Seal ring
The seal ring with recessed grooves and eccentric configuration addresses mold distortion and sticking issues, ensuring low oil leakage and improved moldability for hydraulic systems in ATs and CVTs.
Patent Information
- Application Number
- JP2023047399
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing seal rings for hydraulic systems in automatic transmissions (ATs) and continuously variable transmissions (CVTs) face issues with distortion during continuous injection molding, leading to increased oil leakage and difficulty in mold removal due to sticking, especially when inclined surfaces are involved.
The seal ring design features recessed grooves on the inner peripheral surface, with shallower depths at opposing parts compared to adjacent parts, and an eccentric configuration to facilitate easy mold release and prevent distortion, while maintaining low oil leakage.
The design effectively reduces mold sticking and distortion, ensuring low oil leakage and improved moldability, thereby enhancing the reliability and efficiency of hydraulic systems.
Smart Images

Figure 2024136315000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a seal ring used to seal fluid in devices that utilize the fluid pressure of fluid such as hydraulic oil, such as automatic transmissions (hereinafter referred to as AT) and continuously variable transmissions (hereinafter referred to as CVT). [Background technology]
[0002] In devices such as ATs and CVTs, oil seal rings are attached at key locations to seal hydraulic oil. For example, they are attached to a pair of spaced apart annular grooves provided on a rotating shaft inserted into a shaft hole in a housing, and the side and inner circumferential surfaces of both seal rings receive hydraulic oil supplied from an oil passage between the two annular grooves, while the side and outer circumferential surfaces of the opposite sides seal the side wall of the annular groove and the inner circumferential surface of the housing. Each seal surface of the seal rings maintains the hydraulic pressure of the hydraulic oil between the two seal rings while making sliding contact with the side wall of the annular groove and the inner circumferential surface of the housing, respectively. This seal ring is an annular body with a roughly rectangular cross section, and has a joint at one point in the circumferential direction.
[0003] In recent years, the automobile industry has accelerated the development of fuel-efficient vehicles against the backdrop of environmental issues. As part of this, the need for low oil leakage is increasing with the increase in demand for idling stops. For example, Patent Document 1 describes a resin seal ring with excellent quality that reduces the amount of leakage while reducing rotational sliding friction and maintains stable sealing performance for a long period of time. As a specific configuration, a line contact portion that linearly abuts against the side wall of the annular groove on the non-sealed fluid side is continuously provided on the side of the ring from one side of the joint to the other side, and the line contact portion provided on one side of the joint and the line contact portion provided on the other side of the joint are provided radially apart. Patent Document 1 also describes a seal ring in which the corners between the outer circumferential surface and the ring side are chamfered to form an inclined surface.
[0004] The above-mentioned resin seal ring is obtained, for example, by injection molding of a resin composition. Here, a process diagram of a molding die for a seal ring having an inclined surface on the outer circumferential surface is shown in FIG. 12. FIG. 12(a) shows the time of resin filling, FIG. 12(b) shows the time of mold opening, and FIG. 12(c) shows the time of product removal. As shown in FIG. 12(a), the molding die has a fixed side die 51, a movable side die 52, and a core pin 53, which are collided to form a cavity 54. A molten resin composition is filled into the cavity 54, and after pressure dwell, the cavity is cooled for a certain period of time to obtain a molded body 55. An inclined surface 55a is formed from the outer circumferential surface of the molded body 55 to the ring side surface.
[0005] Next, in the mold opening, the movable mold 52 and the core pin 53 are moved in the X direction relative to the fixed mold 51. At this time, the molded body 55 would normally move in the X direction in accordance with the movement of the core pin 53, but the molded body 55 may be attracted to the fixed mold 51 and stick to it (see FIG. 12(b)). If such sticking occurs, the seal ring becomes more likely to deform, and for example, the flatness of the ring side surface may deteriorate, and oil leakage may increase. In addition, the sticking may affect the removal of the subsequent product (see FIG. 12(c)), making continuous molding difficult. Such sticking is more likely to occur in a seal ring with an inclined surface than in a seal ring without an inclined surface, since the contact area with the fixed mold 51 increases when the mold is divided.
[0006] As a seal ring that solves such problems, the technologies disclosed in Patent Documents 2 and 3 are disclosed. Patent Documents 2 and 3 disclose a seal ring in which a recess is formed on the inner peripheral surface of the seal ring. This seal ring prevents the molded body from partially sticking to the fixed mold when manufactured by injection molding, which causes the seal ring to have a distorted shape. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2004 / 011827 [Patent Document 2] Patent Publication No. 2022-013442 [Patent Document 3] Patent Publication No. 2022-146093 Summary of the Invention [Problem to be solved by the invention]
[0008] However, even with the techniques disclosed in Patent Documents 2 and 3, the seal ring may still become distorted during continuous injection molding over a long period of time. In detail, in Fig. 3(d) of Patent Document 2, when the engagement portion 16a of the removal hand 16 is engaged with a part of the ring side surface 15b of the molded body 15 and moved in the Z direction to remove the molded body 15 from the core pin 13, the seal ring may become distorted due to the engagement between the recess 15a of the molded body 15 and the protrusion 13a of the core pin 13.
[0009] The present invention has been made in consideration of the above circumstances, and aims to provide a seal ring that suppresses the occurrence of sticking when the mold is opened, does not deform into an irregular shape even when removed, and as a result, can maintain low oil leakage properties. [Means for solving the problem]
[0010] The seal ring of the present invention is a seal ring that is mounted in an annular groove provided on a rotating shaft that is inserted into an axial hole of a housing, and is in slidable contact with the side wall surface on the non-sealed fluid side of the annular groove and in contact with the inner surface of the axial hole, thereby sealing the annular gap between the rotating shaft and the axial hole, and is an injection-molded body of a resin composition, and is provided with a joint in part of the circumferential direction, and has a recess that is recessed in the ring radial direction on its inner surface, and is characterized in that the depth of the recess at the opposing portion of the joint (hereinafter the opposing portion of the joint may be simply referred to as the "opposing portion") is shallower than the depth at the vicinity of the joint (hereinafter the vicinity of the joint may be simply referred to as the "proximal portion").
[0011] The vicinity of the gap is, for example, a portion included in a range of 45° on both sides of the position of the central angle 0° (a range of 315° from 45° via 0° in 360° notation) from the position of the central angle 0° when the central angle of the gap intermediate portion with respect to the circumferential center point O of the seal ring is 0°, preferably a portion included in a range of 30°, more preferably a portion included in a range of 15°, and may be a portion where a pair of ends constituting the gap overlap each other. A recess is formed in such a vicinity of the gap. Moreover, the facing portion of the gap is, for example, a portion included in a range of 45° on both sides of the position of the central angle 180° (a range of 225° from 135° via 180° in 360° notation) when the central angle of the gap intermediate portion with respect to the circumferential center point O of the seal ring is 0°, preferably a portion included in a range of 30°, more preferably a portion included in a range of 15°, and may be a portion where the gap faces each other. A recess is also formed in such a facing portion of the gap.
[0012] The depth of the vicinity of the gap is characterized in being 1.1 to 2.2 times the depth of the opposing portion of the gap.
[0013] The recess is a groove formed continuously in the circumferential direction from one end to the other end constituting the gap, and is characterized in that the depth of the groove increases continuously or stepwise from the opposing portion of the gap to the portion in the vicinity of the gap.
[0014] The recess is a groove that is continuously formed in the circumferential direction from one end to the other end that constitutes the gap, and the groove is characterized in that its circumferential center point is formed eccentrically toward the gap with respect to the circumferential center point of the seal ring.
[0015] The recess has a first recess formed in the vicinity of the gap and a second recess formed at the opposing portion of the gap, the first recess and the second recess are not connected, and no recess is formed on the inner surface between them.
[0016] It is characterized by having an inclined portion on at least one end side of the outer circumferential surface. Effect of the Invention
[0017] The seal ring of the present invention is an injection molded product of a resin composition, and has a joint in a part of the circumferential direction and a recessed portion recessed in the ring radial direction on the inner peripheral surface, so that the occurrence of sticking during mold opening can be suppressed. Furthermore, since the depth of the recess is shallower at the portion facing the joint than at the portion near the joint, when the molded product is removed from the core pin with a removal hand, the recess can be easily removed from the protruding portion of the core pin by widening the joint at the portion near the joint. In addition, since the recess at the portion facing the joint is shallow, the joint widens, and the recess is easily released from the protruding portion of the core pin, making it easier to remove from the protruding portion of the core pin. As a result, even if the inner peripheral surface of the molded product sticks to the outer peripheral surface of the core pin during the removal process of the molded product, it is not removed in an irregular shape, and the seal ring can be prevented from becoming irregular. Therefore, the low oil leakage property of the seal ring can be maintained.
[0018] In addition, the recess at the opposing portion of the joint can be made shallower than before, which prevents a decrease in strength at the opposing portion of the joint. This reduces the risk of the seal ring breaking at the opposing portion of the joint even if the joint is widened when the seal ring is fitted into the annular groove of the rotor, and reduces the rate of defects when the seal ring is assembled.
[0019] Since the depth in the vicinity of the joint is 1.1 to 2.2 times the depth in the opposing part of the joint, even if the inner surface of the molded body is stuck to the outer surface of the core pin during the removal process of the molded body, the timing of the seal ring coming off the core pin is almost simultaneous in the vicinity of the joint and the opposing part, so the seal ring is not removed in an irregular shape, and the seal ring can be further prevented from becoming irregular in shape.
[0020] In one form, the recess is a groove that is formed continuously in the circumferential direction from one end to the other end that constitutes the gap, and the groove is formed with its circumferential center point eccentric to the gap side relative to the circumferential center point of the seal ring.Therefore, even if the inner surface of the molded body is stuck to the outer surface of the core pin during the molded body removal process, the seal ring is removed from the core pin at almost the same time in the vicinity of the gap and the opposing portion, so that the seal ring is not removed in an irregular shape, and the seal ring can be further prevented from becoming irregular in shape.
[0021] In another embodiment, the recess has a first recess formed in the vicinity of the joint and a second recess formed on the opposing side of the joint, and the first recess and the second recess are not connected, and no recess is formed on the inner surface between them. This reduces the volume of the recess in the seal ring, suppresses sticking when the mold is opened, and maintains ease of removal from the core pin.
[0022] When the seal ring is assembled into the housing, the side surface of the ring comes into contact with the end surface of the housing, which may cause problems such as galling of the seal ring, thereby affecting the sealing performance. In this regard, the seal ring has an inclined portion on at least one end side of the outer circumferential surface, and the inclined portion has an inclined surface connected to the side surface of the ring, so that the corners are chamfered and the occurrence of galling can be suppressed. On the other hand, the formation of the inclined surface increases the concern of sticking to the fixed side mold when the mold is opened, but the presence of the recess on the inner circumferential surface makes it possible to suppress sticking. [Brief description of the drawings]
[0023] [Figure 1] FIG. 2 is a plan view showing an example of the seal ring of the present invention. [Diagram 2] 2A to 2C are cross-sectional views of the seal ring of FIG. 1. [Diagram 3] FIG. 4 is a schematic plan view illustrating a recess in an example of a seal ring of the present invention. [Figure 4] 13 is a schematic plan view illustrating a recess in another example of the seal ring of the present invention. FIG. [Diagram 5] FIG. 2 is a process diagram of a molding die for the seal ring of the present invention. [Figure 6] 4 is a cross-sectional view showing a state in which the seal ring of the present invention is installed in an annular groove. [Figure 7] 4A and 4B are a cross-sectional view and a partially enlarged view of another example of the seal ring of the present invention. [Figure 8] 8 is an explanatory diagram of the positional relationship between an inclined surface and a step surface of the seal ring in FIG. 7. [Figure 9] FIG. 2 is a schematic plan view of Examples 1 and 2. [Figure 10] 1 is a schematic plan view of Comparative Example 1 and an end view of Comparative Example 2. FIG. [Figure 11] FIG. 4 is a schematic diagram of a test for measuring the amount of oil leakage from a seal ring. [Figure 12] FIG. 11 is a process diagram of a conventional molding die for a seal ring. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] An example of the seal ring of the present invention will be described with reference to Figs. 1 and 2. Fig. 1 is a plan view of the seal ring. The seal ring 1 is formed by injection molding using a mold, and is an annular body having a substantially rectangular cross section. The seal ring 1 is a cut-type ring having a joint 9 at one location in the circumferential direction, and is fitted into an annular groove with its diameter expanded by expanding the joint 9.
[0025] The joint 9 is composed of a pair of ends 8, 8'. The shape of the pair of ends 8, 8' can be straight cut, angle cut, etc., but it is preferable to adopt the compound step cut shown in Fig. 1 because of its excellent oil sealing properties. In the compound step cut, one end 8 has an abutting surface on the inner diameter surface side of the seal ring, and a lip protruding from the abutting surface and a recessed pocket on the outer diameter surface side, while the other end 8' has an abutting surface, pocket and lip formed to complementarily fit with the above abutting surface, lip and pocket.
[0026] The size of the seal ring (outer diameter φ, inner diameter φ, ring thickness T (radial length), ring width W (axial length), etc.) is appropriately set depending on the application, etc. For example, the inner diameter φ of the seal ring is 9 mm to 75 mm, and the outer diameter φ is 13 mm to 80 mm.
[0027] In the seal ring 1, the ring side surface 4 or 4' (see FIG. 2) becomes a sliding surface with the side wall surface of the annular groove. As shown in the cross-sectional view of FIG. 2, at the corners between the ring inner peripheral surface 2 and the ring side surfaces 4, 4', there are provided step portions 5, 5' which become protruding portions from the mold during injection molding. In FIG. 2, the step portions 5, 5' are provided at both ends in the ring axial direction and are recessed portions in the ring radial direction. In addition, at the corners on both sides between the ring outer peripheral surface 3 and the ring side surfaces 4, 4', there are provided inclined surfaces 6, 6' as inclined portions. The inclined surfaces 6, 6' are provided over the entire circumference of the ring and become non-contact portions with the side wall surface of the annular groove. In addition, a plurality of lubrication grooves consisting of recesses may be formed at the inner diameter side ends of the ring side surfaces 4, 4' at intervals in the circumferential direction.
[0028] The depth of the inclined surfaces 6, 6' from the sliding surface (the ring side surface 4 or 4') becomes deeper toward the outside in the ring radial direction. In the axial cross section of the seal ring 1, the inclination angle α of the inclined surfaces 6, 6' with respect to the ring outer peripheral surface 3 is, for example, 20 degrees to 60 degrees. The inclination angle α is preferably 30 degrees to 50 degrees, more preferably 30 degrees to 45 degrees, and even more preferably 40 degrees to 45 degrees. If the inclination angle α is less than 20 degrees, the seal ring is likely to hit the end face of the housing when the seal ring is largely eccentric (protruding from the annular groove) during assembly into the housing, and there is a risk of galling. Also, if the inclination angle α exceeds 60 degrees, there is a risk that the seal ring will not be smoothly guided when it hits the end face of the housing.
[0029] Here, the seal ring 1 has a recess 7 recessed in the ring radial direction on the ring inner peripheral surface 2, specifically, the recess 7 is on the ring inner peripheral surface 2 between a pair of steps 5, 5'. As shown in Fig. 5 described later, the recess 7 is an undercut portion when the molding die is opened. The undercut portion is an engagement allowance with the die (e.g., a core pin), that is, a portion that is caught by the die.
[0030] In the present invention, in the seal ring 1, the recess 7 is shallower in the portion facing the gap than in the vicinity of the gap. First, the location where the recess is formed will be described with reference to FIG.
[0031] Fig. 3 is a schematic plan view of an example of the seal ring of the present invention, showing the location where the recess is formed. In Fig. 3, the line connecting the deepest part of the recess at the circumferential position of the ring is shown by a dotted line. Note that in Fig. 3, the step and the inclined surface are omitted.
[0032] As shown in FIG. 3, the recess 7 is formed along the circumferential direction of the ring, and more specifically, it is a recessed groove that is continuously formed in the circumferential direction from one end 8 to the other end 8' that constitutes the joint 9. In FIG. 3, the recess 7 opens to the butted surfaces of the ends 8 and 8', respectively. In FIG. 3, the depth of the recess 7 becomes continuously deeper from the opposing portion of the joint 9 to the vicinity of the joint 9. Specifically, it is deepest near the 0° position where the middle portion of the joint 9 is located, and is shallowest at the opposing position of the joint 9 (180° position). In addition, the intermediate positions on the circumference between the joint 9 and its opposing position (two positions; each at 90°) have an average depth of the depth near the 0° position and the depth of the opposing position.
[0033] In FIG. 3, the depth of recess 7 may become deeper stepwise from the portion facing joint 9 to the portion in the vicinity of joint 9.
[0034] 3, the recess 7 is characterized in that its circumferential center point P is formed eccentrically toward the joint 9 by the gap g with respect to the circumferential center point O of the seal ring 1. Such a recess 7 can be easily formed, for example, by making the protrusion serving as the transfer portion of the recess formed in the core pin larger by a predetermined amount than the outer diameter dimension of the core pin and forming it slightly eccentric from the central axis of the core pin.
[0035] Next, the depth of the recess will be described with reference to Fig. 2. Fig. 2(a) shows a cross-sectional view of the vicinity of the gap (cross-sectional view taken along line AA in Fig. 1), and Fig. 2(b) shows a cross-sectional view of the opposing portion of the gap. Note that Fig. 2(b) shows a view obtained by inverting the cross-sectional view taken along line BB in Fig. 1. Fig. 2(a) and Fig. 2(b) are the same except for the configuration of the recess, and reference numerals are omitted in Fig. 2(b). Note that in Figs. 2(a) and (b), the sizes of the inclined surfaces 6, 6', the steps 5, 5', and the recess 7 are exaggerated for the purpose of explanation and are not actual size.
[0036] 2(a) and (b), the recess 7 is not open to the steps 5, 5' on both sides, but is a closed recess groove within the inner peripheral surface of the ring. The shape of the recess groove is not particularly limited, and it may be an arc-shaped groove or a triangular groove with a triangular cross section.
[0037] As shown in FIG. 2, the recess 7 has a depth t a Depth t at the opposing part of the gap b The portion near the joint can be made deeper than the depth of the recess at the opposing portion of the joint because the recess can be easily removed from the protrusion of the core pin by widening the joint when the molded body is removed from the core pin with a removal hand.
[0038] In the present invention, the depth t a The depth t of the grooves at the opposing portions of the grooves is the length of a perpendicular line drawn from the deepest point of the grooves to a hypothetical surface F of the inner circumferential surface of the ring, assuming that no grooves are formed. brefers to the length of a perpendicular line drawn from the deepest point of the recess to an imaginary plane F on the inner circumferential surface of the ring as if the recess were not formed, when viewed in an axial cross section of the opposing parts of the joint.
[0039] Depth t in the neighborhood a is the depth t at the opposing part b For example, it is 1.1 to 4.0 times, preferably 1.1 to 3.0 times, and more preferably 1.1 to 2.2 times.
[0040] Depth t at opposing part b is, for example, 0.50% to 5.0% of the ring thickness T. b If the thickness is less than 0.50%, the anchor effect is not obtained easily when the mold is opened, and sticking may occur. b If the thickness exceeds 5.0%, the mold may become more strongly caught, and ultimately it may become difficult to remove the mold from the die. b is preferably 1.5% to 3.0% of the ring thickness T.
[0041] From another point of view, the depth t b is preferably shallower than the depth (radial length) of the stepped portions 5 and 5'. b The specific value of is about 0.01 mm to 0.10 mm. The stepped portions 5, 5' are portions that protrude from the die, and their depth (radial length) is set to exceed 10% of the ring thickness T in order to prevent deformation of the seal ring when ejected.
[0042] Depth t in the neighborhood a is, for example, 0.55% to 11%, preferably 1.2% to 10%, and more preferably 2.0% to 6.0% of the ring thickness T. The ring thickness T refers to the maximum thickness of the seal ring 1 in the ring radial direction, and is the length between the ring inner peripheral surface 2 and the ring outer peripheral surface 3 in FIG.
[0043] The width of the recess 7 in the ring axial direction is not particularly limited, and in FIG. 2, it is a constant width (w a =w b ) where width w a , w b If the width w is too short, the recess 7 may be scratched when the mold is opened. a , w b If the width w of the recess 7 is too long, the anchor effect is not obtained and sticking may occur. a , w b is preferably 2% to 60%, and more preferably 5% to 40% of the ring width W. The ring width W refers to the maximum width of the seal ring 1 in the ring axial direction, and in FIG. 2, it is the length between one ring side surface 4 and the other ring side surface 4'. a , w b is the width in the ring axial direction of the portion that opens to the ring inner circumferential surface 2. The recess 7 is also expressed as the ratio (%) of its depth to the ring thickness T and the width w a , w b It is desirable that the product of this ratio (%) to the ring width W is in the range of 10 to 500. If it is less than 10, it is difficult to obtain an anchor effect when the mold is opened, and there is a risk of sticking. If it exceeds 500, the strength of the seal ring decreases significantly, which is not preferable.
[0044] In FIG. 2, the width of the recess 7 in the ring axial direction is constant, but the width w a , w b For example, the width w a Width w at the opposing part b It is okay if the length is shorter (w a >w b ).
[0045] As shown in Fig. 3, the recess 7 can be formed over the entire inner circumference of the seal ring 1 in the circumferential direction of the ring. However, taking into consideration that the larger the volume of the recess, the more difficult it becomes to remove it from the core pin, the recess can be formed in two areas, the area near the joint and the area facing it, with no recess formed between them. Note that the area near the joint is divided into two areas in the circumferential direction with the joint at the center, but in this specification, the areas on both circumferential directions are combined and considered to be one area. An example of the area where the recess is formed is shown in Fig. 4.
[0046] Fig. 4 is a schematic plan view of the seal ring similar to Fig. 3, and shows the location where the recesses are formed. Note that the step and inclined surfaces are also omitted in Fig. 4. In Fig. 4, the seal ring is divided into regions of a predetermined angle on the circumference, and the presence or absence of the recesses and the depth of the recesses are distinguished between these regions.
[0047] Specifically, when the central angle of the middle part of the joint 19 relative to the circumferential center point O of the seal ring 11 is set to 0°, straight lines of 45° are drawn on both sides in the circumferential direction from the position of the central angle of 0° to divide the seal ring 11 into four equal parts. In this case, the area near joint 19 is a 0° area (an area extending from 45° on one side to 45° on the other side (in 360° notation, an area extending from 45° to 0° to 315°)), the area facing joint 19 is a 180° area (an area extending from 135° on one side to 135° on the other side (in 360° notation, an area extending from 135° to 180° to 225°)), and the remaining two areas are 90° areas (an area extending from 45° to 135° each (in 360° notation, an area extending from 45° to 90° to 135°, and an area extending from 225° to 270° to 315°)).
[0048] In FIG. 4, the recess 17 has a first recess 15 and a second recess 16 that is shallower than the first recess 15, the first recess 15 being formed in the 0° region, and the second recess 16 being formed in the 180° region. On the other hand, no recess is formed in the two 90° regions. That is, the first recess 15 and the second recess 16 are not connected, and no recess is formed on the inner circumferential surface between them. In FIG. 4, the depth of the first recess 15 is formed constant in the 0° region, and the depth of the second recess 16 is formed constant in the 180° region. Even when the depth of each recess is changed, the second recess 16 is set to be shallower than the first recess 15.
[0049] In FIG. 4, the angular range of each region is set to 90°, that is, within a range of 45° on both sides in the circumferential direction from the center of each region (such as the middle part of the joint or the opposing position of the joint), but it may be set to a range smaller than 45° on both sides in the circumferential direction.
[0050] In addition, a cross-sectional view of a portion near the gap and a cross-sectional view of a portion facing the gap in the configuration of FIG. 4 are similar to the cross-sectional views shown in FIG.
[0051] The seal ring of the present invention is an injection molded article of a resin composition. Any synthetic resin that can be injection molded can be used as the base resin of the resin composition. For example, thermoplastic polyimide resin, polyether ketone (PEK) resin, polyether ether ketone (PEEK) resin, polyphenylene sulfide (PPS) resin, polyamide imide (PAI) resin, polyamide (PA) resin, polybutylene terephthalate (PBT) resin, polyethylene terephthalate (PET) resin, polyethylene (PE) resin, polyacetal (POM) resin, phenol (PF) resin, etc. can be mentioned. These resins may be used alone or may be mixed with two or more kinds to form a polymer alloy. Among these resins, it is preferable to use PEK resin, PEEK resin, PPS resin, or PAI resin as the base resin, since they are particularly excellent in friction and wear properties, flexural modulus, heat resistance, and sliding properties. These resins have a high elastic modulus and are unlikely to crack even when expanded in diameter when fitted into the annular groove. They can also be used when the temperature of the hydraulic oil to be sealed is high, and there is no risk of solvent cracking.
[0052] If necessary, the base resin may be blended with fibrous reinforcing materials such as carbon fiber, glass fiber, and aramid fiber, spherical fillers such as spherical silica and spherical carbon, scaly reinforcing materials such as mica and talc, and microfiber reinforcing materials such as potassium titanate whiskers. In addition, solid lubricants such as polytetrafluoroethylene (PTFE) resin, graphite, and molybdenum disulfide, sliding reinforcing materials such as calcium phosphate and calcium sulfate, and pigments such as carbon black may also be blended. These may be blended alone or in combination.
[0053] The above-mentioned raw materials are melt-kneaded to form molding pellets, which are then molded into a desired shape by injection molding. Figure 5 shows a process diagram of the molding die. As shown in Figure 5(a), the molding die has a fixed die 21, a movable die 22, and a core pin 23, which are brought into collision to form a cavity 24. A molten resin composition is filled into the cavity 24, and after pressure retention, the molded body 25 is cooled for a certain period of time to obtain a molded body 25. A recess 25a is provided on the inner peripheral surface of the molded body 25, and a protrusion 23a is formed on the core pin 23 corresponding to the recess of the recess 25a.
[0054] 5(b), the movable mold 22 and the core pin 23 are moved in the X direction relative to the fixed mold 21. At this time, the recess 25a is caught by the protrusion 23a of the core pin 23, so that the molded body 25 also moves in the X direction following the movement of the core pin 23. In this way, the recess 25a becomes an undercut portion and the molded body 25 is physically fixed, so that the molded body 25 is prevented from sticking to the fixed mold 21.
[0055] Thereafter, as shown in FIG. 5(c), the core pin 23 is advanced in the Y direction toward the fixed die 21, so that the molded body 25 is released from the movable die 22. Then, as shown in FIG. 5(d), the engagement portion 26a of the removal hand 26 is engaged with a part of the ring side surface 25b of the molded body 25 and moved in the Z direction, so that the molded body 25 is removed from the core pin 23. At this time, as described above, the depth of the recess in the portion facing the joint is shallower than the depth of the recess in the vicinity of the joint, so that the core pin is prevented from getting caught at that portion, making it easier to remove. The joint of the removed molded body 25 has a pair of ends separated from each other, but is closed by heat fixing or the like, and the seal ring 1 shown in FIG. 1 is obtained.
[0056] The outline of the use of the seal ring will be explained with reference to FIG. 6. The seal ring 1 is mounted in an annular groove 31a provided in a rotating shaft 31 inserted into an axial hole 32a of a housing 32. The arrow in the figure indicates the direction in which pressure from the hydraulic oil is applied, and the right side in the figure is the non-sealed fluid side. The seal ring 1 is in slidable contact with the side wall surface 31b of the annular groove 31a on the non-sealed fluid side at its ring side surface 4. In addition, the ring outer peripheral surface 3 is in contact with the inner peripheral surface of the axial hole 32a. This seal structure seals the annular gap between the rotating shaft 31 and the axial hole 32a. In addition, the type of hydraulic oil used is appropriate depending on the application, and is used under conditions of, for example, an oil temperature of about -30 to 150°C, an oil pressure of about 0 to 3 MPa, and a rotation speed of the rotating shaft of about 0 to 7000 rpm.
[0057] As shown in Fig. 6, in the seal ring 1, no recesses that would become undercuts are formed on the ring outer peripheral surface 3 or ring side surface 4, which are related to oil leakage, and low oil leakage can be maintained by forming recesses 7 on the ring inner peripheral surface 2. Furthermore, the recesses 7 suppress adhesion to the fixed die when the die is opened, so that deformation due to adhesion and further deformation due to catching on a core pin when removing the molded body, such as deterioration in flatness of the ring side surface 4, can be suppressed, which results in maintaining low oil leakage.
[0058] The seal ring 41 shown in Fig. 7 has a different configuration of the inclined portion provided on the outer peripheral surface compared to the seal ring 1 in Fig. 2. Fig. 7(a) is a cross-sectional view of the seal ring, and Fig. 7(b) is an enlarged view of a part of it. Note that a description of the configuration other than the inclined portion will be omitted.
[0059] As shown in Figure 7, the inclined portion has an inclined surface 46 connected to the ring side surface 44, a step surface 48 connected perpendicularly to the ring outer peripheral surface 43, and a connection surface 49. The step surface 48 is a surface formed by parting the dies (also called a parting surface), and in this configuration, the parting surfaces of the fixed side die and the movable side die are positioned on an extension line of the step surface 48 of the seal ring 41. The provision of the step surface 48 reduces variation in the outer diameter dimension of the seal ring. On the other hand, if the parting step is large, there is a risk of the seal ring seizing when assembled to the housing, so the height t of the step surface 48 in the radial direction of the ring is set to 100 mm. c (See FIG. 7(b)) is preferably 0.1 mm or less, and more preferably 0.01 mm to 0.05 mm.
[0060] The seal ring 41 shown in Fig. 7 has inclined portions on both sides of the ring outer circumferential surface 43. Of the inclined portions on both sides, one of the inclined portions has a step surface 48, and the other inclined portion is composed only of an inclined surface. It is preferable that the step surface 48 is formed on the inclined portion on at least one side, and it may be formed symmetrically on the inclined portions on both sides. In this case, the inclined portions on both sides have a step surface, eliminating dependency on the assembly direction.
[0061] 7, a connection surface 49 perpendicular to the ring side surface 44 is provided between the inclined surface 46 and the step surface 48. By providing the connection surface 49, the step surface 48 can be easily accommodated within the inclined portion. The connection surface 49 may be a surface that is approximately perpendicular to the ring side surface 44, and may be formed as a flat surface or a curved surface. The width w of the connection surface 49 in the ring axial direction is c (See FIG. 7(b)) is, but is not limited to, the height t c It is preferable that the width w c For example, the thickness is preferably 0.05 mm to 0.3 mm, and more preferably 0.05 mm to 0.1 mm.
[0062] 8(a) illustrates the positional relationship between the inclined surface and the step surface. As shown in FIG. 8(a), if an imaginary plane extending from the inclined surface 46 is f, the step surface 48 is located radially inward of the imaginary plane f. In other words, the corner P, which is the boundary between the ring outer peripheral surface 43 and the step surface 48, does not protrude radially outward from the imaginary plane f. By positioning the step surface 48 on the inside of the inclined portion in this manner, even when the inclined surface 46 is pressed against the tapered portion of the housing, the step surface 48 (including the corner P) can be prevented from hitting the end surface of the housing, and seizing can be prevented.
[0063] FIG. 8(b) shows a modified example of the step surface of the inclined portion. As shown in FIG. 8(b), the step surface 48' is formed by a curved surface that is approximately perpendicular to the ring outer peripheral surface 43, and the boundary between the ring outer peripheral surface 43 and the step surface 48' is formed in an R-shape. The step surface 48' is obtained, for example, by polishing the corner P shown in FIG. 8(a) by barrel polishing or the like. By making the boundary portion R-shaped, it is possible to further prevent the step surface 48' from being scuffed. Note that, even in the modified example of FIG. 8(b), the step surface 48' is located inside the imaginary plane f in the ring radial direction.
[0064] 1 to 8 show a seal ring having an inclined portion on the outer circumferential surface of the ring, but the seal ring of the present invention is not limited to this and can also be applied to a seal ring that does not have the inclined portion, that is, a seal ring whose corners are not chamfered. Also, while the seal ring of the present invention has a pair of steps recessed in the ring radial direction at both ends in the ring axial direction, the seal ring of the present invention is not limited to this and can also be applied to a seal ring that does not have the steps.
[0065] Further, a method for manufacturing a seal ring according to the present invention includes a molding step of clamping a movable die and a core pin against a fixed die and filling a cavity formed by these with molten resin to mold a seal ring, a die opening step of moving the movable die and the core pin in one direction relative to the fixed die to open the die, and an ejection step of moving the core pin in the opposite direction to the die opening step to eject an inner diameter side end of the seal ring with a step provided on an outer circumferential surface of the core pin, wherein the core pin has a convex portion that protrudes radially outward on its outer circumferential surface on the tip side beyond the step, and the die opening step In the ejection step, the convex portion is caught in a concave portion formed in the inner peripheral surface of the seal ring corresponding to the convex portion, so that the seal ring moves together with the core pin. The method includes a removal step of, after the ejection step, engaging a jig with a side surface of the seal ring held by the core pin and moving the jig to remove the seal ring from the core pin, the height of the convex portion at the opposing portion of the gap is lower than the height of the convex portion at the vicinity of the gap, and in the removal step, the gap is removed from the core pin while expanding in diameter. In the removal step, it is preferable that the timing of the seal ring coming off the core pin is almost the same at the vicinity of the gap and the opposing portion of the gap. The shape of the convex portion of the core pin is configured to correspond to the shape of the concave portion of the seal ring described above.
[0066] The molding die for the seal ring according to the present invention includes the above-mentioned fixed die, the above-mentioned movable die, and the above-mentioned core pin. EXAMPLES
[0067] Examples 1 and 2, Comparative Examples 1 and 2 Seal rings of various shapes were manufactured by injection molding using a resin composition in which PEEK resin was blended with PTFE powder and carbon fiber. The dimensions of the seal rings in each Example (see FIG. 9) and Comparative Example (see FIG. 10) were an outer diameter of φ41 mm, a ring width (axial length) of 2.1 mm, and a ring thickness (radial length) of 1.95 mm, and the joint shape was the composite step cut shown in FIG. 1. The step and inclined surfaces are omitted from the illustration in FIG. 9 and FIG. 10(a).
[0068] In Examples 1 and 2, the cross-sectional shapes in the vicinity and the opposing portion are as shown in FIG. 2. In Example 1, a groove is formed as a recess over the entire circumference, and the circumferential center point of the groove is eccentrically formed toward the joint side with respect to the circumferential center point of the seal ring. In Example 2, a first recess is formed in the 0° region, and a second recess that is shallower than the first recess is formed in the 180° region, and the depth of each recess is constant. Comparative Example 1 is positioned as a conventional example, and the groove is formed with a constant depth over the entire circumference. In Example 2 and Comparative Example 1, the width of each recess is constant, and in Example 1, the width of the recess in the opposing portion is shorter than the width of the recess in the vicinity. In Comparative Example 2, no recess is formed on the inner peripheral surface as an undercut portion. The molds of each Example and Comparative Example are common except for the core pin.
[0069] In Example 1, the depth of the recess in the vicinity was 4.6% of the ring thickness, the depth of the recess in the facing portion was 1.5% of the ring thickness, and the depth of the recess in the vicinity was about three times the depth of the recess in the facing portion. In Example 2, the depth of the recess in the vicinity was 4.1% of the ring thickness, the depth of the recess in the facing portion was 1.5% of the ring thickness, and the depth of the recess in the vicinity was about 2.7 times the depth of the recess in the facing portion.
[0070] <Injection moldability test> The seal rings of each Example and Comparative Example were manufactured by injection molding. Before manufacturing the seal rings of each Example and Comparative Example, the mold was cleaned, and no mold release agent was used in each test. Continuous injection molding was performed from the first shot up to an upper limit of 1000 shots, and the presence or absence of sticking to the mold up to that point was confirmed. The presence or absence of sticking was determined by observing the fixed side mold when the mold was opened, and the number of shots at which sticking occurred was entered in Table 1. Continuous operation was performed twice for each Example and Comparative Example 1, and only once for Comparative Example 2. The results are shown in Table 1.
[0071] [Table 1]
[0072] As shown in Table 1, Examples 1 and 2 were able to perform more continuous molding than Comparative Example 1 with the conventional configuration. The reason for this is believed to be that Examples 1 and 2 were able to correct the imbalance in releasability from the core pin between the adjacent and opposing parts in Comparative Example 1. In Comparative Example 2, sticking occurred within 30 shots, so the second continuous operation was omitted.
[0073] <Oil leak test> The oil leakage amount of each seal ring obtained in the injection moldability test was evaluated by a test machine shown in FIG. 11. FIG. 11 is a schematic diagram of the test machine. Two seal rings that were injection molded last in each of two injection moldability tests (continuous operation) were used, and these were thermally fixed with the joints closed, and then mounted in the annular groove of the mating shaft 33. In the oil leakage test, the housing 34 was rotated by a motor (not shown) with the mating shaft 33 fixed, oil was pumped from the hydraulic unit 36 and supplied to the annular gap between the seal rings 35 and 35', and the oil leakage amount (ml / min) was measured. The test conditions were an oil pressure of 2 MPa, a rotation speed of 2000 rpm, and an oil temperature of 120°C, and ATF was used as the oil. The results are shown in Table 2. The oil leakage test of the seal ring of Comparative Example 2 was omitted.
[0074] [Table 2]
[0075] As shown in Table 2, Examples 1 and 2 had a lower amount of oil leakage than Comparative Example 1. This is thought to be because, of the seal rings used in the oil leakage test, Comparative Example 1 used two seal rings that had become stuck in the injection moldability test, while Example 1 used two seal rings that had not become stuck, and Example 2 used one seal ring that had become stuck. It is thought that even in Comparative Example 1, if a seal ring that did not become stuck to the core pin had been used, the amount of oil leakage would have been about the same as Example 1.
[0076] Looking at the depth of the recesses (see Table 1), the depth of the recesses in the vicinity is deeper in Examples 1 and 2 than in Comparative Example 1. Also, the depth of the recesses in the opposing portion is shallower in Examples 1 and 2 than in Comparative Example 1. In this way, by making the depth of the recesses different depending on the circumferential position of the seal ring, in other words, by considering that the gap widens, the depth of the portion near the gap is made deeper and the depth of the portion opposing the gap is made shallower, so that the recesses do not stick to the fixed mold and can be easily removed from the protrusion of the core pin.
[0077] As described above, in each of the examples, the seal ring did not stick to the mold and was easy to remove from the mold, so deformation of the seal ring was suppressed and low oil leakage was maintained. [Industrial Applicability]
[0078] The seal ring of the present invention suppresses the occurrence of sticking when the mold is opened, and does not deform into an irregular shape when removed, so that it can maintain low oil leakage, and can be used as a seal ring where low oil leakage is required between a rotating shaft and a housing. In particular, it can be suitably used for hydraulic equipment such as AT and CVT in automobiles, etc., to improve fuel efficiency. [Explanation of symbols]
[0079] 1 Seal ring 2 Ring inner surface 3 Ring outer surface 4, 4' Ring side 5, 5' stepped section 6 Slope 7 Recess 8, 8' ends 9 Joint 11 Seal ring 12 Ring inner surface 13 Ring outer surface 14 Ring side 15 First recess 16 Second recess 17 Recess 18, 18' ends 19 Joint 21 Fixed side mold 22 Movable mold 23 Core pin 24 Cavity 25 Molded body 26 Removal Hand 31 Rotation axis 32 Housing 33 Mating shaft 34 Housing 35, 35' Seal ring 36 Hydraulic Unit
Claims
1. A seal ring is attached to an annular groove provided in a rotating shaft inserted into a shaft hole of a housing, and slidably contacts a side wall surface on a non-sealed fluid side of the annular groove and also contacts an inner peripheral surface of the shaft hole to seal an annular gap between the rotating shaft and the shaft hole, The seal ring is an injection-molded body of a resin composition, has a joint in part of its circumferential direction, and has a recess on its inner circumferential surface that is recessed in the radial direction of the ring, and the depth of the recess is shallower at the portion facing the joint than at the portion near the joint.
2. 2. The seal ring according to claim 1, wherein the depth of the portion adjacent to the gap is 1.1 to 2.2 times the depth of the portion facing the gap.
3. 3. The seal ring according to claim 1, wherein the recess is a groove formed continuously in the circumferential direction from one end to the other end constituting the gap, and the depth of the groove increases continuously or stepwise from the opposing portion of the gap to the portion in the vicinity of the gap.
4. 3. The seal ring according to claim 1, wherein the recess is a groove formed continuously in the circumferential direction from one end to the other end constituting the gap, and the groove is formed so that its circumferential center point is eccentric toward the gap with respect to the circumferential center point of the seal ring.
5. 3. The seal ring according to claim 1, characterized in that the recess has a first recess formed in the vicinity of the gap and a second recess formed opposite the gap, the first recess and the second recess being unconnected and no recess is formed on the inner circumferential surface between them.
6. 3. The seal ring according to claim 1, further comprising an inclined portion on at least one end of the outer circumferential surface.
Citation Information
Patent Citations
Seal ring
JP2022013442A
Manufacturing method of seal ring and molding metal mold
JP2022146093A
Seal ring
WO2004011827A1