Curable resin composition

The curable resin composition with organically modified silicone oil and silane compound maintains matte finish and mechanical properties across a wide temperature range, addressing the issue of high-temperature gloss loss in existing compositions.

JP2024136473APending Publication Date: 2024-10-04SHARP KAGAKU INDS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023047600
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing curable resin compositions used for waterproofing and surface protection lose their matte finish at high temperatures, compromising mechanical properties and design integrity.

Method used

A curable resin composition containing specific ratios of an organically modified silicone oil, a silane compound, and a polymer with hydrolyzable silicon groups, which maintains matte finish and mechanical properties across a wide temperature range.

Benefits of technology

The composition provides a stable matte surface and maintains mechanical properties from 0 to 80°C, ensuring durability and design consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136473000001
    Figure 2024136473000001
  • Figure 2024136473000002
    Figure 2024136473000002
  • Figure 2024136473000003
    Figure 2024136473000003
Patent Text Reader

Abstract

To provide a curable resin composition capable of providing a further sufficient matte state to a surface after curing at any temperature from high temperature to low temperature without compromising mechanical properties (e.g., mechanical properties as a sealant, an adhesive and a coating material).SOLUTION: The curable resin composition contains 100 pts.wt. of a polymer having a hydrolyzable silicon group, 0.5 to 8.0 pts.wt. of an organically modified silicone oil, and 2.0 to 15.0 pts.wt. of a silane compound represented by a specific general formula.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition, and more particularly to a curable resin composition that imparts a matte surface after curing. [Background technology]

[0002] Curable resin compositions containing a curable resin such as a polyurethane resin or a modified silicone resin are widely used for the purpose of waterproofing and surface protection of buildings, civil engineering structures, etc. Curable resin compositions are useful as sealant compositions, waterproofing compositions, coating compositions, etc. After these curable resin compositions are cast or applied to the application site, if dust or dirt adheres to the composition during curing, the surface becomes contaminated and causes design defects. In addition, matte materials are often used for components of buildings, civil engineering structures, etc. to give a calm texture, and sand-like (sand-like, sandstone-like) materials are often used to give a luxurious feel. If a glossy curable resin composition is used for such components, the gloss of the component may be noticeable, causing design defects.

[0003] As a method for imparting a matte finish, it is known to add a filler or porous material with a relatively large particle size. Such fillers and porous materials include, for example, glass beads, silica beads, alumina beads, carbon beads, styrene beads, phenol beads, acrylic beads, porous silica, shirasu balloons, glass balloons, silica balloons, saran balloons, acrylic balloons, and the like, each having an average particle size of 10 to 80 μm (see Patent Documents 1 and 2). However, when such fillers or porous materials are added, there are drawbacks such as a decrease in mechanical properties such as tensile properties, making it difficult to obtain a material having sufficient properties as a sealing material.

[0004] In order to address the above problems, for example, a room-temperature curable composition having a matte surface after curing has been disclosed that comprises a propylene oxide polymer having a crosslinkable hydrolyzable silyl group at its terminal, one or more compounds selected from the group consisting of an amine compound having a melting point of 10 to 200°C, an amide compound having a melting point of 10 to 200°C, a fatty acid having a melting point of 10 to 200°C, an alcohol having a melting point of 10 to 200°C, and a fatty acid ester having a melting point of 10 to 200°C (see Patent Document 3). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-100408 [Patent Document 2] JP 2001-262125 A [Patent Document 3] JP 2004-124093 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, such room temperature curable compositions have a new problem in that when exposed to high temperatures of 50°C or higher, which simulates the extremely hot conditions of summer, the matting agent covering the cured surface melts and the surface layer disappears, resulting in the failure to achieve a matte finish.

[0007] Therefore, an object of the present invention is to provide a curable resin composition that can impart a sufficiently matte state to the surface after curing at any temperature, from high to low, without impairing the mechanical properties (e.g., the mechanical properties as a sealant, adhesive, and coating material). [Means for solving the problem]

[0008] The present invention relates to The present invention relates to a curable resin composition comprising 100 parts by weight of a polymer having a hydrolyzable silicon group, 0.5 to 8.0 parts by weight of an organic modified silicone oil, and 2.0 to 15.0 parts by weight of a silane compound represented by general formula (1).

[0009] [ka]

[0010] (In formula (1), m and n each independently represent an integer of 1 to 10; a, b and c each independently represent 1 or 2, and the relationship c=4-ab is satisfied; R 1 is a monovalent hydrocarbon radical; R 2 is a hydrogen atom or a monovalent hydrocarbon group. Effect of the Invention

[0011] The curable resin composition of the present invention can impart a sufficiently matte state to the surface after curing, even at a temperature of, for example, 0 to 80° C. (particularly, 5 to 70° C.), without impairing the mechanical properties of the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described in detail. The curable resin composition of the present invention contains a polymer having a hydrolyzable silicon group (hereinafter, sometimes referred to as "component A"), an organically modified silicone oil (hereinafter, sometimes referred to as "component B"), and a specific silane compound (hereinafter, sometimes referred to as "component C").

[0013] Component A is a polymer having a hydrolyzable silicon group, and more specifically, the main chain contains an oxyalkylene polymer (or an oxyalkylene polymer portion) or a vinyl polymer (or a vinyl polymer portion). The oxyalkylene polymer can be one or more repeating units selected from -CH2CHO-, -CH2CH(CH3)O-, -CH2CH(C2H5)O-, -CH(CH3)CHO-, -CH(C2H5)CHO-, -CH2CH2CH2O-, and -CH2CH2CH2CH2O-. -CH2CH(CH3)O- is preferred. The vinyl polymer can be polyethylene, polypropylene, polyisobutylene, poly(meth)acrylate, polystyrene, polyvinyl chloride, polyvinylidene chloride, polybutadiene, polyisoprene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, and copolymers containing two or more of the monomers constituting these polymers as monomer components. Preferably, it is a poly(meth)acrylate.From the viewpoints of further improving the matte property and mechanical properties as well as improving adhesion, a preferred component A is an oxyalkylene polymer having a hydrolyzable silicon group.

[0014] In this specification, the matte property includes the matte visibility and gloss resistance of a cured product formed from a curable resin composition, and is a property based on both of these properties. The matte visibility refers to a property in which when a curable resin composition is molded into a sheet of 3 mm thickness, left to stand for 24 hours at 5°C, 23°C or 70°C, and the cured product obtained is visually observed, the surface of the cured product obtained at any temperature has no gloss. Gloss resistance refers to the property that, when a curable resin composition is molded into a sheet of 3 mm thickness and allowed to stand at 23°C for 7 days, the surface gloss of the resulting cured product is measured with a 60° specular gloss meter, and the surface gloss shows a smaller value. The mechanical properties include the maximum strength and maximum elongation of a cured product formed from the curable resin composition, and are properties based on both of these properties. More specifically, the mechanical properties refer to the properties that, when the curable resin composition is molded into a sheet of 3 mm thickness, allowed to stand at 23°C for 24 hours, and the resulting cured product is subjected to a tensile test based on JIS K6251, both the maximum strength and the maximum elongation exhibit larger values. The adhesion is a property based on the adhesion between a cured product formed from a curable resin composition and a coating film formed on the surface of the cured product. More specifically, the adhesion refers to a property in which the paint peels off less when the curable resin composition is molded into a 3 mm thick sheet, left to stand at 23°C for 24 hours, the surface of the resulting cured product is coated with a urethane paint, left to stand at 23°C for 7 days to form a coating film, and then subjected to an adhesion test based on JIS K5600-5-6.

[0015] When an oxyalkylene polymer is used in the main chain, the molecular weight of component A is usually 500 to 30000, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving the adhesion, it is preferably 5000 to 20000, more preferably 10000 to 20000, and even more preferably 12000 to 18000. Here, the molecular weight of component A is a number average molecular weight calculated based on the hydroxyl value-converted molecular weight of the hydroxyl-terminated oxyalkylene polymer used as the raw material.

[0016] When a vinyl polymer is used in the main chain, the number average molecular weight of component A is usually 3,000 to 50,000, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving the adhesion, it is preferably 5,000 to 40,000. Here, the molecular weight of component A is a number average molecular weight calculated based on the gel permeation chromatography (GPC) method.

[0017] Component A has a hydrolyzable silicon group as a terminal group of the main chain. In component A, the introduction rate of the hydrolyzable silicon group to the molecular chain terminal is sufficient if it is 50% or more, and from the viewpoint of further improving the matte property and mechanical properties and improving the adhesion, it is preferably 70% or more, more preferably 80% or more, even more preferably 90% or more, and particularly preferably 95% or more. The introduction rate is the ratio of the number of terminals to which the hydrolyzable silicon group is introduced to the number of terminals of all the component A molecules. Here, when the terminal group of the main chain is a hydroxyl group, the introduction rate of the hydrolyzable silicon group to the molecular chain terminal can be measured by calculating the unreacted hydroxyl group after the introduction of the hydrolyzable silicon group using a hydroxyl value analysis method. In addition, as a method that is not limited to the type of terminal group, a method of calculating by quantifying the terminal group after the introduction of the hydrolyzable silicon group using an IR method or an NMR method can also be used.

[0018] The hydrolyzable silicon group can be represented, for example, by the following general formula (2).

[0019] [ka]

[0020] In formula (2), R is usually an alkyl group having 1 to 20 carbon atoms, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably an alkyl group having 1 to 10 carbon atoms, more preferably 1 to 6, still more preferably 1 to 5, and particularly preferably 1 to 3. Examples of such an alkyl group include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a tert-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group. X is a hydroxyl group or an alkoxy group having 1 to 6 carbon atoms, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably an alkoxy group having 1 to 5 carbon atoms, particularly preferably 1 to 3. Examples of such alkoxy groups include a methoxy group, an ethoxy group, an n-propoxy group, an iso-propoxy group, an n-butoxy group, an iso-butoxy group, a tert-butoxy group, an n-pentyloxy group, and an n-hexyloxy group. a is 1, 2 or 3, and from the viewpoints of further improving the matte properties and mechanical properties as well as improving adhesion, a is preferably 2 or 3, and more preferably 3.

[0021] For example, the hydrolyzable silicon group can be an alkyl dialkoxysilyl group or a trialkoxysilyl group.From the viewpoint of further improving matte finish and mechanical properties and improving adhesion, the alkyl dialkoxysilyl group is more preferably a methyl dimethoxysilyl group or a methyl diethoxysilyl group, and more preferably a methyl dimethoxysilyl group.From the viewpoint of further improving matte finish and mechanical properties and improving adhesion, the trialkoxysilyl group is more preferably a trimethoxysilyl group.

[0022] Component A can be prepared by known methods or can be obtained commercially.

[0023] As a method for introducing hydrolyzable silicon groups into an oxyalkylene polymer, a known method can be used, such as a method of producing an oxyalkylene diol by ring-opening polymerization of a cyclic ether in the presence of a bifunctional initiator, and introducing hydrolyzable silicon groups into the hydroxyl groups of this diol. In addition, as a method for introducing hydrolyzable silicon groups into a vinyl polymer, a method of copolymerizing a vinyl monomer and a hydrolyzable silicon group-containing monomer can be used. As a method for changing the introduction rate of hydrolyzable silicon groups, in the case of an oxyalkylene polymer, the molar number of hydrolyzable silicon groups relative to the hydroxyl groups of a diol can be changed. In addition, in the case of a vinyl polymer, the introduction rate of hydrolyzable silicon groups can be changed by changing the blending ratio of the hydrolyzable silicon group-containing monomer to be copolymerized.

[0024] Commercially available products of component A are marketed as modified silicone resins, and examples thereof include, but are not limited to, the following: Kaneka Corporation MS Polymer S203 (oxyalkylene polymer with methyldimethoxysilyl group) Kaneka Corporation's Silyl MA440 (a mixture of oxyalkylene polymers having methyldimethoxysilyl groups and acrylic polymers having alkoxysilyl groups) Kaneka Corporation Silyl SAX580 (oxyalkylene polymer with trimethoxysilyl group) Asahi Glass Co., Ltd. EXCESTAR S2420 (oxyalkylene polymer with methyldimethoxysilyl group) Wacker Chemie GENIOSIL STP-E30 (oxyalkylene polymer with trimethoxysilyl group)

[0025] Component B is an organically modified silicone oil, which is a non-reactive silicone oil. The term "non-reactive" refers to the reactivity with the hydrolyzable silicon group of component A described above and the Si(OR 2 ) cThis means that it has no reactivity with groups. For example, a silicone oil having a non-reactive organic group introduced into the side chain and / or end of a silicone chain (or polysiloxane chain) can be used as such a non-reactive silicone oil. For example, the non-reactive organic group can be one or more organic groups selected from the group consisting of an alkyl group, a fluoroalkyl group, a phenyl group, a polyether group, and the like.

[0026] In Component B, the alkyl group as the non-reactive organic group is an alkyl group having 1 to 10 carbon atoms, and from the viewpoints of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably an alkyl group having 1 to 6 carbon atoms, more preferably 1 to 5, and even more preferably 1 to 3. Specific examples of such alkyl groups include the same alkyl groups as those explained as R in formula (2).

[0027] In Component B, the fluoroalkyl group as the non-reactive organic group is a fluoroalkyl group having 1 to 10 carbon atoms, and from the viewpoints of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably a fluoroalkyl group having 1 to 6 carbon atoms, more preferably 1 to 5, and even more preferably 1 to 3 carbon atoms. Specific examples of such fluoroalkyl groups include fluorinated alkyl groups in which any one or more, for example 1 to 3 hydrogen atoms in the same alkyl groups as those explained as R in formula (2) have been substituted with fluorine atoms.

[0028] The polyether group as the non-reactive organic group in component B may be a polyethylene glycol group, a polypropylene glycol group, or a composite group thereof, and is preferably a polyethylene glycol group from the viewpoint of further improving the matte property and mechanical properties as well as improving the adhesion. The number of repeating units in such a polyether group is not particularly limited, and may be, for example, a value such that the molecular weight of component B is 1000 or more (particularly 4000 to 15000).

[0029] Specific examples of non-reactive silicone oils include alkyl-modified silicone oils with alkyl groups introduced as organic groups, fluoroalkyl-modified silicone oils with fluoroalkyl groups introduced as organic groups, phenyl-modified silicone oils with phenyl groups introduced as organic groups, and polyether-modified silicone oils with polyether groups introduced as organic groups. Component B is preferably polyether-modified silicone oil from the viewpoint of further improving matte properties and mechanical properties as well as improving adhesion.

[0030] In Component B, the introduction rate of the non-reactive organic group is not particularly limited, and may be, for example, such that the HLB value of the Component B molecule is 5 to 15, particularly 5 to 10. In this specification, the HLB value is a value based on "20 x sum of formula weights of hydrophilic moieties / molecular weight".

[0031] The viscosity of the organic modified silicone oil (component B) is 1500 mm from the viewpoint of further improving the matte finish and mechanical properties as well as improving adhesion. 2 / s or less is preferable, and 1300 mm 2 / s or less is preferable, and 1200mm 2 More preferably, the viscosity is 400 mm / s or less. 2 / s or more (especially 800mm 2 / s or more).

[0032] The viscosity is measured at 23° C. using a rotational viscometer.

[0033] Component B is commercially available or can be produced by a known method. Examples of commercially available products of component B include, but are not limited to, the following: Dow Toray DOWSIL L-7002 (polyether modified silicone oil in which polyethylene glycol groups have been introduced into silicone oil) Momentive Performance Materials Japan COATOSIL7510 (polyether modified silicone oil in which polyethylene glycol groups have been introduced into silicone oil)

[0034] The content of component B is 0.5 to 8.0 parts by weight relative to 100 parts by weight of component A, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably 0.5 to 4.0 parts by weight, more preferably 1.5 to 4.0 parts by weight, and even more preferably 2.0 to 3.5 parts by weight. If the content is too small, the matte properties (particularly matte properties at relatively high temperatures) decrease. If the content is too large, the matte properties (particularly matte properties at relatively high temperatures) decrease. Component B may contain two or more types of components B having different structures, and in that case, the total amount thereof may be within the above range.

[0035] Component C is a silane compound represented by general formula (1) (hereinafter sometimes simply referred to as "silane compound (1)").

[0036] [ka]

[0037] In formula (1), m is an integer of 1 to 10, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, m is preferably an integer of 1 to 6, more preferably an integer of 1 to 5, and even more preferably an integer of 2 to 4. n is an integer of 1 to 10, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, n is preferably an integer of 1 to 6, more preferably an integer of 1 to 5, and even more preferably an integer of 1 to 3.

[0038] In formula (1), a is an integer of 1 or 2, and is preferably 1 from the viewpoint of further improving the matte finish and mechanical properties as well as improving adhesion. n -NH-(CH2) mWhen a has a substituent (a-), the amino group-containing hydrocarbon groups may be independently selected. When a is 0 or an integer of 3 or more, at least one of the matte properties and the mechanical properties is reduced. b is an integer of 1 or 2, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably 1. When b is 0 or an integer of 3 or more, the matte properties decrease. c is a value corresponding to "4-ab" and is usually an integer of 1 or 2, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably 2. When c is 0 or an integer of 3 or more, the matte properties decrease.

[0039] In formula (1), R 1 R is a monovalent hydrocarbon group. 1 Specifically, R may be a monovalent saturated or unsaturated aliphatic hydrocarbon group, or may be a monovalent aromatic hydrocarbon group, and is preferably a monovalent saturated aliphatic hydrocarbon group from the viewpoint of further improving the matte property and mechanical properties as well as improving adhesion. Examples of the monovalent saturated aliphatic hydrocarbon group include alkyl groups having 1 to 10 carbon atoms, specifically including methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups. 1 From the viewpoint of further improving the matte property and mechanical properties and improving adhesion, R is preferably an alkyl group having 1 to 6 carbon atoms, more preferably 1 to 5 carbon atoms, and even more preferably 1 to 3 carbon atoms (particularly a linear alkyl group). Examples of the monovalent unsaturated aliphatic hydrocarbon group include an alkenyl group having 2 to 10 carbon atoms, preferably 2 to 7 carbon atoms, more preferably 2 to 5 carbon atoms, and even more preferably 2 to 3 carbon atoms. Specific examples of such alkenyl groups include a vinyl group, etc. Examples of the monovalent aromatic hydrocarbon group include an aryl group having 6 to 14 carbon atoms, preferably 6 to 10 carbon atoms, and even more preferably 6 carbon atoms. Specific examples of such aryl groups include a phenyl group, a naphthyl group, etc. When the silane compound (1) has a plurality of R1 If R 1 may each be independently selected.

[0040] In formula (1), R 2 R is a hydrogen atom or a monovalent hydrocarbon group. 2 The monovalent hydrocarbon group as R in formula (1) 1 From the viewpoint of further improving the matte property and mechanical properties as well as improving the adhesion, preferred R 2 R in formula (1) is a hydrogen atom, a monovalent saturated aliphatic hydrocarbon group, or a monovalent aromatic hydrocarbon group, and more preferably a hydrogen atom or a monovalent saturated aliphatic hydrocarbon group. 2 Preferred monovalent saturated and unsaturated aliphatic hydrocarbon groups and monovalent aromatic hydrocarbon groups are R 1 The preferred monovalent saturated and unsaturated aliphatic hydrocarbon groups and monovalent aromatic hydrocarbon groups are the same as those of the preferred monovalent saturated and unsaturated aliphatic hydrocarbon groups and monovalent aromatic hydrocarbon groups. 2 If R 2 may be independently selected. 2 From the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, is preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms (particularly a linear alkyl group), more preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms (particularly a linear alkyl group), even more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms (particularly a linear alkyl group), and sufficiently preferably an alkyl group having 1 to 3 carbon atoms (particularly a linear alkyl group).

[0041] Specific examples of component C include 3-(2-aminoethylamino)propylmethyldimethoxysilane, 3-(2-aminoethylamino)propylmethyldiethoxysilane, and mixtures thereof.

[0042] Component C is commercially available or can be produced by known methods. Examples of commercially available products of component C include, but are not limited to, the following: Wacker Chemie GENIOSIL GF95 (3-(2-aminoethylamino)propylmethyldimethoxysilane) Dow Toray DOWSIL Z6436 (3-(2-aminoethylamino)propylmethyldimethoxysilane)

[0043] The content of component C is 2.0 to 15.0 parts by weight relative to 100 parts by weight of component A, and from the viewpoint of further improving the matte property and mechanical properties and improving the adhesion, it is preferably 2.0 to 8.0 parts by weight, more preferably 4.0 to 7.0 parts by weight, and even more preferably 4.0 to 6.0 parts by weight. If the content is too small, the matte property (particularly the matte property under relatively high temperatures) decreases. If the content is too large, the matte property (particularly the matte property under relatively high temperatures) decreases. Component C may contain two or more types of components C having different structures, and in that case, the total amount thereof may be within the above range.

[0044] The composition of the present invention may further contain known additives such as solvents, curing catalysts, fillers, tackifiers, plasticizers, dehydrating agents, and colorants.

[0045] As the solvent, naphthenic, isoparaffinic, and aromatic solvents can be used. An example of a naphthenic solvent is Exxol manufactured by ExxonMobil Corporation. An example of an isoparaffin-based solvent is Isopar manufactured by ExxonMobil. An example of an aromatic solvent is Solvesso manufactured by ExxonMobil. The solvent is preferably a naphthenic solvent (particularly Exxol D80) from the viewpoint of further improving the matte finish and mechanical properties as well as improving adhesion.

[0046] The content of the solvent is not particularly limited, and is usually 20 parts by weight or less (particularly 0 to 20 parts by weight) relative to 100 parts by weight of component A. From the viewpoint of further improving the matte property and mechanical properties and improving the adhesion, it is preferably 0.1 to 10 parts by weight, more preferably 1 to 8 parts by weight, and even more preferably 2 to 6 parts by weight. The solvent may contain two or more kinds of solvents, in which case the total amount thereof may be within the above range.

[0047] The curing catalyst is a compound for promoting the curing reaction. For example, metal salts such as alkyl titanate, organosilicon titanate, and bismuth tris-2-ethylhexanoate (manufactured by Matsumoto Fine Chemical Co., Ltd.; Orgatics); acidic compounds such as phosphoric acid, p-toluenesulfonic acid, and phthalic acid; aliphatic monoamines such as butylamine, hexylamine, octylamine, decylamine, laurylamine, and stearylamine (manufactured by Kao Corporation; Farmin); aliphatic diamines such as ethylenediamine and hexanediamine; aliphatic polyamines such as diethylenetriamine, triethylenetetramine, and tetraethylenepentamine; heterocyclic amines such as piperidine and piperazine; aromatic amines such as metaphenylenediamine; alcohol amines such as ethanolamine; trialkylamines such as triethylamine; and amine compounds such as various modified amines used as curing agents for epoxy resins. Also included are mixtures of organic alkyl tin salts such as tin dioctylate, tin dinaphthenate, and tin distearate with the above amines, such as one or more amines selected from aliphatic monoamines, aliphatic diamines, aliphatic polyamines, heterocyclic amines, aromatic amines, alcohol amines, and trialkylamines. Also included are reaction products of organic alkyl tin oxides with ester compounds such as ethyl silicate, dimethyl maleate, diethyl maleate, dioctyl maleate, dimethyl phthalate, diethyl phthalate, and dioctyl phthalate. Also included are reaction products of chelate tin compounds with alkoxysilanes.

[0048] The content of the curing catalyst is not particularly limited and is usually 10 parts by weight or less (particularly 0 to 10 parts by weight) relative to 100 parts by weight of component A, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably 5 parts by weight or less (particularly 0 to 5 parts by weight, more preferably 3 parts by weight or less (particularly 0 to 3 parts by weight), still more preferably 1 part by weight or less (particularly 0 to 1 part by weight), and particularly preferably 0 part by weight. Two or more types of curing catalysts may be contained, in which case the total amount thereof may be within the above range.

[0049] As the filler, known fillers can be used. For example, calcium carbonate (manufactured by Shiraishi Kogyo Co., Ltd.; Whiten), such as calcium carbonate whose surface has been treated with a fatty acid or a resin acid-based organic substance, which has been further pulverized into fine powder, such as gelatinous calcium carbonate having an average particle size of 1 μm or less, light calcium carbonate produced by a precipitation method having an average particle size of 1 to 3 μm, and heavy calcium carbonate having an average particle size of 1 to 20 μm; powder-like fillers such as fumed silica, precipitated silica, anhydrous silicic acid, hydrated silicic acid, magnesium carbonate, diatomaceous earth, calcined clay, clay, talc, titanium oxide, bentonite, organic bentonite, ferric oxide, zinc oxide, activated zinc oxide, shirasu balloon, wood flour, pulp, cotton chips, mica, walnut flour, rice flour, graphite, aluminum fine powder, and flint powder; and fibrous fillers such as glass fiber, glass filament, carbon fiber, Kevlar fiber, and polyethylene fiber. These fillers may be used alone or in combination of two or more. The filler is preferably calcium carbonate (particularly Viscolite OS) from the viewpoints of further improving the matte finish and mechanical properties as well as improving adhesion.

[0050] The content of the filler is not particularly limited, and is usually 500 parts by weight or less (particularly 0 to 500 parts by weight) relative to 100 parts by weight of component A. From the viewpoint of further improving the matte property and mechanical properties and improving the adhesion, it is preferably 10 to 400 parts by weight, more preferably 50 to 350 parts by weight, further preferably 100 to 350 parts by weight, and particularly preferably 200 to 350 parts by weight. Two or more kinds of fillers may be contained, and in that case, the total amount thereof may be within the above range.

[0051] As the tackifier, known tackifiers such as phenol resins, terpene resins, petroleum-based resins, and rosin-based resins can be used.

[0052] The content of the tackifier is not particularly limited and is usually 10 parts by weight or less (particularly from 0 to 10 parts by weight) relative to 100 parts by weight of Component A, and from the viewpoint of further improving the matte properties and mechanical properties as well as improving adhesion, it is preferably 5 parts by weight or less (particularly from 0 to 5 parts by weight, more preferably 3 parts by weight or less (particularly 0 to 3 parts by weight), even more preferably 1 part by weight or less (particularly 0 to 1 part by weight), and particularly preferably 0 part by weight. Two or more types of tackifiers may be contained, in which case the total amount thereof may be within the above range.

[0053] The hardness can be adjusted using a plasticizer. Examples of the plasticizer include alkyl phthalates such as dioctyl phthalate, dibutyl phthalate, dinonyl phthalate, and butyl benzyl phthalate; alkyl aliphatic carboxylates such as dioctyl adipate, diisodecyl succinate, dibutyl sebacate, and butyl oleate; pentaerythritol esters; phosphates such as trioctyl phosphate and tricresyl phosphate; epoxy plasticizers such as epoxidized soybean oil and epoxy benzyl stearate; polypropylene glycol; polyethylene glycol; and chlorinated paraffin. These plasticizers may be used alone or in combination of two or more. The plasticizer is preferably an alkyl phthalate ester (especially dinonyl phthalate) from the viewpoint of further improving the matte property and mechanical properties as well as improving adhesion.

[0054] The content of the plasticizer is not particularly limited, and is usually 300 parts by weight or less (particularly 0 to 300 parts by weight) relative to 100 parts by weight of component A. From the viewpoint of further improving the matte property and mechanical properties and improving the adhesion, it is preferably 1 to 200 parts by weight, more preferably 10 to 150 parts by weight, further preferably 50 to 150 parts by weight, and particularly preferably 80 to 120 parts by weight. Two or more kinds of plasticizers may be contained, and in that case, the total amount thereof may be within the above range.

[0055] As the dehydrating agent, a hydrolyzable silicon compound can be added arbitrarily for the purpose of adjusting the physical properties, curability and storage stability of the cured product.Specific examples include, but are not limited to, tetramethyl silicate, vinyltrimethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and the like, and compounds in which the methoxy group of these is replaced with an ethoxy group.In terms of further improving matte properties and mechanical properties and improving adhesion, the dehydrating agent is preferably vinyltrimethoxysilane.

[0056] The content of the dehydrating agent is not particularly limited, and is usually 100 parts by weight or less (particularly 0 to 100 parts by weight) relative to 100 parts by weight of component A. From the viewpoint of further improving the matte property and mechanical properties and improving the adhesion, it is preferably 1 to 50 parts by weight, more preferably 2 to 20 parts by weight, and even more preferably 5 to 15 parts by weight. Two or more kinds of dehydrating agents may be contained, and in that case, the total amount thereof may be within the above range.

[0057] Examples of the colorant include carbon black (for example, manufactured by Asahi Carbon Co., Ltd.) etc. The colorant is preferably carbon black from the viewpoints of further improving the matte properties and mechanical properties as well as improving the adhesion.

[0058] The content of the colorant is not particularly limited, and is usually 100 parts by weight or less (particularly 0 to 100 parts by weight) relative to 100 parts by weight of component A. From the viewpoint of further improving the matte property and mechanical properties as well as improving the adhesion, it is preferably 1 to 50 parts by weight, more preferably 5 to 30 parts by weight, and even more preferably 10 to 20 parts by weight. Two or more kinds of colorants may be contained, and in that case, the total amount thereof may be within the above range.

[0059] The curable resin composition of the present invention may be included in an adhesive or a sealant. The curable resin composition of the present invention being included in an adhesive or a sealant means that the curable resin composition of the present invention constitutes a part or the whole of the adhesive or sealant.

[0060] An adhesive is a material for bonding or joining two or more members (or components). An adhesive containing the curable resin composition of the present invention is particularly useful for bonding or joining members made of metal, plastic, stone, etc.

[0061] When the adhesive contains the curable resin composition of the present invention, the content of the curable resin composition of the present invention relative to the total amount of the adhesive is usually 1 to 100% by weight, and from the viewpoint of further improving the matte property and mechanical properties as well as improving adhesion, it is preferably 10 to 100% by weight, more preferably 50 to 100% by weight, even more preferably 80 to 100% by weight, and particularly preferably 100% by weight. The content of the curable resin composition of the present invention relative to the total amount of the adhesive being 100% by weight means that the adhesive contains only the curable resin composition of the present invention.

[0062] A sealant is a material that is applied to a structure such as a building or civil engineering structure for the purpose of waterproofing and / or surface protection of the structure. The sealant containing the curable resin composition of the present invention is particularly useful for waterproofing and surface protection of structures made of metal, plastic, stone, etc.

[0063] When a sealant contains the curable resin composition of the present invention, the content of the curable resin composition of the present invention relative to the total amount of the sealant is usually 1 to 100% by weight, and from the viewpoint of further improving the matte property and mechanical properties as well as improving adhesion, it is preferably 10 to 100% by weight, more preferably 50 to 100% by weight, even more preferably 80 to 100% by weight, and particularly preferably 100% by weight. The content of the curable resin composition of the present invention relative to the total amount of the sealant being 100% by weight means that the sealant contains only the curable resin composition of the present invention.

[0064] Preferred embodiments of the present invention are described below. <1> A curable resin composition comprising 100 parts by weight of a polymer having a hydrolyzable silicon group, 0.5 to 8.0 parts by weight of an organic modified silicone oil, and 2.0 to 15.0 parts by weight of a silane compound represented by the general formula (1). <2> In the formula (1), m and n each independently represent an integer of 1 to 5. a and b are 1, c is 2, R 1 is an alkyl group having 1 to 5 carbon atoms, R 2 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; <1> The curable resin composition according to claim 1. <3> The silane compound includes at least one of 3-(2-aminoethylamino)propylmethyldimethoxysilane or 3-(2-aminoethylamino)propylmethyldiethoxysilane. <1> or <2> The curable resin composition according to claim 1. <4> The hydrolyzable silicon group is represented by the general formula (2): <1> ~ <3> The curable resin composition according to any one of the preceding claims. <5> The polymer having a hydrolyzable silicon group is a polymer having a hydrolyzable silicon group represented by the general formula (2) and containing an oxyalkylene polymer or a vinyl polymer as a main chain. <1> ~ <4> The curable resin composition according to any one of the preceding claims. <6> The hydrolyzable silicon group is a methyldimethoxysilyl group or a trimethoxysilyl group. <1> ~ <5> The curable resin composition according to any one of the preceding claims. <7> The organic modified silicone oil has one or more organic groups selected from the group consisting of an alkyl group, a fluoroalkyl group, a phenyl group, and a polyether group introduced into the side chain and / or the end of the silicone chain. <1> ~ <6> The curable resin composition according to any one of the preceding claims. <8> The organic modified silicone oil is a polyether modified silicone oil having a polyether group introduced as an organic group, and the polyether group is a polyethylene glycol group, a polypropylene glycol group, or a composite group thereof. <1> ~ <7> The curable resin composition according to any one of the preceding claims. <9> The content of the organic modified silicone oil is 0.5 to 4.0 parts by weight, The content of the silane compound is 2.0 to 8.0 parts by weight. <1> ~ <8> The curable resin composition according to any one of the preceding claims. <10> The content of the organic modified silicone oil is 1.5 to 4.0 parts by weight, The content of the silane compound is 4.0 to 7.0 parts by weight. <1> ~ <9> The curable resin composition according to any one of the preceding claims. <11> The curable resin composition is contained in an adhesive or a sealant. <1> ~ <10> The curable resin composition according to any one of the preceding claims. EXAMPLES

[0065] The present invention will be described below using examples, but the present invention is not limited to the following examples. There is none.

[0066] Example 1 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 2.5 g of DOWSIL L-7002 (Dow-Toray: modified silicone oil), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 5 g of GENIOSIL GF95 (Wacker Chemie: 3-(2-aminoethylamino)propylmethyldimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0067] GENIOSIL STP-E30 (manufactured by Wacker Chemie) as component A is an oxyalkylene polymer having a trimethoxysilyl group as a terminal group, and has a number average molecular weight of 15,000 and an introduction rate of hydrolyzable silicon groups of 97%. DOWSIL L-7002 (manufactured by Dow Toray) as component B is a polyether modified silicone oil in which a polyethylene glycol group has been introduced into silicone oil, and has a viscosity of 1200 mm 2 / s and HLB value of 8. GENIOSIL GF95 (manufactured by Wacker Chemie) as component C is represented by the general formula (1), in which m is 3, n is 2, a and b are 1, c is 2, and R 1 and R 2 was a methyl group.

[0068] Example 2 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 1 g of DOWSIL L-7002 (Dow-Toray: modified silicone oil), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 5 g of GENIOSIL GF95 (Wacker Chemie: 3-(2-aminoethylamino)propylmethyldimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0069] Example 3 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 2.5 g of DOWSIL L-7002 (Dow-Toray: modified silicone oil), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 2.5 g of GENIOSIL GF95 (Wacker Chemie: 3-(2-aminoethylamino)propylmethyldimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0070] Example 4 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 5 g of DOWSIL L-7002 (Dow-Toray: modified silicone oil), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 5 g of GENIOSIL GF95 (Wacker Chemie: 3-(2-aminoethylamino)propylmethyldimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0071] Example 5 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 2.5 g of DOWSIL L-7002 (Dow-Toray: modified silicone oil), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 10 g of GENIOSIL GF95 (Wacker Chemie: 3-(2-aminoethylamino)propylmethyldimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0072] Example 6 and Comparative Examples 7 to 8 Compositions were prepared in the same manner as in Example 1, except that the contents of the various components and additives were changed to the amounts shown in Table 1.

[0073] Comparative Example 1 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 2.5 g of DOWSIL L-7002 (Dow-Toray: modified silicone oil), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 5 g of GENIOSIL GF91 (Wacker Chemie: 3-(2-aminoethylamino)propyltrimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0074] Comparative Example 2 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 2.5 g of DOWSIL L-7002 (Dow-Toray: modified silicone oil), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 5 g of GENIOSIL XL972 (Wacker Chemie: (phenylaminomethyl)methyldimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0075] Comparative Example 3 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 2.5 g of DOWSIL L-7002 (Dow-Toray: modified silicone oil), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 1 g of GENIOSIL GF95 (Wacker Chemie: 3-(2-aminoethylamino)propylmethyldimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0076] Comparative Example 4 100g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15g of NBK-1215 (manufactured by Nikko Bix: carbon black), 200g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), and 100g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate) were mixed by stirring with a planetary stirrer. 4g of Exxol D80 (manufactured by Exxon Mobil Corp.: naphthenic solvent), 10g of GENIOSIL XL10 (manufactured by Wacker Chemie: vinyltrimethoxysilane), and 5g of GENIOSIL GF95 (manufactured by Wacker Chemie: 3-(2-aminoethylamino)propylmethyldimethoxysilane) were added to the mixture to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0077] Comparative Example 5 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate), and 50 g of Hardlite B-03 (manufactured by Showa Chemical Industry Co., Ltd.: inorganic hollow filler) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 5 g of GENIOSIL GF91 (Wacker Chemie: 3-(2-aminoethylamino)propyltrimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0078] Comparative Example 6 100 g of GENIOSIL STP-E30 (manufactured by Wacker Chemie: modified silicone resin), 100 g of DINP (manufactured by New Japan Chemical: dinonyl phthalate), 15 g of NBK-1215 (manufactured by Nichiko Bicks: carbon black), 200 g of Viscolite OS (manufactured by Shiraishi Kogyo Co., Ltd.: calcium carbonate), 100 g of R heavy carbon (manufactured by Maruo Calcium Co., Ltd.: heavy calcium carbonate), and 2 g of Farmin 80S (manufactured by Kao Chemical Co., Ltd.: stearylamine) were each mixed by stirring with a planetary stirrer. To the mixture, 4 g of Exxol D80 (Exxon Mobil: naphthenic solvent), 10 g of GENIOSIL XL10 (Wacker Chemie: vinyltrimethoxysilane), and 5 g of GENIOSIL GF91 (Wacker Chemie: 3-(2-aminoethylamino)propyltrimethoxysilane) were added to prepare a composition. The composition of the obtained composition is shown in Table 1.

[0079] (Test Method) The produced compositions were evaluated for matte visibility, gloss resistance (surface gloss), mechanical properties (tensile test), and adhesion by the following methods.

[0080] Matte: The evaluation result of the matte property was determined based on the lower evaluation result of the matte visibility and the gloss resistance.

[0081] Matte Visibility: A mold was made to have a length of 40 mm, a width of 40 mm, and a thickness of 3 mm, and the composition was poured into the mold and the surface was smoothed to form a sheet. The sheets were left to stand at temperatures of 5°C, 23°C, and 70°C for 24 hours, and the degree of matteness of the surface after the composition (sealant) hardened was visually confirmed. The evaluation method was performed according to the following criteria. ◎: Matte ×: Glossy

[0082] Gloss resistance (surface gloss): A mold was made to have a length of 40 mm, a width of 40 mm, and a thickness of 3 mm, and the composition was poured into the mold and the surface was smoothed to form a sheet. The sheet was left at 23°C for 7 days and the surface gloss was measured. The surface gloss was measured using a 60° mirror gloss meter. The smaller the surface gloss value, the lower the light reflectance and the lower the surface gloss, i.e., the better the gloss resistance. The evaluation method was performed according to the following criteria. ◎: Glossiness 0 to 5; ○: Gloss level is more than 5 and less than 10; △: Glossiness is more than 10 and less than 20; ×: Glossiness over 20.

[0083] Matte: ⊚: The evaluation results for both matte visibility and gloss resistance were ⊚; ○: The lower evaluation result of matte visibility and gloss resistance was ○; △: The lower evaluation result of the matte visibility and gloss resistance was △; ×: Of the evaluation results for matte visibility and gloss resistance, the lower evaluation result was marked ×.

[0084] Mechanical properties (tensile test): A formwork was made to have dimensions of 40 mm length, 40 mm width, and 3 mm thickness, and the composition was poured into the formwork and the surface was smoothed to form a sheet. The sheet was left to stand at 23°C for 7 days. After curing, a dumbbell-shaped No. 3 test piece was punched out. The maximum tensile strength (N / mm 2 The mechanical properties were evaluated based on the following criteria. The mechanical properties were evaluated based on the lower of the maximum strength and maximum elongation.

[0085] ·Maximum strength ◎: 1.65N / mm 2 More than; ○:Maximum strength 1.20N / mm 2 More than 1.65N / mm 2 less than; △:Maximum strength 1.00)N / mm 2 greater than or equal to 1.20; ×: Maximum strength 1.00N / mm 2 less than.

[0086] Maximum elongation rate ◎: 700% or more; ○: 600% or more but less than 700%; △: 500% or more but less than 600%; ×: Less than 500%.

[0087] ·Mechanical properties ◎: The evaluation results for both maximum strength and maximum elongation were ◎; ○: The lower evaluation result of the maximum strength and maximum elongation was ○; △: The lower evaluation result of the maximum strength and maximum elongation was △; ×: Of the evaluation results of maximum strength and maximum elongation, the lower evaluation result was marked ×.

[0088] comprehensive evaluation The overall evaluation result was determined based on the lower evaluation result of the matte property and the mechanical properties. ⊚: The evaluation results for both matte finish and mechanical properties were ⊚; ○: The lower evaluation result of the matte property and the mechanical properties was ○; △: The lower evaluation result of the matte property and the mechanical properties was △; ×: The lower evaluation result of the matte property and the mechanical properties was marked ×.

[0089] Adhesion: A formwork was prepared with dimensions of 40 mm length x 40 mm width x 3 mm thickness, and the prepared composition was poured into the formwork and the surface was smoothed to form a sheet. The prepared sheet was left to stand at 23°C for 24 hours. After 24 hours, paint (SK Chemical Co., Ltd.: Clean Mild Urethane) was applied with a brush and left to stand at 23°C for 7 days. The adhesion between the paint and the cured product of the composition (sealant) was confirmed in accordance with JIS K5600-5-6. The evaluation method was performed according to the following criteria. In addition, for Comparative Examples 1 to 4, no matte properties were exhibited, so adhesion tests were not performed. ○: Paint peeling 0-20% △: Paint peeling 21-50% ×: More than 51% of the paint has peeled off

[0090] [Table 1]

[0091] (result) The results are shown in Table 1. Examples 1 to 6, which are related to the cured resin compositions containing components A to C, were excellent in both matte visibility and gloss resistance, and as a result, it was confirmed that the matte properties were good. Furthermore, the curable resin compositions of Examples 1 to 6 were good not only in mechanical properties but also in adhesion. [Industrial Applicability]

[0092] The curable resin composition of the present invention has good matt properties over a wide range from low to high temperatures. The curable resin composition of the present invention also has good mechanical properties and adhesion. Therefore, the curable resin composition of the present invention is useful for applications such as adhesives and sealants in fields such as housing and vehicles where design is important.

Claims

1. A curable resin composition comprising 100 parts by weight of a polymer having a hydrolyzable silicon group, 0.5 to 8.0 parts by weight of an organic modified silicone oil, and 2.0 to 15.0 parts by weight of a silane compound represented by general formula (1). [Formula 1] (In formula (1), m and n each independently represent an integer from 1 to 10; a, b and c each independently represent 1 or 2, and the relationship c=4-a-b is satisfied; R 1 is a monovalent hydrocarbon group; R 2 is a hydrogen atom or a monovalent hydrocarbon group.

2. In the formula (1), m and n each independently represent an integer of 1 to 5. a and b are 1; c is 2; R 1 is an alkyl group having 1 to 5 carbon atoms, R 2 The curable resin composition according to claim 1, wherein is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.

3. The curable resin composition according to claim 1, wherein the silane compound comprises at least one of 3-(2-aminoethylamino)propylmethyldimethoxysilane or 3-(2-aminoethylamino)propylmethyldiethoxysilane.

4. The curable resin composition according to claim 1 , wherein the hydrolyzable silicon group is represented by the following general formula (2): [Case 2] (In formula (2), R is an alkyl group having 1 to 20 carbon atoms; X is a hydroxyl group or an alkoxy group having 1 to 6 carbon atoms; and a is 1, 2, or 3.)

5. The curable resin composition according to claim 1, wherein the polymer having a hydrolyzable silicon group is a polymer having a hydrolyzable silicon group represented by the general formula (2) and containing an oxyalkylene polymer or a vinyl polymer as a main chain.

6. The curable resin composition according to claim 1 , wherein the hydrolyzable silicon group is a methyldimethoxysilyl group or a trimethoxysilyl group.

7. The curable resin composition according to claim 1, wherein the organic modified silicone oil has one or more organic groups selected from the group consisting of an alkyl group, a fluoroalkyl group, a phenyl group, and a polyether group introduced into a side chain and / or an end of a silicone chain.

8. 2. The curable resin composition according to claim 1, wherein the organic modified silicone oil is a polyether modified silicone oil having a polyether group introduced as an organic group, and the polyether group is a polyethylene glycol group, a polypropylene glycol group, or a composite group thereof.

9. The content of the organic modified silicone oil is 0.5 to 4.0 parts by weight, The curable resin composition according to claim 1, wherein the content of the silane compound is 2.0 to 8.0 parts by weight.

10. The content of the organic modified silicone oil is 1.5 to 4.0 parts by weight, The curable resin composition according to claim 1, wherein the content of the silane compound is 4.0 to 7.0 parts by weight.

11. The curable resin composition according to any one of claims 1 to 10, wherein the curable resin composition is contained in an adhesive or a sealant.

Citation Information

Patent Citations

  • Room temperature-curable composition

    JP1997100408A

  • Sealant composition

    JP2001262125A

  • Curable composition

    JP2004124093A