Friction stir joining method
The method addresses hole formation in friction stir welding by using a second tool to seal the hole left by the first tool, ensuring seamless welding without additional tool removal steps.
Patent Information
- Application Number
- JP2023047422
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
The existing friction stir welding method leaves holes at the end position when the tool is withdrawn, requiring time and effort to remove tabs.
A method involving a first tool for welding and a second tool for closing the hole, where the second tool is left with a probe in the hole to seal it, and the first tool is replaced or broken to minimize hole formation.
The method effectively seals the hole without additional tools and reduces the need for grinding, allowing for efficient and seamless welding without tool remnants.
Smart Images

Figure 2024136334000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for friction stir welding two or more workpieces. [Background technology]
[0002] Friction stir welding (FSW) is a type of solid-state joining method developed by TWI in the UK in 1991, and has various features not found in conventional welding methods. For example, the maximum temperature reached does not reach the melting point, and joining occurs in a solid state, so there is less loss of strength in the joint compared to welding methods.
[0003] Patent Document 1 discloses a method for friction stir welding two or more workpieces. In this method, a rotating tool is first pressed into the workpieces. The pressing of the rotating tool generates frictional heat between the tool and the workpieces, and the temperature of the workpieces (materials) around the tool rises. When the material is heated sufficiently to a temperature at which it can start plastic flow, it flows around the rotating tool in the direction of the tool's rotation. At this time, parts of the material on the left and right of the tool are forcibly mixed together, realizing welding in the peripheral area of the tool. When the tool is moved along the welding line, a weld is continuously formed on the rear side of the tool's movement. When the tool reaches the desired end position, the tool is pulled out to complete the welding.
[0004] However, when the tool is withdrawn, a hole of the tool remains at the end position where the tool was withdrawn. In order to prevent the hole of the tool from remaining, in the friction stir welding method described in Patent Document 1, a tab is provided at the end position of the workpieces, the tool is moved to the tab, and the tool is withdrawn from the tab so that the hole of the tool does not remain in the workpieces. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2002-539949 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the friction stir welding method described in Patent Document 1 has a problem in that it takes time and effort to remove the tab.
[0007] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a friction stir welding method that can plug holes in the workpieces caused by withdrawal of the tool, or that does not cause holes in the workpieces even when the tool is withdrawn. [Means for solving the problem]
[0008] In order to solve the above-mentioned problems, one aspect of the present invention is a friction stir welding method comprising the steps of: pushing a rotating first tool into two or more workpieces, moving the first tool along a welding line, and withdrawing the first tool from the workpieces; replacing the first tool with a second tool; pushing the rotating second tool into a hole created by the withdrawal of the first tool; and leaving at least a probe of the second tool in the hole.
[0009] Another aspect of the present invention is a friction stir welding method comprising the steps of: pressing a rotating tool into two or more workpieces; and breaking the tool to leave a probe of the tool in the workpieces. Effect of the Invention
[0010] According to one aspect of the present invention, the probe of the second tool is left in the hole formed by the withdrawal of the first tool, so that the hole can be plugged by the probe. Also, since the first tool and the second tool are exchanged, it is possible to use tools suitable for each of the first tool for friction stir welding and the second tool for plugging the hole.
[0011] According to another aspect of the present invention, the tool is broken and the probe of the tool is left in the workpieces, so that no hole is formed in the workpieces even when the tool is pulled out. Also, because the tool is broken, the part of the tool that needs to be removed with a grinder or the like can be reduced. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a process diagram of a friction stir welding method according to a first embodiment of the present invention (showing a process of joining two workpieces by using a first tool). [Diagram 2] FIG. 2 is a process diagram of the friction stir welding method according to the first embodiment of the present invention (showing a process of closing a hole by using a second tool). [Diagram 3] 5A to 5C are process diagrams of a friction stir welding method according to a second embodiment of the present invention. [Figure 4] FIG. 13 is a perspective view showing an example of joining a pipe material as a workpiece. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, a friction stir welding method according to an embodiment of the present invention will be described with reference to the accompanying drawings. However, the friction stir welding method according to the present invention can be embodied in various forms and is not limited to the embodiments described in this specification. This embodiment is provided with the intention of enabling a person skilled in the art to fully understand the invention by fully disclosing the specification. (First embodiment)
[0014] 1 and 2 show process diagrams of a friction stir welding method according to a first embodiment of the present invention. Fig. 1 shows steps (S1 to S4) of joining two workpieces 1, 2 using a first tool 11. Fig. 2 shows steps (S5 to S7) of sealing a hole 4 formed by withdrawing the first tool 11 using a second tool 12. Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1.
[0015] The workpieces 1 and 2 are metal plate materials. The workpieces 1 and 2 may be pipe materials. The material of the workpieces 1 and 2 is not particularly limited, and may be, for example, iron, steel, stainless steel, aluminum, aluminum alloy, etc.
[0016] The joining of the workpieces 1 and 2 begins with steps (S1, S2) of pressing a rotating first tool 11 into the workpieces 1 and 2. The first tool 11 is attached to a holder 13 that rotates about an axis L by a set screw 14 or the like. The first tool 11 attached to the holder 13 rotates together with the holder 13 about the axis L.
[0017] The first tool 11 includes a probe 11b (also called a pin) and a shoulder 11a. The probe 11b penetrates the workpieces 1 and 2 to generate frictional heat and induce plastic flow around the probe 11b. The shoulder 11a comes into contact with the surfaces of the workpieces 1 and 2 to generate frictional heat and induce plastic flow near the surfaces of the workpieces 1 and 2.
[0018] The first tool 11 is made of a material that is stronger than the workpieces 1 and 2 and can withstand the frictional heat generated during joining. For example, when the workpieces 1 and 2 are steel or stainless steel, the tool 11 is made of PCBN, a ceramic material, a cemented carbide, or the like. When the workpieces 1 and 2 are aluminum or an aluminum alloy, the first tool 11 is made of tool steel, or the like.
[0019] As the rotating first tool 11 is pressed in, frictional heat is generated between the first tool 11 and the workpieces 1, 2, causing the temperature of the workpieces 1, 2 (material) around the first tool 11 to rise. When the material is sufficiently heated to a temperature at which it can start to plastically flow, the material flows around the rotating first tool 11 in the direction of rotation of the first tool 11. At this time, parts of the material arranged on the left and right of the first tool 11 are forcibly mixed, and the workpieces 1, 2 are joined in the peripheral area of the first tool 11.
[0020] When the first tool 11 is moved along the joint line, a joint 3 is continuously formed behind the movement of the first tool 11 (S3). When the first tool 11 reaches the target end position, it is pulled out from the workpieces 1 and 2 (S4), and a hole 4 is formed in the joint 3 by the pulling out of the first tool 11.
[0021] 2, the first tool 11 is replaced with the second tool 12 (S5). For example, the set screw 14 is loosened to remove the first tool 11 from the holder 13, the second tool 12 is attached to the holder 13, and the set screw 14 is tightened to fix the second tool 12 to the holder 13.
[0022] The second tool 12 is made of the same material as the workpieces 1 and 2. That is, if the workpieces 1 and 2 are iron, the second tool 12 is also iron, if the workpieces 1 and 2 are steel, the second tool 12 is also steel, if the workpieces 1 and 2 are stainless steel, the second tool 12 is also stainless steel, if the workpieces 1 and 2 are aluminum, the second tool 12 is also aluminum, and if the workpieces 1 and 2 are aluminum alloy, the second tool 12 is also aluminum alloy.
[0023] The second tool 12 is preferably of the same standard and the same grade or higher as the materials to be welded 1, 2. For example, if the materials to be welded 1, 2 are SM490, the second tool 12 is preferably of SM490 or higher (SM490, SM520, etc.). SM material is a rolled steel material for welded structures specified in JIS G 3106:2015. Also, if the materials to be welded 1, 2 are pipe materials and are API X52, the second tool 12 is preferably of API X52 or higher (X52, X60, X65, etc.). API is a standard established by the American Petroleum Institute. Line pipes are standardized in API.
[0024] The second tool 12 includes a probe 12b and a shoulder 12a, similar to the first tool 11. The diameter of the probe 12b of the second tool 12 is preferably the same as the probe 11b of the first tool 11 or 0 to 20% larger. The inventors have confirmed through experiments that the probe 12b of the second tool 12 can be friction stir welded to the hole 4 of the workpieces 1 and 2 when the diameter of the probe 12b of the second tool 12 is the same as the probe 11b of the first tool 11, when it is 5% larger, or when it is 10% larger. In addition, when it is 20% larger, it has been confirmed that the probe 12b of the second tool 12 does not enter the hole 4 and is broken.
[0025] Next, the rotating second tool 12 is pressed into the hole 4 of the workpieces 1, 2 (S6). The pressure and rotation of the second tool 12 are then maintained for a predetermined time, for example, 5 to 15 seconds. As the rotating second tool 12 is pressed into place, frictional heat is generated between the second tool 12 and the workpieces 1, 2 around the hole 4 (joint portion 5 shown by the thick line in FIG. 2 (S6)), inducing plastic flow or melting. When the rotation of the second tool 12 is stopped, the second tool 12 and the workpieces 1, 2 are joined at the joint portion 5 shown by the thick line in FIG. 2 (S6).
[0026] Next, when the second tool 12 is pulled out from the workpieces 1 and 2, the second tool 12 breaks and the probe 12b of the second tool 12 is left in the hole 4, and the hole 4 is blocked by the probe 12b (S7). Here, the second tool 12 breaks at the boundary between the shoulder 12a and the probe 12b. This is because the boundary between the shoulder 12a and the probe 12b is a portion with a discontinuous shape and is a stress concentration portion. In order to break the second tool 12 at a desired position, a microcrack may be formed in advance at a desired position of the second tool 12.
[0027] When the rotating second tool 12 is pressed into the hole 4 of the workpieces 1, 2, the back sides of the workpieces 1, 2 may be preheated by a panel heater, laser heating, induction heating, gas burner, or the like (not shown). By preheating the back sides of the workpieces 1, 2, heat can be supplied to the workpieces 1, 2 on the tip side of the second tool 12 where frictional heat is less likely to be generated, and plastic flow or melting can be promoted in this portion.
[0028] If micro defects occur in the joint 5 of the thick wire, the hole 4 may be filled with powder 6 made of the same material as the workpieces 1 and 2 (S5), and then the rotating second tool 12 may be pressed into the hole 4 filled with the powder 6. The definition of "same material" is as described above. By filling the hole 4 with powder 6 made of the same material as the workpieces 1 and 2, the micro defects in the joint 5 are improved.
[0029] 1, the back sides of the workpieces 1 and 2 may be welded along the butt joints. By welding the back sides of the workpieces 1 and 2 along the butt joints, it is possible to prevent streaks from appearing on the back sides of the workpieces 1 and 2 due to differences in plate thickness, etc.
[0030] The probe 12b and shoulder 12a of the second tool 12 may be configured to be separate and to fit into each other, so that when the second tool 12 is pulled out from the workpieces 1 and 2, the shoulder 12a of the second tool 12 is separated from the probe 12b without breaking the second tool 12. Also, only the holder 13 may be pulled out, and the shoulder 12a and probe 12b of the second tool 12 integrated together may be left in the hole 4 of the workpieces 1 and 2. The effects of the friction stir welding method of this embodiment will be described below.
[0031] Since the probe 12b of the second tool 12 is left in the hole 4 created by the withdrawal of the first tool 11, the hole 4 can be blocked by the probe 12b. Furthermore, since the first tool 11 and the second tool 12 are exchanged, it is possible to use tools suitable for the first tool 11 for friction stir welding and the second tool 12 for blocking the hole 4. For example, a tool having a higher strength than the workpieces 1 and 2 and capable of withstanding frictional heat generated during welding can be used for the first tool 11, and a tool made of the same material as the workpieces 1 and 2 can be used for the second tool 12.
[0032] Since the second tool 12 is broken and the probe 12b of the second tool 12 is left in the hole 4, the portion of the second tool 12 to be removed by a grinder or the like can be reduced.
[0033] Since the diameter of the probe 12 b of the second tool 12 is equal to or larger than the diameter of the probe 11 b of the first tool 11 , plastic flow or melting can be induced around the second tool 12 .
[0034] Since the hole 4 is filled with powder 6 made of the same material as the workpieces 1 and 2, minute defects in the joint portion 5 of the thick wire can be improved.
[0035] Since the rear surfaces of the workpieces 1 and 2 are preheated, the plastic flow or melting of the workpieces 1 and 2 on the tip side of the second tool 12 can be promoted. Second Embodiment
[0036] 3 shows a process diagram of a friction stir welding method according to a second embodiment of the present invention. The friction stir welding method according to the second embodiment is friction stir spot welding. Reference numerals 1 and 2 denote workpieces, reference numeral 13 denotes a holder, and reference numeral 12 denotes a tool. The configurations of the holder 13 and the tool 12 are the same as those of the holder 13 and the second tool 12 in the first embodiment, so the same reference numerals are used and the description thereof is omitted.
[0037] In the second embodiment, the joining of the workpieces 1 and 2 begins with a step (S1) of pressing a rotating tool 12 into the workpieces 1 and 2. Pressing the rotating tool 12 achieves joining of the workpieces 1 and 2 in the peripheral area of the tool 12. At the same time, frictional heat is generated between the tool 12 and the workpieces 1 and 2 (joint portion 5 shown by the thick line in FIG. 3 (S2)), inducing plastic flow or melting. When the rotation of the tool 12 is stopped, the tool 12 and the workpieces 1 and 2 are joined at the joint portion 5 shown by the thick line.
[0038] Next, when the tool 12, whose rotation has stopped, is pulled out from the workpieces 1 and 2, the tool 12 breaks and the probe 12b remains in the workpieces 1 and 2 (S3). Therefore, even when the tool 12 is pulled out, no holes are formed in the workpieces 1 and 2. In addition, because the tool 12 breaks, the portion of the tool 12 that needs to be removed with a grinder or the like can be reduced.
[0039] It should be noted that the present invention is not limited to the above-described embodiment, and can be embodied in other embodiments without departing from the spirit and scope of the present invention.
[0040] In the above embodiment, an example in which plate materials are joined as the materials to be joined has been described, but pipe materials 21, 22 may also be joined as the materials to be joined, as shown in Fig. 4. When joining the pipe materials 21, 22, the rotating tool 11 is moved in the radial and circumferential directions. The pipe materials 21, 22 may be joined from the outer surface side, or from the inner surface side.
[0041] In the above embodiment, an example has been described in which the workpieces are butted together and joined, but it is also possible to join overlapping workpieces. [Explanation of symbols]
[0042] 1,2…material to be joined 3,5…Joint part 4…Hole 6…Powder 11…1st Tour 11a…Shoulder 11b…Probe 12…2nd Tour 12a…Shoulder 12b…Probe
Claims
1. a step of pressing a rotating first tool into two or more workpieces, moving the first tool along a joining line, and pulling the first tool out of the workpieces; replacing the first tool with a second tool; forcing the rotating second tool into a hole created by withdrawal of the first tool; leaving at least the probe of the second tool in the hole.
2. 2. The friction stir welding method according to claim 1, further comprising the step of breaking the second tool and leaving a probe of the second tool in the hole.
3. 3. The friction stir welding method according to claim 1, wherein the second tool is made of the same material as the workpieces.
4. 3. The friction stir welding method according to claim 1, wherein a diameter of the probe of the second tool is equal to or larger than a diameter of the probe of the first tool.
5. 3. The friction stir welding method according to claim 1, wherein the hole is filled with powder made of the same material as the workpiece, and thereafter, the rotating second tool is pushed into the hole.
6. 3. The friction stir welding method according to claim 1, wherein a rear surface side of the workpieces is preheated when the rotating second tool is pushed into the hole.
7. A step of forcing a rotating tool into two or more workpieces; and breaking the tool to leave a probe of the tool on the workpieces.
8. A joint of two or more workpieces, A joint in which the probe of the broken tool is friction stir welded or fusion welded to the joint.
Citation Information
Patent Citations
Joining method of metal stock
JP1998230372A
Method for bonding ferrous material
JP2012040584A
Junction method
JP2015213930A
Reinforcement method and friction pressure-welding junction structure
JP2022143812A
Method and apparatus for welding two workpieces
JP2002539949A