Metal wire for welding additive manufacturing by metal 3D printer, additive manufacturing product, method for producing additive manufacturing molding
By controlling cooling rates and chemical compositions of duplex stainless steel wires, the method addresses the corrosion resistance issue in additively manufactured products, achieving high corrosion resistance and cost-effectiveness.
Patent Information
- Application Number
- JP2023047747
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Additively manufactured products using duplex stainless steel metal wires experience a decrease in corrosion resistance due to the precipitation of sigma phase and Cr carbonitrides during welding and lamination processes.
A manufacturing method using duplex stainless steel metal wires with controlled cooling rates and specific chemical compositions to suppress the precipitation of sigma phase and Cr carbonitrides, maintaining corrosion resistance by limiting the Cr and Mo residues to 0.1% or less, and employing MIG arc welding with a cooling rate of 1°C/s or more.
The method produces additively manufactured products with excellent corrosion resistance at a low cost, ensuring the necessary corrosion resistance is maintained through controlled chemical composition and cooling rates.
Smart Images

Figure 2024136592000001 
Figure 2024136592000002 
Figure 2024136592000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal wire for deposition additive manufacturing using a metal 3D printer, an additive manufactured product, and a method for manufacturing an additive manufactured product, and relates to an additive manufactured product that uses duplex stainless steel and is inexpensive and maintains the necessary corrosion resistance as an additive manufactured product. [Background technology]
[0002] In recent years, metal 3D printers have been expected to be a revolutionary production technology, and various technologies have been proposed. The main technical methods proposed are those that use metal powder and those that use metal wire.
[0003] When using metal wire, for example, a method of stacking weld beads formed by metal wire to form a three-dimensional part has been disclosed (Patent Document 1). Also, a manufacturing method has been disclosed in which stainless steel metal wire is welded and stacked using two deposition devices to reduce thermal deformation, stress, and internal cracks caused by high heat during deposition (Patent Document 2).
[0004] Patent Document 3 discloses a metal wire for deposition additive manufacturing by a metal 3D printer, which is made of ferritic stainless steel and has excellent heat resistance, heat deformation resistance, material uniformity, intergranular corrosion resistance, and stress corrosion resistance. Patent Document 4 discloses a metal wire for deposition additive manufacturing by a metal 3D printer, which is made of austenitic stainless steel and has excellent heat resistance, toughness, and heat deformation resistance, material uniformity, and intergranular corrosion resistance. Patent Document 5 discloses a method of using a stainless steel metal wire for 3D modeling by deposition and layering using a 3D printer, in which the transformation temperature of the metal structure is controlled to adjust the composition so that a martensite structure with low C and N always appears, and which has excellent heat resistance (thermal deformation resistance), material and metal structure uniformity, internal cracking resistance, and internal void resistance, in a manufacturing method of 3D modeling by deposition and layering using a metal wire.
[0005] Duplex stainless steel is a stainless steel that has both austenite and ferrite phases in the steel structure. Duplex stainless steel has a lower Ni content and higher strength than austenitic stainless steel, which generally has the same corrosion resistance, and is therefore attracting attention as a material that can be made thinner and has lower alloy costs. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2003-266174 A [Patent Document 2] JP 2018-87379 A [Patent Document 3] JP 2020-158842 A [Patent Document 4] JP 2020-164882 A [Patent Document 5] JP 2020-147785 A Summary of the Invention [Problem to be solved by the invention]
[0007] There is a demand for inexpensive, highly corrosion-resistant additive manufacturing products that are 3D-modeled by metal wire deposition and lamination. One possible method is to use a wire made of duplex stainless steel as the welding material for additive manufacturing.
[0008] When using the above-mentioned duplex stainless steel metal wires to manufacture 3D shapes by welding and layering using a 3D printer, a problem occurs in that the corrosion resistance decreases due to the precipitation of sigma phases and Cr carbonitrides. Sigma phases are intermetallic compounds of Cr, Mo, and Fe. When sigma phases precipitate in duplex stainless steel, a chromium-depleted layer forms around them, reducing corrosion resistance. In addition, when Cr carbonitrides precipitate in duplex stainless steel, corrosion resistance also decreases.
[0009] The present invention aims to provide a metal wire for deposition additive manufacturing using a metal 3D printer, an additive manufactured product, and a method for manufacturing an additive manufactured product, which uses a metal wire made of duplex stainless steel and can maintain the corrosion resistance required for additive manufactured products in a 3D printer. [Means for solving the problem]
[0010] As a result of various investigations to solve the above problems, the inventors have discovered that in a manufacturing method in which metal wire made of duplex stainless steel is used and 3D modeling is performed by welding and continuous layering using a 3D printer, additive manufacturing is performed using metal wire made of duplex stainless steel that satisfies specific component composition conditions, the cooling rate in the temperature range where sigma phase and carbonitrides precipitate is controlled to 1°C / s or more, and the total amount of Cr and Mo residues, which affect corrosion resistance, is suppressed to 0.1% or less, and an additive manufacturing product with good corrosion resistance can be obtained.
[0011] That is, the gist of the present invention is as follows. [1] In mass percent, Contains C: 0.005-0.050%, Si: 0.1-1.5%, Mn: 0.1-2.5%, P: 0.10% or less, S: 0.030% or less, Ni: 2.0-12.0%, Cr: 20.0-26.0%, Mo: 0.5-3.5%, Cu: 1.5% or less, Al: 0.003-0.050%, N: 0.05-0.30%, Further, the composition contains one or more of Nb: 0.5 mass% or less, V: 1.0 mass% or less, and W: 1.0 mass% or less in total of 0.05 mass% to 2.00 mass%, The chemical composition is the balance Fe and impurities. A metal wire for use in deposition additive manufacturing with a metal 3D printer, characterized in that the DF value defined by the following formula (1) is 30% to 70%. DF value=7.2(Cr+0.88Mo+0.78Si)-8.9(Ni+0.03Mn+0.72Cu+22C+21N)-44.9 (1) In formula (1), the element symbol indicates the content (mass %) of the corresponding element in the metal wire. [2] Part of the Fe is replaced with further mass% The metal wire for deposition additive manufacturing by a metal 3D printer according to [1], characterized in that it contains one or more of Co: 0.01 to 1.00%, Ti: 0.001 to 0.030%, Ta: 0.005 to 0.200%, Zr: 0.001 to 0.050%, Hf: 0.001 to 0.050%, Sn: 0.001 to 0.100%, B: 0.0001 to 0.0050%, Ca: 0.0005 to 0.0050%, Mg: 0.0001 to 0.0030%, and REM: 0.005 to 0.100%. [3] A metal wire for deposition additive manufacturing by a metal 3D printer as described in [1] or [2], characterized in that when the metal wire is used as a welding material to be MIG arc welded and cooled at an average cooling rate of 1°C / s or more from the end of welding to 500°C, the amount of Cr+Mo residue extracted by an extraction residue method is 0.1 mass% or less.
[0012] [4] An additive manufacturing product, which is formed by deposition of multiple layers having the component composition described in [1] or [2], and is characterized in that the amount of Cr+Mo residue extracted by the extraction residue method is 0.1 mass% or less.
[0013] [5] A method for manufacturing an additive manufacturing product in which the amount of Cr+Mo residue extracted by the extraction residue method is 0.1 mass% or less, the method comprising the steps of: using a metal wire for additive manufacturing by a metal 3D printer described in [1] or [2] as a welding material; carrying out additive manufacturing by MIG arc welding; and then cooling from the end of welding to 500°C at an average cooling rate of 1°C / s or more. Effect of the Invention
[0014] According to the present invention, it is possible to provide reliable additive manufacturing products with excellent corrosion resistance at low cost, even in the case of additive manufacturing products that are made by using duplex stainless steel metal wire, fusing and continuously layering using MIG arc welding with a 3D printer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Each of the requirements of the present invention will be explained below.
[0016] The additive manufacturing product of the present invention can be produced by performing additive manufacturing using MIG arc welding with a metal 3D printer using the metal wire for additive manufacturing with the metal 3D printer of the present invention as a welding material to perform three-dimensional modeling.
[0017] The sigma phase and Cr carbonitride in the steel of the additive manufacturing product will be described. As described above, if the sigma phase or Cr carbonitride is excessively generated in the steel of the additive manufacturing product using duplex stainless steel, the corrosion resistance of the additive manufacturing product will be reduced. It has been found that the degree of the influence of the sigma phase and Cr carbonitride on the corrosion resistance can be evaluated by the amount of Cr+Mo residue extracted by the extraction residue method. Both the sigma phase and Cr carbonitride in the steel are detected as Cr+Mo residue when the precipitates are extracted from the steel by the extraction residue method. If the amount of Cr+Mo residue extracted by the extraction residue method is 0.1% by mass or less, the corrosion resistance of the additive manufacturing product can be suppressed from decreasing. The amount of Cr+Mo residue is preferably 0.05% by mass or less.
[0018] Specifically, the extraction residue method is a method in which the target precipitate is separated from the steel by chemical extraction and separation, then decomposed and dissolved in acid, etc., and extracted. The extracted precipitate is subjected to elemental analysis evaluation by plasma emission spectrometry (ICP) or atomic absorption spectrometry, etc., and the amount of precipitate in the steel as a result of the evaluation is regarded as the "Cr+Mo residue amount" and is expressed as a mass % relative to the steel.
[0019] The corrosion resistance of an additive manufacturing product can be evaluated by evaluating the pitting potential, which is an index of the susceptibility of a material to pitting corrosion, and the critical pitting temperature. The pitting potential is measured to evaluate the pitting corrosion resistance of a metal surface, and the critical pitting temperature is measured to evaluate the pitting corrosion resistance of a metal surface.
[0020] The DF value defined by the following formula (1) is known. The DF value in formula (1) is known as a parameter that indicates the stability of the austenite phase. The metal wire and the additive manufacturing product of the present invention are characterized in that, in addition to containing the component composition specified below, the DF value defined by the following formula (1) is 30% to 70%. By adjusting the DF value within this range, the thermal history conditions during additive manufacturing described below are also satisfied, and thus the precipitation of sigma phase after additive manufacturing can be suppressed. By making the DF value 30% or more, the corrosion resistance (pitting potential, critical pitting temperature) can be improved. In addition, by making the DF value 70% or less, the amount of Cr+Mo residue can be reduced, and the corrosion resistance (pitting potential) can be improved. DF value=7.2(Cr+0.88Mo+0.78Si)-8.9(Ni+0.03Mn+0.72Cu+22C+21N)-44.9 (1) In formula (1), the element symbol indicates the content (mass %) of the corresponding element in the metal wire.
[0021] The metal wire and the additive manufacturing product of the present invention are also characterized by containing at least one of Nb: 0.5 mass% or less, V: 1.0 mass% or less, and W: 1.0 mass% or less in a total amount of 0.05 mass% to 2.00 mass%. This, combined with satisfying the thermal history conditions during additive manufacturing described below, makes it possible to suppress the precipitation of Cr carbonitrides after additive manufacturing. By making the total of Nb, V, and W 0.05 mass% or more, a part of the Cr carbonitrides is replaced with Nb, V, and W carbonitrides, reducing the amount of Cr+Mo residue and improving the corrosion resistance (pitting potential).
[0022] First, the essential component composition of the metal wire and layered manufacturing product of the present invention will be described. In the following description, % means mass % unless otherwise specified.
[0023] C: 0.005 to 0.050% C is an element that dissolves in the austenite phase to increase strength, and is set to 0.005% or more. However, if the C content exceeds 0.050%, it promotes the precipitation of Cr carbonitrides, resulting in poor corrosion resistance (pitting potential) of the additive manufacturing product. Therefore, the C content is set to 0.050% or less. It is preferably set to 0.030% or less, and more preferably set to 0.020% or less.
[0024] Silicon: 0.1 to 1.5% Silicon is contained at 0.1% or more as a deoxidizing element and to improve oxidation resistance. However, if the silicon content exceeds 1.5%, the corrosion resistance (critical pitting temperature) of the additive manufacturing product becomes poor. Therefore, the silicon content is set to 1.5% or less. The silicon content is preferably 1.0% or less.
[0025] Mn: 0.1-2.5% Mn increases the austenite phase and increases the solid solubility of nitrogen, suppressing air bubbles during manufacturing, so it should be included at 0.1% or more. However, if a large amount of Mn is included, it reduces corrosion resistance (pitting potential). Therefore, the Mn content should be 2.5% or less.
[0026] P:0.10% or less P is an element that is inevitably mixed into steel, and is also contained in raw materials such as Cr, so it is difficult to reduce, but a large amount of P reduces formability. The lower the P content, the better, and it is set to 0.10% or less. The P content is preferably 0.040% or less. A lower P content is desirable, but reducing the P content would result in a significant increase in costs, so the P content may be 0.0005% or more.
[0027] S: 0.030% or less S is an element that is inevitably mixed into steel, and it can combine with Mn to form inclusions that can become the starting point for rusting. Therefore, the S content is set to 0.030% or less. The lower the S content, the better the corrosion resistance, so it is preferable to keep it at 0.002% or less.
[0028] Ni: 2.0-12.0% Ni is an austenite stabilizing element and is an important element for ensuring corrosion resistance. Ni also has the effect of improving corrosion resistance. However, a large amount of Ni included increases the raw material cost and may cause problems such as stress corrosion cracking. Therefore, the Ni content is set to 2.0% or more and 12.0% or less. The Ni content is preferably 5.0% or more. Also, the Ni content is preferably 9.5% or less.
[0029] Cr: 20.0~26.0% Cr is an element necessary to ensure corrosion resistance, and is contained at 20.0% or more. However, if a large amount of Cr is contained, the amount of sigma phase precipitation in the additive manufacturing product increases, and the amount of Cr+Mo residue increases, resulting in poor corrosion resistance (pitting potential). Therefore, the Cr content is set to 26.0% or less. The Cr content is preferably 21.0% or more, and more preferably 22.0% or more. In addition, the Cr content is preferably 25.0% or less, and more preferably 24.0% or less.
[0030] Mo: 0.5-3.5% Mo is an element that improves corrosion resistance. However, if a large amount of Mo is contained, it increases the cost of raw materials and causes a problem of reduced corrosion resistance due to the precipitation of sigma phase in the additive manufacturing product. Therefore, the Mo content is set to 0.5% or more and 3.5% or less. In order to obtain the above effect, the Mo content is preferably 2.0% or more. Also, the Mo content is preferably 3.4% or less.
[0031] Cu:1.5% or less Cu is an element that is very effective in improving sulfuric acid resistance, and may be added as necessary. To obtain the above effect, the Cu content is preferably 0.05% or more. On the other hand, excessive addition of Cu may reduce toughness, so the Cu content is set to 1.5% or less. The Cu content is preferably 0.5% or less.
[0032] Al: 0.003 to 0.050% The Al content is set to 0.003% or more for desulfurization and deoxidization. However, if the Al content is too high, it will increase manufacturing defects and raw material costs. Therefore, the Al content is set to 0.050% or less.
[0033] N: 0.05~0.30% N is an element that dissolves in the austenite phase to increase strength and corrosion resistance, thereby contributing to alloy saving, and is contained at 0.05% or more. However, N is an element that greatly affects the precipitation of Cr carbonitrides during cooling in additive manufacturing. If it is contained at more than 0.30%, the amount of Cr carbonitrides precipitated increases. Therefore, the N content is set to 0.30% or less. From the viewpoint of strength and corrosion resistance, the N content may be 0.08% or more, preferably 0.10% or more, and more preferably 0.15% or more. In addition, from the viewpoint of suppressing the precipitation of Cr carbonitrides, the N content is preferably 0.25% or less, and more preferably 0.20% or less.
[0034] As described above, the metal wire and the additive manufacturing product of the present invention are also characterized by further containing 0.05% by mass to 2.00% by mass in total of one or more of 0.5% by mass or less Nb, 1.0% by mass or less V, and 1.0% by mass or less W. This, combined with satisfying the thermal history conditions during additive manufacturing described below, makes it possible to suppress the precipitation of Cr carbonitrides after additive manufacturing.
[0035] Nb: 0.5% by mass or less Nb is an element that has affinity with C and N, and has the effect of suppressing the precipitation of Cr carbonitrides, thereby improving corrosion resistance. If the Nb content is too high, the carbonitrides become excessively coarse, and the desired corrosion resistance cannot be obtained. Therefore, the Nb content is preferably 0.5 mass% or less, and preferably 0.2 mass% or less.
[0036] V: 1.0% or less V is an element that has affinity with C and N, and has the effect of suppressing the precipitation of Cr carbonitrides, thereby improving corrosion resistance. If the V content is too high, the carbonitrides become excessively coarse, and the desired corrosion resistance cannot be obtained. Therefore, the V content is 1.0 mass% or less, preferably 0.5 mass% or less, and more preferably 0.2 mass% or less.
[0037] W: 1.0% or less W has affinity with C and N, has the effect of suppressing the precipitation of Cr carbonitrides, and is an element that improves corrosion resistance like Mo. If the W content is too high, the carbonitrides become excessively coarse, and the desired corrosion resistance cannot be obtained. Therefore, the W content is 1.0 mass% or less, preferably 0.5 mass% or less, and more preferably 0.2 mass% or less.
[0038] The metal wire and the layered product of the present invention are composed of the remainder Fe and impurities. Furthermore, it is preferable that the metal wire and the layered product selectively contain the following components in place of a portion of the Fe.
[0039] Co: 0.01 to 1.00% Co is an effective element for improving corrosion resistance, so it may be contained in an amount of 0.01% or more as necessary. Co is an expensive element, and even if it is contained in an amount exceeding 1.00%, it is difficult to obtain an effect commensurate with the cost, so the Co content is preferably 1.00% or less.
[0040] Ti: 0.001 to 0.030% Ti is an element that improves corrosion resistance, so it may be contained in an amount of 0.001% or more as necessary. However, if Ti is contained in a large amount, Ti nitrides become coarse and the toughness is deteriorated. Therefore, the Ti content is set to 0.030% or less.
[0041] Ta: 0.005 to 0.200% Ta is an element that improves corrosion resistance by modifying inclusions, so it may be contained in an amount of 0.005% or more as necessary. However, if Ta is contained in a large amount, nitrides of Ta will precipitate and deteriorate toughness. Therefore, the Ta content is set to 0.200% or less.
[0042] Zr: 0.001 to 0.050% Zr is an effective element for improving oxidation resistance, so it may be added in an amount of 0.001% or more as necessary. However, if a large amount of Zr is added, coarse Zr nitrides precipitate, which deteriorates toughness. Therefore, the Zr content is set to 0.050% or less.
[0043] Hf: 0.001~0.050% Hf, like Zr, is an effective element for improving oxidation resistance, so it may be added in an amount of 0.001% or more as necessary. However, if a large amount of Hf is added, coarse Hf nitrides precipitate, which deteriorates toughness. Therefore, the Hf content is set to 0.050% or less.
[0044] Sn: 0.001 to 0.100% Sn is an element that improves corrosion resistance, so it may be contained in an amount of 0.001% or more as necessary. However, if a large amount of Sn is contained, it deteriorates hot workability. Therefore, the Sn content is set to 0.100% or less.
[0045] B: 0.0001 to 0.0050% B is an element that has a very strong affinity with N, so it may be contained in an amount of 0.0001% or more as necessary. However, if a large amount of B is contained, the corrosion resistance significantly deteriorates. Therefore, the B content is set to 0.0050% or less. The B content is preferably set to 0.0030% or less.
[0046] Ca: 0.0005~0.0050% Ca may be added in an amount of 0.0005% or more for desulfurization and deoxidization as necessary. However, if a large amount of Ca is added, the corrosion resistance decreases. Therefore, the Ca content is set to 0.0050% or less.
[0047] Mg: 0.0001 to 0.0030% Mg not only has the effect of deoxidizing, but also of refining the solidified structure, so it may be contained in an amount of 0.0001% or more as necessary. However, the inclusion of a large amount of Mg increases the cost of the steelmaking process. Therefore, the Mg content is set to 0.0030% or less.
[0048] REM: 0.005~0.100% REM (rare earth elements) may be added in an amount of 0.005% or more for desulfurization and deoxidization as necessary. However, if a large amount of REM is added, it impairs manufacturability and increases costs. Therefore, the REM content is set to 0.100% or less. The REM content is preferably 0.020% or more, and 0.040% or less. REM is a general term for 17 elements, including Sc, Y, and 15 elements from La to Lu (lanthanoids), and the REM content refers to the total content of these elements. Lanthanoids are added industrially in the form of misch metals.
[0049] The additive manufacturing product of the present invention is formed by additive manufacturing of a plurality of layers having the above-mentioned component composition of the present invention, and is characterized in that the amount of Cr+Mo residue extracted by the extraction residue method is 0.1 mass% or less, as described above. This allows the additive manufacturing product to maintain good corrosion resistance.
[0050] The method for producing an additive manufacturing product of the present invention is characterized in that it uses a metal wire for additive manufacturing by a metal 3D printer, having the composition of the present invention, as a welding material, performs additive manufacturing by MIG arc welding, and then cools at an average cooling rate of 1°C / s or more from the end of welding to 500°C. By using a metal wire having the composition of the present invention and cooling at an average cooling rate of 1°C / s or more from the end of welding after additive manufacturing to the Cr carbide precipitation temperature range of 500°C, the amount of Cr+Mo residue extracted by the extraction residue method can be reduced to 0.1 mass% or less.
[0051] Regarding the metal wire for deposition additive manufacturing by a metal 3D printer of the present invention, when the metal wire is used as a welding material for deposition additive manufacturing by a metal 3D printer and is deposited by deposition additive manufacturing by MIG arc welding, the Cr+Mo residue amount is 0.1 mass% or more when the metal wire is used as a welding material, and cooled at an average cooling rate of 1°C / s or more from the end of welding to the Cr carbide precipitation temperature range of 500°C. When the average cooling rate is cooled at a predetermined cooling rate of 1°C / s or more, if the Cr+Mo residue amount is excessive, the average cooling rate is increased. As a result, if the Cr+Mo residue amount falls within the range of the present invention, it can be confirmed that the present invention applies, and if not, it does not apply.
[0052] The metal wire of the present invention is used for deposition additive manufacturing by a metal 3D printer. That is, the metal wire means a metal wire used as a material when a deposition bead of a metal wire is laminated by a metal 3D printer to form a three-dimensional part.
[0053] According to the present invention as described above, it is possible to provide a metal wire for deposition additive manufacturing using a metal 3D printer, an additive manufactured product, and a method for manufacturing an additive manufactured product, which is an additive manufactured product using duplex stainless steel and capable of retaining the necessary corrosion resistance. EXAMPLES
[0054] Example 1 Steel having the chemical composition shown in Table 1 was melted in a 45 kg vacuum melting furnace and processed into a steel bar having a diameter of 11 mm by hot forging and hot extrusion. Then, wire drawing and annealing were repeated to produce a metal wire having a diameter of 1.2 mm. In Table 1 and Table 2 described later, values outside the range of the present invention are underlined.
[0055] [Table 1]
[0056] Using a robotic MIG arc welding machine, the prototype metal wire was repeatedly welded while continuously stacking it in a spiral shape. A hollow rectangular column was produced by stacking in a stacking direction perpendicular to the welding direction, creating a 3D shape. The arc welding conditions were an Ar+3% oxygen shielding gas, a welding current of 200A, an arc voltage of 30V, and a welding speed of 200cm / min. After the welded additive manufacturing, the product was cooled from the end of welding to 500°C at an average cooling rate of 1°C / s or more. The average cooling rate was measured using an infrared thermograph (thermal imaging camera) by measuring the cooling time from the temperature of the molded product after welding to the Cr carbide precipitation temperature range of 500°C.
[0057] The above-mentioned chemical extraction and separation method was used as the extraction residue method, and the extracted precipitates were subjected to elemental analysis evaluation by inductively coupled plasma spectrometry (ICP). The amount of Cr and Mo precipitates in the steel as a result of the evaluation was taken as the "Cr + Mo residue amount" and expressed as a mass % relative to the steel. When the evaluated Cr+Mo residual amount exceeded 0.1 mass%, the average cooling rate from the end of welding to 500°C was increased within the range of 1°C / s to 20°C / s, resulting in an adjustment to the Cr+Mo residual amount range of the present invention. Some of the comparative examples could not be adjusted to the Cr+Mo residual amount range of the present invention.
[0058] Thereafter, the produced square pillars were subjected to evaluation of the pitting potential and the critical pitting temperature as an evaluation of the corrosion resistance. The pitting potential evaluation was performed in accordance with JIS G0577:2014. A test piece measuring 15 mm x 20 mm was cut from the center of the lamination direction, and then wet polished with #600. Next, the electrode surface (exposed portion) of this test piece was insulated with silicone resin to cover the other portions of the test piece except for the electrode surface, so that the electrode surface was 10 mm x 10 mm, to obtain a test piece for measuring the pitting potential. Next, the pitting potential was measured in an Ar-deaerated 1 mol / L NaCl solution at 30°C, and the current density was 100 μA / cm. 2 The potential at which the sample reached the maximum value was calculated, and the average of the three measured data points was evaluated as the pitting potential. A pitting potential (V vs. SSE) of 0.5 V or greater was considered to be acceptable. The critical pitting temperature evaluation was performed in accordance with JIS G0590:2013. A test piece measuring 15 mm x 20 mm was cut from the center of the lamination direction, and then wet polished with #600. Next, the electrode surface (exposed portion) of this test piece was insulated with silicone resin except for the electrode surface to obtain a test piece for measuring the critical pitting temperature. Next, the anode current density was measured at 1000 μA / cm in an Ar-deaerated 1 mol / L NaCl solution. 2 The critical pitting temperature (CPT) is reached when the current density is 100 μA / cm 2 The liquid temperature at which this temperature exceeded the threshold was determined, and the average of three measured data points was evaluated as the critical pitting temperature. A critical pitting temperature (CPT) of 30°C or higher was considered to be acceptable. The evaluation results are shown in Table 2.
[0059] [Table 2]
[0060] For the additive manufacturing products using the metal wires of invention steels 1 to 10, the amount of Cr+Mo residue was 0.1 mass % or less, and the corrosion resistance was good in terms of both the pitting potential and the critical pitting temperature.
[0061] On the other hand, it is clear that the additively manufactured products using the comparative steels A to K do not have the component compositions within the ranges specified by the present invention and do not satisfy the required characteristics. Comparative steel A had a C content outside the upper limit, comparative steel B had a Mn content outside the upper limit, comparative steel H had a Ni content outside the lower limit, and comparative steel I had a Mo content outside the upper limit and a Nb+V+W content outside the lower limits, and each had poor corrosion resistance (pitting potential). Comparative steel C had a Cr content outside the upper limit, and comparative steels E and J had Nb+V+W contents outside the lower limits. In all cases, the Cr+Mo residue amount was outside the upper limit, and the corrosion resistance (pitting potential) was poor. Comparative steel D had a Si content outside the upper limit, comparative steel G had a Nb content outside the upper limit, and comparative steel K had a Cu content outside the upper limit, and all of them had poor corrosion resistance (critical pitting temperature). Comparative steel F had a Cr content below the lower limit and had poor corrosion resistance (pitting potential and critical pitting temperature).
[0062] Example 2 Additive manufacturing was performed using steel 1 of the present invention shown in Table 1 of Example 1, with the average cooling rate from the end of welding to 500°C being set to five conditions shown in Table 3 below, and the other conditions being the same as those of Example 1. The amount of Cr+Mo residue in each case was evaluated and shown in Table 3. As is clear from Table 3, a relationship can be seen in which the amount of Cr+Mo residue increases as the cooling rate slows.
[0063] [Table 3]
Claims
1. In mass percent, C: 0.005-0.050%, Si: 0.1-1.5%, Mn: 0.1-2.5%, P: 0.10% or less, S: 0.030% or less, Ni: 2.0-12.0%, Cr: 20.0-26.0%, Mo: 0.5-3.5%, Cu: 1.5% or less, Al: 0.003-0.050%, N: 0.05-0.30%, Further, the composition contains one or more of Nb: 0.5% by mass or less, V: 1.0% by mass or less, and W: 1.0% by mass or less in a total amount of 0.05% by mass to 2.00% by mass, The balance has a chemical composition consisting of Fe and impurities, A metal wire for deposition layered manufacturing by a metal 3D printer, characterized in that the DF value defined by the following formula (1) is 30% to 70%. DF value=7.2(Cr+0.88Mo+0.78Si)-8.9(Ni+0.03Mn+0.72Cu+22C+21N)-44.9... (1) In formula (1), the element symbol indicates the content (mass %) of the corresponding element in the metal wire.
2. In place of a part of the Fe, further in mass%: The metal wire for deposition additive manufacturing using a metal 3D printer according to claim 1, characterized in that it contains one or more of Co: 0.01 to 1.00%, Ti: 0.001 to 0.030%, Ta: 0.005 to 0.200%, Zr: 0.001 to 0.050%, Hf: 0.001 to 0.050%, Sn: 0.001 to 0.100%, B: 0.0001 to 0.0050%, Ca: 0.0005 to 0.0050%, Mg: 0.0001 to 0.0030%, and REM: 0.005 to 0.100%.
3. 3. The metal wire for deposition additive manufacturing by a metal 3D printer according to claim 1 or 2, characterized in that when the metal wire is MIG arc welded as a welding material and cooled at an average cooling rate of 1°C / s or more from the end of welding to 500°C, the amount of Cr+Mo residue extracted by an extraction residue method is 0.1 mass% or less.
4. 3. An additive manufacturing product, comprising a plurality of layers having the component composition according to claim 1 or 2, which are fabricated by additive manufacturing, and characterized in that the amount of Cr+Mo residue extracted by the extraction residue method is 0.1 mass% or less.
5. A method for producing an additive manufacturing product in which the amount of Cr + Mo residue extracted by an extraction residue method is 0.1 mass% or less, A method for manufacturing an additive manufacturing product, comprising the steps of: performing additive manufacturing by MIG arc welding using the metal wire for additive manufacturing by a metal 3D printer according to claim 1 or 2 as a welding material; and then cooling from the end of welding to 500°C at an average cooling rate of 1°C / s or more.
Citation Information
Patent Citations
Method for manufacturing three-dimensional shaped material
JP2003266174A
Metal laminate molding system
JP2018087379A
Metallic wire for welded and multilayered molding by metal 3D printer
JP2020147785A
Metal wire for welded and laminated shaping with metal 3D printer
JP2020158842A
Metal wire for welded and laminated shaping by metal 3D printer
JP2020164882A