Polymer electrolyte material, polymer electrolyte molding therewith, electrolyte membrane with catalyst layer, membrane electrode assembly, solid state polymer fuel battery and water electrolysis type hydrogen generator

A block copolymer-based electrolyte material with a phase-separated structure addresses the trade-off between proton conductivity and mechanical durability in hydrocarbon-based membranes, achieving high performance and stability under low humidification conditions.

JP2024136654AActive Publication Date: 2024-10-04TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023047836
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

Conventional hydrocarbon-based polymer electrolyte membranes for fuel cells face a trade-off between proton conductivity and mechanical durability, particularly under low humidification conditions, making it difficult to achieve both high power generation performance and mechanical stability simultaneously.

Method used

A polymer electrolyte material composed of a block copolymer with specific phase-separated structures, containing ionic and non-ionic segments, which has an ion exchange capacity of 2.4 meq/g or less, crystallinity, and a phase-separated structure with an average periodic size of 60 nm to 110 nm, enhancing both proton conductivity and mechanical durability.

Benefits of technology

The proposed electrolyte material maintains good power generation performance under low humidity conditions while ensuring excellent mechanical durability, overcoming the trade-off limitations of previous materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136654000001_ABST
    Figure 2024136654000001_ABST
Patent Text Reader

Abstract

To provide a polymer electrolyte material having relatively excellent level of power generation performance under low humidity condition and excellent mechanical durability.SOLUTION: A polymer electrolyte material made of a block copolymer having a segment containing an ionic group (hereinafter referred to as "ionic segment") and a segment not containing the ionic group (hereinafter referred to as "nonionic segment"), has an ion exchange capacity of 2.4 meq / g or less, and satisfies both of the following conditions 1 and 2:<Condition 1>The polymer electrolyte material has a heat of crystallization of 0.1 J / g or more or a crystallinity of 0.5% or more. <Condition 2>The polymer electrolyte material has a phase-separated structure (bicontinuous M1, lamellar M2, cylindrical M3 or sea-island M4), and the average periodic size of the phase-separated structure observed by a transmission electron microscope is 60 nm or more and less than 110 nm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer electrolyte material, a polymer electrolyte molded body using the same, an electrolyte membrane with a catalyst layer, a membrane electrode assembly, a solid polymer fuel cell, and a water electrolysis type hydrogen generation device. [Background technology]

[0002] Fuel cells are a type of power generation device that extracts electrical energy by electrochemically oxidizing fuels such as hydrogen and methanol, and have been attracting attention in recent years as a clean energy supply source. Among them, solid polymer fuel cells have a low standard operating temperature of around 100°C and a high energy density, so they are expected to be widely used as power generation devices for relatively small-scale distributed power generation facilities and mobile objects such as automobiles and ships. Solid polymer fuel cells are also attracting attention as power sources for small mobile and portable devices, and are expected to be used as an alternative to secondary batteries such as nickel-metal hydride batteries and lithium-ion batteries in mobile phones and personal computers.

[0003] Fuel cells are usually constructed as a unit, with a cell in which a membrane electrode assembly (MEA) is sandwiched between separators. The MEA has catalyst layers arranged on both sides of an electrolyte membrane, and gas diffusion layers arranged on both sides of the electrolyte membrane. In the MEA, a pair of electrode layers is composed of a catalyst layer and a gas diffusion layer arranged on both sides of the electrolyte membrane, one of which is an anode electrode and the other is a cathode electrode. Electricity is generated by an electrochemical reaction when a fuel gas containing hydrogen comes into contact with the anode electrode and air comes into contact with the cathode electrode. The electrolyte membrane is mainly composed of a polymer electrolyte material. Polymer electrolyte materials are also used as binders for the catalyst layers.

[0004] Conventionally, the fluorine-based polymer electrolyte "Nafion" (registered trademark) (manufactured by Chemours Corporation) has been widely used as a polymer electrolyte material. On the other hand, development of inexpensive hydrocarbon-based electrolyte materials with excellent membrane properties that can replace "Nafion" (registered trademark) has been active in recent years. Hydrocarbon-based electrolyte materials have low gas permeability and excellent heat resistance, and electrolyte materials using aromatic polyether ketones and aromatic polyether sulfones have been particularly actively studied. However, while conventional hydrocarbon-based electrolyte materials exhibit proton conductivity equivalent to or superior to that of fluorine-based electrolyte materials under high humidification conditions, their proton conductivity under low humidification conditions is insufficient. For example, if the proton conductivity is insufficient, good power generation performance may not be obtained. In addition, high mechanical durability may be required for electrolyte membranes applied to fuel cells, water electrolysis devices, etc.

[0005] In response to the above-mentioned problems, electrolyte membranes having a phase-separated structure have been proposed as hydrocarbon-based polymer electrolyte membranes with improved proton conductivity and mechanical durability (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2008 / 018487 [Patent Document 2] International Publication No. 2013 / 031675 Summary of the Invention [Problem to be solved by the invention]

[0007] The polymer electrolyte membranes disclosed in the above patent documents are expected to have improved proton conductivity and mechanical durability.

[0008] However, in general, there is a trade-off between proton conductivity and mechanical durability, that is, increasing proton conductivity reduces mechanical durability, and conversely, increasing mechanical durability reduces proton conductivity, and even when the electrolyte membranes described in Patent Documents 1 and 2 are used, it is difficult to achieve both of these properties at a relatively high level. In particular, increasing proton conductivity (power generation performance) under low humidification conditions can sometimes reduce mechanical durability. In other words, it is difficult to achieve both mechanical durability and power generation performance under low humidification conditions.

[0009] In view of the above background of the prior art, an object of the present invention is to provide a polymer electrolyte material that has a relatively good level of power generation performance under low humidification conditions and also has excellent mechanical durability. [Means for solving the problem]

[0010] In order to solve the above problems, the polymer electrolyte material of the present invention has the following configuration. [1] A polymer electrolyte material comprising a block copolymer having a segment containing an ionic group (hereinafter referred to as an "ionic segment") and a segment not containing an ionic group (hereinafter referred to as a "nonionic segment"), the polymer electrolyte material having an ion exchange capacity of 2.4 meq / g or less and satisfying both of the following conditions 1 and 2: <Condition 1> The heat of crystallization of the polymer electrolyte material measured by differential scanning calorimetry (DSC) is 0.1 J / g or more, or the degree of crystallinity of the polymer electrolyte material measured by wide-angle X-ray diffraction is 0.5% or more. <Condition 2> The polymer electrolyte material has a phase-separated structure, and the average periodic size of the phase-separated structure observed with a transmission electron microscope is 60 nm or more and less than 110 nm. [2] The polymer electrolyte material according to [1], wherein the phase-separated structure is bicontinuous or lamellar. [3] The polymer electrolyte material according to [1] or 2, wherein the ionic segment and the nonionic segment contain an aromatic polyether ketone-based polymer. [4] The polymer electrolyte material according to any one of [1] to [3], wherein the ionic segment contains a structure represented by the following general formula (S1):

[0011] [ka]

[0012] (In general formula (S1), Ar 1 ~Ar 4 each independently represents a substituted or unsubstituted arylene group; Ar 1 ~Ar 4 At least one of Y has an ionic group. 1 and Y 2 each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to the general formula (S1) or another structural unit. [5] The polymer electrolyte material according to [4], wherein the structure represented by general formula (S1) is a structure represented by the following general formula (S2):

[0013] [ka]

[0014] (In general formula (S2), Y 1 and Y 2 each independently represents a ketone group or a protecting group that can be derived to a ketone group. M 1 ~M 4 Each of n1 to n4 independently represents a hydrogen atom, a metal cation or an ammonium cation. Each of n1 to n4 independently represents 0 or 1, and at least one of n1 to n4 is 1. * represents a bond to general formula (S2) or another structural unit. [6] The polymer electrolyte material according to any one of [1] to [5], wherein the nonionic segment contains a structure represented by the following general formula (S3):

[0015] [ka]

[0016] (In general formula (S3), Ar 5 ~Ar 8 each independently represents a substituted or unsubstituted arylene group. 5 ~Ar 8 None of Y has an ionic group. 3 and Y 4 each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to general formula (S3) or another structural unit. [7] The polymer electrolyte material according to [6], wherein the structure represented by general formula (S3) is a structure represented by the following general formula (S4):

[0017] [ka]

[0018] (In general formula (S4), Y 3 and Y 4 each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to general formula (S4) or another structural unit. [8] The polymer electrolyte material according to any one of [1] to [7], wherein the block copolymer has a linker moiety that bonds between the ionic segment and the nonionic segment. [9] A polymer electrolyte molded product comprising the polymer electrolyte material according to any one of [1] to [8].

[10] An electrolyte membrane with a catalyst layer, which is formed using the polymer electrolyte molded product according to [9].

[11] A membrane electrode assembly formed using the polymer electrolyte molded article according to [9].

[12] A solid polymer fuel cell constructed using the polymer electrolyte molded article according to [9].

[13] A water electrolysis hydrogen generation device comprising the polymer electrolyte molded body according to [9]. Effect of the Invention

[0019] According to the present invention, it is possible to provide a polymer electrolyte material which has a relatively good level of power generation performance under low humidification conditions and also has excellent mechanical durability. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic diagram of a phase-separated structure in a polymer electrolyte material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments and can be modified and implemented in various ways depending on the purpose and application.

[0022] The polymer electrolyte material according to the embodiment of the present invention is made of a block copolymer having a segment containing an ionic group (hereinafter referred to as an "ionic segment") and a segment not containing an ionic group (hereinafter referred to as a "nonionic segment"). A polymer electrolyte material made of such a block copolymer has the advantage that it easily forms a phase-separated structure. Hereinafter, the polymer electrolyte material may be simply referred to as an "electrolyte material".

[0023] For example, in an electrolyte membrane formed using an electrolyte material, there is generally a trade-off between power generation performance and mechanical durability, as described above. For example, taking the ion exchange capacity (hereinafter sometimes abbreviated as "IEC") of an electrolyte material as an example, the power generation performance tends to be high when the IEC is large and tends to be low when the IEC is small, while the mechanical durability tends to be low when the IEC is large and tends to be high when the IEC is small.

[0024] Therefore, the present invention has discovered that mechanical durability is improved by the synergistic effect of the electrolyte material having crystallinity and an IEC of 2.4 meq / g or less, and that even if the electrolyte material has an IEC of 2.4 meq / g or less, the power generation performance can be maintained at a relatively good level by the electrolyte material having a phase-separated structure with an average periodic size of 60 nm or more and less than 110 nm.

[0025] In the present invention, an electrolyte material having crystallinity means that it satisfies condition 1. <Condition 1> The heat of crystallization of the electrolyte material measured by differential scanning calorimetry (DSC) is 0.1 J / g or more, or the crystallinity of the electrolyte material measured by wide-angle X-ray diffraction is 0.5% or more. In the following description, satisfaction of condition 1 will be replaced with "having crystallinity."

[0026] In the present invention, confirmation of the phase separation structure of the electrolyte material, confirmation and measurement of the crystallinity of the electrolyte material, and evaluation of the mechanical durability and power generation performance of the electrolyte material were performed using a membrane (hereinafter referred to as "electrolyte membrane") obtained by applying a solution in which the electrolyte material was dissolved or dispersed in an appropriate solvent onto a support substrate and drying the applied solution. In the following description, the electrolyte material may be replaced with the electrolyte membrane.

[0027] In the present invention, good mechanical durability means that the wet-dry dimensional change rate of the electrolyte membrane made of the electrolyte material is small. Here, the wet-dry dimensional change rate of the electrolyte membrane can be obtained by the following measurement. A dry-wet cycle in which a test piece of the electrolyte membrane is alternately exposed to a dry atmosphere (30% RH) and a humid atmosphere (90% RH) while applying a constant stress to the test piece is repeated, and the dimensional change rates (%) at 30% RH and 90% RH are measured at the 10th cycle, and the difference between them is taken as the wet-dry dimensional change rate (%).

[0028] In the present invention, good power generation performance means that a high voltage is exhibited in the power generation performance evaluation described below.

[0029] [Ion exchange capacity (IEC)] The polymer electrolyte material according to the embodiment of the present invention has an IEC of 2.4 meq / g or less. From the viewpoint of mechanical durability, a lower IEC is preferable. That is, the IEC of the polymer electrolyte material according to the embodiment of the present invention is preferably 2.3 meq / g or less, and more preferably 2.2 meq / g or less. Furthermore, from the viewpoint of ensuring good power generation performance, the IEC is preferably greater than 1.5 meq / g, more preferably greater than 1.7 meq / g, and particularly preferably greater than 1.9 meq / g.

[0030] IEC is the molar amount of ion exchange groups introduced per unit dry mass of an electrolyte material (block copolymer). IEC can be measured by elemental analysis, neutralization titration, etc. When the ion exchange group is a sulfonic acid group, it can be calculated from the S / C ratio using elemental analysis, but it is difficult to measure when a sulfur source other than sulfonic acid groups is contained. Therefore, in the present invention, IEC is defined as a value obtained by neutralization titration, which will be described later.

[0031] The IEC of the electrolyte material can be adjusted by controlling, for example, the density of the sulfonic acid group in the block copolymer, the content of the ionic segment in the block copolymer, and the like.

[0032] [Crystalline] The polymer electrolyte material according to the embodiment of the present invention has crystallinity. Here, "having crystallinity" means any one of (i) being capable of being crystallized when heated, (ii) having a property capable of being crystallized, and (iii) already being crystallized.

[0033] The above (i) and (ii) can be determined by the heat of crystallization of the electrolyte material measured by differential scanning calorimetry (DSC). The above (iii) can be determined by the crystallinity of the electrolyte material measured by wide-angle X-ray diffraction. In other words, in the present invention, the electrolyte material having crystallinity means that the heat of crystallization of the electrolyte material measured by differential scanning calorimetry (DSC) is 0.1 J / g or more, or the crystallinity of the electrolyte material measured by wide-angle X-ray diffraction is 0.5% or more (satisfying the above-mentioned <Condition 1>).

[0034] The degree of crystallinity of the electrolyte material is preferably high from the viewpoint of mechanical durability. For example, in the case of the heat of crystallization, it is preferably 1 J / g or more, more preferably 5 J / g or more, and particularly preferably 10 J / g or more. Moreover, if the heat of crystallization is too large, the electrolyte membrane tends to become brittle, so it is preferably 35 J / g or less, more preferably 30 J / g or less, and particularly preferably 25 J / g or less.

[0035] In the case of the crystallinity, it is preferably 1% or more, more preferably 3% or more, and particularly preferably 5% or more. Also, if the crystallinity is too high, the electrolyte membrane tends to become brittle, so it is preferably 30% or less, more preferably 27% or less, and particularly preferably 25% or less.

[0036] The crystallinity of the electrolyte material (block copolymer) can be increased by increasing the molecular chain length of the nonionic segment or by increasing the content of the nonionic segment in the block copolymer. It can also be increased by selecting the molecular structure. Regarding the above molecular structure, it is preferable that the ionic segment and the nonionic segment each contain an aromatic hydrocarbon-based polymer, and further preferably contain an aromatic polyether-based polymer, and particularly preferably contain an aromatic polyether ketone-based polymer. Details will be described later.

[0037] [Phase separation structure] The polymer electrolyte material according to the embodiment of the present invention has a phase-separated structure. Here, the term "the electrolyte material has a phase-separated structure" means that the phase-separated structure can be confirmed when the electrolyte membrane is observed with a transmission electron microscope (TEM).

[0038] Examples of the phase-separated structure of an electrolyte membrane are shown in Figure 1. Phase-separated structures are broadly classified into four types: co-continuous (M1), lamellar (M2), cylindrical (M3), and sea-island (M4). The polymer electrolyte material according to the embodiment of the present invention has any one of the phase-separated structures (M1) to (M4).

[0039] In (M1) to (M4) in FIG. 1, the continuous phase (phase 1) in the white portion is formed by one segment selected from the ionic segment and the nonionic segment, and the continuous or dispersed phase (phase 2) in the gray portion is formed by the other segment.

[0040] The above phase-separated structure is described, for example, in Annual Review of Physical Chemistry, 41, 1990, p. 525.

[0041] By controlling the higher-order structure and shape of the ionic and nonionic segments, it is possible to achieve excellent proton conductivity even under low humidity and low temperature conditions. In other words, by having an electrolyte membrane with a phase-separated structure of (M1) to (M4), it is possible to form continuous proton-conducting channels, improving proton conductivity.

[0042] In the phase separation structure consisting of cocontinuous (M1) and lamellar (M2), both the ionic segment and the nonionic segment form a continuous phase. An electrolyte membrane having such a phase separation structure has excellent proton conductivity due to the formation of continuous proton conductive channels, and at the same time, has excellent mechanical durability due to the crystallinity of the domains consisting of the nonionic segments. That is, the polymer electrolyte material according to the embodiment of the present invention preferably has a cocontinuous (M1) or lamellar (M2) phase separation structure, and particularly preferably has a cocontinuous (M1) phase separation structure.

[0043] The above-mentioned domain refers to a cluster formed by the aggregation of similar segments in one or more polymer chains.

[0044] The electrolyte membrane can be confirmed to have a bicontinuous (M1) or lamellar (M2) phase separation structure by the following method. Specifically, it is defined that the electrolyte membrane has the structure when a desired image is observed by the following method. The method is to compare three digital slice views cut from three directions, vertical, horizontal, and height, with a three-dimensional view obtained by TEM tomography observation. For example, in an electrolyte membrane containing a block copolymer having an ionic segment and a nonionic segment, when the phase separation structure is bicontinuous (M1) or lamellar (M2), both the hydrophilic domain containing the ionic segment and the hydrophobic domain containing the nonionic segment form a continuous phase in all three views.

[0045] In the case of the bicontinuous phase (M1), each of the continuous phases shows an intricate pattern, and in the case of the lamellar phase (M2), each of the continuous phases shows a layered pattern. Here, the continuous phase means a phase in which the individual domains are not isolated from each other when viewed macroscopically, but it is acceptable for there to be some parts that are not connected.

[0046] On the other hand, in the case of the cylindrical structure (M3) or the sea-island structure (M4), one of the domains does not form a continuous phase on at least one surface, so it can be distinguished from the above-mentioned cocontinuous-like (M1) and lamellar-like (M2) structures, and the structures can also be distinguished from the patterns shown in each of the three-dimensional views.

[0047] In observing the phase-separated structure, in order to clarify the aggregation state and contrast of the ionic and nonionic segments, for example, the electrolyte membrane can be immersed in a 2 wt % lead acetate aqueous solution for two days to ion-exchange the ionic groups with lead, and then observed with a transmission electron microscope (TEM) and TEM tomography.

[0048] The size of the phase-separated structure can be expressed as the periodic size of the hydrophilic domains containing ionic segments and the hydrophobic domains containing nonionic segments. The periodic size of such a phase-separated structure can be estimated from the autocorrelation function given by image processing of the phase-separated structure obtained by transmission electron microscope (TEM) observation. The periodic size of the phase-separated structure obtained by transmission electron microscope (TEM) observation is the size in a vacuum atmosphere.

[0049] The average periodic size of the phase-separated structure in the polymer electrolyte material (electrolyte membrane) according to the embodiment of the present invention is 60 nm or more and less than 110 nm. <Condition 2> The polymer electrolyte material has a phase-separated structure, and the average periodic size of the phase-separated structure observed by a transmission electron microscope is 60 nm or more and less than 110 nm. In this way, by increasing the average periodic size of the phase separation structure, high power generation performance can be obtained even if the IEC is 2.4 meq / g or less.

[0050] In the polymer electrolyte material according to the embodiment of the present invention, the average periodic size of the phase separation structure is preferably 63 nm or more, more preferably 65 nm or more, and particularly preferably 70 nm or more, from the above viewpoint. On the other hand, if the average periodic size of the phase separation structure is 110 nm or more, the mechanical durability decreases. In addition, as described above, a cocontinuous phase separation structure is preferable, but if the average periodic size of the phase separation structure is large, such as 110 nm or more, it becomes difficult to form a cocontinuous phase separation structure. Therefore, from the viewpoint of obtaining a cocontinuous phase separation structure, the average periodic size is less than 110 nm. Furthermore, from the above viewpoint, the average periodic size of the phase separation structure is more preferably less than 100 nm.

[0051] The average periodic size of the phase-separated structure in a block copolymer correlates with the IEC, and the periodic size tends to become smaller as the IEC becomes smaller. Until now, there has been no specific disclosure of a block copolymer having crystallinity and an IEC of 2.4 meq / g or less in which the average periodic size of the phase-separated structure is 60 nm or more and less than 110 nm. Therefore, the present invention has succeeded in obtaining a block copolymer having crystallinity and an IEC of 2.4 meq / g or less, but with an average periodic size of the phase-separated structure in the above range, and has found that an electrolyte material made of this block copolymer has excellent mechanical durability and relatively good power generation performance under low humidification conditions.

[0052] Such a block copolymer can be obtained, for example, by increasing the molecular chain length of each of the ionic and nonionic segments of the block copolymer, or by increasing the ratio of the molecular chain length of the nonionic segment to the molecular chain length of the ionic segment, as described in detail below.

[0053] [Block copolymer] The polymer electrolyte material according to the embodiment of the present invention is made of a block copolymer having an ionic segment and a nonionic segment. In the present invention, a segment is a partial structure in a block copolymer of a macromonomer used in synthesizing the block copolymer. Although the nonionic segment is described as not containing an ionic group, it may contain a small amount of ionic groups as long as it does not adversely affect the effects of the present invention, particularly the crystallinity.

[0054] The block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention is a polymer chain formed by linking two or more mutually incompatible segment chains, i.e., an ionic segment which is a hydrophilic segment and a nonionic segment which is a hydrophobic segment. In the block copolymer, the short-range interaction caused by the repulsion between the chemically different segment chains causes phase separation into nano- or micro-domains consisting of the respective segment chains. Since the segment chains are covalently bonded to each other, a long-range interaction occurs, and due to this effect, each domain is arranged with a specific order. The higher-order structure created by the aggregation of the domains consisting of each segment chain is called a nano- or micro-phase separation structure. Here, a domain means a mass formed by the aggregation of similar segments in one or more polymer chains. For the ion conduction of the electrolyte membrane, the spatial arrangement of the ion-conducting segments in the membrane, i.e., the nano- or micro-phase separation structure, is important.

[0055] [Ionic segment] From the viewpoints of crystallinity and mechanical durability, the ionic segment in the block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention preferably contains a hydrocarbon-based polymer, where "hydrocarbon-based" means a polymer other than a perfluoro-based polymer, and "hydrocarbon-based polymer" means a polymer other than a perfluoro-based polymer.

[0056] Furthermore, from the viewpoints of crystallinity and mechanical durability, the ionic segment preferably contains a hydrocarbon polymer having an aromatic ring in the main chain (hereinafter referred to as an "aromatic hydrocarbon polymer").

[0057] The aromatic ring contained in the aromatic hydrocarbon polymer may contain not only a hydrocarbon aromatic ring but also a heterocycle. In addition, some aliphatic units may constitute the polymer together with the aromatic ring unit. Specific examples of aromatic hydrocarbon polymers include polymers having a structure selected from polysulfone, polyethersulfone, polyphenylene oxide, polyarylene ether polymer, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene polymer, polyarylene ketone, polyether ketone, polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole, polybenzothiazole, polybenzimidazole, polyamide, polyimide, polyetherimide, and polyimide sulfone in the main chain together with an aromatic ring. Among these, aromatic polyether polymers are preferred from the viewpoints of cost and polymerizability.

[0058] The aromatic polyether polymer refers to a polymer mainly composed of aromatic rings, in which the repeating unit contains at least an ether bond as a mode of linking the aromatic ring units. Examples of the structure of the aromatic polyether polymer include, but are not limited to, aromatic polyether, aromatic polyether ketone, aromatic polyether imide, aromatic polyether sulfone, etc. From the viewpoint of crystallinity, aromatic polyether ketone polymers are preferable.

[0059] The aromatic polyetherketone polymer refers to a polymer mainly composed of aromatic rings, in which the repeating units contain at least an ether bond and a ketone bond as a mode of linking the aromatic ring units. The aromatic polyetherketone polymer includes aromatic polyetherketone, aromatic polyetheretherketone, aromatic polyetherketoneketone, aromatic polyetheretherketoneketone, aromatic polyetherketoneetherketoneketone, and aromatic polyetherketoneetherketoneketone.

[0060] The ionic segment used in the present invention can be synthesized by an aromatic nucleophilic substitution reaction, a coupling reaction, or the like.

[0061] As described above, the ionic segment preferably contains an aromatic polyether ketone polymer, and the polymer preferably contains a structure represented by the following general formula (S1).

[0062] [ka]

[0063] In general formula (S1), Ar 1 ~Ar 4 each independently represents a substituted or unsubstituted arylene group; Ar 1 ~Ar 4 At least one of Y has an ionic group. 1 and Y 2 each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to general formula (S1) or another structural unit.

[0064] Here, Ar 1 ~Ar 4Examples of the arylene group represented by the formula (1) include, but are not limited to, hydrocarbon arylene groups such as phenylene, naphthylene, biphenylene, and fluorenediyl groups, and heteroarylene groups such as pyridinediyl, quinoxalinediyl, and thiophenediyl. The ionic group is preferably an atomic group having a negative charge, and is preferably one having proton exchange ability. Examples of such functional groups include, but are not limited to, sulfonic acid groups, sulfonimide groups, sulfuric acid groups, phosphonic acid groups, phosphoric acid groups, and carboxylic acid groups.

[0065] The above ionic groups include those in the form of salts. Examples of cations that form such salts include any metal cation, NR4 + (R is any organic group) and the like can be given as examples. There is no particular limitation on the metal cation, but Na, K, and Li, which are inexpensive and can be easily proton-substituted, are preferred.

[0066] Two or more types of these ionic groups can be contained in the ionic segment, and the combination is appropriately determined depending on the structure of the block copolymer, etc. Among them, it is more preferable to contain at least a sulfonic acid group, a sulfonimide group, or a sulfate group from the viewpoint of high proton conductivity, and it is particularly preferable to contain a sulfonic acid group from the viewpoint of raw material costs.

[0067] In addition, in the general formula (S1), Y 1 and Y 2 From the viewpoint of forming a phase-separated structure, it is preferable that the ionic segment is a ketone group or a protecting group that can be derived to a ketone group. That is, the ionic segment is preferably an aromatic polyether ketone polymer. The protecting group that can be derived to a ketone group will be described later.

[0068] The structure represented by the above general formula (S1) is preferably a structure represented by the following general formula (P1) in terms of raw material availability, and among these, a structure represented by the following general formula (S2) is more preferable in terms of raw material availability and polymerizability.

[0069] [ka]

[0070] In general formula (P1) and general formula (S2), Y 1 and Y 2 each independently represents a ketone group or a protecting group that can be derived to a ketone group. M 1 ~M 4 each independently represents a hydrogen atom, a metal cation or an ammonium cation. n1 to n4 each independently represent 0 or 1, provided that at least one of n1 to n4 is 1. * represents a bond to general formula (P1) or (S2) or another structural unit.

[0071] Furthermore, in terms of raw material availability and polymerizability, it is most preferable that n1=1, n2=1, n3=0, and n4=0 or n1=0, n2=0, n3=1, and n4=1.

[0072] Examples of ionic monomers used to synthesize the constituent units of the ionic segment include aromatic active dihalide compounds. It is preferable to use a compound obtained by introducing an ionic acid group into an aromatic active dihalide compound as the aromatic active dihalide compound used in the ionic segment in terms of chemical stability, production cost, and the ability to precisely control the amount of ionic groups. Suitable specific examples of monomers having a sulfonic acid group as an ionic group include, but are not limited to, 3,3'-disulfonate-4,4'-dichlorodiphenyl sulfone, 3,3'-disulfonate-4,4'-difluorodiphenyl sulfone, 3,3'-disulfonate-4,4'-dichlorodiphenyl ketone, 3,3'-disulfonate-4,4'-difluorodiphenyl ketone, 3,3'-disulfonate-4,4'-dichlorodiphenyl phenyl phosphine oxide, and 3,3'-disulfonate-4,4'-difluorodiphenyl phenyl phosphine oxide.

[0073] From the standpoint of proton conductivity and hydrolysis resistance, the ionic group is most preferably a sulfonic acid group, but the monomer having the above ionic group may also have another ionic group.

[0074] Among the above-mentioned monomers having a sulfonic acid group, 3,3'-disulfonate-4,4'-dichlorodiphenyl ketone and 3,3'-disulfonate-4,4'-difluorodiphenyl ketone are more preferred from the viewpoints of chemical stability and mechanical durability, and 3,3'-disulfonate-4,4'-difluorodiphenyl ketone is most preferred from the viewpoint of polymerization activity.

[0075] The ionic segment synthesized using 3,3'-disulfonate-4,4'-dichlorodiphenyl ketone and 3,3'-disulfonate-4,4'-difluorodiphenyl ketone as monomers having an ionic group contains a constitutional unit represented by the following general formula (p1), and is preferably used. The aromatic polyether polymer is a component having better hot water resistance than a sulfone group in addition to the high crystallinity characteristic of the ketone group, and is more preferably used in terms of mechanical durability under high temperature and high humidity conditions. It is preferable that these sulfonic acid groups are salts with monovalent cationic species during polymerization. The monovalent cationic species may be sodium, potassium, other metal species, various amines, etc., and are not limited thereto. These aromatic active dihalide compounds can be used alone, but it is also possible to use multiple aromatic active dihalide compounds in combination.

[0076] [ka]

[0077] In general formula (p1), M 1 and M. 2 represents hydrogen, a metal cation or an ammonium cation, and a1 and a2 represent integers of 1 to 4. The constitutional unit represented by general formula (p1) may be optionally substituted.

[0078] In addition, it is also possible to control the ionic group density by copolymerizing aromatic active dihalide compounds having an ionic group with those having no ionic group. However, it is more preferable not to copolymerize aromatic active dihalide compounds having no ionic group as the ionic segment from the viewpoint of ensuring the continuity of the proton conductive path.

[0079] More preferred specific examples of aromatic active dihalide compounds having no ionic group include 4,4'-dichlorodiphenyl sulfone, 4,4'-difluorodiphenyl sulfone, 4,4'-dichlorodiphenyl ketone, 4,4'-difluorodiphenyl ketone, 4,4'-dichlorodiphenyl phenyl phosphine oxide, 4,4'-difluorodiphenyl phenyl phosphine oxide, 2,6-dichlorobenzonitrile, 2,6-difluorobenzonitrile, etc. Among them, 4,4'-dichlorodiphenyl ketone and 4,4'-difluorodiphenyl ketone are more preferred from the viewpoint of crystallinity and mechanical durability, and 4,4'-difluorodiphenyl ketone is most preferred from the viewpoint of polymerization activity. These aromatic active dihalide compounds can be used alone, but it is also possible to use multiple aromatic active dihalide compounds in combination.

[0080] Polymer electrolyte materials synthesized using 4,4'-dichlorodiphenyl ketone or 4,4'-difluorodiphenyl ketone as an aromatic active dihalide compound further contain a constituent part represented by the following general formula (p2), and are preferably used. The constituent unit is a component that imparts intermolecular cohesive force and crystallinity, and is preferably used because it is a material with excellent mechanical durability under high temperature and high humidity conditions.

[0081] [ka]

[0082] The constitutional unit represented by general formula (p2) may be optionally substituted, but does not contain an ionic group.

[0083] Examples of nonionic monomers used to synthesize the ionic segment include aromatic diphenol compounds, and aromatic diphenol compounds having a protecting group, which will be described later, are particularly preferred.

[0084] The monomers used to synthesize the building blocks of the ionic segment have been described above.

[0085] The ionic segment or the structural units constituting the ionic segment may include structures represented by the following general formulas (T1) and (T2) in addition to the structure represented by general formula (S1).

[0086] [ka]

[0087] In the general formulas (T1) and (T2), B represents a divalent organic group containing an aromatic ring. 5 and M. 6 each independently represents a hydrogen atom, a metal cation, or an ammonium cation.

[0088] In this aromatic polyether ketone copolymer, the ion exchange capacity can be controlled by changing the composition ratio of the structural units represented by general formulas (T1) and (T2).

[0089] It is particularly preferred that the ionic segment has a structure represented by general formula (P1) and a structure represented by general formula (T1) and (T2). In such an ionic segment, when the amounts of the structural units represented by general formula (P1), (T1) and (T2) are p1, t1 and t2, respectively, the total molar amount of t1 and t2 is 100 molar parts, and p1 is preferably 75 molar parts or more, more preferably 90 molar parts or more, and even more preferably 100 molar parts or more.

[0090] Examples of the divalent organic group B containing an aromatic ring in general formulae (T1) and (T2) include residues of various dihydric phenol compounds that can be used in the polymerization of aromatic polyether polymers by aromatic nucleophilic substitution reactions, and residues of such dihydric phenol compounds into which a sulfonic acid group has been introduced. Preferred specific examples of the divalent organic group B containing an aromatic ring include groups represented by the following general formulas (X'-1) to (X'-6), but are not limited to these.

[0091] [ka]

[0092] These may have an ionic group or an aromatic group. These may also be used in combination as necessary. Among them, from the viewpoints of crystallinity, mechanical durability, and chemical stability, the groups represented by the general formulae (X'-1) to (X'-4) are more preferable, and the groups represented by the general formulae (X'-2) and (X'-3) are most preferable.

[0093] [Non-ionic segment] From the viewpoints of crystallinity and mechanical durability, the nonionic segment constituting the block copolymer of the present invention preferably contains a hydrocarbon polymer, and more preferably contains an aromatic hydrocarbon polymer, where the definition of the hydrocarbon polymer and specific examples of the aromatic hydrocarbon polymer are as described above.

[0094] Among aromatic hydrocarbon polymers, aromatic polyether polymers are preferred from the viewpoints of cost and polymerizability, and aromatic polyether ketone polymers are more preferred from the viewpoints of crystallinity and mechanical durability.

[0095] As described above, the nonionic segment preferably contains an aromatic polyether ketone polymer, and the polymer preferably contains a structure represented by the following general formula (S3).

[0096] [ka]

[0097] In general formula (S3), Ar 5 ~Ar 8 each independently represents a substituted or unsubstituted arylene group. 5 ~Ar 8 None of Y has an ionic group. 3 and Y 4 each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to general formula (S3) or another structural unit.

[0098] Here, Ar 5 ~Ar 8 Examples of the arylene group represented by the formula (I) include hydrocarbon arylene groups such as a phenylene group, a naphthylene group, a biphenylene group, and a fluorenediyl group, and heteroarylene groups such as pyridinediyl, quinoxalinediyl, and thiophenediyl, but are not limited thereto.

[0099] In addition, in the general formula (S3), Y 3 and Y 4 From the viewpoint of forming a phase-separated structure, since is a ketone group or a protecting group that can be derived to a ketone group, the block copolymer has crystallinity and is likely to form a phase-separated structure. In other words, the nonionic segment is preferably an aromatic polyether ketone polymer.

[0100] The structure represented by the above general formula (S3) preferably contains a structure represented by the following general formula (P2) in terms of raw material availability, and among these, it is more preferable that it contains a constitutional unit represented by the following general formula (S4) in terms of crystallinity.

[0101] [ka]

[0102] In the general formulas (P2) and (S4), Y 3 and Y 4each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to general formulae (P2) and (S4) or other structural units.

[0103] The content of the structure represented by general formula (P2) or (S4) in the nonionic segment is preferably 20 mol % or more, more preferably 50 mol % or more, and particularly preferably 80 mol % or more, from the viewpoints of crystallinity and mechanical durability.

[0104] Preferred examples of the protecting group that can be derived to a ketone group include those containing at least one type selected from the following general formulae (P3) and (P4).

[0105] [ka]

[0106] In the general formulas (P3) and (P4), Ar 11 ~Ar 14 is any divalent arylene group, R 1 and R 2 is at least one group selected from H and an alkyl group; R 3 represents any alkylene group, each of which may represent two or more types of groups. The groups represented by general formulae (P3) and (P4) may be optionally substituted.

[0107] R in general formula (P3) 1 and R 2 From the viewpoint of stability, R is preferably an alkyl group, further preferably an alkyl group having 1 to 6 carbon atoms, and most preferably an alkyl group having 1 to 3 carbon atoms. 3 From the viewpoint of stability, R is more preferably an alkylene group having 1 to 7 carbon atoms, and most preferably an alkylene group having 1 to 4 carbon atoms. 3Specific examples include, but are not limited to, -CH2CH2-, -CH(CH3)CH2-, -CH(CH3)CH(CH3)-, -C(CH3)2CH2-, -C(CH3)2CH(CH3)-, -C(CH3)2O(CH3)2-, -CH2CH2CH2-, -CH2C(CH3)2CH2-, and the like.

[0108] Ar in general formulas (P3) and (P4) 11 ~Ar 14 The preferred organic group for is a phenylene group, a naphthylene group, or a biphenylene group. These may be optionally substituted. As the aromatic polyether polymer, the Ar 13 and Ar 14 More preferably, both are phenylene groups, and most preferably, Ar 13 and Ar 14 Both are p-phenylene groups.

[0109] Here, the method of protecting the ketone moiety with a ketal includes a method of reacting a precursor compound having a ketone group with a monofunctional and / or difunctional alcohol in the presence of an acid catalyst. For example, it can be produced by reacting the ketone precursor 4,4'-dihydroxybenzophenone with a monofunctional and / or difunctional alcohol, aliphatic or aromatic hydrocarbon, or the like in a solvent in the presence of an acid catalyst such as hydrogen bromide. The alcohol is an aliphatic alcohol having 1 to 20 carbon atoms.

[0110] An improved process for preparing ketal monomers involves reacting the ketone precursors 4,4'-dihydroxybenzophenone with a difunctional alcohol in the presence of an alkyl orthoester and a solid catalyst.

[0111] The method of deprotecting at least a part of the ketone moiety protected by ketal to obtain a ketone moiety is not particularly limited. The deprotection reaction can be carried out in the presence of water and acid under heterogeneous or homogeneous conditions, but from the viewpoint of mechanical durability and solvent resistance, a method of forming into a membrane or the like and then treating with acid is more preferable. Specifically, the formed membrane can be deprotected by immersing in an aqueous hydrochloric acid solution or an aqueous sulfuric acid solution, and the concentration of the acid and the temperature of the aqueous solution can be appropriately selected.

[0112] The weight ratio of the acidic aqueous solution required to the polymer is preferably 1 to 100 times, but larger amounts of water can also be used. The acid catalyst is preferably used at a concentration of 0.1 to 50% by weight of the water present. Suitable acid catalysts include strong mineral acids such as hydrochloric acid, nitric acid, fluorosulfonic acid, sulfuric acid, etc., and strong organic acids such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, etc. The amounts of acid catalyst and excess water, reaction pressure, etc. can be appropriately selected depending on the film thickness of the polymer, etc.

[0113] For example, in the case of a membrane having a thickness of 50 μm, it is possible to easily deprotect almost the entire amount by immersing it in an acidic aqueous solution such as a 6N hydrochloric acid aqueous solution and heating it at 95° C. for 1 to 48 hours. It is also possible to deprotect most of the protecting groups by immersing it in a 1N hydrochloric acid aqueous solution at 25° C. for 24 hours. However, the deprotection conditions are not limited to these, and deprotection may be performed using an acidic gas, an organic acid, or the like, or by heat treatment.

[0114] Even when the aromatic polyether polymer contains a bonding type other than an ether bond, such as a direct bond, the position of the protective group to be introduced is preferably the aromatic ether polymer portion from the viewpoint of improving processability.

[0115] Specifically, for example, aromatic polyether polymers containing structural units represented by general formulas (P3) and (P4) can be synthesized by using compounds represented by the following general formulas (P3-1) and (P4-1) as aromatic diphenol compounds, respectively, and subjecting them to aromatic nucleophilic substitution reaction with aromatic active dihalide compounds. The structural units represented by general formulas (P3) and (P4) may be derived from either the aromatic diphenol compound or the aromatic active dihalide compound, but it is more preferable to use those derived from aromatic diphenol compounds in consideration of the reactivity of the monomers.

[0116] [ka]

[0117] In the general formulae (P3-1) and (P4-1), Ar 11 ~Ar 14 is any divalent arylene group, R 1 and R 2 is at least one group selected from H and an alkyl group; R 3 represents any alkylene group. The compounds represented by general formula (P3-1) and general formula (P4-1) may be optionally substituted.

[0118] [Details of block copolymers] In the block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention, both the ionic segment and the nonionic segment are preferably aromatic polyether-based polymers, and more preferably aromatic polyether ketone-based polymers.

[0119] In particular, it is preferable that the block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention contains an ionic segment containing a constitutional unit represented by the above general formula (S1) and a nonionic segment containing a constitutional unit represented by the above general formula (S3).

[0120] When the nonionic segment contains a constituent unit represented by general formula (S3), it is a crystalline segment, and the crystallinity can be adjusted to the desired level by controlling the molecular weight of this nonionic segment or its content in the block copolymer.

[0121] A block copolymer containing a nonionic segment containing a constitutional unit represented by general formula (S3) can be produced, for example, by molding a block copolymer precursor in which a protective group has been introduced at least into the nonionic segment, and then deprotecting at least a part of the protective group contained in the molded product. Since block copolymers tend to have poorer processability than random copolymers due to crystallization of the polymer that has formed domains, it is preferable to introduce a protective group at least into the nonionic segment to improve processability, and it is also preferable to introduce a protective group into the ionic segment when the processability is poor.

[0122] The block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention has a phase separation structure. That is, in the block copolymer of the present invention having ionic segments and nonionic segments, the hydrophilic domain formed by aggregation of the ionic segments has a locally high ionic group concentration and exhibits excellent power generation performance. The hydrophobic domain formed by aggregation of the nonionic segments has a strong intermolecular interaction due to crystallinity and exhibits excellent mechanical durability.

[0123] When both the ionic segment and the nonionic segment constituting the block copolymer are aromatic polyether polymers, preferably aromatic polyether ketone polymers, a phase separation structure is easily formed. From the above viewpoint, the block copolymer of the present invention preferably contains an ionic segment containing a constitutional unit represented by the above general formula (S1) and a nonionic segment containing a constitutional unit represented by the above general formula (S3).

[0124] In addition, the block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention preferably contains one or more linker moieties connecting the ionic segment and the nonionic segment. Such a block copolymer is likely to form a bicontinuous phase-separated structure, and the periodic size of the phase-separated structure is likely to become large. Hereinafter, the linker moiety connecting the ionic segment and the nonionic segment may be referred to as "linker (R1)". Meanwhile, as described later, the linker moiety connecting the structural units in the ionic segment may be referred to as "linker (R2)".

[0125] The linker (R1) is defined as a moiety that connects between an ionic segment and a nonionic segment and has a chemical structure different from that of the ionic segment or the nonionic segment.

[0126] The linker (R1) has the function of linking different segments while suppressing randomization of the copolymer by ether exchange reaction, segment cleavage, and other side reactions that may occur during the synthesis of the copolymer. Therefore, by using a compound that gives such a linker (R1) as a raw material, a block copolymer can be obtained without lowering the molecular weight of each segment. The compound that gives the linker (R1) is preferably a halide compound, and examples thereof include, but are not limited to, decafluorobiphenyl, hexafluorobenzene, 4,4'-difluorodiphenylsulfone, and 2,6-difluorobenzonitrile.

[0127] By controlling the number average molecular weight of the ionic segment and the number average molecular weight of the nonionic segment constituting the block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention, the IEC, the average periodic size of the crystalline and phase-separated structures of the block copolymer can be adjusted to the desired range described above. For example, the number average molecular weight of the ionic segment is preferably in the range of 40,000 to 150,000, more preferably in the range of 45,000 to 130,000, and particularly preferably in the range of 50,000 to 120,000, from the viewpoint of adjusting the average periodic size of the IEC and phase-separated structures to the desired range. On the other hand, the number average molecular weight of the nonionic segment is preferably in the range of 15,000 to 60,000, more preferably in the range of 20,000 to 50,000, and particularly preferably in the range of 22,000 to 45,000, from the viewpoint of adjusting the average periodic size of the crystalline and phase-separated structures to the desired range.

[0128] In order to make the number average molecular weight of the ionic segment relatively large, for example, to make the number average molecular weight 50,000 or more, it is preferable to make the structure in which the structural units in the ionic segment are linked with a linker site (linker (R2)). By using the linker (R2), the synthesis of a long-chain polymer becomes relatively easy. As a compound that provides the linker (R2), a halide compound is preferable, and examples thereof include, but are not limited to, decafluorobiphenyl, hexafluorobenzene, 4,4'-difluorodiphenylsulfone, and 2,6-difluorobenzonitrile.

[0129] In the block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention, i.e., in the block copolymer having crystallinity with an IEC of 2.4 meq / g or less, a phase separation structure having an average periodic size of 60 nm or more and less than 110 nm is easily formed by, for example, designing Mn1 and Mn2 in the above-mentioned ranges and designing the ratio of Mn1 to Mn2 (Mn1 / Mn2) in the range of 1.50 to 4.00, where Mn1 is the number average molecular weight of the ionic segment of the block copolymer and Mn2 is the number average molecular weight of the nonionic segment. The ratio (Mn1 / Mn2) is preferably in the range of 1.50 to 3.70. When the ratio (Mn1 / Mn2) is in the range of 1.50 to 4.00, Mn2 is preferably 20,000 or more, more preferably 22,000 or more.

[0130] Specific examples of methods for synthesizing the block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention are given below, although the present invention is not limited thereto.

[0131] Each segment in the block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention is preferably synthesized by an aromatic nucleophilic substitution reaction because the process is easy. The aromatic nucleophilic substitution reaction is a method in which a monomer mixture of a dihalide compound and a diol compound is reacted in the presence of a basic compound. The polymerization can be carried out at a temperature range of 0 to 350°C, but a temperature of 50 to 250°C is preferable. The reaction can be carried out without a solvent, but is preferably carried out in a solvent. Examples of solvents that can be used include aprotic polar solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, sulfolane, 1,3-dimethyl-2-imidazolidinone, and hexamethylphosphontriamide, but are not limited thereto, and any solvent that can be used as a stable solvent in an aromatic nucleophilic substitution reaction may be used. These organic solvents may be used alone or as a mixture of two or more kinds.

[0132] Examples of basic compounds include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, etc., but any compound that can convert diols into an active phenoxide structure can be used without being limited thereto. In addition, in order to increase the nucleophilicity of the phenoxide, it is also preferable to add a crown ether such as 18-crown-6. Crown ethers can be preferably used because they can coordinate with the sodium ion or potassium ion of the sulfonic acid group to improve the solubility of the sulfonate portion of the monomer or polymer in an organic solvent.

[0133] In aromatic nucleophilic substitution reactions, water may be produced as a by-product. In this case, water can be removed from the system as an azeotrope by coexisting toluene or the like in the reaction system, regardless of the polymerization solvent. A water absorbent such as a molecular sieve can also be used to remove water from the system.

[0134] The block copolymer constituting the polymer electrolyte material according to the embodiment of the present invention can be produced by synthesizing a block copolymer precursor and then deprotecting at least a part of the protective groups contained in the precursor. The method for producing the block copolymer and block copolymer precursor of the present invention preferably includes at least the following steps (1) and (2). By including these steps, it is possible to achieve improvement in mechanical durability by increasing the molecular weight, and to obtain a block copolymer in which the phase separation structure and domain size are strictly controlled by alternately introducing both segments. Such a block copolymer has good power generation performance even if its IEC is 2.4 meq / g or less.

[0135] Step (1): A step of reacting the -OM groups at both ends of one of an ionic segment having -OM groups (M represents a hydrogen atom, a metal cation, or an ammonium cation) at both ends and a nonionic segment having -OM groups at both ends with a compound that provides a linker (R1) to introduce the linker (R1) into both ends of the segment. Step (2): A step of producing a block copolymer or a block copolymer precursor having an ionic segment and a nonionic segment by polymerizing the linker (R1) at both ends of the segment into which the linker (R1) synthesized in step (1) has been introduced with the -OM groups at both ends of the other segment.

[0136] Specific examples of the ionic segments represented by general formulae (S1) and (S2) having -OM groups at both ends, and the nonionic segments represented by general formulae (S3) and (S4) having -OM groups at both ends, include segments having structures represented by the following general formulae (H3-1) and (H3-2), respectively. In addition, examples of structures obtained after reacting the segments having structures represented by general formulae (H3-1) and (H3-2) with a compound that provides a linker (R1) include structures represented by the following general formulae (H3-3) and (H3-4), respectively. However, the present invention is not limited to these.

[0137] [ka]

[0138] In the above general formulas (H3-1) to (H3-4), N1, N2, N3, and N4 each independently represent an integer of 1 to 200.

[0139] A specific example of an ionic segment having a linker (R2) connecting its constituent units is shown in the following general formula (H3-1L), and a specific example of this ionic segment to which a linker (R1) has been introduced in the above step (1) is shown in general formula (H3-3L). However, the present invention is not limited to these. The steps of introducing the linker (R2) and the linker (R1) into the ionic segment can be carried out in a single reaction step.

[0140] [ka]

[0141] In the above general formulae (H3-1L) and (H3-3L), N5 and N6 each independently represent an integer of 1 to 200.

[0142] In the general formulae (H3-1) to (H3-4), (H3-1L) and (H3-3L), the halogen atom is represented by F, the terminal -OM group is represented by -OK group, and the alkali metal is represented by Na and K, but they can be used without being limited to these. In addition, these general formulae are inserted for the purpose of aiding the reader's understanding, and do not necessarily accurately represent the chemical structure, exact composition, arrangement, position, number and molecular weight of the polymerization components of the polymer, and are not limited to these.

[0143] Furthermore, in the general formulae (H3-1) to (H3-4), (H3-1L) and (H3-3L), a ketal group is introduced as a protecting group to each segment, but in the present invention, a protecting group may be introduced to a component having high crystallinity and low solubility. Therefore, the ionic segment does not necessarily require a protecting group, and from the viewpoint of mechanical durability, a segment without a protecting group can also be preferably used.

[0144] [Polymer electrolyte molded body] The polymer electrolyte material according to the embodiment of the present invention is suitable as a polymer electrolyte molded body. Here, the polymer electrolyte molded body means a molded body containing the polymer electrolyte material according to the embodiment of the present invention. Such polymer electrolyte molded bodies can take various forms depending on the application, such as membranes (including films and film-like ones), plates, fibers, hollow fibers, particles, blocks, microporous, coatings, foams, etc. Among these, membranes are preferable because they can be applied to a wide range of applications. Hereinafter, a membrane-type polymer electrolyte molded body is referred to as an "electrolyte molded membrane". The "electrolyte membrane" for evaluating the properties of the electrolyte material described above is included in the above "electrolyte molded membrane". Hereinafter, an electrolyte molded membrane will be described as a representative example of a polymer electrolyte molded body, but the present invention is not limited thereto.

[0145] Methods for producing an electrolyte membrane include a method for forming a membrane from a solution state at a stage where the electrolyte has a protecting group such as ketal, and a method for forming a membrane from a molten state. In the former method, for example, an electrolyte material is dissolved in a solvent such as N-methyl-2-pyrrolidone, and the solution is cast onto a glass plate or a polyethylene terephthalate film (hereinafter, PET film), and the solvent is removed to form a membrane.

[0146] The solvent used for membrane formation may be any solvent that dissolves the electrolyte material and can be subsequently removed, and examples of suitable solvents include aprotic polar solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, sulfolane, 1,3-dimethyl-2-imidazolidinone, and hexamethylphosphontriamide, ester solvents such as γ-butyrolactone and butyl acetate, carbonate solvents such as ethylene carbonate and propylene carbonate, alkylene glycol monoalkyl ethers such as ethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether, and alcohol solvents such as isopropanol, water, and mixtures thereof, but aprotic polar solvents are the most soluble and are preferred. In addition, in order to increase the solubility of the ionic segment, it is also suitable to add a crown ether such as 18-crown-6.

[0147] As a method for converting the polymer electrolyte material according to the embodiment of the present invention into an electrolyte molding membrane, for example, a membrane made of the electrolyte material is formed by the above-mentioned method, and then at least a part of the sites protected by the protecting groups is deprotected. For example, when the protecting group has a ketal site, at least a part of the ketone site protected by the ketal is deprotected to obtain a ketone site. This method enables solution membrane formation of a block copolymer with poor solubility.

[0148] In addition, after forming a membrane in a state in which the ionic groups contained therein form salts with cations of an alkali metal or an alkaline earth metal, a step of exchanging the cations of the alkali metal or the alkaline earth metal with protons may be carried out. This step is preferably a step of contacting the formed membrane with an acidic aqueous solution, and more preferably a step of immersing the formed membrane in the acidic aqueous solution. In this step, the protons in the acidic aqueous solution are replaced with cations ionically bonded to the ionic groups, and the remaining water-soluble impurities, remaining monomers, solvents, remaining salts, etc. are simultaneously removed.

[0149] The acidic aqueous solution is not particularly limited, but it is preferable to use sulfuric acid, hydrochloric acid, nitric acid, acetic acid, trifluoromethanesulfonic acid, methanesulfonic acid, phosphoric acid, citric acid, etc. The temperature, concentration, etc. of the acidic aqueous solution should also be appropriately determined, but from the viewpoint of productivity, it is preferable to use an aqueous sulfuric acid solution of 3 mass % or more and 30 mass % or less at a temperature of 0° C. or more and 80° C. or less.

[0150] The thickness of the electrolyte membrane in the present invention is preferably 1 μm or more, more preferably 2 μm or more, and particularly preferably 3 μm or more, from the viewpoint of mechanical durability. On the other hand, from the viewpoint of power generation performance, it is preferably 200 μm or less, more preferably 100 μm or less, and particularly preferably 50 μm or less. In particular, when the electrolyte membrane is applied to a fuel cell, the thickness is preferably less than 20 μm, more preferably less than 15 μm, and particularly preferably less than 10 μm, from the viewpoint of power generation performance. Thus, when the thickness of the electrolyte membrane is reduced, the mechanical durability is reduced, but the mechanical durability can be improved by using the polymer electrolyte material according to the embodiment of the present invention.

[0151] The electrolyte membrane may also contain additives such as crystallization nucleating agents, plasticizers, stabilizers, antioxidants, and release agents that are commonly used in polymer compounds, within the scope of the present invention.

[0152] The electrolyte membrane may contain various polymers, elastomers, fillers, fine particles, various additives, etc., for the purpose of improving mechanical strength, thermal stability, processability, etc., within the range that does not adversely affect the above-mentioned various properties. The electrolyte membrane may also be reinforced with a microporous membrane, a nonwoven fabric, a mesh, etc.

[0153] The electrolyte molded membrane can be applied to various applications. For example, it can be applied to medical applications such as artificial skin, filtration applications, ion exchange resin applications such as chlorine-resistant reverse osmosis membranes, various structural material applications, electrochemical applications, humidification membranes, anti-fogging membranes, antistatic membranes, oxygen removal membranes, solar cell membranes, and gas barrier membranes. Among them, it can be preferably used for various electrochemical applications. Examples of electrochemical applications include solid polymer fuel cells, redox flow batteries, water electrolysis devices, chloroalkali electrolysis devices, electrochemical hydrogen pumps, and water electrolysis hydrogen generation devices.

[0154] In a solid polymer electrolyte fuel cell, an electrochemical hydrogen pump, and a water electrolysis hydrogen generation device, an electrolyte membrane is used in a structure in which a catalyst layer, an electrode substrate, and a separator are laminated in sequence on both sides. Among these, an electrolyte membrane in which a catalyst layer is laminated on both sides (i.e., a layer structure of catalyst layer / electrolyte membrane / catalyst layer) is called a catalyst-coated electrolyte membrane (CCM), and an electrolyte membrane in which a catalyst layer and a gas diffusion substrate are laminated in sequence on both sides (i.e., a layer structure of gas diffusion substrate / catalyst layer / electrolyte membrane / catalyst layer / gas diffusion substrate) is called a membrane electrode assembly (MEA). The polymer electrolyte material according to the embodiment of the present invention is particularly suitable as an electrolyte membrane constituting such a CCM and MEA.

[0155] The electrolyte membrane can be produced, for example, by casting an electrolyte solution in which an electrolyte material is dissolved or dispersed in a suitable solvent onto a supporting substrate (such as a glass plate or a PET film) and drying the resulting electrolyte membrane. If necessary, the electrolyte membrane thus obtained is subjected to an acid treatment, washed with water, and dried. EXAMPLES

[0156] The present invention will be specifically described with reference to examples. However, the present invention is not limited to these examples. The measurement methods used in the examples are shown below. In the following measurement methods, when it is difficult to measure using a block copolymer or there is a concern about the measurement accuracy, the following electrolyte membranes were used as specimens instead of block copolymers.

[0157] <Preparation of electrolyte membrane (specimen)> A 25% by weight N-methylpyrrolidone (NMP) solution in which the block copolymer was dissolved was pressure filtered using a glass fiber filter, and then cast onto a glass substrate and dried for 4 hours at 100° C. to obtain a membrane. Next, this membrane was immersed in a 10% by weight aqueous sulfuric acid solution at 80° C. for 24 hours to cause proton substitution and deprotection reactions, and then immersed in a large excess of pure water for 24 hours for thorough washing to obtain an electrolyte membrane with a thickness of 8 μm.

[0158] (1) Molecular weight of the polymer The number average molecular weight and weight average molecular weight of the polymer were measured by GPC. The HLC-8022GPC manufactured by Tosoh Corporation was used as an integrated device of an ultraviolet detector and a differential refractometer, and the TSKgelGuardColumnSuperH-H (inner diameter 4.6 mm, length 3.5 cm) manufactured by Tosoh Corporation was used as a guard column. Two TSKgelSuperHM-H (inner diameter 6.0 mm, length 15 cm) manufactured by Tosoh Corporation were used as GPC columns. The measurements were performed in N-methyl-2-pyrrolidone solvent (N-methyl-2-pyrrolidone solvent containing 10 mmol / L lithium bromide) at a sample concentration of 0.1 wt%, a flow rate of 0.2 mL / min, a temperature of 40°C, and a measurement wavelength of 265 nm. The number average molecular weight and weight average molecular weight were calculated based on standard polystyrene.

[0159] (2) Ion exchange capacity (IEC) The measurements were performed using the neutralization titration method shown in 1) to 4) below. The measurements were performed three times and the average value was taken. 1) After the proton exchange and thorough washing with pure water, the water was wiped off from the block copolymer, which was then vacuum dried at 100°C for 12 hours or more, and the dry weight was determined. 2) 50 mL of a 5 wt % aqueous solution of sodium sulfate was added to the block copolymer, and the mixture was allowed to stand for 12 hours to carry out ion exchange. 3) The resulting sulfuric acid was titrated using 0.01 mol / L sodium hydroxide solution. 0.1 w / v% commercially available phenolphthalein solution for titration was added as an indicator, and the end point was when the solution turned a light reddish purple color. 4) IEC was calculated using the following formula. IEC (meq / g) = [concentration of sodium hydroxide solution (mmol / mL) × amount dropped (mL)] / dry weight of sample (g).

[0160] (3) Crystallization calorimetry by differential scanning calorimetry (DSC) 10 mg of the electrolyte membrane (specimen) was pre-dried in the DSC apparatus at 110°C for 3 hours, and then the specimen was heated to 200°C under the following conditions without being removed from the DSC apparatus, and a temperature-modulated differential scanning calorimetry analysis was performed during the heating stage. Measurement temperature range: 30℃~200℃ Temperature control: AC temperature control Heating rate: 2℃ / min ·Amplitude: ±3℃ ·Applied frequency: 0.02Hz Sample pan: Aluminum crimp pan Measurement and pre-drying atmosphere: Nitrogen 100mL / min.

[0161] (4) Crystallinity measurement by wide-angle X-ray diffraction (XRD) The electrolyte membrane (specimen) was set in a diffractometer and X-ray diffraction measurement was performed under the following conditions. X-ray diffraction equipment: Rigaku Corporation RINT2500V X-ray: Cu-Kα X-ray output: 50kV-300mA Optical system: Concentration optical system Scan speed: 2θ=2° / min Scan method: 2θ-θ Scan range: 2θ=5~60° Slits: Divergence slit-1 / 2°, receiving slit-0.15mm, scattering slit-1 / 2° The components were separated by profile fitting of the X-ray diffraction measurement results, and the diffraction angle and integrated intensity of each component were determined. The crystallinity was calculated from the obtained crystalline peak and the integrated intensity of the amorphous halo according to the following general formula (s2).

[0162] Crystallinity (%) = (sum of integrated intensities of all crystalline peaks) / (sum of integrated intensities of all crystalline peaks and amorphous halo) × 100···(s2).

[0163] (5) Observation of phase-separated structure using a transmission electron microscope (TEM) The phase separation structure was confirmed using an electrolyte membrane (specimen). A sample piece was immersed in a 2 wt% aqueous solution of lead acetate as a staining agent and left at 25°C for 72 hours. The stained sample was taken out and embedded in epoxy resin. An ultramicrotome was used to cut a thin section of 80 nm at room temperature, and the obtained thin section was collected on a Cu grid and subjected to TEM observation. Observation was performed at an accelerating voltage of 100 kV, and images were taken at a magnification of 10,000 to 100,000 times. The above magnification was appropriately set according to the size of the phase separation structure. The equipment used was HT7700 (manufactured by Hitachi High-Tech Corporation).

[0164] In addition, the TEM image was subjected to a fast Fourier transform (FFT), and the spatial frequency in the TD and ZD directions was measured from the obtained ring-shaped FFT pattern, from which the periodic size of the phase separation structure was calculated. The spatial frequency was measured as the distance from the center of the image to the center of the thickness of the ring. DigitalMicrograph (Gatan) was used for FFT and length measurement.

[0165] (6) Observation of phase-separated structures by transmission electron microscope (TEM) tomography The thin specimen prepared by the method described in (5) above was mounted on a collodion film and observed under the following conditions. Equipment: High-resolution field emission electron microscope (HRTEM) JEM 2100F manufactured by JEOL Ltd. Image acquisition: DigitalMicrograph (Gatan) System: Marker method Accelerating voltage: 200 kV Imaging magnification: 30,000 times Tilt angle: +60° to -62° Reconstruction resolution: 0.71 nm / pixel For the three-dimensional reconstruction process, the marker method was applied. As the alignment marker during the three-dimensional reconstruction, Au colloid particles deposited on the collodion film were used. Based on the marker, CT reconstruction processing was performed based on a total of 124 TEM images obtained from a series of continuous tilt images in which the sample was tilted at 1° intervals from +61° to -62° and TEM images were taken, and the three-dimensional phase separation structure was observed.

[0166] (7) Evaluation of power generation performance In evaluating the power generation performance, a catalyst-coated electrolyte membrane (CCM) and a membrane electrode assembly (MEA) were fabricated in the following manner.

[0167] <Fabrication of CCM> An anode catalyst decal was overlaid on one surface of the electrolyte membrane, and a cathode catalyst decal was overlaid on the other surface, followed by heat pressing at 150 °C and 5 MPa for 3 minutes for bonding. Thereafter, the polytetrafluoroethylene films of the respective catalyst decals were peeled off to obtain a CCM.

[0168] <Fabrication of anode catalyst decal> 10 parts by mass of platinum catalyst-supported carbon particles TEC10E50E (platinum loading rate 50% by mass) manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. and 5 parts by mass in terms of solid content of a fluorine-based polymer electrolyte (“Nafion” (registered trademark) manufactured by Chemours Co., Ltd.) were dispersed using a bead mill in a mixed solvent (mass ratio of water to 1-propyl alcohol 4:6) to prepare Catalyst Ink 1 with a solid content concentration of 10% by mass. This Catalyst Ink 1 was applied to a commercially available polytetrafluoroethylene film and dried to fabricate an anode catalyst decal. The platinum amount in the catalyst layer was 0.4 mg / cm 2 was.

[0169] <Fabrication of cathode catalyst decal> The platinum amount in the catalyst layer was 0.7 mg / cm 2It was prepared in the same manner as the anode catalyst decal, except that it was changed to

[0170] <Fabrication of MEA> A commercially available gas diffusion layer 24BCH manufactured by SGL was overlaid on both sides of the CCM prepared above, and heat pressing was performed at 160 °C and 4.5 Ma for 5 minutes to fabricate an MEA. Using this MEA, the power generation performance was evaluated in the following manner.

[0171] <Evaluation of Power Generation Performance> The MEA was set in a JARI standard cell "Ex-1" manufactured by Eiwa Corporation (electrode area 25 cm 2 ) to form a power generation evaluation module. Hydrogen gas was supplied as a fuel gas to the anode electrode, and air was supplied as an oxidizing gas to the cathode electrode. Power generation evaluation was performed under the following conditions, and the current was swept from 0 A / cm 2 to 1.2 A / cm 2 until the voltage reached 0.2 V or less. In the present invention, the voltage at a current density of 1.2 A / cm 2 was read and evaluated. Electronic load device; Electronic load device "PLZ664WA" manufactured by Kikusui Electronics Industry Co., Ltd. Cell temperature; 80 °C Relative humidity of the supplied gas (hydrogen gas and air); 30% RH Back pressure of the supplied gas (hydrogen gas and air): 150 kPa Gas utilization rate; 70% of stoichiometry for the anode and 40% of stoichiometry for the cathode. From the viewpoint of obtaining good power generation performance under low humidity conditions, the power generation voltage measured above is preferably 0.58 V or more, more preferably 0.60 V or more, and particularly preferably 0.61 V or more.

[0172] (8) Dry and wet dimensional change rate The electrolyte membrane (specimen) was cut into a rectangle of 3 mm x 20 mm to prepare a sample piece. The long side of the sample piece was placed in the sample holder of a thermomechanical analyzer TMA / SS6100 (manufactured by Hitachi High-Tech Science Co., Ltd.) with a furnace with temperature and humidity control function so that the measurement direction was the direction of measurement, and a stress of 20 mN was applied. The sample was stabilized in the furnace at 23°C and 50% RH for 1 hour, and the length of the sample piece was set as the zero point. The temperature inside the furnace was fixed at 23°C, and the humidity was adjusted to 30% RH (dry condition) over 30 minutes and held for 30 minutes. Next, the humidity was adjusted to 90% RH (humidified condition) over 30 minutes and held for 30 minutes. This dry-wet cycle (30% RH-90% RH) was considered as one cycle, and the difference between the dimensional change rate (%) at 30% RH and the dimensional change rate (%) at 90% RH in the 10th cycle was taken as the dry-wet dimensional change rate (%). From the viewpoint of obtaining excellent mechanical durability, the wet / dry dimensional change rate measured above is preferably 5.0% or less, more preferably 4.5% or less, and particularly preferably 4.2% or less.

[0173] [Polymer synthesis] The structures of the compounds obtained in the following synthesis examples are 1 The purity was confirmed by H-NMR, and quantitative analysis was performed by capillary electrophoresis (organic substances) and ion chromatography (inorganic substances).

[0174] <Synthesis Example 1> (Synthesis of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane (K-DHBP) represented by the following formula (G1)) In a 500 mL flask equipped with a stirrer, a thermometer, and a distillation tube, 49.5 g of 4,4'-dihydroxybenzophenone, 134 g of ethylene glycol, 96.9 g of trimethyl orthoformate, and 0.50 g of p-toluenesulfonic acid monohydrate were charged to obtain a solution. The mixture was then stirred at 78-82°C for 2 hours. The internal temperature was gradually raised to 120°C, and kept at 120°C until the distillation of methyl formate, methanol, and trimethyl orthoformate completely stopped. After cooling the reaction solution to room temperature, the reaction solution was diluted with ethyl acetate. The organic layer was washed with 100 mL of a 5% aqueous potassium carbonate solution and separated, and the solvent was distilled off. 80 mL of dichloromethane was added to the residue to precipitate crystals, which were filtered and dried to obtain 52.0 g of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane. The purity was 99.9%.

[0175] [ka]

[0176] <Synthesis Example 2> (Synthesis of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone represented by the following formula (G2)) 109.1g of 4,4'-difluorobenzophenone (Aldrich reagent) was reacted in 150mL of fuming sulfuric acid (50% SO3) (Wako Pure Chemicals reagent) at 100℃ for 10 hours. After that, it was poured little by little into a large amount of water, neutralized with NaOH, and then 200g of table salt (NaCl) was added to precipitate the synthesized product. The resulting precipitate was filtered and recrystallized with an ethanol aqueous solution to obtain disodium-3,3'-disulfonate-4,4'-difluorobenzophenone. The purity was 99.3%.

[0177] [ka]

[0178] <Synthesis Example 3> (Synthesis of 3,3'-disulfonic acid sodium salt-4,4'-difluorodiphenyl sulfone represented by the following formula (G3)) 109.1g of 4,4-difluorodiphenylsulfone (Aldrich reagent) was reacted in 150mL of fuming sulfuric acid (50% SO3) (Wako Pure Chemicals reagent) at 100℃ for 10 hours. After that, it was poured little by little into a large amount of water, neutralized with NaOH, and then 200g of salt was added to precipitate the synthesized product. The resulting precipitate was filtered and recrystallized with an ethanol aqueous solution to obtain 3,3'-disulfonic acid sodium salt-4,4'-difluorodiphenylsulfone. The purity was 99.3%.

[0179] [ka]

[0180] [Example 1] <Synthesis of nonionic oligomer a1 represented by the following general formula (G4)> In a 2,000 mL SUS polymerization apparatus equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 16.59 g of potassium carbonate (Aldrich reagent, 120 mmol), 25.83 g (100 mmol) of K-DHBP obtained in Synthesis Example 1, and 21.47 g of 4,4'-difluorobenzophenone (Aldrich reagent, 98 mmol) were placed. After replacing the atmosphere in the apparatus with nitrogen, 300 mL of N-methylpyrrolidone (NMP) and 100 mL of toluene were added, and the mixture was dehydrated at 150°C, heated to remove toluene, and polymerized at 170°C for 3 hours. The mixture was purified by reprecipitation in a large amount of methanol to obtain a terminal hydroxyl group of nonionic oligomer a1. The number average molecular weight of the terminal hydroxyl group of this nonionic oligomer a1 was 27,000.

[0181] In a 500 mL three-neck flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 1.1 g of potassium carbonate (Aldrich reagent, 8 mmol) and 27.0 g (1 mmol) of the terminal hydroxyl group of the nonionic oligomer a1 were placed. After replacing the inside of the apparatus with nitrogen, 100 mL of NMP and 30 mL of toluene were added, and the mixture was dehydrated at 100°C, and then heated to remove the toluene. Furthermore, 1.1 g of hexafluorobenzene (Aldrich reagent, 6 mmol) was placed, and the reaction was carried out at 105°C for 12 hours. The mixture was purified by reprecipitation with a large amount of isopropyl alcohol to obtain a nonionic oligomer a1 (terminal: fluoro group) represented by the following general formula (G4). The number average molecular weight of this nonionic oligomer a1 was 28,000. In addition, in the general formula (G4), m represents an integer of 1 or more.

[0182] [ka]

[0183] <Synthesis of ionic oligomer a2 represented by the following general formula (G5)> In a 2,000 mL SUS polymerization apparatus equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 27.64 g of potassium carbonate (Aldrich reagent, 200 mmol), 12.91 g (50 mmol) of K-DHBP obtained in Synthesis Example 1, 9.31 g (Aldrich reagent, 50 mmol) of 4,4'-biphenol, 41.64 g (98.6 mmol) of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone obtained in Synthesis Example 2, and 26.40 g (100 mmol) of 18-crown-6 were placed. After replacing the inside of the apparatus with nitrogen, 300 mL of NMP and 100 mL of toluene were added, and the mixture was dehydrated at 150°C, heated to remove toluene, and polymerization was carried out at 170°C for 6 hours. The product was purified by reprecipitation with a large amount of isopropyl alcohol to obtain an ionic oligomer a2 (terminal: OM group) represented by the following general formula (G5). The number average molecular weight of this ionic oligomer a2 was 46,000. In the general formula (G5), M represents a hydrogen atom, Na or K, and n represents an integer of 1 or more.

[0184] [ka]

[0185] <Synthesis of ionic oligomer a2' represented by the following general formula (G6)> 0.56g of potassium carbonate (Aldrich reagent, 400mmol) and 49.0g of ionic oligomer a2 were placed in a 2,000mL SUS polymerization apparatus equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap. After replacing the atmosphere in the apparatus with nitrogen, 500mL of NMP was added, and the contents were dissolved at 60°C, and then 19.8g of hexafluorobenzene / NMP solution (1wt%) was added. The reaction was carried out at 80°C for 18 hours to obtain an NMP solution containing ionic oligomer a2' (terminal: OM group) represented by general formula (G6). The number average molecular weight of this ionic oligomer a2' was 92,000. In addition, in general formula (G6), M represents a hydrogen atom, Na or K, and n represents an integer of 1 or more.

[0186] [ka]

[0187] <Synthesis of block copolymer b1> The block copolymer b1 contains the above oligomer a2' as an ionic segment and the above oligomer a1 as a non-ionic segment.

[0188] 49.0 g of ionic oligomer a2' and 8.17 g of nonionic oligomer a1 were placed in a 2,000 mL SUS polymerization apparatus equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap, and NMP was added so that the total amount of oligomers was 7 wt%, and the reaction was carried out at 105 ° C. for 24 hours. Reprecipitation was carried out in a large amount of isopropyl alcohol / NMP mixed liquid (weight ratio 2 / 1), and purification was carried out with a large amount of isopropyl alcohol to obtain a block copolymer b1. The number average molecular weight of this block copolymer was 160,000, and the weight average molecular weight was 420,000.

[0189] The IEC of block copolymer b1 was 2.3 meq / g. The electrolyte membrane prepared using block copolymer b1 was confirmed to have a bicontinuous phase-separated structure (hydrophilic domains containing ionic groups and hydrophobic domains not containing ionic groups both formed a continuous phase). The average periodic size of the phase-separated structure was 83 nm. A crystallization peak was observed by DSC, and the heat of crystallization was 14.8 J / g. Furthermore, no crystalline peak was observed by wide-angle X-ray diffraction (crystallinity 0%). In other words, block copolymer b1 is crystalline.

[0190] [Example 2] <Synthesis of nonionic oligomer a3 represented by the above general formula (G4)> The terminal hydroxy compound of oligomer a3 was obtained in the same manner as in the synthesis of the terminal hydroxy compound of oligomer a1, except that the amount of 4,4'-difluorobenzophenone used was 21.51 g. The number average molecular weight of the terminal hydroxy compound of oligomer a3 was 29,000.

[0191] A nonionic oligomer a3 (terminal: fluoro group) represented by the general formula (G4) was obtained in the same manner as in the synthesis of oligomer a1, except that 29.0 g of the terminal hydroxy group of oligomer a3 was used instead of the terminal hydroxy group of oligomer a1. The number average molecular weight of this nonionic oligomer a3 was 30,000.

[0192] <Synthesis of ionic oligomer a4 represented by the above general formula (G5)> Ionic oligomer A4 was obtained in the same manner as in the synthesis of ionic oligomer A2, except that the amount of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone used was 41.38 g (98.0 mmol). The number average molecular weight of this ionic oligomer A4 was 35,000.

[0193] <Synthesis of ionic oligomer a4' represented by the following general formula (G7)> 0.56g of potassium carbonate (Aldrich reagent, 400mmol) and 37.16g of ionic oligomer a4 were placed in a 2,000mL SUS polymerization apparatus equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap. After replacing the atmosphere in the apparatus with nitrogen, 400mL of NMP was added, and the contents were dissolved at 60°C, and then 11.4g of 2,6-difluorobenzonitrile / NMP solution (1wt%) was added. The reaction was carried out at 80°C for 18 hours to obtain an NMP solution containing ionic oligomer a4' (terminal: OM group) represented by general formula (G7). The number average molecular weight of this ionic oligomer a4' was 70,000. In addition, in general formula (G7), M represents a hydrogen atom, Na or K, and n represents an integer of 1 or more.

[0194] [ka]

[0195] <Synthesis of block copolymer 2> The block copolymer b2 contains the above oligomer a4' as an ionic segment and the above oligomer a3 as a non-ionic segment.

[0196] Block copolymer b2 was obtained in the same manner as block copolymer b1, except that ionic oligomer a4' (40.89 g) was used instead of ionic oligomer a2' (49.0 g) and nonionic oligomer a3 (12.39 g) was used instead of nonionic oligomer a1 (7.65 g). The number average molecular weight of this block copolymer was 160,000 and the weight average molecular weight was 390,000.

[0197] The IEC of block copolymer b2 was 2.0 meq / g. The electrolyte membrane prepared using block copolymer b2 was confirmed to have a bicontinuous phase-separated structure (hydrophilic domains containing ionic groups and hydrophobic domains not containing ionic groups both formed a continuous phase). The average periodic size of the phase-separated structure was 79 nm. A crystallization peak was observed by DSC, and the heat of crystallization was 17.8 J / g. Furthermore, no crystalline peak was observed by wide-angle X-ray diffraction (crystallinity 0%). In other words, block copolymer b2 is crystalline.

[0198] [Example 3] <Synthesis of nonionic oligomer a5 represented by the above general formula (G4)> The terminal hydroxy compound of oligomer a5 was obtained in the same manner as in the synthesis of the terminal hydroxy compound of oligomer a1, except that the amount of 4,4'-difluorobenzophenone used was 21.43 g. The number average molecular weight of the terminal hydroxy compound of oligomer a5 was 25,000.

[0199] A nonionic oligomer a5 (terminal: fluoro group) represented by the general formula (G4) was obtained in the same manner as in the synthesis of oligomer a1, except that 25.0 g of the terminal hydroxy group of oligomer a5 was used instead of the terminal hydroxy group of oligomer a1. The number average molecular weight of this nonionic oligomer a5 was 26,000.

[0200] <Synthesis of block copolymer b3> The block copolymer b3 contains the above oligomer a2' as an ionic segment and the above oligomer a5 as a non-ionic segment.

[0201] Block copolymer b3 was obtained in the same manner as block copolymer b1, except that nonionic oligomer a5 (12.25 g) was used instead of nonionic oligomer a1 (7.65 g). The number average molecular weight of this block copolymer was 150,000 and the weight average molecular weight was 380,000.

[0202] The IEC of block copolymer b3 was 2.1 meq / g. The electrolyte membrane prepared using block copolymer b3 was confirmed to have a bicontinuous phase-separated structure (hydrophilic domains containing ionic groups and hydrophobic domains not containing ionic groups both formed a continuous phase). The average periodic size of the phase-separated structure was 62 nm. A crystallization peak was observed by DSC, and the heat of crystallization was 15.7 J / g. In addition, no crystalline peak was observed by wide-angle X-ray diffraction (crystallinity 0%). In other words, block copolymer b3 is crystalline.

[0203] [Example 4] <Synthesis of nonionic oligomer a6 represented by the above general formula (G4)> The terminal hydroxy compound of oligomer a6 was obtained in the same manner as in the synthesis of the terminal hydroxy compound of oligomer a1, except that the amount of 4,4'-difluorobenzophenone used was 21.55 g. The number average molecular weight of the terminal hydroxy compound of oligomer a6 was 34,000.

[0204] A nonionic oligomer a6 (terminal: fluoro group) represented by the general formula (G4) was obtained in the same manner as in the synthesis of oligomer a1, except that 34.0 g of the terminal hydroxy group of oligomer a6 was used instead of the terminal hydroxy group of oligomer a1. The number average molecular weight of this nonionic oligomer a6 was 35,000.

[0205] <Synthesis of block copolymer b4> The block copolymer b4 contains the above oligomer a4' as an ionic segment and the above oligomer a6 as a non-ionic segment.

[0206] Block copolymer B4 was obtained in the same manner as block copolymer B1, except that ionic oligomer A4' (35.58 g) was used instead of ionic oligomer A2' (49.0 g) and nonionic oligomer A6 (14.23 g) was used instead of nonionic oligomer A1 (7.65 g). The number average molecular weight of this block copolymer was 160,000 and the weight average molecular weight was 400,000.

[0207] The IEC of block copolymer b4 was 1.9 meq / g. The electrolyte membrane prepared using block copolymer b4 was confirmed to have a bicontinuous phase-separated structure (hydrophilic domains containing ionic groups and hydrophobic domains not containing ionic groups both formed a continuous phase). The average periodic size of the phase-separated structure was 77 nm. A crystallization peak was observed by DSC, and the heat of crystallization was 19.4 J / g. In addition, no crystalline peak was observed by wide-angle X-ray diffraction (crystallinity 0%). In other words, block copolymer b4 is crystalline.

[0208] [Comparative Example 1] <Synthesis of nonionic oligomer a7 represented by the above general formula (G4)> The terminal hydroxy compound of oligomer a7 was obtained in the same manner as in the synthesis of the terminal hydroxy compound of oligomer a1, except that the amount of 4,4'-difluorobenzophenone used was 21.27 g. The number average molecular weight of the terminal hydroxy compound of oligomer a7 was 17,000.

[0209] A nonionic oligomer a7 (terminal: fluoro group) represented by the general formula (G4) was obtained in the same manner as in the synthesis of oligomer a1, except that 17.0 g of the terminal hydroxy group of oligomer a7 was used instead of the terminal hydroxy group of oligomer a1. The number average molecular weight of this nonionic oligomer a7 was 18,000.

[0210] <Synthesis of ionic oligomer a8 represented by the above general formula (G5)> Ionic oligomer A8 was obtained in the same manner as in the synthesis of ionic oligomer A2, except that the amount of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone used was 41.6 g (98.5 mmol). The number average molecular weight of this ionic oligomer A8 was 40,000.

[0211] <Synthesis of ionic oligomer a8' represented by the above general formula (G7)> In a 2,000 mL SUS polymerization apparatus equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap, 0.56 g of potassium carbonate (Aldrich reagent, 400 mmol) and 49.00 g of ionic oligomer a8 were placed. After replacing the atmosphere in the apparatus with nitrogen, 400 mL of NMP was added, and the contents were dissolved at 60°C, and then 11.4 g of 2,6-difluorobenzonitrile / NMP solution (1 wt%) was added. The reaction was carried out at 80°C for 18 hours to obtain an NMP solution containing ionic oligomer a4' (terminal: OM group) represented by general formula (G7). The number average molecular weight of this ionic oligomer a8' was 80,000.

[0212] <Synthesis of block copolymer b5> The block copolymer b5 contains the above oligomer a8' as an ionic segment and the above oligomer a7 as a non-ionic segment.

[0213] A block copolymer b5 was obtained in the same manner as in Example 1, except that the nonionic oligomer a1 was changed to a7 and its amount was changed to 5.57 g. The number average molecular weight of this block copolymer was 140,000 and the weight average molecular weight was 360,000.

[0214] The IEC of block copolymer B5 was 2.6 meq / g. The electrolyte membrane prepared using block copolymer B4 was confirmed to have a bicontinuous phase-separated structure (hydrophilic domains containing ionic groups and hydrophobic domains not containing ionic groups both formed a continuous phase). The average periodic size of the phase-separated structure was 61 nm. A crystallization peak was observed by DSC, and the heat of crystallization was 10.1 J / g. In addition, no crystalline peak was observed by wide-angle X-ray diffraction (crystallinity 0%). In other words, block copolymer B5 is crystalline.

[0215] [Comparative Example 2] <Synthesis of nonionic oligomer a9 represented by the above general formula (G4)> The terminal hydroxy compound of oligomer a9 was obtained in the same manner as in the synthesis of the terminal hydroxy compound of oligomer a1, except that the amount of 4,4'-difluorobenzophenone used was 21.25 g. The number average molecular weight of the terminal hydroxy compound of oligomer a9 was 16,000.

[0216] A nonionic oligomer a9 (terminal: fluoro group) represented by the general formula (G4) was obtained in the same manner as in the synthesis of oligomer a1, except that 17.0 g of the terminal hydroxy group of oligomer a9 was used instead of the terminal hydroxy group of oligomer a1. The number average molecular weight of this nonionic oligomer a9 was 17,000.

[0217] <Synthesis of ionic oligomer a10 represented by the above general formula (G5)> Ionic oligomer A10 was obtained in the same manner as in the synthesis of ionic oligomer A2, except that the amount of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone used was 41.30 g (97.8 mmol). The number average molecular weight of this ionic oligomer A10 was 30,000.

[0218] <Synthesis of ionic oligomer a10' represented by the above general formula (G6)> An NMP solution containing an ionic oligomer a10' (terminal: OM group) represented by the general formula (G6) was obtained in the same manner as in the synthesis of the ionic oligomer a2', except that the ionic oligomer a24' was replaced with the ionic oligomer a10 (37.16 g), the amount of NMP used was 400 mL, and the amount of hexafluorobenzene / NMP solution (1 wt%) used was 15.3 g. The number average molecular weight of this oligomer a24' was 60,000.

[0219] <Synthesis of block copolymer b6> The block copolymer b6 contains the above oligomer a10' as an ionic segment and the above oligomer a9 as a non-ionic segment.

[0220] Block copolymer b6 was obtained in the same manner as in the synthesis of block copolymer b1, except that ionic oligomer a10' (37.16 g) was used instead of ionic oligomer a2' (49.0 g) and nonionic oligomer a9 (5.80 g) was used instead of nonionic oligomer a1 in a 2,000 mL SUS polymerization apparatus equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap. The number average molecular weight of this block copolymer was 130,000, and the weight average molecular weight was 340,000.

[0221] The IEC of the block copolymer b6 was 2.3 meq / g. The electrolyte membrane prepared using the block copolymer b6 was confirmed to have a bicontinuous phase-separated structure (hydrophilic domains containing ionic groups and hydrophobic domains not containing ionic groups both formed a continuous phase). The average periodic size of the phase-separated structure was 52 nm. A crystallization peak was observed by DSC, and the heat of crystallization was 16.2 J / g. In addition, no crystalline peak was observed by wide-angle X-ray diffraction (crystallinity 0%). In other words, the block copolymer b6 has crystallinity.

[0222] [Comparative Example 3] <Synthesis of nonionic oligomer a11 represented by the following general formula (G8)> A nonionic oligomer a11 (terminal: fluoro group) represented by the general formula (G8) was obtained in the same manner as in the synthesis of the terminal hydroxyl form of the nonionic oligomer a1, except that the amount of K-DHBP used was 25.22 g and the amount of 4,4'-difluorobenzophenone used was 21.82 g. The number average molecular weight of this ionic oligomer a11 was 17,000.

[0223] [ka]

[0224] <Synthesis of ionic oligomer a12 represented by the above general formula (G5)> In a 2,000 mL SUS polymerization apparatus equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 27.64 g of potassium carbonate (Aldrich reagent, 200 mmol), 12.91 g (50 mmol) of K-DHBP obtained in Synthesis Example 1, 9.31 g (Aldrich reagent, 50 mmol) of 4,4'-biphenol, 41.47 g (98.2 mmol) of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone obtained in Synthesis Example 2, and 26.40 g (100 mmol) of 18-crown-6 were placed. After replacing the inside of the apparatus with nitrogen, 300 mL of NMP and 100 mL of toluene were added, and the mixture was dehydrated at 150°C, heated to remove toluene, and polymerization was carried out at 170°C for 6 hours. The ionic oligomer a12 (terminal: hydroxy group) represented by formula (G5) was obtained by reprecipitation with a large amount of isopropyl alcohol, and the number average molecular weight of the ionic oligomer a12 was 42,000.

[0225] <Synthesis of block copolymer b7> Block copolymer b7 contains oligomer a12 as an ionic segment and oligomer a11 as a non-ionic segment.

[0226] 43.57g of ionic oligomer a12 and 10.89g of nonionic oligomer a11 were placed in a 2,000mL SUS polymerization apparatus equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap, and NMP was added so that the total amount of oligomers was 21wt%, and the reaction was carried out at 180°C for 24 hours. Reprecipitation was carried out in a large amount of isopropyl alcohol / NMP mixed liquid (weight ratio 2 / 1), and purification was carried out with a large amount of isopropyl alcohol to obtain block copolymer b7. The number average molecular weight of this block copolymer was 90,000, and the weight average molecular weight was 210,000.

[0227] The IEC of block copolymer b7 was 2.1 meq / g. An island-like phase-separated structure was confirmed in the electrolyte membrane prepared using the block copolymer b7. The average periodic size of the phase-separated structure was 120 nm. A crystallization peak was observed by DSC, and the heat of crystallization was 3.6 J / g. Furthermore, no crystalline peak was observed by wide-angle X-ray diffraction (crystallinity 0%). In other words, block copolymer b7 is crystalline.

[0228] [Comparative Example 4] <Synthesis of nonionic oligomer a13 represented by the following general formula (G9)> A terminal hydroxyl group of nonionic oligomer a13 was obtained in the same manner as in the synthesis of the terminal hydroxyl group of nonionic oligomer a1, except that 23.65 g of 4,4-difluorodiphenyl sulfone was used instead of 4,4'-difluorobenzophenone. The number average molecular weight of the terminal hydroxyl group of nonionic oligomer a13 was 10,000.

[0229] A nonionic oligomer a13 (terminal fluoro group) represented by general formula (G9) was obtained in the same manner as in the synthesis of nonionic oligomer a1, except that 10.0 g of the terminal hydroxyl group of nonionic oligomer a13 was used instead of 20.0 g of the terminal hydroxyl group of nonionic oligomer a1. The number average molecular weight of this nonionic oligomer a13 was 11,000. In addition, in general formula (G9), m represents an integer of 1 or more.

[0230] [ka]

[0231] <Synthesis of ionic oligomer a14 represented by the following general formula (G10)> An ionic oligomer a14 (terminal: OM group) represented by general formula (G10) was obtained in the same manner as in the synthesis of ionic oligomer a2, except that 44.94 g (98.1 mmol) of 3,3'-disulfonic acid sodium salt-4,4'-difluorodiphenyl sulfone obtained in Synthesis Example 3 was used instead of 41.60 g of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone. The number average molecular weight of this ionic oligomer a14 was 41,000. In addition, in general formula (G10), M represents a hydrogen atom, Na or K, and n represents an integer of 1 or more.

[0232] [ka]

[0233] <Synthesis of block copolymer b8> The block copolymer b8 contains the above oligomer a14 as an ionic segment and the above oligomer a13 as a non-ionic segment.

[0234] Ionic oligomer a14 (45.76 g) and nonionic oligomer a13 (8.93 g) were placed in a 2,000 mL SUS polymerization apparatus equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap, and NMP was added so that the total amount of oligomers was 7 wt%, and the reaction was carried out at 105 ° C. for 24 hours. Reprecipitation was carried out in a large amount of isopropyl alcohol / NMP mixed liquid (weight ratio 2 / 1), and purification was carried out with a large amount of isopropyl alcohol to obtain block copolymer b8. The number average molecular weight of this block copolymer b8 was 120,000, and the weight average molecular weight was 290,000.

[0235] The IEC of block copolymer b8 was 2.4 meq / g. A bicontinuous phase-separated structure was confirmed in the electrolyte membrane prepared using the block copolymer b8. The average periodic size of the phase-separated structure was 32 nm. No crystallization peak was observed by DSC (heat of crystallization 0 J / g). Furthermore, no crystalline peak was observed by wide-angle X-ray diffraction (degree of crystallinity 0%). In other words, block copolymer b8 does not have crystallinity.

[0236] [Comparative Example 5] <Synthesis of polyethersulfone (PES) block copolymer precursor bp> 1.62 g of anhydrous nickel chloride and 15 mL of dimethyl sulfoxide were mixed and adjusted to 70° C. 2.15 g of 2,2′-bipyridyl was added thereto and stirred at the same temperature for 10 minutes to prepare a nickel-containing solution.

[0237] Here, 1.49 g of 2,5-dichlorobenzenesulfonic acid (2,2-dimethylpropyl) and 0.50 g of "Sumikaexcel" (registered trademark) PES5200P (manufactured by Sumitomo Chemical Co., Ltd., Mn = 40,000, Mw = 94,000) represented by the following formula (G11) were dissolved in 5 mL of dimethyl sulfoxide to obtain a solution, to which 1.23 g of zinc powder was added and adjusted to 70 ° C. The nickel-containing solution was poured into this, and a polymerization reaction was carried out at 70 ° C. for 4 hours. The reaction mixture was added to 60 mL of methanol, and then 60 mL of 6 mol / L hydrochloric acid was added and stirred for 1 hour. The precipitated solid was separated by filtration and dried, and a precursor bp containing segments represented by the following formula (G12) and the following formula (G13) was obtained in a yield of 99%.

[0238] [ka]

[0239] <Synthesis of polyethersulfone (PES)-based block copolymer b9> 0.23 g of the precursor bp was added to a mixed solution of 0.16 g of lithium bromide monohydrate and 8 mL of NMP, and reacted at 120° C. for 24 hours. The reaction mixture was poured into 80 mL of 6 mol / L hydrochloric acid and stirred for 1 hour. The precipitated solid was separated by filtration. The separated solid was dried to obtain a gray-white PES block copolymer b9 consisting of a segment represented by the above general formula (G13) and a segment represented by the following chemical formula (G14). The weight-average molecular weight of this PES block copolymer was 180,000.

[0240] [ka]

[0241] The IEC of the PES block copolymer b9 was 2.1 meq / g. A bicontinuous phase-separated structure was confirmed in the electrolyte membrane prepared using the block copolymer b9. The average periodic size of the phase-separated structure was 60 nm. No crystallization peak was observed by DSC (heat of crystallization 0 J / g). Furthermore, no crystalline peak was observed by wide-angle X-ray diffraction (degree of crystallinity 0%). In other words, the PES block copolymer b8 does not have crystallinity.

[0242] [Measurement results] Table 1 shows the measurement results of the electrolyte materials obtained in the examples and comparative examples.

[0243] [Table 1]

[0244] In the table, "Mn1", "Mn2", and "Mn3" represent the number average molecular weights of the ionic segment, nonionic segment, and block copolymer, respectively, and "Mw" represents the weight average molecular weight of the block copolymer. [Explanation of symbols]

[0245] 1 phase 1 2 phase 2

Claims

1. A polymer electrolyte material comprising a block copolymer having a segment containing an ionic group (hereinafter referred to as an "ionic segment") and a segment not containing an ionic group (hereinafter referred to as a "nonionic segment"), the polymer electrolyte material having an ion exchange capacity of 2.4 meq / g or less and satisfying both of the following conditions 1 and 2: <Condition 1> The heat of crystallization of the polymer electrolyte material measured by differential scanning calorimetry (DSC) is 0.1 J / g or more, or the degree of crystallinity of the polymer electrolyte material measured by wide-angle X-ray diffraction is 0.5% or more. <Condition 2> The polymer electrolyte material has a phase-separated structure, and the average periodic size of the phase-separated structure observed with a transmission electron microscope is 60 nm or more and less than 110 nm.

2. The polymer electrolyte material according to claim 1 , wherein the phase-separated structure is bicontinuous or lamellar.

3. The polymer electrolyte material according to claim 1 , wherein the ionic segment and the nonionic segment comprise an aromatic polyether ketone-based polymer.

4. The polymer electrolyte material according to claim 1 , wherein the ionic segment contains a structure represented by the following general formula (S1): 【Chemistry 1】 (In general formula (S1), Ar 1 ~Ar 4 each independently represents a substituted or unsubstituted arylene group; Ar 1 ~Ar 4 At least one of Y has an ionic group. 1 and Y 2 each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to general formula (S1) or another structural unit.

5. The polymer electrolyte material according to claim 4 , wherein the structure represented by the general formula (S1) is a structure represented by the following general formula (S2): 【Chemistry 2】 (In general formula (S2), Y 1 and Y 2 each independently represents a ketone group or a protecting group that can be derived to a ketone group. M 1 ~M 4 Each of n independently represents a hydrogen atom, a metal cation, or an ammonium cation. 1 ~n 4 are each independently 0 or 1; 1 ~n 4 At least one of the is 1. * represents a bond to the general formula (S2) or another structural unit.)

6. The polymer electrolyte material according to claim 1 , wherein the nonionic segment contains a structure represented by the following general formula (S3): 【Chemistry 3】 (In general formula (S3), Ar 5 ~Ar 8 each independently represents a substituted or unsubstituted arylene group. 5 ~Ar 8 None of Y has an ionic group. 3 and Y 4 each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to general formula (S3) or another structural unit.

7. The polymer electrolyte material according to claim 6 , wherein the structure represented by the general formula (S3) is a structure represented by the following general formula (S4): 【Chemistry 4】 (In general formula (S4), Y 3 and Y 4 each independently represents a ketone group or a protecting group that can be derived to a ketone group. * represents a bond to general formula (S4) or another structural unit.

8. The polymer electrolyte material according to claim 1 , wherein the block copolymer has a linker moiety connecting between the ionic segment and the non-ionic segment.

9. A polymer electrolyte molded product comprising the polymer electrolyte material according to any one of claims 1 to 8.

10. A catalyst layer-attached electrolyte membrane formed using the polymer electrolyte molded product according to claim 9.

11. A membrane electrode assembly formed using the polymer electrolyte molded product according to claim 9.

12. A solid polymer fuel cell constructed using the polymer electrolyte molded product according to claim 9.

13. A water electrolysis hydrogen generating device comprising the polymer electrolyte molded product according to claim 9.

Citation Information

Patent Citations

  • POLYMER ELECTROLYTE COMPOSITION, POLYMER ELECTROLYTE MEMBRANE USING THE SAME, ELECTROLYTE MEMBRANE WITH CATALYST LAYER, MEMBRANE ELECTRODE COMPOSITE, SOLID POLYMER FUEL CELL, SOLID POLYMER WATER ELECTROLYSIS HYDROGEN GENERATOR AND ELECTROCHEMICAL HYDROGEN COMPRESSOR, AND PRODUCTION METHOD OF POLYMER ELECTROLYtE COMPOSITION

    JP2018110108A

  • Polymer electrolyte membrane, electrolyte membrane with catalyst layer using the same, membrane electrode composite, polymer electrolyte fuel cell, and water electrolysis type hydrogen generator

    JP2022167820A

  • Polymer electrolyte membrane, membrane electrode assembly using same, and solid polymer fuel cell

    WO2013031675A1

  • Polymer electrolyte material, polymer electrolyte molded product using the polymer electrolyte material and method for manufacturing the polymer electrolyte molded product, membrane electrode composite, and solid polymer fuel cell

    WO2008018487A1