Electrolytic polishing method

By employing titanium dummy media at a controlled volume ratio and stirring during electrolytic polishing, the method achieves consistent polishing results, addressing the uniformity issues in existing methods and enhancing product quality for narrow tolerance products.

JP2024136617APending Publication Date: 2024-10-04CITIZEN FINEDEVICE CO LTD +1

Patent Information

Application Number
JP2023047774
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing electrolytic polishing methods face challenges in achieving uniformity of polishing amounts, particularly when manufacturing products with narrow dimensional tolerances, whether using dummy media or not.

Method used

The method involves using titanium dummy media in a ratio exceeding 100% of the volume of the object to be polished, with a specific volume ratio range of 150% to 1000%, and applying a DC voltage while stirring, ensuring controlled current flow and even contact with an anode.

Benefits of technology

This approach results in polished objects with minimal variations in polishing amounts, suitable for products requiring tight dimensional tolerances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136617000001_ABST
    Figure 2024136617000001_ABST
Patent Text Reader

Abstract

To provide an electrolytic polishing method that makes it possible to obtain a polished object with a small variation in the amount of polishing in the electrolytic polishing of an object to be polished made of ferrous metal.SOLUTION: The subject is solved with an electrolytically polishing method for an object to be polished made of ferrous metal by using titanium dummy media comprising a charging process in which multiple object to be polished and multiple titanium dummy media are loaded into a barrel container, and the ratio of the total volume of titanium dummy media to the total volume of object to be polished inside the barrel container is set to be more than 100%, an application process in which the object to be polished and titanium dummy media accommodated inside a barrel container are immersed in an electrolyte solution, an anode is placed so that it is immersed in the electrolyte solution inside the barrel container, and a cathode is placed so that it is immersed in the electrolyte solution outside the barrel container, and then direct current voltage is applied while agitating the object to be polished and the titanium dummy media so that the object to be polished or the titanium dummy media comes into contact with the anode.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for electrolytic polishing of an object to be polished that is made of an iron-based metal. [Background technology]

[0002] Electrolytic polishing is sometimes performed on parts made of ferrous metals such as stainless steel to remove foreign matter and burrs from the surface. This electrolytic polishing is a method in which the object to be polished is immersed in an electrolytic polishing solution (electrolyte) using a barrel container or jig, a voltage is applied between the object to be polished and a counter electrode, and the surface of the object to be polished is smoothed by electrolysis. Although not often performed, electrolytic polishing may be performed by storing media (dummy media) together with the object to be polished in a barrel container or the like.

[0003] For example, Patent Document 1 discloses a method for electrolytic polishing of a stainless steel sheet, in which the stainless steel sheet to be polished is used as the anode and a metal plate as the counter electrode, and the current density pattern applied for electrolytic polishing is characterized in that electrolysis is initially performed at a constant current density of 15% or more and 50% or less of the final current density. Furthermore, Patent Document 2 discloses an electropolishing method characterized by containing an electrolyte, media, and an object to be polished in a container with an open top, and applying a DC voltage to the electrolyte while rocking and vibrating the container. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-287099 [Patent Document 2] Japanese Patent Application Publication No. 5-214600 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in general electrolytic polishing without using dummy media, it is difficult to avoid some variation in the polishing amount. Also, even when electrolytic polishing using dummy media as in Patent Document 2 is performed, there are many cases where a certain degree of variation in the polishing amount occurs between the polished objects (between products) or within the polished object (within the product), and there is room for further improvement, particularly when electrolytic polishing is used to manufacture products with a narrow tolerance range for the required dimensional tolerance.

[0006] Therefore, an object of the present invention is to provide an electrolytic polishing method capable of obtaining a polished object having small variation in the amount of polishing in electrolytic polishing of an object made of an iron-based metal. [Means for solving the problem]

[0007] In order to solve the above problems, the present inventors conducted extensive research and discovered that the ratio of the total volume of titanium dummy media to the total volume of the workpieces inside a barrel container when performing electrolytic polishing affects the variation in the amount of polishing between and within the resulting polished objects. Further research led to the completion of the present invention.

[0008] That is, the present invention provides the following <1> ~ <5> It is. <1> A method for electrolytically polishing a workpiece made of an iron-based metal using titanium dummy media, the method comprising: a loading step of loading a plurality of the workpieces and a plurality of the titanium dummy media into a barrel container, and making the ratio of the total volume of the titanium dummy media to the total volume of the workpieces inside the barrel container exceed 100%; and an application step of immersing the workpieces and the titanium dummy media contained inside the barrel container in an electrolyte, positioning an anode so as to be immersed in the electrolyte inside the barrel container, and further positioning a cathode so as to be immersed in the electrolyte outside the barrel container, and applying a DC voltage while stirring the workpieces and the titanium dummy media so that the workpieces or the titanium dummy media come into contact with the anode. <2> In the loading step, a ratio of a total volume of the titanium dummy media to a total volume of the workpieces inside the barrel container is set to 150% or more and 1000% or less. <1> The electrolytic polishing method according to claim 1. <3> In the loading step, the total volume of the workpieces and the titanium dummy media loaded is set to be 2.0% or more and 8.0% or less of the volume of the internal storage area of ​​the barrel container. <1> or <2> The electrolytic polishing method according to claim 1. <4> the titanium dummy media are substantially cylindrical in shape, and the volume of each of the titanium dummy media is different from the volume of each of the workpieces; <1> ~ <3> 13. The electrolytic polishing method according to claim 12 . <5> The titanium dummy media is made of JIS Class 1 or JIS Class 2 pure titanium. <1> ~ <4> 13. The electrolytic polishing method according to claim 12 . Effect of the Invention

[0009] According to the present invention, a polished object made of an iron-based metal can be electrolytically polished to obtain a polished object with small variation in the amount of polishing. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view showing an example of an embodiment of an electrolytic polishing method according to the present invention. [Diagram 2] 1 is a graph showing the change in standard deviation of diameter (Δσ: μm) before and after electrolytic polishing of a stainless steel cylinder under each condition, measured and calculated in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will now be described. The present invention is a method for electrolytically polishing a workpiece (multiple workpieces) made of an iron-based metal using titanium dummy media (multiple titanium dummy media), which comprises a loading step of loading multiple workpieces and multiple titanium dummy media into a barrel container and making the ratio of the total volume of the titanium dummy media to the total volume of the workpieces inside the barrel container exceed 100%, and an application step of immersing the workpieces and titanium dummy media contained inside the barrel container in an electrolyte, arranging an anode so that it is immersed in the electrolyte inside the barrel container, and further arranging a cathode so that it is immersed in the electrolyte outside the barrel container, and applying a DC voltage while stirring the workpieces and titanium dummy media so that the workpieces or titanium dummy media come into contact with the anode (hereinafter, this may also be referred to as the "electrolytic polishing method according to the present invention").

[0012] Hereinafter, an embodiment of each step of the electrolytic polishing method according to the present invention will be described in detail with reference to Fig. 1 etc. Note that the dimensional ratios of the devices, members, etc. shown in the drawings may differ from the actual dimensional ratios in order to facilitate understanding of the invention.

[0013] <Input process> The loading step is a step of loading a plurality of iron-based metals and a plurality of titanium dummy media into a barrel container. The "barrel container" is a container capable of housing and stirring the objects and titanium dummy media inside during electrolytic polishing. Although not limited thereto, examples thereof include a cylindrical container having a substantially circular cross section in the short side direction and capable of rotating around the axis of the substantially center of the cross section, as shown in FIG. 1, and a container in which the diameter of the cross section (i.e., the side wall of the container) tapers from the center to both ends in the longitudinal direction. The container may be capable of vibrating in addition to rotating. Furthermore, the container may be a polygonal cross section (hexagonal, octagonal, etc.) in the short side direction, and may be configured such that the diameter of the polygonal cross section tapers from the center to both ends in the longitudinal direction. The barrel may be configured to allow the electrolyte (described later) to pass between the inside and outside (for example, a container having a mesh-like side wall that allows the electrolyte to pass between the inside and outside but prevents the workpiece and titanium dummy media from passing to the outside). If necessary, the barrel may be provided with a lid or the like to prevent the workpiece and titanium dummy media from being discharged from the barrel during electrolytic polishing.

[0014] Moreover, "iron-based metal" refers to a metal whose main component is iron. And, this "main component" means that the content of the component is 70 mass% or more. Therefore, examples of the polished object (workpiece) made of iron-based metal include members (parts, etc.) made of stainless steel (martensitic stainless steel, austenitic stainless steel, ferritic stainless steel, austenitic-ferritic stainless steel) and chrome steel. In the description of the present invention, the terms "iron-based metal" and "main component" are used in this sense unless otherwise specified.

[0015] Furthermore, the term "titanium dummy media" refers to dummy media made of titanium (pure titanium or titanium alloy). In this way, since the dummy media used by mixing with the workpiece is made of titanium (particularly pure titanium), which is softer than iron-based metals, the workpiece is unlikely to be deformed or scratched even if it collides with the workpiece during stirring. Furthermore, since the dummy media made of titanium (particularly pure titanium) hardly decomposes during electrolytic polishing and has high conductivity, efficient electrolytic polishing can be achieved. In addition, pure titanium is classified into four types from JIS type 1 to JIS type 4 according to the JIS standard (JIS H 4600) depending on the content of impurities such as Fe and O, the titanium dummy media used in the present invention is particularly preferably made of JIS type 1 pure titanium or JIS type 2 pure titanium from the viewpoint of reducing the influence on the workpiece and performing efficient electrolytic polishing. However, this titanium dummy media may be made of a titanium alloy.

[0016] In this charging step, a plurality of the above-mentioned objects to be polished and titanium dummy media are charged, and the ratio of the total volume of the plurality of titanium dummy media to the total volume of the objects to be polished inside the barrel container is set to more than 100%. This narrows down the amount of current flowing through the objects to be polished during electrolytic polishing, and as a result, the polishing speed (electrolysis speed, cumulative current amount) is controlled overall, and an object to be polished with a small variation in the amount of polishing can be obtained. In addition, since this effect is more easily exhibited, the lower limit of the ratio of the total volume of the titanium dummy media to the total volume of the objects to be polished inside the barrel container is more preferably 110% or more, more preferably 120% or more, even more preferably 150% or more, even more preferably 180% or more, even more preferably 200% or more, and even more preferably 230% or more. The upper limit is preferably 30000% or less, more preferably 25000% or less, even more preferably 20000% or less, even more preferably 15000% or less, even more preferably 10000% or less, even more preferably 5000% or less, even more preferably 3000% or less, even more preferably 2500% or less, even more preferably 2000% or less, even more preferably 1800% or less, even more preferably 1500% or less, even more preferably 1300% or less, even more preferably 1000% or less, even more preferably 900% or less, even more preferably 800% or less. For example, it is extremely preferable that the ratio of the total volume of the titanium dummy media to the total volume of the polished object inside the barrel container is 120% or more and 1500% or less, and even more preferably 150% or more and 1000% or less.

[0017] In addition to the above, it is preferable that the total volume of the workpieces and titanium dummy media (total volume of all workpieces and titanium dummy media put into the barrel container) is 2.0% or more and 8.0% or less as a ratio to the volume of the internal storage area of ​​the barrel container (total volume of the area in the barrel container that can store the workpieces and titanium dummy media). This makes it appear that the entire workpieces and titanium dummy media put in (total area including the area of ​​each gap) occupy about 5 to 20% of the total volume of the internal storage area of ​​the barrel container, and during electrolytic polishing, it is easy to stir the workpieces and titanium dummy media in the barrel container evenly by rotation or the like. In particular, it is more preferable that the above ratio is 2.5% or more and 6.0% or less, even more preferable that it is 2.5% or more and 4.5% or less, and even more preferable that it is 2.5% or more and 4.0% or less.

[0018] Although there are no limitations on the volume of each workpiece and each titanium dummy media that are put (stored) in the barrel container, for example, it is preferable that the volume of each titanium dummy media is about 50 to 150% of the volume of each workpiece (100%), since this facilitates efficient electrolytic polishing. It is also preferable that the multiple titanium dummy media have substantially the same volume (approximately the same shape, etc.). Here, in the present invention, the "volume per workpiece" refers to the volume per workpiece (average value) calculated from the total volume and number of the multiple workpieces placed and housed in the barrel container. Similarly, the "volume per titanium dummy media" refers to the volume per workpiece (average value) calculated from the total volume and number of the multiple titanium dummy media placed and housed in the barrel container.

[0019] In addition, since the polished object and the titanium dummy media are easily separated after electrolytic polishing, it is preferable that the volume of each titanium dummy media put into (contained in) the barrel container is different from the volume of each object to be polished. For example, an embodiment in which the volume of each titanium dummy media is 10% or more larger or 10% or more smaller than the volume of each object to be polished (100%) is exemplified. In particular, it is more preferable that the volume of each titanium dummy media is 50 to 90% or 110 to 150% of the volume of each object to be polished (100%). In this case, it is more preferable that the shape of the titanium dummy media is approximately cylindrical, since the above-mentioned separation is easy while maintaining a high efficiency of electrolytic polishing and is also excellent in terms of cost. However, the shape of the titanium dummy media may be approximately spherical, etc.

[0020] <Printing process> The application step is a step of immersing the plurality of objects to be polished and the plurality of titanium dummy media contained in the barrel container by the aforementioned introduction step in an electrolytic solution, arranging an anode so as to be immersed in the electrolytic solution inside the barrel container, and further arranging a cathode so as to be immersed in the electrolytic solution outside the barrel container, and applying a DC voltage while stirring the objects to be polished and the titanium dummy media so that the objects to be polished or the titanium dummy media come into contact with the anode. In other words, it is a step of electrolytically polishing the objects to be polished by applying a DC voltage.

[0021] The electrolyte (electrolytic polishing solution) is not particularly limited and may be any known electrolyte used in electrolytic polishing, but since the effects of the present invention are more easily exhibited, it is preferable to use an electrolyte having phosphoric acid and / or sulfuric acid and water as the main components (in this case, a total of 70 vol% or more) (for example, an electrolyte having phosphoric acid, sulfuric acid, and water as the main components). In particular, an electrolyte having water and phosphoric acid as the main components (phosphoric acid-based electrolyte) is more preferable. However, this does not exclude electrolytes having other components and water as the main components, and may be, for example, an electrolyte having inorganic acids or salts thereof such as hydrochloric acid, chloric acid, perchloric acid, nitric acid, sulfonic acid (e.g., methanesulfonic acid), acetic acid, propionic acid, citric acid, oxalic acid, malic acid, malonic acid, succinic acid, lactic acid, gluconic acid, tartaric acid, fumaric acid, glutaric acid, adipic acid, maleic acid, ascorbic acid, aconitic acid, glyoxylic acid, glycolic acid, or an organic acid or salt thereof and water as the main components. Furthermore, the ink may contain one or more additives such as metal salts, amines, gelatin, monohydric alcohols, polyhydric alcohols, pH adjusters, surfactants, and chelating agents. Furthermore, the viscosity of the electrolyte is not particularly limited as long as it is liquid, and it may be an electrolyte with a viscosity of about 100 cps as well as one with properties close to that of pure water (viscosity of about 1 cps).

[0022] Then, the workpiece and titanium dummy media housed inside the barrel container are immersed in the electrolyte. For example, the barrel container, which contains the workpiece and titanium dummy media and is configured to allow the electrolyte to pass through it, may be immersed in the electrolyte (such as a tank filled with electrolyte) as is. The electrolyte may be used in an amount such that the workpiece and titanium dummy media housed inside the barrel container are always immersed in the electrolyte during electrolytic polishing, but it may also be used in an amount such that 50% or more of the internal storage area of ​​the barrel container is filled with the electrolyte, or it may be used in an amount such that the entire internal storage area is filled with the electrolyte. Furthermore, the electrolyte may be replenished during electrolytic polishing to maintain the above range.

[0023] Furthermore, an anode is disposed so as to be immersed in the electrolyte inside the barrel container, and a cathode is disposed so as to be immersed in the electrolyte outside the barrel container. The anode and the cathode are connected to a DC power source. The anode and the cathode can be any known electrode used in electrolytic polishing, and are not particularly limited, but it is preferable to use titanium as the anode and a phosphor bronze plate or a copper plate as the cathode. Stainless steel (SUS) or nickel (Ni) can also be used as the cathode. The anode is preferably in a shape that does not interfere with the stirring of the polished object and the titanium dummy media in the barrel container, and is preferably in a rod shape as shown in FIG. 1. In addition, when the anode is rod-shaped, the anode may be a single rod-shaped electrode, or may be in a shape in which two or more rod-shaped electrodes are connected or joined to each other at a part thereof. At least one of the plurality of rod-shaped electrodes may be disposed so as to be immersed in the electrolyte. Although this anode comes into contact with the workpiece and the titanium dummy media during electrolytic polishing, it is not directly connected or joined to the workpiece by a jig, conductor, etc. Furthermore, it is more preferable to arrange multiple cathodes so that they are immersed in the electrolyte outside the barrel container (for example, arranging multiple cathodes so that they sandwich the barrel container as shown in Figure 1).

[0024] Furthermore, the power supply to be used is not particularly limited as long as it is a DC power supply capable of at least both voltage control and current control, but it is more preferable to use a DC power supply that can perform voltage control and current control by program operation, as this makes it easier to control the voltage and current.

[0025] After arranging the anode and the cathode in this way, for example, the barrel container is rotated to stir the polished object and the titanium dummy media so that the polished object or the titanium dummy media (at least one part selected from them) comes into contact with the anode, while applying a DC voltage between the anode (the polished object in direct contact with the anode or indirectly through the titanium dummy media) and the cathode. The contact between the anode and the polished object or the titanium dummy media due to this stirring is such that the ratio of the total volume of the titanium dummy media to the total volume of the polished object is within the range described above, so that the frequency of direct contact between the polished object and the anode is relatively low, that is, the frequency of direct contact between the titanium dummy media and the anode is relatively high, and the amount of current flowing through the polished object during electrolytic polishing is narrowed to a certain extent, while the polished object can be uniformly electrified, so that the embodiment can obtain a polished object with a small variation in the polishing amount. In addition, the presence of the titanium dummy media also exerts effects such as suppressing the reaction of electrolytic polishing from proceeding too quickly and making the polished object easier to stir.

[0026] During this application of voltage, the workpiece and the titanium dummy media must be stirred so that at least a part of the workpiece or the titanium dummy media comes into contact with the anode, i.e., stirring is essential when applying voltage, but the stirring method is not particularly limited. For example, an embodiment in which the barrel container is rotated is exemplified. As described above, the barrel container may be vibrated in conjunction with the rotation.

[0027] The temperature of the electrolyte during electrolytic polishing (i.e., during this voltage application step) is not particularly limited, and may be appropriately set depending on the material of the workpiece to be polished, the type of electrolyte, etc. Also, during electrolytic polishing, the electrolyte may be allowed to circulate gently.

[0028] Furthermore, the conditions of the applied voltage are not limited and can be appropriately set depending on the type of electrolyte used, the shape and material of the workpiece, the desired amount of polishing, the polishing state, etc. During electrolytic polishing, the voltage may be constant, or the voltage may be changed during the process.

[0029] After the electrolytic polishing in the voltage application step is completed, the polished object is separated from the titanium dummy media. As described above, this separation can be performed using a sieve or roller sorter when the volume of each titanium dummy media is different from the volume of each object to be polished. Separation can also be performed using a magnet or a device using a camera.

[0030] <Other processes> The electrolytic polishing method according to the present invention includes the above-mentioned charging step and application step, and may include any other steps as long as they do not significantly affect the effects of the present invention. For example, it may further include a cleaning step for cleaning the polished object obtained.

[0031] By using the electrolytic polishing method according to the present invention, which is an embodiment as described above, it is possible to electrolytically polish an object made of an iron-based metal to obtain polished objects with small variations in the amount of polishing. In other words, it is possible to reduce the variations in the amount of polishing between the multiple polished objects obtained and within one polished object obtained. Therefore, the electrolytic polishing method according to the present invention can be preferably used for the manufacture of products with a narrow tolerance range for the required dimensional tolerance (difference between maximum and minimum values).

[0032] Here, a specific example of the electrolytic polishing method according to the present invention is shown in the schematic diagram of FIG. 1. In FIG. 1, a plurality of objects to be polished 31 and a plurality of titanium dummy media 33 are put into a barrel container 41, and the ratio of the total volume of the titanium dummy media 33 (white) to the total volume of the objects to be polished 31 (blackened) inside the barrel container 41 is set to be more than 100%. In addition, the ratio of the total volume of the objects to be polished 31 and the titanium dummy media 33 to the volume of the internal storage area of ​​the barrel container 41 is set to be 2.0% or more and 8.0% or less. Furthermore, the entire barrel container 41 containing the objects to be polished 31 and the titanium dummy media 33 is immersed in the electrolyte 13 in the electrolytic polishing tank 11, the anode 21 (rod-shaped anode) is arranged so as to be immersed in the electrolyte 13 inside the barrel container 41, and the cathode 23 is arranged so as to be immersed in the electrolyte 13 outside the barrel container 41. The anode 21 and the cathode 23 are connected to a DC power source 51. Then, electrolytic polishing is performed by rotating the barrel container 41 on a rotation axis 43 approximately at the center of its short-side cross section (for example, rotating in the direction of the arrow) and applying a DC voltage while stirring the object to be polished 31 or the titanium dummy media 33 so that they come into contact with the anode 21. After completion of electrolytic polishing, the object to be polished and the titanium dummy media 33 are removed from the barrel container 41, and the titanium dummy media 33 are separated using a sieve, a roller sorter, or the like.

[0033] The electrolytic polishing method according to the present invention is preferably the embodiment as described above, but is not limited thereto, and further modifications and the like are possible within the scope that does not significantly affect the effects of the present invention. EXAMPLES

[0034] Hereinafter, examples of the present invention will be described, however, the present invention is not limited to the following examples, and various modifications are possible within the technical concept of the present invention.

[0035] A stainless steel cylinder (φ2.7×7mm: SUS304) with a diameter of 2.7 mm and a length of 7 mm was used as the object to be polished, and a pure titanium cylinder (φ3×7mm: JIS type 1) with a diameter of 3 mm and a length of 7 mm was used as the titanium dummy media. The amount (number) of the object to be polished shown in Table 1 below and 2000 pieces of the titanium dummy media were put into a barrel container (volume of the internal storage area is 4 L) with a mesh-like side wall and stored. The ratio of the total volume of the titanium dummy media to the total volume of the object to be polished inside the barrel container (dummy volume ratio) is also shown in Table 1 below. For example, when 2000 pieces of the object to be polished and 2000 pieces of the titanium dummy media are put into the barrel container, the ratio of the total volume of the titanium dummy media to the total volume of the object to be polished inside the barrel container is about 123%.

[0036] Then, as shown in Figure 1, the barrel container containing the workpiece and titanium dummy media was immersed in an electrolyte whose main components were water and phosphoric acid (a mixture of EP-13 manufactured by Okuno Pharmaceutical Co., Ltd. and phosphoric acid), a rod-shaped anode (titanium) was placed so that it was immersed in the electrolyte inside the barrel container, and two cathodes (phosphor bronze plates) were placed on either side of the barrel container so that they were immersed in the electrolyte outside the barrel container, and the barrel container was rotated, and a DC voltage was applied while stirring the workpiece and titanium dummy media so that the workpiece or titanium dummy media came into contact with the anode. Note that a DC power supply capable of controlling both voltage and current was used as the power source, and electrolytic polishing was performed by applying a DC voltage while adjusting the temperature of the electrolyte to be constant.

[0037] After the electrolytic polishing, the diameters (μm) of all the polished objects were measured by image measurement to calculate the standard deviation (σ), and the standard deviation (σ) was compared with the standard deviation (σ) calculated from the diameters (μm) of all the polished objects previously measured by the same method to calculate the change in standard deviation (Δσ: μm). The results are shown in Table 1 and Figure 2 below.

[0038] As a result, the standard deviation change (Δσ) was less than 0.8 μm in all cases. Therefore, by making the total volume of the titanium dummy media relative to the total volume of the workpieces contained in the barrel container more than 100%, a polished product with a small standard deviation change (Δσ) before and after electrolytic polishing, that is, a polished product with a small variation in the polishing amount, could be obtained. In particular, when the total volume of the titanium dummy media relative to the total volume of the workpieces contained in the barrel container is about 123% to about 1235%, a polished product with a fairly small variation in the polishing amount could be obtained, and further, when the total volume of the titanium dummy media relative to the total volume of the workpieces is about 247% and about 617%, a polished product with an extremely small variation in the polishing amount could be obtained. Therefore, it was suggested that the total volume of the titanium dummy media relative to the total volume of the workpieces contained in this barrel container is more preferably about 120% or more and 1500% or less, and particularly preferably about 150% or more and 1000% or less.

[0039] [Table 1] [Explanation of symbols]

[0040] 11 Electropolishing tank 13 Electrolyte 21 Anode (rod anode) 23 Cathode 31 Object to be polished 33 Titanium Dummy Media 41 Barrel Container 43 Rotational Axis 51 DC power supply

Claims

1. A method for electrolytically polishing an object to be polished made of an iron-based metal using a titanium dummy media, comprising the steps of: a step of loading a plurality of the objects to be polished and a plurality of the titanium dummy media into a barrel container, and setting a ratio of a total volume of the titanium dummy media to a total volume of the objects to be polished inside the barrel container to be more than 100%; and an application step of immersing the workpiece and the titanium dummy media contained inside the barrel container in an electrolytic solution, arranging an anode so as to be immersed in the electrolytic solution inside the barrel container, and further arranging a cathode so as to be immersed in the electrolytic solution outside the barrel container, and applying a DC voltage while stirring the workpiece and the titanium dummy media so that the workpiece or the titanium dummy media come into contact with the anode. Electrolytic polishing method.

2. 2. The electrolytic polishing method according to claim 1, wherein in the loading step, a ratio of a total volume of the titanium dummy media to a total volume of the workpieces inside the barrel container is set to 150% or more and 1000% or less.

3. 3. The electrolytic polishing method according to claim 1, wherein in the loading step, the total volume of the workpiece and the titanium dummy media loaded is 2.0% or more and 8.0% or less of the volume of the internal storage area of ​​the barrel container.

4. 3. The electrolytic polishing method according to claim 1, wherein the titanium dummy media are substantially cylindrical, and the volume of each of the titanium dummy media is different from the volume of each of the workpieces.

5. 3. The electrolytic polishing method according to claim 1, wherein the titanium dummy media is made of JIS Class 1 or JIS Class 2 pure titanium.

Citation Information

Patent Citations

  • Electrolytic grinding method and device therefor

    JP1993214600A

  • Method of electrolytic grinding wigh high efficiency for stainless steel sheet

    JP1997287099A

Cited By

  • CMP Disk Recycling Method

    KR102878443B1

  • CMP Disk Recycling Device

    KR102901007B1

  • Method for recycling CMP disk

    WO2026225725A1