Laminate paper, method for manufacturing laminate paper, and recycling method of laminate paper

The laminated paper design with a pseudo-adhesive thermoplastic resin layer allows for solvent-free separation of the paper base material and resin layer, addressing recycling challenges by minimizing residue and enhancing recyclability.

JP2024136636APending Publication Date: 2024-10-04LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023047800
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing laminated papers with a thermoplastic resin layer face challenges in recycling due to the difficulty in separating the paper base material and the thermoplastic resin layer without using solvents, leading to increased processing steps and high residue of the paper base material in the resin layer, which hinders effective recycling.

Method used

The laminated paper design includes a thermoplastic resin layer with a pseudo-adhesive force of 150 mN/50 mm to 1500 mN/50 mm, allowing for easy separation from the paper base material without solvents, using a polyolefin resin with specific properties such as melt flow rate and density, and a manufacturing process that avoids adhesion-promoting treatments on the paper base material.

Benefits of technology

This design enables efficient separation of the paper base material and thermoplastic resin layer, reducing the residue to 6% by mass or less, facilitating effective recycling of both components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136636000001_ABST
    Figure 2024136636000001_ABST
Patent Text Reader

Abstract

To provide laminate paper which enables separation of a paper base material and a thermoplastic resin layer containing polyolefin without using a solvent, and suppresses an amount of the paper base material remaining in the thermoplastic resin layer.SOLUTION: Laminate paper 100 including a thermoplastic resin layer 30 includes a paper base material 10, and a thermoplastic resin layer 30 which is provided on at least one surface of the paper base material 10 and is pseudo-bonded to the paper base material 10, where the thermoplastic resin layer 30 contains a polyolefin resin, and pseudo-adhesive force when being peeled at an interface between the paper base material 10 and the thermoplastic resin layer 30 is 150 mN / 50 mm or more and 1,500 mN / 50 mm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to laminated paper, a method for manufacturing laminated paper, and a method for recycling laminated paper. [Background technology]

[0002] Laminated materials in which a thermoplastic resin and a different material are laminated are used in various applications. Laminated paper in which a thermoplastic resin is laminated on a paper base material is also used in various applications, and an example of the application of the laminated paper is release paper.

[0003] Patent Document 1 discloses a polyolefin laminated paper for release paper, which has a structure in which a polyolefin resin layer is formed by extrusion lamination on at least one surface of a paper substrate. The polyolefin laminated paper for release paper disclosed in Patent Document 1 has a multi-layered polyolefin resin layer, and among the polyolefin resin layers of the multi-layered structure, the layer made of the lowest density polyolefin resin is located on the paper substrate side. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-116718 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, interest in recycling has been increasing from the viewpoint of reducing the environmental impact associated with the treatment of plastic waste. It is also required to recover and recycle the paper base material and the thermoplastic resin layer of laminated paper having a thermoplastic resin layer. When recycling laminated paper, the thermoplastic resin layer and the paper base material are usually separated using a solvent such as water. When the thermoplastic resin layer and the paper base material are separated using a solvent, the number of processing steps is increased because a processing step such as immersing the laminated paper in the solvent for separation is required. In addition, when the thermoplastic resin layer and the paper base material are separated from the laminated paper and the separated paper base material and the thermoplastic resin layer are recovered, it is desirable that the amount of the paper base material remaining in the thermoplastic resin layer is small.

[0006] Laminated paper having a thermoplastic resin layer laminated on a paper substrate is usually required to have excellent adhesion between the paper substrate and the thermoplastic resin. For example, the polyolefin laminated paper for release paper described in Patent Document 1 is said to be able to suppress or prevent peeling between the paper substrate and the polyolefin resin layer even when heat treatment is performed. Thus, the polyolefin laminated paper for release paper described in Patent Document 1 is a technology for preventing heat-resistant peeling, so separation between the paper substrate and the polyolefin resin layer is not considered. In addition, since the polyolefin laminated paper for release paper described in Patent Document 1 has excellent adhesion between the paper substrate and the polyolefin resin layer, even when separation between the paper substrate and the polyolefin resin layer is attempted in the polyolefin laminated paper for release paper described in Patent Document 1, a large amount of the paper substrate remains in the thermoplastic resin layer. For this reason, it has been difficult to separate the polyolefin resin layer from the polyolefin laminated paper for release paper and recycle the separated polyolefin resin layer.

[0007] The object of the present invention is to provide a laminated paper in which the paper base material and the thermoplastic resin layer containing polyolefin can be separated without using a solvent, and in which the amount of the paper base material remaining in the thermoplastic resin layer is reduced, a method for producing the laminated paper, and a method for recycling the laminated paper. [Means for solving the problem]

[0008] [1] A laminated paper having a thermoplastic resin layer, A paper substrate; A thermoplastic resin layer provided on at least one surface of the paper base material and pseudo-adhered to the paper base material; Equipped with the thermoplastic resin layer contains a polyolefin resin, The pseudo-adhesion strength when peeled off at the interface between the paper base material and the thermoplastic resin layer is 150 mN / 50 mm or more and 1500 mN / 50 mm or less; Laminated paper.

[0009] [2] [1] The laminated paper according to the present invention, The thickness of the thermoplastic resin layer is 13 μm or more. Laminated paper.

[0010] [3] In the laminated paper according to [1] or [2], The polyolefin resin has at least one of a structural unit derived from ethylene and a structural unit derived from propylene. Laminated paper.

[0011] [4] In the laminated paper according to any one of [1] to [3], The melt flow rate of the polyolefin resin is 3 g / 10 min or more and 45 g / 10 min or less. Laminated paper.

[0012] [5] In the laminated paper according to any one of [1] to [4], The polyolefin resin is an unmodified polyolefin resin that is not acid-modified. Laminated paper.

[0013] [6] [1] to [5], the laminated paper according to any one of the above, A release paper or a wrapping paper. Laminated paper.

[0014] [7] A method for producing the laminated paper according to any one of [1] to [6], Providing the paper substrate; preparing the polyolefin resin; A step of melt-extruding the polyolefin resin melted at a temperature of 230° C. or more and 320° C. or less onto the paper base material without subjecting the paper base material to an easy-adhesion treatment; having How laminated paper is manufactured.

[0015] [8] A method for recycling the laminated paper according to any one of [1] to [6], Separating the laminated paper into the paper base material and the thermoplastic resin layer without using a solvent; A step of recovering the separated paper base material and the separated thermoplastic resin layer, respectively; having In the step of separating the paper base material from the thermoplastic resin layer, when the paper base material and the thermoplastic resin layer are separated, the amount of residue adhering to the thermoplastic resin layer is represented by the following formula (Mathematical Formula 1): The amount of the residue is 6% by mass or less based on the total mass of the paper base material. How to recycle laminated paper. R=[{TP W -((TP T / 10 4 )×TP ρ ×L S )} / {L W -((TP T / 10 4 )×TP ρ ×L S )}]×100 (number 1) (In the above formula (Math. 1), R is the amount of residue (unit: mass %), TP W is the mass of the thermoplastic resin layer after separation (unit: g), TP T is the thickness of the thermoplastic resin layer (unit: μm), TP ρ is the density of the thermoplastic resin layer (unit: g / cm 3 ), L S is the area of ​​the thermoplastic resin layer in the laminated paper before separation (unit: cm 2 ), L W indicates the mass of the laminated paper before separation (unit: g). Effect of the Invention

[0016] According to one aspect of the present invention, it is possible to separate a paper base material from a thermoplastic resin layer containing a polyolefin without using a solvent, and it is possible to provide laminated paper in which the amount of paper base material remaining in the thermoplastic resin layer is reduced, a manufacturing method for the laminated paper, and a recycling method for the laminated paper. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic cross-sectional view showing an example of a laminate paper according to an embodiment of the present invention. [Diagram 2] 2 is a schematic diagram showing an example of a method for manufacturing laminated paper according to the present embodiment. FIG. [Diagram 3] FIG. 2 is a schematic diagram showing an example of a method for recycling laminated paper according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] [Laminated paper] The laminated paper according to the present embodiment includes a thermoplastic resin layer. The laminated paper according to the present embodiment includes a paper base material and a thermoplastic resin layer provided on at least one surface of the paper base material and pseudo-adhered to the paper base material, the thermoplastic resin layer including a polyolefin resin. The pseudo-adhesion strength when peeled off at the interface between the paper base material and the thermoplastic resin layer is 150 mN / 50 mm or more and 1500 mN / 50 mm or less.

[0019] The laminated paper according to the present embodiment has the above-mentioned configuration, and when using the laminated paper according to the present embodiment, the adhesiveness of the thermoplastic resin layer to the paper substrate is sufficient, but when the paper substrate and the thermoplastic resin layer are separated, the adhesiveness is moderate so that the two can be easily separated. Therefore, when the laminated paper according to the present embodiment is separated from the thermoplastic resin layer containing polyolefin, the paper substrate can be easily separated without using a solvent, and the amount of the paper substrate remaining in the thermoplastic resin layer is suppressed (for example, the amount of residue represented by the formula (Mathematical formula 1) is 6% by mass or less). Since the adhesiveness of the thermoplastic resin layer to the paper substrate is sufficient, the laminated paper according to the present embodiment can withstand use when applied to various applications (for example, applications such as release paper, wrapping paper, and label surface substrate).

[0020] In this specification, the above-mentioned solvent includes various liquids such as water, an aqueous solution containing water, a liquid having a high affinity for water, a mixture of water and a liquid having a high affinity for water, and a liquid having a low affinity for water.

[0021] The laminated paper according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are shown enlarged or reduced in size to facilitate explanation. Referring to Fig. 1, an example of the laminated paper according to the present embodiment is shown. Fig. 1 is a schematic cross-sectional view of the laminated paper 100.

[0022] The laminated paper 100 shown in FIG. 1 comprises a paper substrate 10 and a thermoplastic resin layer 30 containing a polyolefin resin provided on one surface (first substrate surface 11) of the paper substrate 10. The thermoplastic resin layer 30 is laminated directly on the paper substrate 10, and the thermoplastic resin layer 30 is pseudo-adhered to the paper substrate 10. The interface between the paper substrate 10 and the thermoplastic resin layer 30 is a pseudo-adhesive interface. Specifically, in the laminated paper 100, the contact surface between the first substrate surface 11 and the second thermoplastic resin layer surface 32 is the pseudo-adhesive interface. The pseudo-adhesive strength when peeled off at the interface between the paper substrate 10 and the thermoplastic resin layer 30 is in the range of 150 mN / 50 mm or more and 1500 mN / 50 mm or less. In the laminated paper 100, the thermoplastic resin layer 30 is not provided on the second paper substrate surface 12, which is the surface opposite to the first paper substrate surface 11 of the paper substrate 10, and the second paper substrate surface 12 is exposed. In addition, the first thermoplastic resin layer surface 31, which is the surface opposite to the second thermoplastic resin layer surface 32 of the thermoplastic resin layer 30, is also exposed.

[0023] Although an example of the laminated paper according to the present embodiment has been described above with reference to FIG. 1, the laminated paper according to the present embodiment is not limited thereto. The laminated paper according to the present embodiment may adopt various forms as long as it has the above-mentioned configuration. For example, the laminated paper 100 has a thermoplastic resin layer 30 provided on the first paper substrate surface 11 side of the paper substrate 10, but the thermoplastic resin layer 30 may be provided not only on the first paper substrate surface 11 side but also on the second paper substrate surface 12 side. When the thermoplastic resin layer 30 is provided on the second paper substrate surface 12 as well, it is preferable that the thermoplastic resin layer 30 provided on the second paper substrate surface 12 is in direct contact with the paper substrate 10 and is pseudo-adhered to the paper substrate 10. When a thermoplastic resin layer 30 is also provided on the second paper substrate surface 12, the thermoplastic resin layer 30, the paper substrate 10, and the thermoplastic resin layer 30 are laminated in this order in the thickness direction, and it is preferable that the interface between the thermoplastic resin layer 30 provided on the second paper substrate surface 12 side and the paper substrate 10 and the interface between the thermoplastic resin layer 30 provided on the first paper substrate surface 11 side and the paper substrate 10 are both pseudo-adhesive interfaces, and it is preferable that the pseudo-adhesive strength at each of these pseudo-adhesive interfaces is 150 mN / 50 mm or more and 1500 mN / 50 mm or less.

[0024] Furthermore, when the laminated paper 100 is used as a release paper, a release agent layer (not shown) may be provided on the first thermoplastic resin layer surface 31. The release agent layer preferably contains a silicone-based release agent. In addition, when the laminated paper 100 is used as wrapping paper, a decorative layer such as a printed layer (not shown) may be provided on at least one of the first thermoplastic resin layer surface 31 and the second paper base material surface 12, if necessary.

[0025] (Paper base material) The paper substrate is not particularly limited as long as it can support the thermoplastic resin layer, and examples of the paper substrate include kraft paper, fine paper, glassine paper, and coated paper (e.g., art paper, clay-coated paper, and cast-coated paper).

[0026] In this specification, the coated paper comprises a base paper mainly composed of pulp fibers and a pigment coating layer provided on the base paper. The base paper is obtained by adding the desired additives to, for example, pulp fibers as the main component, using a known method. The pigment coating layer is provided on the base paper by a known method. The pigment coating layer may have a single-layer structure or a multi-layer structure. The pigment coating layer contains, for example, an adhesive such as an aqueous resin in a range of 2 parts by mass or more and 50 parts by mass or less per 100 parts by mass of one or more pigments such as calcium carbonate, kaolin, clay, talc, satin white, titanium oxide, and plastic pigment. In this specification, the aqueous resin refers to a resin that can be dispersed in water or a resin that can be dissolved in water. The aqueous resin includes not only water-soluble resins, but also resins that can be dispersed in water, such as emulsion type and dispersion type.

[0027] The basis weight of the paper substrate is not particularly limited. The basis weight of the paper substrate is, for example, 50 g / m 2 It is preferable that the thickness is 60 g / m or more. 2 More preferably, it is equal to or greater than this. The basis weight of the paper base material is, for example, 200 g / m 2 It is preferable that the thickness is less than 150 g / m 2 It is more preferable that:

[0028] The thickness of the paper substrate is not particularly limited, but is preferably, for example, 50 μm or more, and more preferably 60 μm or more. The thickness of the paper base material is, for example, preferably 200 μm or less, and more preferably 150 μm or less.

[0029] (thermoplastic resin layer) The thermoplastic resin layer contains a polyolefin resin. The thermoplastic resin layer is preferably provided in direct contact with the paper substrate. The polyolefin resin is not particularly limited. For example, the polyolefin resin may be a polymer polymerized from a monomer containing an olefin monomer having 2 to 18 carbon atoms.

[0030] Examples of the polyolefin resin include homopolymers of olefin monomers such as ethylene, propylene, butene, hexene, octene, decene, and 4-methyl-1-pentene. Examples of the polyolefin resin include copolymers of olefin monomers selected from the group consisting of ethylene, propylene, butene, hexene, octene, decene, and 4-methylpentene. Examples of the copolymers of olefin monomers include copolymers of ethylene and α-olefins having 3 to 18 carbon atoms (for example, at least one olefin monomer selected from the group consisting of propylene, butene, hexene, octene, decene, and 4-methylpentene). The copolymers of olefin monomers may be a combination of two or more olefin monomers. The polyolefin resin may be a single resin or a combination of two or more resins. From the viewpoint of easy recycling, it is preferable that the polyolefin resin is a single resin.

[0031] Examples of polyolefin resins include copolymers of one or more olefin monomers such as ethylene, propylene, butene, hexene, octene, and 4-methyl-1-pentene with one or more monomers having a hydroxyl group, a carboxyl group, a vinyl acetate structure, an acid anhydride structure, or the like.

[0032] Specific examples of the polyolefin resin include at least one selected from the group consisting of polyethylene (low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, etc.), polypropylene, poly-1-butene, poly-2-butene, poly-1-hexene, poly-1-octene, poly(4-methyl-1-pentene), ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, and ethylene-(meth)acrylic acid ester copolymer.

[0033] Among these, the polyolefin resin is preferably a resin having at least one of a structural unit derived from ethylene and a structural unit derived from propylene. Specifically, the polyolefin resin is more preferably at least one selected from the group consisting of polyethylene, polypropylene, and an ethylene-vinyl acetate copolymer, and further preferably at least one selected from the group consisting of polyethylene and polypropylene. When polyethylene is used as the polyolefin resin, the polyolefin resin is preferably at least one of low-density polyethylene and medium-density polyethylene, and more preferably either low-density polyethylene or medium-density polyethylene.

[0034] The paper substrate and the thermoplastic resin layer can be separated without using a solvent, and from the viewpoint of easily suppressing the amount of the paper substrate remaining in the thermoplastic resin layer, the polyolefin resin is preferably an unmodified polyolefin resin, and more preferably an unmodified polyolefin resin that is not acid-modified. The unmodified polyolefin resin includes, for example, a polyolefin resin obtained by polymerizing a monomer containing an olefin monomer such as ethylene, propylene, butene, hexene, octene, and 4-methyl-1-pentene, in which functional groups such as one or more structures such as a hydroxyl group, a carboxyl group, a vinyl acetate structure, and an acid anhydride structure are not introduced. Specifically, for example, an acid-modified polymer obtained by polymerizing a monomer containing an olefin monomer and modifying it with an unsaturated carboxylic acid compound or an anhydride of an unsaturated carboxylic acid compound is a modified polyolefin resin, and is not an unmodified polyolefin resin that is not acid-modified.

[0035] The unmodified polyolefin resin is preferably at least one selected from the group consisting of unmodified polyethylene, unmodified polypropylene, and unmodified ethylene-vinyl acetate copolymer, and more preferably at least one selected from the group consisting of unmodified polyethylene and unmodified polypropylene.

[0036] The density of the polyolefin resin is not particularly limited and is, for example, 0.85 g / cm 3 More than 0.97g / cm 3 It is preferable that: When the polyolefin resin is polyethylene, for example, the density is 0.91 g / cm 3 More than 0.93g / cm 3 Low density polyethylene, with a density of less than 0.93 g / cm 3 More than 0.942g / cm 3 Medium density polyethylene with a density of less than 0.942 g / cm 3 More than 0.97g / cm 3 Any of the following high density polyethylenes may be used: When the polyolefin resin is polypropylene, for example, the density is 0.90 g / cm 3 More than 0.91g / cm 3 The following polypropylene is preferred: When the polyolefin resin is an ethylene-vinyl acetate copolymer, the resistance is 0.92 g / cm 3 More than 0.95g / cm 3 The following ethylene-vinyl acetate copolymers are preferred: The density of the polyolefin resin can be measured in accordance with JIS K7112:1999.

[0037] The melt flow rate (MFR) of the polyolefin resin is preferably 3 g / 10 min or more and 45 g / 10 min or less. The MFR of the polyolefin resin is more preferably 3.5 g / 10 min or more, further preferably 7 g / 10 min or more, and more preferably 42 g / 10 min or less.

[0038] The MFR of a polyolefin resin can be measured, for example, as follows. When the polyolefin resin is, for example, polyethylene, the MFR of the polyethylene represents the MFR at a temperature of 190° C. and a load of 2.16 kg. The MFR of the polyethylene can be measured in accordance with JIS K6922-1, JIS K6922-2:2018, and JIS K7210-1:2011. When the polyolefin resin is, for example, polypropylene, the MFR of the polypropylene represents the MFR at a temperature of 230° C. and a load of 2.16 kg. The MFR of the polypropylene can be measured in accordance with JIS K6921-1:2018, JIS K6921-2:2018, and JIS K7210-1:2011. When the polyolefin resin is, for example, an ethylene-vinyl acetate copolymer, the MFR of the ethylene-vinyl acetate copolymer represents the MFR at a temperature of 190° C. and a load of 2.16 kg. The MFR of the ethylene-vinyl acetate copolymer can be measured in accordance with JIS K6924-1:1997, JIS K6924-2:1997, and JIS K7210-1:2011.

[0039] The thickness of the thermoplastic resin layer is not particularly limited. From the viewpoint of ease of recovery of the thermoplastic resin layer, the thickness of the thermoplastic resin layer is preferably 13 μm or more. If the thickness of the thermoplastic resin layer is 13 μm or more, for example, it is easy to separate the paper base material and the thermoplastic resin layer from the roll-shaped laminated paper, and the separated thermoplastic resin layer is easy to recover as a roll-shaped thermoplastic resin layer. From the viewpoint of making the thermoplastic resin layer easier to recover, the thickness of the thermoplastic resin layer is more preferably 13 μm or more, and further preferably 18 μm or more. The upper limit of the thickness of the thermoplastic resin layer is not particularly limited, and the thickness of the thermoplastic resin layer may be, for example, 50 μm or less.

[0040] The content of the polyolefin resin in the thermoplastic resin layer is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 99 mass% or more, and even more preferably 100 mass%, based on the total amount of the thermoplastic resin layer. If the content of polyolefin resin in the thermoplastic resin layer is 100% by mass (that is, the thermoplastic resin layer is a layer consisting of only polyolefin resin), the thermoplastic resin layer containing polyolefin resin can be easily recycled.

[0041] The thermoplastic resin layer may contain additives, if necessary, in addition to the polyolefin resin. Examples of additives include antioxidants, lubricants, ultraviolet absorbers, colorants, and antiblocking agents. When the thermoplastic resin layer contains additives, the additives may be contained alone or in combination.

[0042] (pseudo adhesive strength) In the laminated paper according to this embodiment, the pseudo-adhesion strength when peeled at the interface between the paper base material and the thermoplastic resin layer is 150 mN / 50 mm or more and 1500 mN / 50 mm or less. If the pseudo-adhesion strength is in the range of 150 mN / 50 mm or more and 1500 mN / 50 mm or less, the paper substrate and the thermoplastic resin layer can be easily separated, and the amount of the paper substrate remaining in the thermoplastic resin layer can be easily reduced. In addition, if the pseudo-adhesion strength is 150 mN / 50 mm or more, a strength sufficient for use can be obtained. From the viewpoint of obtaining a strength that can withstand further use, the pseudo-adhesive strength is preferably 220 mN / 50 mm or more, and more preferably 250 mN / 50 mm or more. From the viewpoint of making it possible to more easily separate the paper substrate from the thermoplastic resin layer and making it easier to suppress the amount of the paper substrate remaining in the thermoplastic resin layer, the pseudo-adhesion strength is preferably 1300 mN / 50 mm or less, and more preferably 1000 mN / 50 mm or less. The pseudo-adhesion strength when peeled off at the interface between the paper substrate and the thermoplastic resin layer can be measured by the method described in the examples below.

[0043] (Uses of laminated paper) The use of the laminated paper according to the present embodiment is not particularly limited, and examples thereof include release paper and wrapping paper. When the laminated paper according to the present embodiment is used as a release paper or wrapping paper, the release paper or wrapping paper includes the laminated paper according to the present embodiment. The release paper can be used for general release sheet applications. The release paper can be used as a process paper used in a process of forming a sheet-like object on the release surface of the release agent layer of the release paper. Specifically, the release paper can be used as various process papers when producing various resin sheets, synthetic leather, or various composite materials.

[0044] When the laminated paper according to the present embodiment is applied as a release paper, the laminated paper according to the present embodiment itself may be applied as a release paper, or may be applied as a base material of the release paper. When the laminated paper according to the present embodiment is applied as a base material of the release paper, it is preferable to provide a release agent layer on the thermoplastic resin layer in the laminated paper according to the present embodiment. For example, the release agent layer may be laminated so as to be in direct contact with the thermoplastic resin layer in the laminated paper according to the present embodiment. For example, the release agent layer may be provided by providing an intermediate layer on the thermoplastic resin layer in the laminated paper according to the present embodiment, and the release agent layer may be laminated on the intermediate layer. Examples of the intermediate layer include an easy-adhesion layer such as a primer layer.

[0045] The release agent contained in the release agent layer is not particularly limited, and examples thereof include known release agents such as silicone resins, alkyd resins, acrylic resins, long-chain alkyl resins, unsaturated polyester resins, polyolefin resins, and waxes. Among these, from the viewpoint of release properties, the release agent is preferably a silicone-based release agent using a silicone resin. The silicone-based release agent is not particularly limited, and can be used in any form of solvent type, solventless type, or emulsion type.

[0046] The silicone resin used in the silicone-based release agent may be a silicone resin having a basic skeleton of dimethylpolysiloxane. Examples of the silicone resin include addition reaction type, condensation reaction type, ultraviolet curing type, and electron beam curing type. When an addition reaction type silicone resin is used as the release agent, it is preferable to use a crosslinking agent and a catalyst in combination. Examples of the crosslinking agent include organopolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule. Examples of the catalyst include platinum metal compounds such as platinum group metals, palladium, and rhodium.

[0047] When the laminated paper according to the present embodiment is used as a release paper, it can be obtained by a manufacturing method including a step of applying a coating solution of a release agent composition to at least one surface of the laminated paper according to the present embodiment to form a coating film, and a step of curing the obtained coating film to form a release agent layer. As a method for applying the release agent composition, for example, a coating method such as a gravure coating method, a bar coating method, a knife coating method, a roll coating method, and a die coating method can be used. As a drying condition for the coating film, a condition under which the coating film can be dried can be used.

[0048] When the silicone-based release agent is a solvent-based release agent, a coating liquid is prepared by mixing an organic solvent such as toluene, ethyl acetate, methyl ethyl ketone, hexane, or heptane with a release agent composition containing the solvent-based silicone-based release agent, and the coating liquid is applied onto the thermoplastic resin layer of the laminated paper according to this embodiment by a known coating method, followed by drying and heating.

[0049] The release agent composition containing the release agent may contain various additives, such as an antioxidant, an ultraviolet absorber, an inorganic or organic filler, an antistatic agent, and a surfactant, as necessary.

[0050] In general, conventionally used normal laminated paper is manufactured so as to have excellent adhesion between the paper base material and the thermoplastic resin layer, and it is assumed that the paper base material and the thermoplastic resin layer do not peel off. For this reason, when normal laminated paper is applied to the use of release paper, for example, separation of the paper base material and the thermoplastic resin layer from normal laminated paper that becomes waste such as used paper is not considered. In addition, even when the paper base material and the thermoplastic resin layer are separated from the normal laminated paper, for example, when the paper base material and the thermoplastic resin layer are separated, destruction (so-called paper layer destruction) occurs in the paper base material, and the amount of the paper base material remaining in the thermoplastic resin layer increases. For this reason, in normal laminated paper, even if separation of the paper base material and the thermoplastic resin layer and recovery and recycling of the separated paper base material are considered, recovery and recycling of the separated thermoplastic resin layer are not considered.

[0051] In contrast, in the laminated paper according to the present embodiment, since the thermoplastic resin layer is pseudo-adhered to the paper substrate, even when the paper substrate and the thermoplastic resin layer are separated, the amount of the paper substrate remaining in the thermoplastic resin layer is suppressed (for example, the amount of residue described below is 6% by mass or less). Therefore, even if the laminated paper according to the present embodiment is discarded after being used as a release paper, the thermoplastic resin layer separated from the laminated paper can be recovered and recycled.

[0052] When the laminated paper according to the present embodiment is used as a wrapping paper, for example, the laminated paper according to the present embodiment itself may be used as a wrapping paper, or a decorative layer such as a printed layer may be provided on at least one of the surface of the paper substrate opposite the thermoplastic resin layer side (second paper substrate surface) and the surface of the thermoplastic resin layer opposite the paper substrate side (first thermoplastic resin layer surface) in the laminated paper according to the present embodiment. By providing a printed layer as a decorative layer, information regarding the contents of the packaged item and other information can be displayed by printing on the laminated paper.

[0053] In addition, even when the laminated paper of this embodiment is applied to applications in which adhesion between a paper base material and a thermoplastic resin layer is required without peeling the paper base material from the thermoplastic resin layer, not limited to applications as release paper and wrapping paper, the laminated paper of this embodiment has the advantage over conventionally used ordinary laminated paper that the thermoplastic resin layer separated from the laminated paper can be recovered and recycled.

[0054] (Laminated paper manufacturing method) An example of a preferred method for producing the laminated paper according to the present embodiment is the following production method: A preferred method for producing the laminated paper according to the present embodiment includes the steps of preparing a paper base material, preparing the polyolefin resin, and melt-extruding the polyolefin resin molten at a temperature of 230° C. or higher and 320° C. or lower onto the paper base material without subjecting the paper base material to an easy-adhesion treatment.

[0055] The paper base material may be prepared by the above-described paper base material. The paper base material may be obtained by a known manufacturing method.

[0056] In the step of preparing the polyolefin resin, the polyolefin resin described above in relation to the thermoplastic resin layer may be prepared. The polyolefin resin may be obtained by a known manufacturing method.

[0057] In the process of melt-extruding the polyolefin resin, the surface of the paper substrate is not subjected to an easy-adhesion treatment such as corona treatment, plasma treatment, or flame treatment. By not subjecting the surface of the paper substrate to an easy-adhesion treatment, pseudo-adhesion between the paper substrate and the thermoplastic resin layer is easily obtained, and the paper substrate and the thermoplastic resin layer are easily separated. The method of melt-extruding the molten polyolefin resin onto the paper substrate that is not subjected to the easy-adhesion treatment is not particularly limited, and for example, a method using a T-die can be mentioned.

[0058] In the process of melt-extruding a polyolefin resin, the temperature of the molten polyolefin resin is the extrusion resin temperature when the polyolefin resin is melted and extruded. That is, the temperature of the polyolefin when the molten polyolefin resin is melt-extruded onto a paper substrate is 230° C. or higher and 320° C. or lower. The temperature when the polyolefin resin is melted and extruded (extrusion resin temperature) is the temperature of the thermoplastic resin when it is extruded from the die, and can be measured as the temperature of the polyolefin resin in the die of the extruder. The temperature at which the polyolefin resin is melted and extruded is preferably 240° C. or higher, and more preferably 250° C. or higher. The temperature at which the polyolefin resin is melted and extruded is preferably 310° C. or lower, and more preferably 300° C. or lower.

[0059] The step of melt-extruding the polyolefin resin also includes a step of cooling the melt-extruded polyolefin resin (cooling step). In the cooling step, the heated and melted polyolefin resin is brought into contact with a cooling means such as a cooling roll to form a thermoplastic resin layer containing the polyolefin resin. The cooling roll has a cylindrical body with a metal outer circumferential surface. The cooling roll has a cooling function by passing cooling water or the like through the inside of the cylindrical body. When a cooling roll is used as the cooling means, the polyolefin resin melt-extruded onto the paper substrate may be cooled by directly contacting the outer circumferential surface of the cooling roll, or the paper substrate may be directly contacted with the outer circumferential surface of the cooling roll to indirectly cool the polyolefin resin. In addition, in the cooling step, the melt-extruded polyolefin resin may be cooled by air cooling.

[0060] The cooling temperature of the polyolefin resin is preferably 15° C. or higher and 40° C. or lower, and more preferably 20° C. or higher and 35° C. or lower. When a cooling roll is used as the cooling means, the cooling temperature is the temperature of cooling water passed through the cooling roll. When the polyolefin resin is cooled by air cooling, the cooling temperature is the temperature of the atmosphere in which the melt-extruded polyolefin resin is placed, and when temperature-controlled air is forcibly blown onto the polyolefin resin, the cooling temperature is the temperature of that air.

[0061] When a cooling roll is used as the cooling means, the time (cooling time) during which the molten polyolefin resin is directly or indirectly brought into contact with the outer peripheral surface of the cooling roll can be controlled by the speed at which the laminated paper in which the paper substrate and the polyolefin resin are laminated is conveyed. The conveying speed is, for example, preferably 40 m / min or more and 180 m / min or less, and more preferably 50 m / min or more and 160 m / min or less.

[0062] Through the above steps, the laminated paper according to this embodiment can be obtained.

[0063] Here, an example of a manufacturing method of laminated paper according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are illustrated enlarged or reduced in size to facilitate explanation. Referring to Fig. 2, Fig. 2 shows a schematic diagram of a main part of a process in which a laminating device 200 is used to melt-extrude a molten polyolefin resin onto a paper substrate 10 unwound from a roll-shaped paper substrate 10A, thereby providing a thermoplastic resin layer 30 on the paper substrate 10.

[0064] The laminating apparatus 200 includes an extruder 202 equipped with a T-die 204, a cooling roll 208, a touch roll 206 adjacent to the cooling roll 208 at an interval, a payout roll 210, and a take-up roll 212. The roll-shaped paper base material 10A is wound up so that the surface on which the thermoplastic resin layer 30 is to be provided faces the core, and the opposite surface faces the outer circumferential surface.

[0065] The paper substrate 10 is unwound from the roll-shaped paper substrate 10A by the unwinding roll 210. The unwound paper substrate 10 passes through a guide roll (not shown) and reaches the gap between the cooling roll 208 and the touch roll 206. The paper substrate 10 that reaches the gap between the cooling roll 208 and the touch roll 206 is not subjected to an easy-adhesion treatment such as corona treatment. After the paper substrate 10 reaches the gap between the cooling roll 208 and the touch roll 206, the molten polyolefin resin is extruded in a film shape from the T-die 204 toward the paper substrate 10. The temperature of the polyolefin when extruded from the T-die 204 is 230°C or higher and 320°C or lower. The extruded thermoplastic resin comes into contact with the paper substrate 10, and the thermoplastic resin supplied in a film shape is pressure-bonded onto the paper substrate 10 in the gap between the cooling roll 208 and the touch roll 206. As a result, a laminated paper 100 is formed in which the thermoplastic resin layer 30 is laminated on the paper substrate 10. In the laminated paper 100, the thermoplastic resin layer 30 is pseudo-adhered to the paper substrate 10. The pseudo-adhesion strength when the paper substrate 10 and the thermoplastic resin layer 30 are peeled off at the interface between them is 150 mN / 50 mm or more and 1500 mN / 50 mm or less. The laminated paper 100, in which the thermoplastic resin layer 30 is laminated on the paper substrate 10, passes through a guide roll (not shown) and is wound up by a winding roll 212 to form a roll-shaped laminated paper 100A. The roll-shaped laminated paper 100A is wound up so that the paper substrate 10 is on the core side and the thermoplastic resin layer 30 is on the outer peripheral surface side.

[0066] The cooling temperature by the cooling roll 208 is preferably within the range of the cooling temperature of the polyolefin resin described above. The winding speed of the laminate paper 100 is preferably within the range of the speed at which the laminate paper is transported described above. The gap between the cooling roll 208 and the touch roll 206 can be adjusted, for example, so that the thermoplastic resin layer 30 has a predetermined thickness.

[0067] Although an example of the manufacturing method of the laminated paper according to the present embodiment has been described above with reference to FIG. 2, the manufacturing method of the laminated paper according to the present embodiment is not limited thereto. For example, the roll-shaped paper base material 10A may be wound up so that the surface on which the thermoplastic resin layer 30 is to be provided is the outer peripheral surface side and the opposite surface is the core side. The roll-shaped laminated paper 100A may be wound up so that the paper base material 10 is the outer peripheral surface side and the thermoplastic resin layer 30 is the core side. The manufacturing method of the laminated paper according to the present embodiment may adopt various forms as long as the thermoplastic resin layer 30 can be pseudo-adhered to the paper base material 10 and the thermoplastic resin layer 30 can be laminated on the paper base material 10 so that the pseudo-adhesion force when peeled off at the interface between the paper base material 10 and the thermoplastic resin layer 30 is within the above-mentioned specific range.

[0068] (How to recycle laminated paper) An example of a preferred method for recycling the laminated paper according to this embodiment is the following method. A preferred method for recycling the laminated paper according to this embodiment includes a step of separating the laminated paper according to this embodiment into the paper base material and the thermoplastic resin layer without using a solvent, and a step of recovering the separated paper base material and the thermoplastic resin layer, respectively. In the step of separating the paper base material and the thermoplastic resin layer, when the paper base material and the thermoplastic resin layer are separated, the amount of residue adhering to the thermoplastic resin layer is 6 mass% or less with respect to the total mass of the paper base material. The amount of residue is expressed by the following mathematical formula (Mathematical Formula 1).

[0069] R=[{TP W -((TP T / 10 4 )×TP ρ ×L S )} / {L W -((TP T / 10 4 )×TP ρ ×L S )}]×100 (number 1) (In the above formula (Math. 1), R is the amount of residue (unit: mass %), TP Wis the mass of the thermoplastic resin layer after separation (unit: g), TP T is the thickness of the thermoplastic resin layer (unit: μm), TP ρ is the density of the thermoplastic resin layer (unit: g / cm 3 ), L S is the area of ​​the thermoplastic resin layer in the laminated paper before separation (unit: cm 2 ), L W indicates the mass of the laminated paper before separation (unit: g).

[0070] In the above formula (Mathematical formula 1), when the thermoplastic resin layer is a single layer of polyolefin resin, the density may be measured in accordance with JIS K7112: 1999. When different types of polyolefin resins are laminated, the density may be measured in accordance with JIS K7112: 1999 and the average value of the densities may be used.

[0071] A preferred method for recycling the laminated paper according to the present embodiment also includes a step of preparing the laminated paper according to the present embodiment. The laminated paper can be obtained, for example, by the preferred manufacturing method of the laminated paper described above. The laminated paper to be prepared can be a waste laminated paper. Specifically, an example of the laminated paper to be prepared is (1) a form of used laminated paper, (2) another example is a form of laminated paper that is a product loss when manufacturing the laminated paper according to the present embodiment, and (3) another example is a form of a stock disposal item of the laminated paper according to the present embodiment. The laminated paper to be prepared can be a long laminated paper wound in a roll, a long laminated paper folded, or a sheet-like laminated paper cut to a predetermined size.

[0072] In the process of separating the laminated paper, the paper substrate and the thermoplastic resin layer are separated without using a solvent. In the laminated paper according to the present embodiment, the paper substrate and the thermoplastic resin layer are pseudo-adhered to each other, so that the adhesion between the paper substrate and the thermoplastic resin layer is sufficient during use. On the other hand, when the laminated paper according to the present embodiment is separated into the paper substrate and the thermoplastic resin layer, the paper substrate and the thermoplastic resin layer can be easily peeled off, and a physical separation process can be performed without a chemical separation process. For example, when the laminated paper according to the present embodiment becomes waste, the laminated paper according to the present embodiment can be separated into the paper substrate and the thermoplastic resin layer by hand or machine.

[0073] In the process of separating the laminated paper, when the paper base material and the thermoplastic resin layer are separated, the amount of residue adhering to the thermoplastic resin layer is 6% by mass or less relative to the total mass of the paper base material. The amount of residue is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0 (zero) mass%. The amount of residue is preferably 0% by mass or more and 6% by mass or less. The amount of residue is expressed by the above-mentioned mathematical formula (Mathematical Formula 1).

[0074] The breaking strength of the thermoplastic resin layer separated in the process of separating the laminated paper is preferably 2.0 MPa or more. If the breaking strength is 2.0 MPa or more, the paper base material and the thermoplastic resin layer are separated from the rolled laminated paper, and the rolled paper base material and the rolled thermoplastic resin layer can be easily recovered. The upper limit of the breaking strength of the thermoplastic resin layer separated in the process of separating the laminate paper is not particularly limited, and may be, for example, 20 MPa or less.

[0075] In the process of recovering the separated paper base material and the thermoplastic resin layer, the paper base material and the thermoplastic resin layer separated in the process of separating the laminated paper are recovered. For example, when the paper base material and the thermoplastic resin layer are separated from the rolled laminated paper, the paper base material and the thermoplastic resin layer can be recovered as the rolled paper base material and the rolled thermoplastic resin layer, respectively. When the paper base material and the thermoplastic resin layer are separated from the folded laminated paper that is not in a roll shape, they can also be recovered as the rolled paper base material and the rolled thermoplastic resin layer, respectively. In addition, for example, when the paper base material and the thermoplastic resin layer are separated from the sheet-shaped laminated paper, the paper base material and the thermoplastic resin layer can be recovered as the sheet-shaped paper base material and the sheet-shaped thermoplastic resin layer, respectively. Both the recovered paper base material and the thermoplastic resin layer can be recycled. In particular, the amount of residual paper base material remaining in the thermoplastic resin layer separated from the laminated paper according to this embodiment is suppressed to 6% by mass or less, so that the recovered thermoplastic resin layer is easy to recycle.

[0076] An example of a method for recovering laminated paper according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are illustrated enlarged or reduced to facilitate explanation. Referring to FIG. 3, FIG. 3 shows a schematic diagram of a main part of a process in which a laminated paper separation device 300 is used to separate a paper base material 10 and a thermoplastic resin layer 30 from a rolled laminated paper 100B, and the paper base material 10B and the thermoplastic resin layer 30B are recovered, respectively.

[0077] The separation device 300 includes a payout roll 310, a take-up roll 301 for taking up the separated paper substrate 10, and a take-up roll 303 for taking up the separated thermoplastic resin layer 30. The roll-shaped laminated paper 100B is a laminated paper that has come to be discarded, and is waste of the laminated paper. The roll-shaped laminated paper 100B is taken up so that the thermoplastic resin layer 30 is on the core side and the paper substrate 10 is on the outer peripheral surface side. When the paper substrate 10 and the thermoplastic resin layer 30 are separated from the roll-shaped laminated paper 100B, the thermoplastic resin layer 30 passes through a guide roll (not shown) and is taken up by the take-up roll 303 for taking up the thermoplastic resin layer 30, and the paper substrate 10 passes through a guide roll (not shown) and is taken up by the take-up roll 301 for taking up the paper substrate 10. The rolled thermoplastic resin layer 30B and the rolled paper base material 10B are each collected. The collected rolled thermoplastic resin layer 30B and the rolled paper base material 10B are each recycled.

[0078] An example of the method for recovering laminated paper according to the present embodiment has been described above with reference to FIG. 3, but the method for recovering laminated paper according to the present embodiment is not limited thereto. The laminated paper 100B is wound up so that the thermoplastic resin layer 30 is on the core side and the paper base material 10 is on the outer peripheral surface side, but the present invention is not limited thereto, and the paper base material 10 may be wound up so that the thermoplastic resin layer 30 is on the outer peripheral surface side. Also, with reference to FIG. 3, an example of the method for recovering laminated paper according to the present embodiment has been described using a roll-shaped laminated paper 100B as an example, but the present invention is not limited thereto. For example, the paper base material and the thermoplastic resin layer may be separated from the folded long laminated paper using a separation device capable of separating the paper base material and the thermoplastic resin layer. For example, the paper base material and the thermoplastic resin layer may be separated from the sheet-shaped laminated paper using a separation device capable of separating the paper base material and the thermoplastic resin layer. The separation of the paper base material and the thermoplastic resin layer may be performed, for example, by machine, by hand, or by a combination of both. The method for recovering laminated paper according to the present embodiment may adopt various forms as long as the paper base material and the thermoplastic resin layer can be separated without using a solvent.

[0079] The present invention is not limited to the above-described embodiment, and may include modifications and improvements within the scope of the present invention. EXAMPLES

[0080] Examples will be described below, but the present invention is not limited to these examples in any way.

[0081] The following raw materials were prepared as raw materials for producing the laminated paper of each Example and Comparative Example.

[0082] (Paper base material) "P-1": High-quality paper (manufactured by Nippon Paper Industries Co., Ltd., "WM Seal 64.0G", basis weight 64g / m 2 ) "P-2": Glassine paper (glassine made by Lintec Corporation, basis weight 73g / m 2 )

[0083] (thermoplastic resin layer) "PE-1": Low-density polyethylene (manufactured by Japan Polyethylene Co., Ltd., "LC8001", MFR: 20g / 10min, density: 0.917g / cm 3 ) "PE-2": Low-density polyethylene (manufactured by Sumitomo Chemical Co., Ltd., "L405", MFR: 3.7 g / 10 min, density: 0.924 g / cm 3 ) "PE-3": Low-density polyethylene (manufactured by Japan Polyethylene Co., Ltd., "LC605Y", MFR: 7.3 g / 10 min, density: 0.918 g / cm 3 ) "PE-4": Low-density polyethylene (manufactured by Japan Polyethylene Co., Ltd., "LC621", MFR: 5.5 g / 10 min, density: 0.923 g / cm 3 ) "PE-5": Medium density polyethylene (manufactured by Sumitomo Chemical Co., Ltd., "L5721", MFR: 7.5 g / 10 min, density: 0.937 g / cm 3 ) "PP-1": Polypropylene (manufactured by SunAllomer Co., Ltd., "PHA03A", MFR: 42g / 10min, density: 0.90g / cm 3 ) "PP-2": Polypropylene (manufactured by Japan Polypropylene Corporation, "OX0167", MFR: 15g / 10min, density: 0.910g / cm 3 ) "EVA-1": Ethylene-vinyl acetate copolymer (manufactured by Tosoh Corporation, "Ultrathene 537", MFR: 8.5 g / 10 min, density: 0.925 g / cm 3 )

[0084] <Example 1> Polyethylene (PE-1) was heated and melted as a polyolefin resin, and the melted polyethylene was extruded from a T-die at an extrusion resin temperature of 280° C. to form a thermoplastic resin layer having a thickness of 25 μm on one side of a paper substrate (P-1: wood-free paper). In this way, the laminated paper of Example 1 was obtained, which had a thermoplastic resin layer laminated directly in contact with the paper substrate. The thickness of the thermoplastic resin layer was controlled by adjusting the back pressure of the extruder screw. Cooling water adjusted to 23°C was passed through a water-cooled roll, and the thermoplastic resin layer on the substrate was brought into contact with the surface of the water-cooled roll, thereby cooling and solidifying the molten thermoplastic resin layer. The conveying speed of the paper substrate (P-1) when laminating the polyethylene (PE-1) was 150 m / min.

[0085] <Examples 2 to 6> The laminated paper of each example was obtained in the same manner as in Example 1, except that at least one of the conditions of the type of paper base material, the type of polyolefin resin forming the thermoplastic resin layer, the thickness of the thermoplastic resin, and the extrusion resin temperature was changed according to Table 1.

[0086] <Comparative Example 1> The laminated paper of Comparative Example 1 was obtained in the same manner as in Example 1, except that the type of polyolefin resin forming the thermoplastic resin layer, the thickness of the thermoplastic resin layer, and the extrusion resin temperature conditions were changed according to Table 1.

[0087] <Comparative Examples 2 to 7> For Comparative Examples 2 to 5, the type of polyolefin resin forming the thermoplastic resin layer, the thickness of the thermoplastic resin layer, and the extrusion resin temperature conditions were changed according to Table 1, and further, before the molten thermoplastic resin was extruded onto one side of the paper substrate, a corona treatment was performed on the side of the paper substrate on which the thermoplastic resin layer was to be formed. Except for this, the laminated papers of each Comparative Example were obtained in the same manner as in Example 1. For Comparative Examples 6 and 7, the laminated papers of each Comparative Example were obtained in the same manner as in Example 1, except for the change in the extrusion resin temperature conditions.

[0088] <Evaluation of pseudo-adhesive strength> The pseudo-adhesive strength was measured according to the 180° peel adhesion test specified in JIS Z0237:2009. Specifically, the thermoplastic resin layer side of the laminated paper prepared in each example was first fixed to a stainless steel plate using double-sided tape. Then, the paper substrate of the laminated paper was peeled off from the thermoplastic resin layer under the following conditions: peel speed: 300 mm / min, peel angle: 180°. The magnitude of the force (peeling force) required for this peeling was measured, and the measured peeling force was taken as the pseudo-adhesive strength (unit: mN / 50 mm). In addition, when the pseudo-adhesive strength could not be measured due to the occurrence of paper layer destruction between the paper base material and the thermoplastic resin layer, it was indicated as F.

[0089] <Breaking strength of thermoplastic resin layer> The laminated paper prepared in each example was cut into a test piece with a length of 150 mm (MD direction) and a width of 15 mm (TD direction). The paper base material and the thermoplastic resin layer were separated from the test piece, and the separated thermoplastic resin was clamped with the chuck of a universal testing machine (Shimadzu Corporation, Autograph AG-IS 500N) and the breaking strength (unit: MPa) in the MD direction of the thermoplastic resin layer was measured in accordance with JIS K7127:1999 under the conditions of a chuck distance of 100 mm and a tensile speed of 200 mm / min. When the residue adhering to the thermoplastic resin layer exceeded 6% by mass, it was not suitable as the breaking strength of the separated thermoplastic resin, and therefore was not measurable (indicated as F in Table 2).

[0090] <Residue amount evaluation> The laminated paper obtained in each example was cut to a size of 100 mm x 100 mm to prepare a sample for evaluating the amount of residue on the paper substrate. The weight of the sample for evaluating the amount of residue was measured. The sample for evaluating the amount of residue was then peeled off by hand, and the weight of the thermoplastic resin layer was measured. The mass of the sample for evaluating the amount of residue measured before peeling off by hand (L in Equation (1)) was W (corresponding to TP in Equation 1) and the mass of the thermoplastic resin layer measured after peeling it off by hand. W From the above-mentioned formula (equation 1), the amount of residue adhered to the thermoplastic resin layer was calculated. TP in formula (1) ρ The value to be substituted is the density of the polyolefin resin used in the thermoplastic resin layer. T As the value to be substituted for, the thickness of the thermoplastic resin layer after separation from the sample for evaluating the amount of residue was measured. Also, TP in formula (1) T The thickness of the thermoplastic resin layer after separation from the sample for evaluating the amount of residue was measured as a value to be substituted for . The thickness of the thermoplastic resin layer was measured at a total of five locations, near the four corners and one location near the center of the thermoplastic resin layer, avoiding the area where the residue was present, and the average value was used. When there was a large amount of residue adhering to the thermoplastic resin layer, the thickness of the thermoplastic resin layer formed by extrusion from the above-mentioned T-die was used as the thickness of the thermoplastic resin layer. The amount of residue was evaluated according to the following evaluation criteria.

[0091] (Evaluation Criteria) "5": Residue amount is 6% by mass or less. "4": Residue amount is more than 6% by mass and less than 30% by mass. "3": Residue amount is more than 30% by mass and 50% by mass or less. "2": Residue amount is more than 50% by mass and 70% by mass or less. "1": Residue amount is more than 70% by mass and 99% by mass or less.

[0092] <Release agent hardening evaluation> (Preparation of release paper) A release agent composition containing a silicone-based release agent (KS-847, manufactured by Shin-Etsu Chemical Co., Ltd.) was applied to the surface of the thermoplastic resin layer of the laminated paper obtained in each example using an applicator so that the silicone-based release agent was applied in an amount of 0.5 g / m2 after drying. 2 and drying to provide a release agent layer, thereby preparing a release paper. (Evaluation of hardening of release agent layer) For the release paper prepared above, the surface of the release agent layer was rubbed with a finger 10 times, and the presence or absence of cloudiness (smear) and peeling off of the release agent layer (rub-off) was visually confirmed, and the hardening property of the release agent layer was evaluated according to the following criteria. "A": Neither smear nor rub-off was observed. "F": At least one of smear and rub-off was observed.

[0093] <Evaluation of lifting and peeling> The laminated paper obtained in each example was cut to a size of 300 mm x 300 mm. The cut laminated paper was then subjected to a punching process (a circular shape with an inner diameter of 30 mm). The laminated paper after cutting and punching was visually inspected for the presence or absence of lifting or peeling between the paper base material and the thermoplastic resin, and was evaluated according to the following criteria. "A": No lifting or peeling was observed after cutting or punching. "F": Lifting and peeling were observed at least either after cutting or after punching.

[0094] [Table 1]

[0095] [Table 2]

[0096] In each example, pseudo-adhesion was obtained, and therefore the paper substrate and the thermoplastic resin layer could be peeled off by hand at the interface between the paper substrate and the thermoplastic resin layer. On the other hand, the paper base material and the thermoplastic resin layer were firmly bonded to each other in Comparative Examples 1 to 5. Therefore, when the paper base material and the thermoplastic resin layer were peeled off by hand, a large amount of the paper base material remained on the thermoplastic resin layer. Therefore, each Example was evaluated to have a better amount of residue than Comparative Examples 1 to 5, and it is understood that both the paper base material and the thermoplastic resin layer are recyclable. On the other hand, in Comparative Example 6, the pseudo-adhesion was too weak, and the evaluation results for lifting and peeling were F, making it unsuitable for use. In Comparative Example 7, although the pseudo-adhesion could be measured, the pseudo-adhesion was too strong, with the amount of paper base remaining on the thermoplastic resin layer exceeding 6% by mass, resulting in a large amount of residue. From the above results, it can be seen that the laminated paper of this embodiment is capable of separating the paper base material from the thermoplastic resin layer containing polyolefin without using a solvent, and the amount of paper base material remaining in the thermoplastic resin layer is suppressed. [Explanation of symbols]

[0097] 10, 10A, 10B...paper substrate, 11...first paper substrate surface, 12...second paper substrate surface, 30, 30A, 30B...thermoplastic resin layer, 31...first thermoplastic resin layer surface, 32...second thermoplastic resin layer surface, 100, 100A, 100B...laminated paper, 200...laminating device, 202...extruder, 204...T-die, 206...touch roll, 208...cooling roll, 210, 310...delivery roll, 212, 301, 303...winding roll, 300...separation device.

Claims

1. A laminated paper having a thermoplastic resin layer, A paper substrate; A thermoplastic resin layer provided on at least one surface of the paper base material and pseudo-adhered to the paper base material; Equipped with the thermoplastic resin layer contains a polyolefin resin, The pseudo-adhesion strength when peeled off at the interface between the paper base material and the thermoplastic resin layer is 150 mN / 50 mm or more and 1500 mN / 50 mm or less. Laminated paper.

2. The laminated paper according to claim 1, The thickness of the thermoplastic resin layer is 13 μm or more. Laminated paper.

3. The laminated paper according to claim 1 or 2, The polyolefin resin has at least one of a structural unit derived from ethylene and a structural unit derived from propylene. Laminated paper.

4. The laminated paper according to claim 1 or 2, The melt flow rate of the polyolefin resin is 3 g / 10 min or more and 45 g / 10 min or less. Laminated paper.

5. The laminated paper according to claim 1 or 2, The polyolefin resin is an unmodified polyolefin resin that is not acid-modified. Laminated paper.

6. The laminated paper according to claim 1 or 2, A release paper or a wrapping paper. Laminated paper.

7. A method for producing the laminated paper according to claim 1 or 2, comprising the steps of: Providing the paper substrate; preparing the polyolefin resin; A step of melt-extruding the polyolefin resin molten at a temperature of 230° C. or more and 320° C. or less onto the paper base material without subjecting the paper base material to an easy-adhesion treatment; having How laminated paper is manufactured.

8. A method for recycling the laminated paper according to claim 1 or 2, comprising: Separating the laminated paper into the paper base material and the thermoplastic resin layer without using a solvent; A step of recovering the separated paper base material and the separated thermoplastic resin layer, respectively; having In the step of separating the paper base material from the thermoplastic resin layer, when the paper base material and the thermoplastic resin layer are separated, the amount of residue adhering to the thermoplastic resin layer is represented by the following formula (Mathematical Formula 1): The amount of the residue is 6% by mass or less based on the total mass of the paper base material; How to recycle laminated paper. R = [{TP W - ((TP T / 10 4 ) × TP ρ × L S )} / {L W - ((TP T / 10 4 ) × TP ρ × L S )}] × 100... (Equation 1) (In the above formula (Math. 1), R is the amount of residue (unit: mass %), TP W is the mass of the thermoplastic resin layer after separation (unit: g), TP T is the thickness of the thermoplastic resin layer (unit: μm), TP ρ is the density of the thermoplastic resin layer (unit: g / cm 3 ), L S is the area of ​​the thermoplastic resin layer in the laminated paper before separation (unit: cm 2 ), L W represents the mass (unit: g) of the laminated paper before separation.

Citation Information

Patent Citations

  • Polyolefin laminated paper for release paper, release paper and pressure-sensitive adhesive sheet

    JP2006116718A