Method for producing modified cross-section acrylic fiber

The method of solution polymerization in organic solvents with controlled discharge into a coagulation bath addresses productivity and yellowing issues, resulting in high-quality acrylic fibers with irregular cross-sections and enhanced texture.

JP2024136655AInactive Publication Date: 2024-10-04TORAY INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023047838
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing acrylic fibers with irregular cross-sections face issues of low productivity, yellowing due to thermal history, and compromised texture.

Method used

A method involving solution polymerization of acrylonitrile-based polymers in organic solvents, using a spinning stock solution discharged into a coagulation bath with specific solvent concentration and velocity to create acrylic fibers with irregular cross-sections, characterized by at least two recesses.

Benefits of technology

Produces acrylic fibers with improved productivity, whiteness, and texture, maintaining a soft and firm feel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136655000001_ABST
    Figure 2024136655000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a modified cross-section acrylic fiber having an excellent feeling, anti-pilling property, and whiteness.SOLUTION: In the method for producing the modified cross-section acrylic fiber whose cross-sectional shape includes at least two recessed parts, an acrylonitrile-based polymer containing acrylonitrile as a main repeating unit is discharged from an atypical-hole nozzle into a coagulation bath having an organic solvent concentration of 40-60 wt%, using a spinning dope obtained by solution polymerization in an organic solvent, within a range of a spinning dope discharge velocity satisfying the formula (1). Formula (1): 4.70≤discharge linear velocity / fineness≤7.90.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an excellent modified cross-section acrylic fiber. [Background technology]

[0002] Acrylic fibers have a texture similar to that of wool, and are used in clothing products such as sweaters and socks, or as pile materials for animal-hair-like raised-pile products that make use of the texture and luster of animal hair, making them a major synthetic fiber. The cross-sectional shape of the fiber contributes greatly to the appearance of the final product, especially its texture, and can determine the characteristics of the product. The cross-sectional shapes of acrylic fibers include circular, broad bean, and flat types, and among these, dumbbell-shaped (dog-bone) cross-sections are known to be characterized by softness, firmness, and slimy feel, and to give an extremely good texture.

[0003] As a method for obtaining acrylic fibers with a dumbbell cross section, Patent Document 1 discloses a method using a dry spinning method, while Patent Document 2 and Patent Document 3 disclose methods using a wet spinning method in which the ratio of the take-up speed to the discharge speed of the spinning dope from the nozzle is set within a specific range. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 53-147818 [Patent Document 2] Japanese Patent Application Publication No. 11-217723 [Patent Document 3] JP 2003-301322 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the method described in Patent Document 1 has a problem of being inferior in productivity to the wet spinning method. The methods described in Patent Documents 2 and 3 have a problem of increasing the thermal history and causing the fibers to take on a yellowish tinge because the acrylonitrile polymer is dried once and then dissolved in an organic solvent again.

[0006] Therefore, an object of the present invention is to provide a method for producing a modified cross-section acrylic fiber which is excellent in productivity, whiteness and texture. [Means for solving the problem]

[0007] As a result of investigations aimed at solving the above problems, the present inventors discovered that the problems could be solved by the following means, and thus arrived at the present invention.

[0008] The present invention is a method for producing an acrylic fiber having a modified cross section in which the cross-sectional shape of the fiber has at least two recesses, characterized in that a spinning dope obtained by solution polymerization of an acrylonitrile-based polymer, the main repeating unit of which is acrylonitrile, in an organic solvent is extruded from a modified hole spinneret into a coagulation bath having an organic solvent concentration of 40 to 60% by weight at a spinning dope extrusion speed range that satisfies the following formula (1):

[0009] 4.70≦Discharge linear velocity / fineness≦7.90 Formula (1) Effect of the Invention

[0010] According to the present invention, a modified cross section acrylic fiber excellent in productivity and whiteness can be produced, and a fiber product having a good feel can be obtained from the fiber obtained therefrom. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional photograph of an example of a modified cross-section acrylic fiber obtained by the production method of the present invention. [Diagram 2] 1 is a representative schematic diagram of a modified cross section obtained by the manufacturing method of the present invention, in which the shaded areas indicate recesses. [Diagram 3] FIG. 2 is a schematic diagram of an example of a dumbbell-shaped cross section obtained by the manufacturing method of the present invention, showing line portion A and line portion B for evaluating the degree of irregularity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The method for producing a modified cross-section acrylic fiber of the present invention is characterized in that a spinning dope of an acrylic polymer, the main repeating unit of which is acrylonitrile, obtained by solution polymerization in an organic solvent, is discharged from a modified hole spinneret into a coagulation bath having an organic solvent concentration of 40 to 60% by weight at a spinning dope discharge speed range which satisfies the following formula (1): 4.70≦Discharge linear velocity / fineness≦7.90 Formula (1) In the present invention, a spinning solution (hereinafter, sometimes simply referred to as "spinning solution") in which an acrylic polymer is dissolved in a solvent is used. The acrylic polymer is one that is composed of acrylonitrile units as the main repeating unit and is composed of vinyl monomers that can be copolymerized with the acrylic polymer. The acrylic polymer used contains 80 mol % or more of acrylonitrile, more preferably 85 mol % or more, and even more preferably 90 mol % or more.

[0013] As the copolymerizable vinyl monomer, acrylic acid, methacrylic acid or their esters, olefin monomers such as itaconic acid, acrylamide, methacrylamide, vinyl acetate, vinyl chloride, vinylidene chloride, or unsaturated sulfonic acids such as allylsulfonic acid, vinylsulfonic acid, acrylsulfonic acid, methallylsulfonic acid, and p-styrenesulfonic acid or their salts can be used, and methyl acrylate and sodium methallylsulfonate are particularly preferably used. For clothing and materials, from the viewpoint of dyeing and imparting functionality, it is preferable to copolymerize at least one of the above components, with a preferred lower limit of 1 mol%, more preferably 2 mol%. If the copolymerization component is too high, spinnability may be impaired, and a preferred upper limit is 20 mol%, more preferably 15 mol%.

[0014] If necessary, the acrylic polymer used in the present invention may contain additives such as a polymerization initiator, a pH adjuster, and a molecular weight adjuster.

[0015] The spinning solution used in the present invention is obtained by solution polymerization of acrylonitrile and a copolymerization monomer in an organic solvent. Aqueous suspension polymerization is also a common method for obtaining an acrylic polymer, but since the polymer particles are dried once, the thermal history is high and the spinning solution and fibers are yellowish, so this method is not suitable for the present invention. In the present invention, an acrylic polymer is obtained by solution polymerization, and the polymer solution is used as the spinning solution as is or after concentration adjustment without drying, so that the thermal history can be reduced. The organic solvent used in the solution polymerization may be one or more selected from the group consisting of dimethyl sulfoxide (DMSO), dimethylformamide, and dimethylacetamide. In a more preferred embodiment of the present invention, the diffusion coefficient of the organic solvent into water is preferably in the range of 2.5 to 8.0, and from this viewpoint, the organic solvent is preferably dimethyl sulfoxide.

[0016] In the present invention, it is necessary to extrude into a coagulation bath having an organic solvent concentration of 40 to 60% by weight. When the organic solvent concentration is below 40% by weight, the fiber surface is coagulated very quickly, and the internal coagulation does not proceed, so that the spinnability is significantly reduced. The preferred lower limit of the organic solvent concentration is 42% by weight, and the more preferred lower limit is 44% by weight. On the other hand, when the organic solvent concentration exceeds 60% by weight, the coagulation is slowed down, so that the desired irregular cross section cannot be obtained. The preferred upper limit of the organic solvent concentration is 58% by weight, and more preferably 56% by weight. It is preferable that the organic solvent used in the coagulation bath is the same as the organic solvent used in the polymerization from the viewpoint of separation, recovery, and reuse of the coagulation bath liquid.

[0017] The modified hole die used in the present invention can be appropriately selected by a person skilled in the art as long as it is a die that forms a desired modified cross section having at least two recesses. Examples of modified cross sections having at least two recesses include dumbbell-shaped, trilobal, cross-shaped, and flattened multi-lobed types. The recess here refers to a part where the actual fiber periphery has a recess on the inside, as shown in FIG. 2, with respect to the figure of the periphery of the fiber cross section drawn at the shortest distance. In other words, triangular and hexagonal cross sections do not fall under modified cross sections having recesses. In addition, when there is only one recess, for example, a broad bean-shaped cross section, is also inappropriate. When there are not two or more recesses, it is inappropriate because the desired softness, firmness, and sliminess are lacking.

[0018] The degree of the recess in the modified cross-section acrylic fiber of the present invention is expressed differently depending on the cross-sectional shape, but for example, in the case of a dumbbell-shaped fiber, as shown in Fig. 3, when the longest line portion perpendicular to the longest line portion in the fiber cross section (dumbbell-shaped cross section) is designated as A and the shortest line portion is designated as B, the degree of irregularity is A / B, and the larger this value is, the larger the recess is, and the higher the degree of irregularity can be considered to be. In the modified cross-section acrylic fiber of the present invention, in the case of a dumbbell-shaped fiber, it is preferable that A / B is 1.15 or more.

[0019] In the present invention, it is necessary to extrude the spinning dope from the modified hole die within a range of extrusion linear velocity that satisfies the following formula (1). 4.70≦Discharge linear velocity / fineness≦7.90 Formula (1) Here, the fineness is the fineness (dtex) of the obtained fiber, and the discharge linear velocity (cm / sec) is the volumetric discharge amount of the spinning dope per hole (cm 3 / sec) to the opening area per hole (cm 2 ) when this value is below 4.70 cm / (sec·dtex), cross-section formation and spinnability change drastically depending on the coagulation bath conditions, making it difficult to stably spin acrylic fibers with irregular cross-sections. The lower limit is preferably 5.00 cm / (sec·dtex), and more preferably 5.50 cm / (sec·dtex). When this value exceeds 7.90 cm / (sec·dtex), the ballast effect immediately after discharge from the spinneret hole increases, making it impossible to obtain a clear irregular cross-section.

[0020] The spun yarn is taken up at a constant speed by a take-up facility, and is then continuously stretched, washed with water, dried and densified, oiled, crimped, heat-relaxed, and dried to obtain fibers. A cross-sectional photograph of an example (dumbbell-shaped) of the modified cross-section acrylic fiber obtained by the manufacturing method of the present invention is shown in FIG. 1. The preferred range of the fineness of the modified cross-section acrylic fiber obtained by the manufacturing method of the present invention is 1.0 dtex to 5.5 dtex. The fibers may be in a tow state or cut into staples.

[0021] In addition, in a preferred embodiment of the modified cross-section acrylic fiber obtained by the production method of the present invention, the color tone b value, which is an index of yellowness, is in the range of 1.5 to 6.0, more preferably in the range of 2.0 to 5.0. In the production method of the present invention, since the thermal history can be reduced as described above, yellowing of the fiber can be suppressed, and the color tone b value can be set in the above range.

[0022] In addition, those skilled in the art can appropriately adjust the polymerization and spinning conditions for carrying out the present invention. EXAMPLES

[0023] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0024] (1) Single fiber size (dtex) Measurements were performed in accordance with the method described in JIS L1015:2010, Chemical Fiber Staple Test Method.

[0025] (2) Color tone b value Samples were prepared according to the whiteness measurement method described in JIS L1015:2010 Chemical fiber staple test method, and the b value was measured using a Suga Corporation "Color Computer; Model SM-3."

[0026] (3) Spinnability The take-up speed was gradually increased under the same extrusion conditions, and the speed at which yarn breakage occurred at the nozzle surface was defined as the upper limit spinnable speed (m / min), and the result was judged as follows: Good (A): 10.0≦Upper limit spinning speed Possible (B): 8.0<Upper limit spinning speed<10.0 Defective (C): Upper limit spinning speed ≦8.0 The results were judged on the three-point scale above, with A being good and B being fair.

[0027] (4) Atypicality The longest line perpendicular to the longest line in the fiber cross section (dumbbell-shaped cross section) was designated as A, and the shortest line was designated as B. The irregularity degree was A / B, and a ratio of 1.15 or more was considered to be acceptable.

[0028] (5) Overall evaluation The spinnability and the degree of irregularity were evaluated comprehensively. Those for which the degree of irregularity was acceptable and the spinnability was good were rated "good", those for which the degree of irregularity was acceptable and the spinnability was fair were rated "passable", and those for which either the spinnability or the degree of irregularity was poor were rated "poor".

[0029] [Examples 1 to 5, Comparative Examples 1 to 4] An acrylic polymer consisting of 93.8% by mass of acrylonitrile, 5.0% by mass of methyl acrylate, and 1.2% by mass of sodium methallylsulfonate was obtained by DMSO-based solution polymerization. DMSO was added to the DMSO solution of the obtained acrylic polymer to adjust the concentration of the acrylic polymer solution to 22% by mass, and used as a spinning dope. The spinning dope was adjusted to 60°C, and spun using a dumbbell-shaped spinneret hole under various conditions shown in Table 1. After that, the tow was stretched 5.0 times, washed with soft water, dried and densified, and oil was added. The tow was then heated to 75°C by wet heat treatment with steam, crimped with a push-in crimper, dried, and cut to obtain an acrylic fiber. The characteristics of the obtained fiber are shown in Table 1. In addition, in the degree of irregularity in Table 1, those in which no recesses were formed on the fiber cross section were given a value of 1. In addition, FIG. 1 is a cross-sectional photograph of the irregular cross-section acrylic fiber obtained in Example 2.

[0030] The manufacturing methods of Examples 1 to 5 showed that acrylic fibers having a modified cross section and an excellent degree of irregularity could be obtained while maintaining good spinnability. In Comparative Examples 1 and 2, the value of extrusion linear velocity / fineness was high, and a good degree of irregularity could not be obtained even when the coagulation bath conditions were set to a low concentration. In Comparative Example 3, a relatively good degree of irregularity was obtained, but the spinnability was inferior and stable spinning could not be achieved. In Comparative Example 4, when the organic solvent concentration was set to a concentration exceeding the specified concentration of the present invention, the spinnability was improved compared to Comparative Example 3, but a good degree of irregularity could not be obtained.

[0031] [Table 1] [Explanation of symbols]

[0032] 1: Recess 2: The longest line in the fiber cross section (dumbbell-shaped cross section)

Claims

1. A method for producing a modified cross-section acrylic fiber having a cross-sectional shape of at least two recesses, the method being characterized in that a spinning dope of an acrylic polymer, the main repeating unit of which is acrylic, obtained by solution polymerization in an organic solvent, is extruded from a modified hole spinneret into a coagulation bath having an organic solvent concentration of 40 to 60% by weight at a linear extrusion velocity within the range that satisfies the following formula (1): 4.70≦discharge linear velocity / fineness≦7.90 Formula (1)

2. The method for producing a modified cross-section acrylic fiber according to claim 1, characterized in that the diffusion coefficient of the organic solvent into water is in the range of 2.5 to 8.

0.

3. The method for producing a modified cross section acrylic fiber according to claim 1 or 2, wherein the shape of the modified hole is dumbbell-shaped.

4. 3. A modified cross-section acrylic fiber, obtained by the method according to claim 1 or 2, characterized in that the color tone b value is 1.5 to 6.0.

Citation Information

Patent Citations

  • Production of acrylic fiber

    JP1978147818A

  • Acrylic fiber tow material and its production

    JP1999217723A

  • Acrylic modified cross section high-fineness fiber and method producing same

    JP2003301322A