difference are also suppressed.

[0060] In this embodiment, the thickness (height) of the adhesive tape may be set to a thickness that can suppress the effects of differences in height on the surface. When the workpiece is a wafer on which a convex electrode is formed, it is preferable to set the thickness of the adhesive tape according to the height of the convex electrode. Specifically, when the thickness of the adhesive tape is H1 and the height of the convex electrode is Hb, H1 is set to Hb / 8

[0061] In addition, when the workpiece is a chip-on-wafer or a half-trim wafer, it is preferable to set the thickness of the adhesive tape according to the difference in height between the inner circumference and the outer circumference of the wafer surface. Specifically, when the thickness of the adhesive tape is H1 and the difference in height between the inner circumference and the outer circumference is Hd, H1 is expressed as Hd / 1.2

[0062] ​​The reason why H1 differs depending on the type of workpiece is presumed to be, for example, the following reasons. When comparing the convex electrode and the chip constituting the chip-on-wafer, the chip occupies a larger area and volume of the unevenness on the wafer than the convex electrode. In other words, the chip is arranged more densely on the wafer than the convex electrode. Therefore, even if the convex electrode and the chip form unevenness of the same height, the chip is more likely to lift up the surface protection sheet when attached than the convex electrode, especially at the inner periphery of the wafer, and cracks are more likely to occur during back grinding. As a result, H1 is controlled to the above range due to the difference in the ease of cracking.

[0063] As long as the adhesive tape is applied to an area on the surface of the wafer where the influence of the height difference can be suppressed (in this embodiment, an area lower in height than the inner circumference of the wafer), multiple adhesive tapes may be applied. That is, when the adhesive tape is viewed in plan in FIG. 3A, multiple adhesive tapes may be applied intermittently.

[0064] In the present embodiment, the adhesive tape preferably has a ring-like shape in plan view, which can reduce the time required for application compared to the case where multiple pieces of adhesive tape are applied.

[0065] Although the adhesive tape can be formed over the entire outer periphery (outside the area where the circuit and convex electrode are formed, or outside the area where the chip is formed), it is preferable to form the adhesive tape away from the circuit and convex electrode or chip, from the viewpoints of the time required for application being long and the risk of the adhesive tape coming into contact with the circuit and convex electrode, chip, etc. In other words, it is preferable for the outer periphery to include an area where the adhesive tape is not formed.

[0066] In this embodiment, the adhesive tape 3 preferably has a base material 3a and an adhesive layer 3b. The adhesive tape having such a configuration is easy to handle, and even if stress is applied during back grinding, it is easy to maintain the suppression of the height difference. In particular, when the adhesive layer is formed on both main surfaces of the base material, it is difficult to handle during application, so it is preferable that the adhesive layer 3b is formed only on one main surface of the base material 3a, as shown in FIG. 3C.

[0067] The width of the adhesive tape may be set to a width that can suppress the influence of the height difference, taking into consideration the width of the outer periphery, etc. In this embodiment, the width of the adhesive tape is preferably 0.5 mm or more and 10 mm or less.

[0068] (1.2.1. Base material) The substrate (substrate for tape) is a member that is responsible for the rigidity of the adhesive tape. As described above, the substrate only needs to have a rigidity sufficient to maintain the suppression of the height difference even when stress is applied during back grinding. In this embodiment, various resin films used as substrates for back grinding tapes are exemplified. The substrate may be made of a single-layer film made of one resin film, or may be made of a multi-layer film in which multiple resin films are laminated.

[0069] In this embodiment, examples of the material of the substrate include polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, wholly aromatic polyesters, polyamides, polycarbonates, polyacetals, modified polyphenylene oxides, polyphenylene sulfides, polysulfones, polyether ketones, biaxially oriented polypropylenes, etc. Among these, polyesters are preferred, and polyethylene terephthalate is more preferred.

[0070] The thickness of the substrate may be set depending on the rigidity of the adhesive tape, the material of the substrate, the range of the height H1 of the adhesive tape described above, etc. In this embodiment, the thickness of the substrate is preferably 1 μm or more and 500 μm or less, more preferably 5 μm or more and 300 μm or less, and even more preferably 10 μm or more and 100 μm or less.

[0071] At least one of the main surfaces of the substrate may be subjected to an adhesion treatment such as a corona treatment in order to improve adhesion with a layer formed on the main surface. Also, at least one of the main surfaces of the substrate may be provided with an easy-adhesion layer in order to improve adhesion with a layer formed on the main surface.

[0072] (1.2.2. Adhesive Layer) The adhesive layer (adhesive layer for tape) is attached to a surface having a height difference and is fixed on the surface until it is peeled off from the surface. As a result, the height difference is suppressed, and even if a surface protection sheet is attached to the surface, the height difference reflected in the surface protection sheet can be reduced. Therefore, the TTV of the wafer after back grinding can be reduced. The adhesive layer may be composed of one layer (single layer) or may be composed of two or more layers.

[0073] The thickness of the adhesive layer may be set to a thickness that allows the adhesive tape to be fixed on the surface of the wafer, taking into consideration the thickness of the substrate, the range of the height H1 of the adhesive tape described above, etc. In this embodiment, the thickness of the adhesive layer is preferably 1 μm or more and 300 μm or less, and more preferably 3 μm or more and 50 μm or less. The thickness of the adhesive layer means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer composed of multiple layers means the total thickness of all layers that make up the adhesive layer.

[0074] The composition of the adhesive layer is not limited as long as it has an adhesive strength sufficient to fix the adhesive tape on the surface of the wafer. The adhesive layer may be composed of, for example, an acrylic adhesive, a urethane adhesive, a rubber adhesive, a silicone adhesive, etc. In particular, in consideration of the surface protection sheet peeling step (step 3) described later, it is preferable that the adhesive has an adhesive strength sufficient to be peeled off from the surface together with the peeling of the surface protection sheet. In this embodiment, it is preferable that the adhesive layer is composed of an acrylic adhesive containing an acrylic polymer.

[0075] The acrylic adhesive may be energy ray curable or non-energy ray curable. For example, the acrylic adhesive described in the adhesive layer (sheet adhesive layer) of the surface protection sheet described later can be used as the energy ray curable acrylic adhesive. In addition, for example, the non-energy ray curable acrylic adhesive can be used as an acrylic adhesive that does not contain a component that reacts with energy rays, such as an acrylic polymer having an energy ray curable group introduced therein, or an energy ray curable compound.

[0076] (1.3. Surface protection sheet) The surface protection sheet attached to the surface may be configured to protect the circuits and the like on the wafer surface. In this embodiment, as shown in FIG. 4A, the surface protection sheet 10 preferably has a base material 11 (sheet base material 11) and an adhesive layer 12 (sheet adhesive layer 12). The adhesive layer is attached to the wafer surface, so that the wafer surface is reliably protected. The adhesive layer may or may not conform to the height difference of the wafer surface.

[0077] For example, when the workpiece is a wafer on which a convex electrode is formed, it is preferable that the adhesive layer conforms to the height difference and embeds the convex electrode. On the other hand, when the workpiece is a chip-on-wafer, the adhesive layer does not have to conform to the height difference. That is, the adhesive layer does not have to be inserted between the chips. The adhesive tape may be embedded in the surface protection sheet, or a part of the adhesive tape may not be embedded in the surface protection sheet and a part of the adhesive tape may be exposed to the outside.

[0078] 4B, an intermediate layer 13 may be disposed between the substrate 11 and the adhesive layer 12 in the surface protection sheet 10. The intermediate layer makes it easy to suppress the height difference on the wafer surface. In particular, when the workpiece is a wafer on which a convex electrode is formed, the convex electrode can be reliably embedded.

[0079] The surface protection sheet 10 shown in Fig. 4B is described in detail below. Fig. 4B shows a surface protection sheet 10 having a configuration in which an intermediate layer 13 and a pressure-sensitive adhesive layer 12 are laminated in this order on a substrate 11.

[0080] The surface protective sheet 10 may have other layers. For example, another layer may be formed between the substrate 11 and the intermediate layer 13, or another layer may be formed between the intermediate layer 13 and the pressure-sensitive adhesive layer 12.

[0081] The components of surface protection sheet 10 shown in FIG. 4B will be described in detail below.

[0082] (1.3.1. Base material) The substrate (substrate for sheet) is a member that is responsible for the rigidity of the surface protection sheet. The substrate is not limited as long as it is made of a material that can support the workpiece. For example, various resin films used as substrates for backgrinding tapes are exemplified. By using such a resin film, the workpiece can be held without being damaged even if the thickness of the workpiece becomes thin due to grinding. The substrate may be made of a single layer film made of one resin film, or may be made of a multilayer film in which multiple resin films are laminated.

[0083] In this embodiment, examples of the material of the substrate include polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, wholly aromatic polyesters, polyamides, polycarbonates, polyacetals, modified polyphenylene oxides, polyphenylene sulfides, polysulfones, polyether ketones, biaxially oriented polypropylenes, etc. Among these, polyesters are preferred, and polyethylene terephthalate is more preferred.

[0084] The thickness of the substrate affects the rigidity of the surface protection sheet, and may be set according to the material of the substrate. In this embodiment, the thickness of the substrate is preferably 25 μm or more and 200 μm or less, more preferably 35 μm or more and 150 μm or less, and even more preferably 40 μm or more and 150 μm or less.

[0085] At least one of the main surfaces of the substrate may be subjected to an adhesion treatment such as a corona treatment in order to improve adhesion with a layer formed on the main surface. Also, at least one of the main surfaces of the substrate may be provided with an easy-adhesion layer in order to improve adhesion with a layer formed on the main surface.

[0086] (1.3.2. Adhesive Layer) The adhesive layer (sheet adhesive layer) is attached to the surface of the wafer, and protects the surface and supports the wafer until it is peeled off from the surface. In this embodiment, the adhesive layer is closely attached to and fixed to the surface of the wafer. As a result, even if cooling water or the like is used during back grinding, the surface protection sheet can prevent the cooling water from penetrating into the wafer surface and adequately protect the wafer surface. Furthermore, even if the wafer is divided into individual pieces, contact between chips can be suppressed. The adhesive layer may be composed of one layer (single layer) or may be composed of two or more layers.

[0087] The thickness of the adhesive layer is not particularly limited as long as it is thick enough to support the wafer. In this embodiment, the thickness of the adhesive layer is preferably 1 μm or more and 100 μm or less, more preferably 5 μm or more and 50 μm or less. The thickness of the adhesive layer means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer composed of multiple layers means the total thickness of all layers constituting the adhesive layer.

[0088] The composition of the adhesive layer is not limited as long as it has enough adhesiveness to protect the surface of the wafer. In this embodiment, the adhesive layer is preferably composed of, for example, an acrylic adhesive, a urethane adhesive, a rubber adhesive, a silicone adhesive, or the like.

[0089] In addition, the adhesive layer is preferably formed from an energy ray curable adhesive. By forming the adhesive layer of the surface protection sheet from an energy ray curable adhesive, the adhesive layer adheres to the wafer with high adhesive strength when attached to the wafer, and the adhesive strength can be reduced by irradiating energy rays when peeled off from the wafer. Therefore, while appropriately protecting the circuits of the wafer, the circuit on the wafer surface is prevented from being destroyed and the adhesive is prevented from being transferred onto the wafer when the surface protection sheet is peeled off.

[0090] In this embodiment, the energy ray curable adhesive is preferably composed of an adhesive composition containing an acrylic adhesive. As the acrylic adhesive, it is preferable to use an acrylic polymer. As the energy ray curable acrylic adhesive, it may be an acrylic adhesive composed of an acrylic polymer having energy ray curability, or an acrylic adhesive containing an acrylic polymer having energy ray curability and / or an acrylic polymer not having energy ray curability and an energy ray curable compound such as an oligomer having an energy ray curable group. In this embodiment, an acrylic adhesive composed of an acrylic polymer having energy ray curability is preferable.

[0091] The acrylic polymer having energy ray curability may be any known acrylic polymer, but in this embodiment, an acrylic polymer having an energy curable group introduced into a functional group-containing acrylic polymer is preferred. The functional group-containing acrylic polymer may be a homopolymer formed from one type of acrylic monomer, a copolymer formed from multiple types of acrylic monomers, or a copolymer formed from one or multiple types of acrylic monomers and a monomer other than the acrylic monomer.

[0092] In this embodiment, the functional group-containing acrylic polymer is preferably an acrylic copolymer obtained by copolymerizing an alkyl (meth)acrylate with a functional group-containing monomer.

[0093] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and n-octyl (meth)acrylate.

[0094] The functional group-containing monomer is a monomer containing a reactive functional group. The reactive functional group is a functional group capable of reacting with other compounds such as a crosslinking agent described later. Examples of the functional group in the functional group-containing monomer include a hydroxyl group, a carboxyl group, and an epoxy group, and a hydroxyl group is preferred.

[0095] Examples of hydroxyl group-containing monomers include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol.

[0096] Examples of the energy ray curable group include a (meth)acryloyl group and a vinyl group, and a (meth)acryloyl group is preferred. The energy ray curable group is introduced into the acrylic polymer by, for example, adding an energy ray curable compound described later to the functional group-containing acrylic polymer.

[0097] The energy ray-curable compound having an energy ray-curable group is preferably a compound having one or more groups selected from an isocyanate group, an epoxy group, and a carboxy group, and more preferably a compound having an isocyanate group.

[0098] Examples of compounds having an isocyanate group include 2-methacryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate, allyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate; acryloyl monoisocyanate compounds obtained by reacting a diisocyanate compound or a polyisocyanate compound with hydroxyethyl (meth)acrylate; and acryloyl monoisocyanate compounds obtained by reacting a diisocyanate compound or a polyisocyanate compound with a polyol compound and hydroxyethyl (meth)acrylate. The isocyanate group undergoes an addition reaction with the hydroxyl group of the functional group-containing acrylic polymer.

[0099] The pressure-sensitive adhesive composition preferably further contains a crosslinking agent, which reacts with functional groups, for example, to crosslink resins contained in the functional-group-containing acrylic polymer.

[0100] Examples of the crosslinking agent include isocyanate-based crosslinking agents (crosslinking agents having an isocyanate group) such as tolylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates; epoxy-based crosslinking agents (crosslinking agents having a glycidyl group) such as ethylene glycol glycidyl ether; aziridine-based crosslinking agents (crosslinking agents having an aziridinyl group) such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine; metal chelate-based crosslinking agents (crosslinking agents having a metal chelate structure) such as aluminum chelate; and isocyanurate-based crosslinking agents (crosslinking agents having an isocyanuric acid skeleton).

[0101] The crosslinking agent is preferably an isocyanate-based crosslinking agent from the viewpoints of improving the cohesive strength of the pressure-sensitive adhesive and thereby improving the adhesive strength of the pressure-sensitive adhesive layer, and of easy availability.

[0102] The pressure-sensitive adhesive composition may further contain a photopolymerization initiator. When the pressure-sensitive adhesive composition contains a photopolymerization initiator, the curing reaction proceeds sufficiently even when irradiated with relatively low-energy energy rays such as ultraviolet rays.

[0103] Examples of the photopolymerization initiator include photoinitiators such as benzoin compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones.Specific examples include α-hydroxycyclohexyl phenyl ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl diphenyl sulfide, benzyl dimethyl ketal, tetramethylthiuram monosulfide, azobisisobutyronitrile, dibenzyl, diacetyl, β-chloroanthraquinone, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0104] (1.3.3. Middle Layer) The intermediate layer is a layer disposed between the substrate and the pressure-sensitive adhesive layer. In this embodiment, the intermediate layer may be composed of one layer (single layer) or may be composed of two or more layers.

[0105] The thickness of the intermediate layer may be set in consideration of the height difference on the wafer surface. In this embodiment, the thickness of the intermediate layer is preferably 50 μm or more and 600 μm or less, and more preferably 150 μm or more and 500 μm or less. The thickness of the intermediate layer means the thickness of the entire intermediate layer. For example, the thickness of the intermediate layer composed of multiple layers means the total thickness of all layers that compose the intermediate layer.

[0106] In this embodiment, when the surface protective sheet has an intermediate layer, the intermediate layer preferably has the following physical properties.

[0107] (1.3.3.1. Shear storage modulus at 65°C) In this embodiment, the shear storage modulus (G') of the intermediate layer at 65°C is preferably 0.5 MPa or less. The shear storage modulus (G') is one of the indicators of the ease of deformation (hardness) of the intermediate layer. When the shear storage modulus (G') of the intermediate layer at 65°C is within the above range, damage to the wafer or the like during back grinding can be suppressed.

[0108] The shear storage modulus of the intermediate layer at 65° C. is more preferably 0.4 MPa or less, and even more preferably 0.2 MPa or less. Furthermore, from the viewpoint of suppressing exudation of intermediate layer components during storage of the surface protection sheet, the shear storage modulus of the intermediate layer at 65° C. is preferably 0.005 MPa or more.

[0109] The shear storage modulus of the intermediate layer at 65° C. may be measured by a known method. For example, the intermediate layer may be used as a sample of a predetermined size, and the sample may be strained at a predetermined frequency within a predetermined temperature range using a dynamic viscoelasticity measuring device to measure the elastic modulus, and the shear storage modulus may be calculated from the measured elastic modulus.

[0110] (1.3.3.2.Loss tangent at 65°C) In this embodiment, the loss tangent (tan δ) of the intermediate layer at 65° C. is preferably greater than 0.5. The loss tangent is defined as "loss modulus / storage modulus" and is a value measured by the response to stress applied to an object using a dynamic viscoelasticity measuring device. When the loss tangent of the intermediate layer at 65° C. is within the above range, damage to wafers and the like during back grinding can be suppressed.

[0111] The loss tangent of the intermediate layer at 65° C. is more preferably 0.7 or more, and even more preferably 1.0 or more. Also, the loss tangent of the intermediate layer at 65° C. is preferably 2.0 or less.

[0112] The loss tangent of the intermediate layer at 65° C. may be measured by a known method, similar to the shear storage modulus. For example, the intermediate layer is prepared as a sample of a predetermined size, and a dynamic viscoelasticity measuring device is used to apply a strain to the sample at a predetermined frequency within a predetermined temperature range to measure the elastic modulus, and the loss tangent can be calculated from the measured elastic modulus.

[0113] (1.3.4. Composition for intermediate layer) Although the composition of the intermediate layer is not particularly limited, in this embodiment, the intermediate layer is preferably composed of a composition having a resin (intermediate layer composition). The intermediate layer composition preferably contains the following components.

[0114] (1.3.4.1. Urethane (meth)acrylates) The urethane (meth)acrylate is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized by energy ray irradiation. In this embodiment, the urethane (meth)acrylate is a component for imparting flexibility to the intermediate layer.

[0115] The urethane (meth)acrylate may be a monofunctional type or a multifunctional type. In this embodiment, a multifunctional urethane (meth)acrylate is preferred, and a bifunctional urethane (meth)acrylate is preferred.

[0116] The urethane (meth)acrylate may be an oligomer, a polymer, or a mixture thereof. In this embodiment, a urethane (meth)acrylate oligomer is preferred.

[0117] The urethane (meth)acrylate can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting the resulting prepolymer with a hydroxyl group-containing (meth)acrylate. The urethane (meth)acrylate may be used alone or in combination of two or more kinds.

[0118] The content of the urethane (meth)acrylate in the intermediate layer composition is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. The content of the urethane (meth)acrylate in the intermediate layer composition is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 50% by mass or less.

[0119] (1.3.4.2. Polymerizable Monomers) The polymerizable monomer is preferably a polymerizable compound other than the above-mentioned urethane (meth)acrylate, and is a compound that can be polymerized with other components by irradiation with energy rays. In this embodiment, the polymerizable monomer is a compound having one reactive unsaturated double bond group.

[0120] Examples of the polymerizable monomer include (meth)acrylates having an alkyl group having 1 to 30 carbon atoms; (meth)acrylates having a functional group such as a hydroxyl group, an amide group, an amino group, or an epoxy group; (meth)acrylates having an alicyclic structure; (meth)acrylates having an aromatic structure; (meth)acrylates having a heterocyclic structure; and vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam.

[0121] Examples of the (meth)acrylate having an alkyl group having 1 to 30 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0122] Examples of the (meth)acrylate having a functional group include hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-butyl (meth)acrylamide, and N-methylol (meth)acrylamide. Examples of the amide group-containing compounds include acrylamide, N-methylolpropane (meth)acrylamide, N-methoxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; amino group-containing (meth)acrylates such as primary amino group-containing (meth)acrylates, secondary amino group-containing (meth)acrylates, and tertiary amino group-containing (meth)acrylates; and epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.

[0123] Examples of (meth)acrylates having an alicyclic structure include isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, and adamantane (meth)acrylate.

[0124] Examples of the (meth)acrylate having an aromatic structure include phenylhydroxypropyl (meth)acrylate, benzyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.

[0125] Examples of the (meth)acrylate having a heterocyclic structure include tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate.

[0126] In this embodiment, the polymerizable monomer preferably includes a (meth)acrylate having an alkyl group with 1 to 30 carbon atoms and a (meth)acrylate having an alicyclic structure. Among (meth)acrylates having an alkyl group with 1 to 30 carbon atoms, (meth)acrylates having an alkyl group with 4 to 14 carbon atoms are preferred, and as (meth)acrylates having an alicyclic structure, isobornyl (meth)acrylate and trimethylcyclohexyl (meth)acrylate are preferred.

[0127] In addition, when the intermediate layer composition contains a crosslinking agent, a (meth)acrylate having a functional group capable of reacting with the crosslinking agent is not preferred. This is because the crosslinked structure formed by the crosslinking reaction may increase the shear storage modulus of the intermediate layer. For example, a composition for the intermediate layer containing a polyisocyanate-based crosslinking agent and a (meth)acrylate having a hydroxyl group is not preferred.

[0128] The content of the polymerizable monomer in the intermediate layer composition is preferably 20% by mass or more, more preferably 30% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less.

[0129] In addition, the mass ratio of the urethane (meth)acrylate to the polymerizable monomer (urethane (meth)acrylate / polymerizable monomer) in a total of 100 parts by mass of the urethane (meth)acrylate and the polymerizable monomer is preferably from 20 / 80 to 80 / 20, and more preferably from 30 / 70 to 70 / 30.

[0130] (1.3.4.3. Photopolymerization initiator) When the intermediate layer composition contains the above-mentioned urethane (meth)acrylate and polymerizable monomer, the intermediate layer composition preferably contains a photopolymerization initiator. By containing the photopolymerization initiator, polymerization proceeds reliably, and an intermediate layer having the above-mentioned characteristics can be easily obtained.

[0131] Examples of the photopolymerization initiator include photopolymerization initiators such as benzoin compounds, acetophenone compounds, acylphosphinoxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones. Specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. These photopolymerization initiators may be used alone or in combination of two or more.

[0132] The amount of the photopolymerization initiator is preferably 0.05 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total of the urethane (meth)acrylate and the polymerizable monomer.

[0133] (1.3.4.4. Chain transfer agents) The intermediate layer composition preferably contains a chain transfer agent. The chain transfer agent can cause a chain transfer reaction and adjust the progress of the curing reaction of the intermediate layer composition. By containing the chain transfer agent, it becomes possible for components with short molecular chains to remain relatively even after curing, so that the cured polymer has a crosslinked structure with relatively high flexibility. As a result, it becomes easy to set the shear storage modulus of the intermediate layer within the above range.

[0134] Examples of the chain transfer agent include thiol group-containing compounds. Examples of the thiol group-containing compounds include nonyl mercaptan, 1-dodecanethiol, 1,2-ethanedithiol, 1,3-propanedithiol, triazine thiol, triazine dithiol, triazine trithiol, 1,2,3-propane trithiol, tetraethylene glycol-bis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetraki ... Examples of the chain transfer agent include erythritol tetrakis thioglucolate, dipentaerythritol hexakis (3-mercaptopropionate), tris [(3-mercaptopropionyloxy)-ethyl]-isocyanurate, 1,4-bis (3-mercaptobutyryloxy) butane, pentaerythritol tetrakis (3-mercaptobutyrate), and 1,3,5-tris (3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6- (1H,3H,5H)-trione. The chain transfer agent may be used alone or in combination of two or more.

[0135] The amount of the chain transfer agent is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the total of the urethane (meth)acrylate and the polymerizable monomer.

[0136] (1.3.5. Manufacturing of Surface Protection Sheets) The surface protection sheet can be manufactured by a known method. For example, first, the above-mentioned adhesive layer composition (if necessary, intermediate layer composition) is prepared. Next, the prepared composition is applied to the surface of a release sheet, a substrate, etc., using a known coating method, and then dried and cured to obtain a surface protection sheet having a predetermined structure.

[0137] (1.4.Process 2) After a surface protection sheet 10 is applied onto the front surface 1a of the wafer 1 to which the adhesive tape 3 has been applied, the back surface 1b of the wafer is ground.

[0138] 5(B), the wafer 1 with the surface protection sheet 10 attached thereto is placed with the surface 1a side on the chuck table 100. The chuck table 100 has, for example, a porous holding surface, and the surface protection sheet 10 is adsorbed and fixed to the chuck table 100 by suction from the side opposite to the side on which the wafer 1 is placed.

[0139] At this time, because the adhesive tape 3 is attached to the wafer 1, the height difference of the surface protection sheet 10 is suppressed between the inner and outer periphery of the wafer 1. Therefore, even when suction is performed, the outer periphery of the wafer 1 is adsorbed to the chuck table 100 with almost no deformation.

[0140] After the wafer 1 is fixed to the chuck table 100, the back surface 1b of the wafer 1 is ground, for example, by a grinding wheel or the like. The thickness of the wafer 1 after the back surface grinding is, for example, about 25 μm or more and 600 μm or less.

[0141] After grinding, the suction is released and the wafer 1 and surface protection sheet 10 are released from the chuck table 100. In this embodiment, since process A is adopted in step 1, the thickness of the wafer 1 becomes almost uniform from the inner periphery to the outer periphery, as shown in Fig. 5(C). As a result, the TTV of the wafer 1 after grinding is suppressed to a small value.

[0142] (1.5.Step 3) In this embodiment, it is preferable to peel off the surface protection sheet from the wafer after the backside grinding. That is, it is preferable that the method for processing a workpiece according to this embodiment has a step (step 3) of peeling off the surface protection sheet from the wafer after the backside grinding. Step 3 is performed, for example, as follows.

[0143] When the adhesive layer of the surface protection sheet is formed from an energy ray curable adhesive, the adhesive layer is cured and shrunk by irradiating it with energy rays, and the adhesive strength to the adherend (wafer) is reduced. Next, a pick-up tape is attached to the back side of the wafer after the back grinding, and the position and direction are adjusted so that the wafer can be picked up. At this time, a ring frame arranged on the outer periphery of the wafer is also attached to the pick-up tape, and the outer periphery of the pick-up tape is fixed to the ring frame. The wafer and the ring frame may be attached to the pick-up tape at the same time, or may be attached at different times. Next, the surface protection sheet is peeled off from the wafer held on the pick-up tape.

[0144] In this embodiment, when the surface protection sheet is peeled off, it is preferable that at least a part of the adhesive tape attached to the surface of the wafer is peeled off together with the surface protection sheet, and it is particularly preferable that the entire adhesive tape is peeled off. That is, the adhesive tape formed under the surface protection sheet is also peeled off together with the surface protection sheet. This makes it possible to suppress the generation of residue on the surface after peeling.

[0145] (1.6. Steps 4A and 4B) The method for processing a workpiece according to this embodiment is also applicable to DBG or LDBG. In this case, it is preferable to use a surface protection sheet 10 shown in FIG. 4C as the surface protection sheet. In the surface protection sheet 10 shown in FIG. 4C, a buffer layer 14 is formed on a main surface 11b of a substrate 11 opposite to a main surface on which an intermediate layer 12 and an adhesive layer 13 are formed.

[0146] The buffer layer is a layer that is softer than the base material and relieves stress during back grinding of the wafer to prevent cracks and chips from occurring in the wafer. Also, the presence of the buffer layer makes it easier for the wafer to be properly held on the chuck table.

[0147] The thickness of the buffer layer is preferably 1 to 200 μm, more preferably 10 to 100 μm, and further preferably 20 to 80 μm. By setting the thickness of the buffer layer within the above range, the buffer layer can appropriately relieve stress during back grinding.

[0148] The buffer layer may be a layer formed from a buffer layer composition containing an energy ray-polymerizable compound, or may be a film such as a polypropylene film, an ethylene-vinyl acetate copolymer film, an ionomer resin film, an ethylene-(meth)acrylic acid copolymer film, an ethylene-(meth)acrylic acid ester copolymer film, an LDPE film, or an LLDPE film.

[0149] When the workpiece processing method according to this embodiment is applied to DBG or LDBG, it is preferable to have a step of forming a groove on the surface of the wafer (step 4A: DBG) or a step of forming a modified region inside the wafer (step 4B: LDBG) in addition to the above steps 1 and 2. The groove and modified region are formed so as to follow the parting line when the wafer is divided and singulated into chips in the above step 2.

[0150] When grooves are formed on the surface of the wafer by dicing or the like, step 1 (and step A) is performed after step 4A. That is, in step 1, a surface protection sheet is attached to the surface of the wafer having the grooves formed in step 4A described below.

[0151] The grooves formed in step 4A are shallower than the thickness of the wafer. The grooves can be formed by dicing using a conventionally known dicing device or the like. In step 2 described above, the wafer is divided into a plurality of chips along the grooves by the stress applied during back grinding.

[0152] On the other hand, when forming a modified region on the wafer, step 1 (and step A) may be performed before or after step 4 B. In this embodiment, when forming a modified region on the wafer, it is preferable to perform step 1 (and step A) before step 4 B.

[0153] In addition, the modified region is a brittle portion of the wafer, and is the starting point for the wafer to be destroyed and diced into chips when the wafer becomes thinner due to grinding in the grinding process or when stress is applied during backside grinding.

[0154] The modified region is formed inside the wafer by irradiating the laser focused on the inside of the wafer. The laser may be irradiated from the front side or the back side of the wafer. In the embodiment in which the modified region is formed, when step 4B is performed after step 1 and the laser is irradiated from the front side of the wafer, the laser is irradiated to the wafer through the surface protection sheet.

[0155] In DBG, the back grinding in step 2 is performed to thin the wafer at least to the bottom of the grooves. This back grinding turns the grooves into cuts that penetrate the wafer, and the wafer is divided by the cuts into individual chips.

[0156] In LDBG, the grinding surface (wafer back surface) may reach the modified region by grinding, but it does not have to reach the modified region strictly. In other words, it is sufficient to grind to a position close to the modified region so that the wafer is broken and singulated into chips starting from the modified region. For example, the actual singulation of the chips may be performed by attaching the above-mentioned pick-up tape and then stretching the pick-up tape.

[0157] After the back surface grinding is completed, dry polishing may be performed prior to picking up the chips.

[0158] Step 3 may be performed as described above, but the surface protection sheet is peeled off from the individual wafers. Even in this case, damage to the chips is suppressed.

[0159] The shape of the individualized chips (workpiece individualized products) obtained through step 3 may be square or elongated, such as rectangular. The thickness of the individualized chips is not particularly limited, but is preferably about 5 to 100 μm, and more preferably 10 to 45 μm. LDBG makes it easy to make the thickness of the individualized chips 50 μm or less, and more preferably 10 to 45 μm. The size of the individualized chips is not particularly limited, but the chip size is preferably 600 mm or less. 2 Less than 400mm, more preferably 2 Less than 120mm, more preferably 2 is less than.

[0160] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES

[0161] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0162] Example 1 (1) Adhesive tape 100 parts by mass of an acrylic polymer obtained by copolymerizing 99 parts by mass of n-butyl acrylate (BA) and 1 part by mass of acrylic acid (AA) was mixed with 0.5 parts by mass of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") and diluted with methyl ethyl ketone to prepare a coating agent for a composition for adhesive layers.

[0163] The prepared adhesive layer composition was applied to one side of a PET film (thickness: 25 μm) as a substrate, and then dried to form an adhesive layer with a thickness of 5 μm on the PET film. The adhesive layer was then punched out into a ring shape to obtain a ring-shaped adhesive tape with an outer diameter of 299 mm and an inner diameter of 293 mm.

[0164] (2) Surface protection sheet As the surface protective sheet, the surface protective sheet shown below was used.

[0165] A composition for an intermediate layer was obtained by blending 48 parts by mass of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 26 parts by mass of isobornyl acrylate, 16 parts by mass of trimethylcyclohexyl acrylate, and 10 parts by mass of lauryl acrylate, for a total of 100 parts by mass, with 3.4 parts by mass of a photopolymerization initiator (Omnirad1173, manufactured by IGM Resin Co., Ltd.) and 1.0 part by mass of a chain transfer agent (Karenz MT PE1, manufactured by Showa Denko K.K.).

[0166] The obtained intermediate layer composition was applied by knife coating onto a substrate PET film (manufactured by Toray Industries, Inc., thickness 75 μm) to a thickness of 400 μm to form an intermediate layer composition layer. Immediately after application, a PET-based release film (manufactured by Lintec Corporation, SP-PET752150, thickness 75 μm) was further laminated onto the intermediate layer composition layer. Thereafter, a high-pressure mercury lamp was used to illuminate the intermediate layer composition layer at an illumination intensity of 120 mW / cm. 2 , light intensity 240mJ / cm 2 The intermediate layer composition layer was irradiated with ultraviolet light under the conditions of 330 mW / cm illuminance using a metal halide lamp. 2 , light intensity 1260mJ / cm 2 The intermediate layer composition layer was cured by irradiating ultraviolet light under the above conditions, thereby forming an intermediate layer having a thickness of 400 μm on the PET film substrate.

[0167] Next, 80 parts by mass of 2-ethylhexyl acrylate (2EHA) and 20 parts by mass of 2-hydroxyethyl acrylate (HEA) were copolymerized to obtain an acrylic copolymer, to which 2-isocyanatoethyl methacrylate (MOI) was added so that the addition ratio was 80 equivalents relative to the hydroxyl group (100 equivalents) derived from HEA. To the energy ray curable acrylic copolymer (weight average molecular weight: 800,000) obtained by adding 1.5 parts by mass of trimethylolpropane adduct tolylene diisocyanate (manufactured by Tosoh, Coronate L) as a crosslinking agent and 2.2 parts by mass of 2,2-dimethoxy-2-phenylacetophenone (manufactured by IGM Resin, Omnirad651) as a photopolymerization initiator, toluene was further added to adjust the solid content concentration to 30%, and the mixture was stirred for 30 minutes to prepare a pressure-sensitive adhesive composition.

[0168] Next, the prepared solution of the adhesive composition was applied to a PET-based release film (SP-PET382150, manufactured by Lintec Corporation, thickness 38 μm) and dried to form an adhesive layer with a thickness of 10 μm, thereby producing an adhesive sheet.

[0169] The release film on the intermediate layer obtained above was removed, and the intermediate layer was laminated to the adhesive layer of the adhesive sheet to produce a surface protection sheet having a substrate / intermediate layer / adhesive layer configuration.

[0170] Next, a silicon wafer (diameter 12 inches, thickness 760 μm) with bump electrodes having a bump electrode height of 200 μm and a pitch of 400 μm was prepared. A polyimide film having a thickness of 4 μm was formed on the surface of this silicon wafer with bump electrodes. The adhesive tape obtained above was attached to the outer periphery of this silicon wafer with bump electrodes where the bump electrodes were not formed.

[0171] A surface protection sheet was attached to the silicon wafer with bump electrodes after the adhesive tape was attached using a tape laminator (manufactured by Lintec Corporation, RAD-3510F / 12) under the condition that the temperature of the lamination table was 65°C. The wafer with the surface protection sheet attached was placed on the chuck table so that the surface protection sheet was in contact with the chuck table, and the wafer was fixed to the chuck table by suction. Next, the back surface of the wafer was ground with a grinding wheel, and the grinding was stopped when the thickness of the wafer became 150 μm. After grinding was completed, the TTV evaluation shown below was performed.

[0172] (TTV evaluation of the outer periphery of the wafer after grinding) The thickness of the wafer was measured using a digital microscope (Keyence, VHX-7000) in a section 15 mm inward from the edge of the ground wafer, the maximum and minimum values ​​were selected, and the difference between the maximum and minimum values ​​was calculated. This measurement was performed at four locations on the ground wafer, the top, bottom, right, and left (positions obtained by rotating the wafer 90°), and the average value of the differences between the maximum and minimum values ​​was calculated. The results are shown in Table 1.

[0173] (Examples 2 and 3 and Comparative Example 1) In Example 2, the thickness of the adhesive tape substrate was 50 μm, in Example 3, the thickness of the adhesive tape substrate was 75 μm, and in Comparative Example 1, the adhesive tape was not applied to the outer periphery of the wafer. Except for this, back grinding and TTV evaluation of the wafer having bump electrodes were performed in the same manner as in Example 1. The results are shown in Table 1.

[0174] [Table 1]

[0175] From Table 1, it was confirmed that when a surface protection sheet is attached to a wafer having a surface with height differences and then the wafer is background, the TTV of the wafer after backgrounding can be reduced by attaching an adhesive tape to the surface of the wafer to suppress the effect of the height differences. [Explanation of symbols]

[0176] 1...Work (wafer) 2a...Convex electrode, 2b...Chip 3…Adhesive tape 3a...Base material 3b…adhesive layer 10...Surface protection sheet 11...Base material 12...Adhesive layer 13. Middle class 14...Buffer layer

Claims

1. A workpiece has a surface having a height difference and a back surface opposite to the surface, and an adhesive tape is attached to the surface to suppress the effect of the height difference of the surface. A surface protective sheet is attached to the surface of the workpiece. and grinding the back surface of the workpiece to which the surface protection sheet is attached.

2. The method for processing a workpiece according to claim 1 , wherein the adhesive tape has a base material and an adhesive layer.

3. The method for processing a workpiece according to claim 2 , wherein the adhesive layer is formed on only one of the main surfaces of the base material.

4. A method for processing a workpiece as described in any one of claims 1 to 3, wherein the surface has an inner circumference and an outer circumference surrounding the inner circumference, the height of the outer circumference is lower than the height of the inner circumference, and the adhesive tape is attached onto the outer circumference.

5. 4. The method for machining a workpiece according to claim 1, wherein the workpiece has a convex electrode formed on the surface thereof.

6. The method for processing a workpiece according to claim 1 , wherein the surface protection sheet has a base material and an adhesive layer.

7. A step of forming a groove on the surface of the workpiece before the step of attaching a surface protection sheet to the surface of the workpiece, 5. The method for machining a workpiece according to claim 4, wherein in the step of grinding the rear surface of the workpiece, the workpiece is diced into a plurality of workpiece pieces starting from the grooves.

8. A process for forming a modified region inside the workpiece before the process for grinding the back surface of the workpiece, The method for machining a workpiece according to claim 4 , wherein in the step of grinding the rear surface of the workpiece, the workpiece is diced into a plurality of workpiece individual pieces starting from modified regions.

Citation Information

Patent Citations

  • Adhesive tape for semiconductor wafer processing, manufacturing method of adhesive tape for semiconductor wafer processing, and processing method of semiconductor wafer

    JP2017171896A