Carbon dioxide absorbent
A carbon dioxide adsorbent using zeolite and alumina-based particles with surface-supported sodium improves carbon dioxide retention and adsorption at low temperatures, addressing the limitations of conventional zeolite-based adsorbents.
Patent Information
- Application Number
- JP2023047637
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional carbon dioxide adsorbents using zeolite exhibit low carbon dioxide retention at low temperatures.
A carbon dioxide adsorbent comprising zeolite and alumina-based particles with sodium supported on the surface of the alumina particles, with specific ratios and contents of alumina and sodium, enhancing carbon dioxide adsorption and retention at low temperatures.
The adsorbent achieves a significant increase in carbon dioxide adsorption and retention rate at 30°C, outperforming conventional adsorbents in both metrics.
Smart Images

Figure 2024136502000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon dioxide adsorbent. [Background technology]
[0002] One of the causes of global warming is the emission of greenhouse gases. Greenhouse gases include carbon dioxide (CO2), methane (CH4), and fluorocarbons (CFCs, etc.). Carbon dioxide, a representative greenhouse gas, is particularly emitted in large quantities from power plants, steelworks, and oil refineries, so there is growing interest in technologies to reduce carbon dioxide emissions. Meanwhile, apart from technologies to reduce carbon dioxide emissions, there is also interest in technologies to capture and store carbon dioxide (Carbon dioxide Capture and Storage: "CCS").
[0003] In order to store carbon dioxide, it is first necessary to separate the carbon dioxide from a medium (for example, exhaust gas, air, etc.). Known methods for separating carbon dioxide include a chemical absorption method in which carbon dioxide is absorbed in an alkaline solution or an amine solution (for example, Patent Document 1), and a physical adsorption method in which carbon dioxide is adsorbed on an adsorbent and separated (for example, Patent Document 2). In the latter method, an adsorbent containing activated carbon or zeolite is used. In the method using such an adsorbent, carbon dioxide is adsorbed and removed by a temperature-pressure swing method (PTSA method) in which the temperature and pressure are changed, or a pressure swing method (PSA method) in which only the pressure is changed. In general, carbon dioxide is adsorbed on an adsorbent at a low temperature and a high pressure, and carbon dioxide is desorbed from the adsorbent at a temperature higher than the adsorption temperature and a low pressure to regenerate the adsorbent. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. WO2023 / 013397 [Patent Document 2] JP 2001-347123 A Summary of the Invention [Problem to be solved by the invention]
[0005] Conventional carbon dioxide adsorbents using zeolite had the problem that the carbon dioxide retention rate was low at low temperatures.
[0006] Therefore, an object of the present invention is to provide a carbon dioxide adsorbent that has a large carbon dioxide adsorption amount and a high carbon dioxide retention rate at low temperatures. [Means for solving the problem]
[0007] The present inventors have focused on alumina-based particles, which are one of the binder components constituting the carbon dioxide adsorbent, and have found that the above-mentioned problems can be solved by using a carbon dioxide adsorbent containing alumina-based particles with sodium supported on the surface and zeolite. Effect of the Invention
[0008] According to the present invention, it is possible to provide a carbon dioxide adsorbent that has a large carbon dioxide adsorption amount and a high carbon dioxide retention rate at low temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention includes an invention relating to a carbon dioxide adsorbent (hereinafter, also referred to as "the adsorbent of the present invention"). The adsorbent of the present invention will be described in detail below.
[0010] [Adsorbent of the present invention] The adsorbent of the present invention is a molded body containing zeolite and alumina-based particles, the content of the alumina-based particles being in the range of 5 mass% or more and 30 mass% or less relative to 100 mass% of the molded body, sodium being supported on the surfaces of the alumina-based particles, and the sodium content of the alumina-based particles being 0.1 mass% or more relative to 100 mass% of the alumina-based particles.
[0011] Conventional carbon dioxide adsorbents increase the amount of carbon dioxide adsorbed by increasing the ratio of zeolite, which is a component that adsorbs carbon dioxide, even if only slightly. For example, Patent Document 2 proposes that the content of zeolite be 95% or more. In contrast, the adsorbent of the present invention contains alumina-based particles, which are a component other than zeolite, in the range of 5% by mass or more and 30% by mass or less. Furthermore, by using alumina-based particles having sodium supported on the surface of the particles as the alumina-based particles, the amount of carbon dioxide adsorbed and the carbon dioxide retention rate at low temperatures (carbon dioxide retention rate at 30°C) are increased. The adsorbent of the present invention will be described in detail below.
[0012] The adsorbent of the present invention is a molded body containing zeolite and alumina particles. In the adsorption of carbon dioxide, which is the application of the present invention, the adsorbent is filled in a reactor, and a gas containing carbon dioxide is passed through the adsorbent to contact the adsorbent, thereby adsorbing carbon dioxide into the adsorbent. At this time, if the adsorbent is in a powder form, it becomes difficult to pass the gas through the adsorbent, so a molded adsorbent is used.
[0013] The adsorbent of the present invention contains zeolite. Zeolite is a general term for crystalline porous aluminum silicate, and has a large surface area due to its structure. Taking advantage of such characteristics, zeolite is used for adsorption or separation of various substances. In the adsorbent of the present invention, zeolite is used as a component that adsorbs carbon dioxide.
[0014] The structural code of the zeolite contained in the adsorbent of the present invention is preferably at least one selected from A-type (LTA), chabazite (CHA) and faujasite (FAU), and more preferably FAU. FAU is further classified according to the SiO2 / Al2O3 molar ratio, and is classified as Y-type when the SiO2 / Al2O3 molar ratio is 4 or more, and as X-type when the SiO2 / Al2O3 molar ratio is less than 4. In the present invention, X-type zeolite is preferred, and X-type zeolite with a SiO2 / Al2O3 molar ratio of 2 or less is particularly preferred. The adsorbent of the present invention contains such zeolite, thereby increasing the amount of carbon dioxide adsorption and the carbon dioxide retention rate at 30°C.
[0015] The zeolite contained in the adsorbent of the present invention is preferably ion-exchanged with an alkali metal or an alkaline earth metal. Zeolites generally have ion-exchange sites, and it is known that the pore size varies depending on the ion species at the site. In the adsorbent of the present invention, the zeolite is preferably ion-exchanged with sodium (Na). By thus matching the alkali metal ion-exchanged in the zeolite with the alkali metal on the surface of the alumina-based particles, the carbon dioxide adsorption amount and the carbon dioxide retention rate at 30°C can be further increased.
[0016] The adsorbent of the present invention contains alumina-based particles. In the present invention, the alumina-based particles refer to inorganic oxide particles mainly composed of aluminum (Al). In the present invention, the alumina-based particles function as a binder that fills the gaps between zeolite particles contained in the molded body. Specific examples of the alumina-based particles include aluminum oxide and alumina hydrate. In the present invention, alumina hydrate is preferable. Specific examples of alumina hydrate include boehmite, pseudoboehmite, gibbsite, bayerite, etc. In the adsorbent of the present invention, boehmite or pseudoboehmite is preferable. Furthermore, the crystallite diameter of boehmite or pseudoboehmite is preferably 25 nm or less, more preferably 20 nm or less, and particularly preferably 15 nm or less. When boehmite or pseudoboehmite with a small crystallite diameter is contained, the carbon dioxide adsorption amount and the carbon dioxide retention rate at 30°C are further improved.
[0017] The content of the alumina-based particles contained in the adsorbent of the present invention is 1% by mass or more and 30% by mass or less, preferably 5% by mass or more and 30% by mass or less, and more preferably 5% by mass or more and 25% by mass or less, calculated as Al2O3 relative to 100% by mass of the molded body. When the content of the alumina-based particles is within the above-mentioned range, the carbon dioxide adsorption amount and the carbon dioxide retention rate at 30°C are further improved.
[0018] The alumina-based particles contained in the adsorbent of the present invention have sodium supported on their surfaces. By containing such alumina-based particles together with zeolite, the adsorbent of the present invention can achieve the effect of improving the carbon dioxide adsorption amount and the carbon dioxide retention rate at 30°C, which could not be achieved by the conventional combination of zeolite and binder.
[0019] The sodium content of the alumina particles is 0.1% by mass or more, preferably 0.1% by mass or more and 15% by mass or less, and more preferably 0.5% by mass or more and 10% by mass or less, calculated as Na2O relative to 100% by mass of the alumina particles. When the sodium content of the alumina particles is in the above-mentioned range, the carbon dioxide adsorption amount and the carbon dioxide retention rate at 30°C are further improved.
[0020] The sodium content of the adsorbent of the present invention (the total amount of all sodium contained in the adsorbent, such as sodium ion-exchanged in zeolite and sodium present on the surface of alumina-based particles) is preferably 0.01% by mass or more, more preferably 1% by mass or more and 30% by mass or less, and particularly preferably 10% by mass or more and 25% by mass or less, in terms of Na2O, relative to 100% by mass of the molded body. In addition, the content of alkali metals other than Na in the adsorbent of the present invention is preferably 5% by mass or less, more preferably 3% by mass or less, and particularly preferably 1% by mass or less, relative to 100% by mass of the molded body. Furthermore, the content of alkaline earth metals in the adsorbent of the present invention is preferably 5% by mass or less, more preferably 3% by mass or less, and particularly preferably 1% by mass or less, relative to 100% by mass of the molded body, in terms of MeO (Me: alkaline earth metal), relative to 100% by mass of the molded body. When the content of alkali metals and alkaline earth metals other than Na contained in the adsorbent of the present invention is reduced in this way, the effect of sodium becomes more prominent, and the carbon dioxide adsorption amount and carbon dioxide retention rate at 30°C are further improved.
[0021] The molar ratio of Si to Al contained in the adsorbent of the present invention (the molar ratio relative to the total amount of all Si and Al contained in the adsorbent, such as Si and Al contained in the zeolite, and Al contained in the alumina-based particles) is, in terms of the SiO2 / Al2O3 molar ratio, preferably in the range of 0.01 to 5, more preferably in the range of 0.1 to 4, and particularly preferably in the range of 0.5 to 3.5.
[0022] The specific surface area of the adsorbent of the present invention is 400 m2 / g or more, 700m 2 / g or less, and 2 / g or more, 650m 2 / g or less, and more preferably 450m 2 / g or more, 650m 2 It is particularly preferable that the specific surface area is in the range of 1 / g or less. When the specific surface area is in the above-mentioned range, the carbon dioxide adsorption amount is further improved. The specific surface area in the present invention refers to the specific surface area determined by the BET one-point method.
[0023] The pore volume of the adsorbent of the present invention is preferably in the range of 0.20 mL / g or more and 0.60 mL / g or less, more preferably in the range of 0.20 mL / g or more and 0.55 mL / g or less, and particularly preferably in the range of 0.25 mL / g or more and 0.55 mL / g or more. When the pore volume is in the above-mentioned range, the carbon dioxide adsorption amount is further improved. The pore volume in the present invention refers to the total amount of pores having a pore diameter of 1 nm to 500 nm in the pore distribution obtained from the adsorption isotherm obtained by the nitrogen adsorption method.
[0024] The average pore diameter of the adsorbent of the present invention is preferably in the range of 3.0 nm or more and 7.0 nm or less, more preferably in the range of 3.5 nm or more and 6.5 nm or less, and particularly preferably in the range of 3.5 nm or more and 6.0 nm or less. When the average pore diameter is in the above-mentioned range, the carbon dioxide adsorption amount is further improved. The pore volume in the present invention refers to the average pore diameter in the pore distribution obtained from the adsorption isotherm obtained by the nitrogen adsorption method.
[0025] The adsorbent of the present invention is preferably a molded body having a spherical shape, a columnar shape (including a cylindrical shape and a four-lobe shape) or a shape similar thereto. The size (the minimum length of the outer shape of the adsorbent) is preferably in the range of 0.5 mm to 6 mm, more preferably in the range of 1 mm to 5 mm, and particularly preferably in the range of 3 mm to 5 mm. The adsorbent of the present invention molded to such a size has a low pressure loss when passing a gas through it, which is preferable in terms of process design.
[0026] [Method of producing the adsorbent of the present invention] The adsorbent of the present invention can be prepared, for example, by using a production method including the following steps (1) to (3). (1) Alumina-based particle preparation step of preparing alumina-based particles (2) A sodium supporting step of supporting sodium on the surface of the alumina-based particles (3) A molding step of mixing the alumina particles having sodium supported on the surface with zeolite to prepare a molded body.
[0027] Hereinafter, the method for producing the adsorbent of the present invention (hereinafter also referred to as the "production method of the present invention") will be described in detail as an example of this production method, but the production method for the adsorbent of the present invention is not limited to this production method.
[0028] The manufacturing method of the present invention includes a step of preparing alumina-based particles, such as aluminum oxide (Al2O3), boehmite (AlOOH), aluminum hydroxide (Al(OH)3), etc. Alternatively, this step can be substituted by purchasing commercially available alumina-based particles.
[0029] A method for preparing alumina particles can be a known method. For example, boehmite can be prepared by reacting an aqueous solution of an aluminum salt (e.g., aluminum sulfate) with an aqueous solution of a neutralizing agent (e.g., sodium aluminate) in the range of pH 6 to 11. Aluminum oxide having various crystal structures (e.g., gamma) can also be prepared by calcining this boehmite.
[0030] The production method of the present invention includes a sodium supporting step, in which sodium is supported on the surfaces of the alumina-based particles obtained in the above-mentioned alumina-based particle preparation step.
[0031] A conventionally known method can be used for supporting sodium. For example, a method of spraying an aqueous solution containing sodium onto alumina-based particles, a method of mixing alumina-based particles and sodium in an aqueous solution and then removing the water, etc. can be used. The aqueous solution containing sodium can be prepared by dissolving a sodium salt in water. Specific examples of sodium salts include sodium carbonate, sodium hydroxide, and sodium chloride.
[0032] The production method of the present invention includes a molding step in which the alumina-based particles having sodium supported on their surfaces obtained in the sodium supporting step described above are mixed with zeolite to prepare a molded body.
[0033] The molded body can be prepared by a conventional method, for example, a method of mixing alumina particles, zeolite, and a solvent to prepare a kneaded product, and extruding the kneaded product into pellets, or a method of dry-mixing alumina particles and zeolite, and then compression-molding the mixture into pellets.
[0034] After forming into a molded body by the above-mentioned method, the solvent such as water contained in the molded body may be removed by drying. Furthermore, the strength of the molded body can be further increased by firing the molded body in air. The temperature at which the molded body is fired is preferably in the range of 400°C or higher and 650°C or lower. If the firing temperature is too high, the crystal structure of the zeolite may be destroyed, and the amount of carbon dioxide adsorption may decrease.
[0035] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0036] [Measurement method or evaluation method] The various measurements and evaluations were carried out as follows.
[0037] [1] Crystal structure and crystallite size (alumina-based particles) The X-ray diffraction pattern of the alumina hydrate microparticles was measured using MiniFlex manufactured by Rigaku Corporation. The measurement conditions were as follows: the operating axis was 2θ / θ, CuKα was used as the radiation source, and the voltage was 40 kV, the current was 15 mA, the start angle was 2θ=5°, and the end angle was 2θ=50°, the sampling width was 0.02°, and the scan speed was 10.0° / min. The crystallite diameter was calculated from the half-width of the diffraction peak corresponding to the (020) plane at 2θ=14.5° using the Scherrer formula.
[0038] [2] Composition (SiO2 / Al2O3 molar ratio, Na content, K content, Ca content) 3 g of the measurement sample was collected in a 30 ml zirconia bowl with a lid, heated (200°C, 20 min), and sintered (700°C, 5 min), after which 2 g of Na2O2 and 1 g of NaOH were added and melted for 15 min. Further, 25 ml of H2SO4 and 200 ml of water were added to dissolve, and then the mixture was diluted with pure water to 500 ml to prepare a sample. The obtained sample was measured for the content of each component based on the oxide (SiO2, Al2O3, Na2O, K2O, CaO) mass standard using an inductively coupled plasma (ICP) emission spectrometer (Shimadzu Corporation, ICPS-8100, analysis software ICPS-8000).
[0039] [3] Specific surface area Approximately 30 mL of the measurement sample was placed in a magnetic crucible (B-2 type), heated at 600°C for 2 hours, and then cooled to room temperature in a desiccator to obtain a measurement sample. Next, 1 g of this sample was taken and the specific surface area (m 2 / g) was measured by the BET method.
[0040] [4] Pore volume and average pore diameter The pore volume and average pore diameter were measured using BELSORP-mini Ver2.5.6 manufactured by Microtrack-Bell Co., Ltd. Specifically, the measurement sample was heat-treated at 500°C for 2 hours while being evacuated to a vacuum, and nitrogen gas was adsorbed onto the sample. The pore volume (ml / g) and average pore diameter (nm) were calculated from the desorption side isotherm of the relative pressure (P / P0 = 0.99) of the BJH method.
[0041] [5] Carbon dioxide adsorption amount and carbon dioxide retention rate at 30℃ Carbon dioxide adsorption and desorption tests were performed using Microtrack-Bell's "BELCATII." 0.1 g of the measurement sample was placed in the measurement cell, and evacuation was performed at 400°C for 1 hour under a helium gas flow of 50 ml per minute. After that, the temperature was reduced to 30°C, and carbon dioxide gas was introduced for 1 hour to measure the amount of adsorption. Next, helium gas was introduced for 1 hour, and the amount of carbon dioxide desorbed at 30°C (X) was measured, and then the amount of carbon dioxide desorbed with the temperature increase (Y) was measured while the temperature was increased from 30°C to 300°C at a rate of 10°C per minute.
[0042] Carbon dioxide retention rate at 30℃ (%) = (X / (X+Y)) × 100 [Example 1] Alumina-based particle preparation process 500g of sodium gluconate solution with a concentration of 26% by mass was added to 12.7kg of sodium aluminate solution (3% by mass in terms of Al2O3 concentration) while stirring, and 28kg of aluminum sulfate (1.5% by mass in terms of Al2O3 concentration) was added over 5 minutes. Then, stirring was stopped, and the mixture was aged at 60°C for 90 minutes, filtered with a flat filter, and washed with ammonia water with a concentration of 1.5%. The washed cake obtained was mixed with pure water to prepare a suspension with an Al2O3 concentration of 8.0% by mass. This suspension was heated to 95°C, nitric acid with a concentration of 10% was added to adjust the pH to 7.5, and the mixture was stirred for 5 hours while maintaining the temperature at 95°C. Then, acetic acid with a concentration of 20% was added to adjust the pH to 4.0, and the mixture was stirred for 5 hours while maintaining the temperature at 95°C to obtain a suspension of alumina hydrate fine particles. This suspension was adjusted to 35° C., and then spray-dried as droplets in a spray dryer at an inlet temperature of 250° C. and an outlet temperature of 100° C. to obtain alumina-based particles.
[0043] Sodium loading process The alumina-based particles were mixed with pure water to prepare a suspension containing 20.0% by mass of Al2O3. Sodium bicarbonate powder was then added so that the Na content was 0.5% by mass in terms of Na2O relative to 100% by mass of the alumina-based particles, and the mixture was stirred for 30 minutes. The suspension was made into droplets in a spray dryer and spray-dried at an inlet temperature of 250°C and an outlet temperature of 100°C to obtain alumina-based particles (1). The properties of the alumina-based particles (1) were analyzed using the measurement methods described in [1] and [2] above. The results are shown in Table 1.
[0044] Molding process The zeolite has a SiO2 / Al2O3 molar ratio of 2.7, a Na content of 18.0 mass% calculated as Na2O relative to 100 mass% of zeolite, and a specific surface area of 680 m 2 A faujasite-type zeolite (1) of 1000 g / g was prepared. 85 g of this faujasite-type zeolite (1) was mixed with 23 g of the alumina-based particles (1) obtained in the above-mentioned step and 40 g of water, thoroughly kneaded, and extrusion-molded using an extruder (die hole diameter = 2.3 mmφ). The mixture was then dried at 120°C for 24 hours, cut to a length of about 5 mm, and fired at 600°C for 2 hours to obtain a molded body. The properties of this molded body were analyzed using the measurement and evaluation methods described in [1] to [5] above. The results are shown in Table 1.
[0045] [Example 2] Alumina-based particles (2) were obtained in the same manner as in Example 1, except that in the sodium supporting step, sodium bicarbonate powder was added so that the Na content was 1.0 mass% in terms of Na2O relative to 100 mass% of the alumina-based particles.
[0046] A molded body was obtained in the same manner as in Example 1, except that 96 g of the faujasite-type zeolite (1) and 12 g of the alumina-based particles (1) were used in the preparation step of the molded body. The properties of this molded body were analyzed using the measurement and evaluation methods described in the above [1] to [5]. The results are shown in Table 1.
[0047] [Example 3] Alumina-based particles (2) were obtained in the same manner as in Example 1, except that in the sodium supporting step, sodium bicarbonate powder was added so that the Na content was 5.0 mass% in terms of Na2O relative to 100 mass% of the alumina-based particles.
[0048] In the molding process, the zeolite was prepared with a SiO2 / Al2O3 molar ratio of 3.5, a Na content of 17.0 mass% calculated as Na2O, and a specific surface area of 700 m 2 A molded body was obtained in the same manner as in Example 1, except that faujasite-type zeolite (2) of 0.01 g / g was prepared, faujasite-type zeolite (2) was used instead of faujasite-type zeolite (1), and alumina-based particles (2) were used instead of alumina-based particles (1). The properties of this molded body were analyzed using the measurement and evaluation methods described in the above [1] to [5]. The results are shown in Table 1.
[0049] [Example 4] Alumina-based particles (3) were obtained in the same manner as in Example 1, except that in the sodium supporting step, sodium bicarbonate powder was added so that the Na content was 8.0 mass% in terms of Na2O relative to 100 mass% of the alumina-based particles.
[0050] A molded body was obtained in the same manner as in Example 3, except that alumina-based particles (3) were used instead of alumina-based particles (2) in the molding step. The properties of this molded body were analyzed using the measurement and evaluation methods described in the above [1] to [5]. The results are shown in Table 1.
[0051] [Example 5] Alumina-based particle preparation process An alumina boehmite powder having a crystallite size of 25 nm (product name: Catapal-200, manufactured by Sasol) was prepared.
[0052] Sodium loading process The alumina boehmite powder was mixed with pure water to prepare a suspension containing 20.0% by mass of Al2O3. Sodium bicarbonate powder was then added so that the Na content was 5.0% by mass in terms of Na2O relative to 100% by mass of the alumina boehmite powder, and the mixture was stirred for 30 minutes. The suspension was made into droplets in a spray dryer and spray-dried at an inlet temperature of 250°C and an outlet temperature of 100°C to obtain alumina-based particles (4).
[0053] A molded body was obtained in the same manner as in Example 3, except that alumina-based particles (4) were used instead of alumina-based particles (2) in the molding step. The properties of this molded body were analyzed using the measurement and evaluation methods described in the above [1] to [5]. The results are shown in Table 1.
[0054] [Comparative Example 1] Alumina-based particles (5) were obtained in the same manner as in Example 1, except that the sodium supporting step was not carried out. A molded body was obtained in the same manner as in Example 3, except that the alumina-based particles (5) were used instead of the alumina-based particles (2) in the molding step. The properties of this molded body were analyzed using the measurement and evaluation methods described in the above [1] to [5]. The results are shown in Table 1.
[0055] [Comparative Example 2] In the molding process, the zeolite had a SiO2 / Al2O3 molar ratio of 5.1, a Na content of 4.1 mass% in terms of Na2O relative to 100 mass% of zeolite, and a specific surface area of 640 m 2A molded body was obtained in the same manner as in Comparative Example 1, except that faujasite-type zeolite (3) having a molecular weight of 1.001 to 1.001 g was prepared and that faujasite-type zeolite (3) was used instead of faujasite-type zeolite (1). The properties of this molded body were analyzed using the measurement and evaluation methods described in the above [1] to [5]. The results are shown in Table 1.
[0056] [Comparative Example 3] Alumina-based particles (6) were obtained in the same manner as in Example 1, except that in the sodium supporting step, potassium carbonate powder was added instead of sodium carbonate powder so that the K content was 5.0 mass% in terms of K2O relative to 100 mass% of the alumina-based particles.
[0057] A molded body was obtained in the same manner as in Example 3, except that alumina-based particles (6) were used instead of alumina-based particles (2) in the molding step. The properties of this molded body were analyzed using the measurement and evaluation methods described in the above [1] to [5]. The results are shown in Table 1. The properties of the alkali metal-containing alumina hydrate fine particles (5) are shown in Table 1.
[0058] [Reference example] Molecular Sieves 5A (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the zeolite molded body. The properties of this molded body were analyzed using the measurement and evaluation methods described in [1] to [5] above. The results are shown in Table 1.
[0059] [Table 1]
[0060] When the molded body of Example 3 containing alumina-based particles (Na content 5.0% by mass) obtained through the sodium supporting process is compared with Comparative Example 1 containing alumina-based particles (Na content 0.01% by mass) without the sodium supporting process, the carbon dioxide adsorption amount and the carbon dioxide retention rate at 30°C were both Example 3>Comparative Example 1. In addition, looking at the examples and comparative examples as a whole, the molded bodies of Examples 1 to 5 containing alumina-based particles obtained through the sodium supporting process have a carbon dioxide adsorption amount of 0.6 mmol / g or more and a carbon dioxide retention rate at 30°C of 40% or more, whereas the molded bodies of Comparative Examples 1 to 4 containing alumina-based particles without the sodium supporting process did not satisfy both of these. Therefore, it was confirmed that a carbon dioxide adsorbent with a large carbon dioxide adsorption amount and a high carbon dioxide retention rate at low temperatures can be obtained by using alumina-based particles with sodium supported on the surface. In addition, when compared with Comparative Example 3 containing alumina-based particles (K content 5.0% by mass) with potassium supported on the surface, Example 3>Comparative Example 1, and it was confirmed that the effect of sodium is remarkable among alkali metals. Furthermore, it was confirmed that the molded bodies of Examples 1 to 5 were superior in terms of carbon dioxide retention at 30°C in comparison with a commercially available molecular sieve adsorbent (Reference Example).
Claims
[Claim 1] A carbon dioxide adsorbent comprising zeolite and alumina-based particles, the content of the alumina-based particles is in the range of 5% by mass or more and 30% by mass or less with respect to 100% by mass of the molded body, sodium is supported on the surface of the alumina-based particles, The sodium content of the alumina-based particles is 0.1% by mass or more relative to 100% by mass of the alumina-based particles. Carbon dioxide absorbent.
Citation Information
Patent Citations
Composite adsorbent for refining hydrocarbon stream
JP2002253959A
Purification method and purification device of gas
JP2010195616A
Low-reactivity adsorbent and high oxygenate-containing capacity for removing oxygenated substances from olefin streams.
JP2013506554A
Composite adsorbents for purifying hydrocarbon streams
US20020147377A1
Lower Reactivity Adsorbent and Higher Oxygenate Capacity for Removal of Oxygenates from Olefin Streams
US20110079145A1