Pellet, method for producing molding and film

By using polyolefin pellets with a specific angle of repose and a laser marking agent, the method stabilizes the concentration of the marking agent, addressing uneven printing issues in laser-printable containers and films.

JP2024136680APending Publication Date: 2024-10-04TOYOBO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023047866
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for producing laser-printable containers and films often result in unevenness in laser printing due to variations in the concentration of the laser marking agent during the manufacturing process.

Method used

The use of polyolefin pellets containing a laser marking agent with an angle of repose between 25 and 45 degrees, combined with other pellets, to stabilize the feed rate and concentration of the laser marking agent, reducing variations in the extrusion process and minimizing uneven printing.

Benefits of technology

This approach effectively reduces printing unevenness by stabilizing the concentration of the laser marking agent, ensuring consistent printing quality across multiple containers or films produced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136680000004
    Figure 2024136680000004
  • Figure 2024136680000005
    Figure 2024136680000005
  • Figure 2024136680000001
    Figure 2024136680000001
Patent Text Reader

Abstract

To provide a pellet capable of producing moldings (container and film, for instance) capable of reducing printing unevenness that can be caused when laser printing is carried out, a method for producing a molding capable of reducing the printing unevenness that can be caused when the laser printing is carried out, and a film capable of reducing the printing unevenness that can be caused when the laser printing is carried out.SOLUTION: The present invention relates to a pellet containing a polyolefin and a laser marking agent, and having an angle of repose of 25 degrees or more and 45 degrees or less. Since the pellet contains a laser marking agent, it is possible to produce a molded article on which a mark can be formed by a laser, that is, a molded article that can be laser-marked. Since the pellet has an angle of repose of 25 degrees or more and 45 degrees or less, it is possible to produce a molded article that can reduce printing unevenness.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pellet, a method for producing a molded article, and a film. [Background technology]

[0002] Containers that can be marked with a laser are known as containers for foods and beverages (see Patent Documents 1 to 3). Patent Document 1 describes a small bag that can be marked with a laser. Patent Document 2 describes a laminated tube container that can be marked with a laser. Patent Document 3 describes a multi-layer resin container that can be marked with a laser. The manufacturing date, expiration date, lot number, etc. of the food or beverage can be marked on these containers with a laser.

[0003] Films, labels, and lids that can be printed with a laser are also known (see Patent Document 4). By printing on these with a laser, it is possible to add the manufacturing date, expiration date, lot number, and the like.

[0004] To manufacture these, it is known to prepare pellets containing the laser marking agent, i.e., a master batch, and then mix the master batch with pellets that do not contain the laser marking agent (e.g., commercially available polyolefin pellets) and feed the mixture into an extruder (see, for example, Patent Document 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4727414 [Patent Document 2] Patent No. 6592926 [Patent Document 3] Patent No. 6260265 [Patent Document 4] WO / 2021 / 125135A1 Summary of the Invention [Problem to be solved by the invention]

[0006] The inventors discovered that when a roll of film having a certain length (specifically, 500 m) was manufactured and individual pieces of film cut from the roll were laser-printed, uneven printing, i.e., uneven density of the laser printing, could occur on each piece of film.

[0007] The present invention aims to provide pellets that can be used to produce molded articles (such as containers and films) that can reduce printing unevenness that can occur when laser marking is performed.The present invention also aims to provide a method for producing a molded article that can reduce printing unevenness that can occur when laser marking is performed.The present invention also aims to provide a film that can reduce printing unevenness that can occur when laser marking is performed. [Means for solving the problem]

[0008] In order to solve this problem, the present invention has the following configuration [1]. [1] A polyolefin; a laser marking agent; The angle of repose is between 25 degrees and 45 degrees. pellet.

[0009] According to [1], since the pellets contain a laser marking agent, it is possible to produce molded articles on which marks can be formed by a laser, i.e., laser-markable molded articles.

[0010] Moreover, since the repose angle of the pellets is 25 degrees or more and 45 degrees or less, a molded product capable of reducing printing unevenness can be manufactured. This will be explained. Since the repose angle of the pellets is 25 degrees or more and 45 degrees or less, when the pellets of the present invention (i.e., the pellets according to [1]) are mixed with other pellets (e.g., the second pellets) and then fed from a hopper to an extruder, it is possible to suppress the variation over time in the amount of the pellets of the present invention (i.e., the pellets according to [1]) fed per unit time, and the variation over time in the concentration of the laser marking agent in the molten material in the extruder can be suppressed. Therefore, it is possible to suppress the variation in the concentration of the laser marking agent in the molded product, and it is possible to reduce the printing unevenness that may occur when laser marking is performed on the molded product. For example, when the molded product is a roll-shaped film manufactured through a process of extruding a film-shaped molten material, it is possible to suppress the variation in the concentration of the laser marking agent in the length direction of the film. Therefore, when laser marking is performed on a film cut from a roll, it is possible to reduce the printing unevenness that may occur for each film. On the other hand, when the molded product is a container manufactured through blow molding of a parison including a layer extruded by an extruder, it is possible to reduce printing unevenness that may occur from container to container.

[0011] In the present invention, the following configurations [2] to [4] are preferred. [2] The pellet according to [1], wherein the content of the laser marking agent is 1% by mass or more and 50% by mass or less. [3] The pellet according to [1] or [2], wherein the weight of each pellet is 8 mg or more and 20 mg or less. [4] The pellet according to any one of [1] to [3], which is used for producing a container.

[0012] The present invention has the following configuration [5]. [5] A step of mixing at least the pellet according to any one of [1] to [4] and a second pellet; feeding the mixed pellets prepared in the step of mixing at least the pellets and the second pellets from a hopper to an extruder; and melting and extruding the mixed pellets in the extruder. Manufacturing method of molded products.

[0013] In the present invention, the following configurations [6] to [8] are preferable. [6] The method for producing a molded article according to [5], further comprising a step of blow molding a parison including the layer extruded by the extruder. [7] The method for producing a molded product according to [5], wherein in the step of melting and extruding the mixed pellets in the extruder, a film-like molten material is extruded. [8] The method for producing a molded article according to any one of [5] to [7], wherein a difference between an angle of repose of the pellet and an angle of repose of the second pellet is 10 degrees or less in absolute value.

[0014] The present invention has the following configuration [9]. [9] A polyolefin; A film comprising a laser marking agent, the fluctuation range of the content of the main metal element in the laser marking agent in the longitudinal direction of the film is 0.10 mass% or less, and the fluctuation range is the absolute value of the difference between the average value when the content of the main metal element is measured at 50 m intervals in the longitudinal direction of the film and the value farthest from the average value; film. Here, the term "major metal element in the laser marking agent" refers to the metal element that is contained in the largest amount among the metal elements contained in the laser marking agent.

[0015] According to [9], the fluctuation range of the content of major metal elements in the laser marking agent in the longitudinal direction of the film is 0.10 mass% or less, which reduces printing unevenness that may occur when laser marking is performed. Effect of the Invention

[0016] According to the present invention, it is possible to provide pellets that can be used to manufacture molded articles (such as containers and films) that can reduce printing unevenness that can occur when laser marking is performed. According to the present invention, it is also possible to provide a manufacturing method for molded articles that can reduce printing unevenness that can occur when laser marking is performed. According to the present invention, it is also possible to provide a film that can reduce printing unevenness that can occur when laser marking is performed. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a schematic perspective view for explaining the measured length of a pellet having an elliptical cylindrical shape. [Diagram 2] FIG. 2 is a schematic perspective view for explaining the measured length of an ellipsoidal pellet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, embodiments of the present invention will be described in detail.

[0019] <1. Pellets> <1.1. Polyolefin> The pellets of this embodiment include polyolefins. The polyolefins may be homopolymers or copolymers. Examples of polyolefins include polyethylenes such as low-density polyethylene (LDPE), high-density polyethylene (HDPE), and linear low-density polyethylene (LLDPE). In addition, examples of polypropylenes include homopolypropylene and ethylene-propylene copolymers. Examples of polyolefins include olefin-based thermoplastic elastomers and ionomers. The polyolefins may have functional groups. Examples of functional groups include amino groups, isocyanate groups, hydroxyl groups, mercapto groups, ureido groups, glycidyl groups, carboxylic acid groups, carboxylic anhydride groups, carboxylic acid ester groups, and metal carboxylate groups. Examples of polyolefins having functional groups include adhesive polyolefins "Admer (registered trademark)" by Mitsui Chemicals, Inc. It should be noted that one type of polyolefin may be used, or two or more types may be used.

[0020] <1.2. Laser marking agent> The pellets of this embodiment contain a laser marking agent. Since the pellets contain a laser marking agent, it is possible to produce a molded article on which a mark can be formed by a laser, that is, a laser-markable molded article.

[0021] The laser marking agent can be a pigment capable of absorbing a laser. If the laser marking agent is capable of absorbing a laser, it can convert the energy of the laser into heat, and therefore can carbonize the surrounding polyolefin. Of course, the laser marking agent itself may be capable of changing color (e.g., changing color to black). In this way, the laser marking agent may be capable of carbonizing the surrounding polyolefin, may be capable of changing color, or may be capable of both.

[0022] Examples of the laser include a CO2 laser (10600 nm), a YAG laser (1064 nm), a YVO4 laser (1064 nm), a fiber laser (1090 nm), a green laser (532 nm), and an ultraviolet laser (hereinafter sometimes referred to as a "UV laser") (355 nm). Among these, a YAG laser, a YVO4 laser, a fiber laser, a green laser, and a UV laser are preferred, and a Nd:YAG laser, a fiber laser, a green laser, and a UV laser are more preferred.

[0023] The laser marking agent may contain, for example, at least one elemental metal selected from the group consisting of bismuth, gadolinium, neodymium, titanium, antimony, tin, and aluminum, and / or at least one oxide of a metal selected from this group. Of course, the laser marking agent may contain elemental metals or oxides of metals other than these.

[0024] The particle size of the laser marking agent is preferably 0.1 μm or more, more preferably 0.5 μm or more, while the particle size of the laser marking agent is preferably 10 μm or less, more preferably 9 μm or less.

[0025] Commercially available laser marking agents include, for example, "TOMATEC COLOR" from TOMATEC Corporation and "Iriotec (registered trademark)" from Merck Performance Materials LLC. Note that one type of laser marking agent may be used, or two or more types may be used.

[0026] The content of the laser marking agent in the pellet is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more. The content of the laser marking agent may be 10% by mass or more, 15% by mass or more, or 20% by mass or more. On the other hand, the content of the laser marking agent in the pellet is preferably 50% by mass or less, more preferably 35% by mass or less, even more preferably 30% by mass or less, and even more preferably 25% by mass or less. When it is 50% by mass or less, it is possible to prevent the true specific gravity of the pellet from becoming excessively large. The content of the laser marking agent may be 40% by mass or less, 30% by mass or less, or 25% by mass or less.

[0027] <1.3. Pellets properties, weight, etc.> The repose angle of the pellets is 25 degrees or more and 45 degrees or less. By being 25 degrees or more and 45 degrees or less, a molded product capable of reducing printing unevenness can be manufactured. This will be explained. Since the repose angle of the pellets is 25 degrees or more and 45 degrees or less, when the pellets of this embodiment are mixed with other pellets and then fed from a hopper to an extruder, it is possible to suppress the variation over time of the supply amount of the pellets of this embodiment per unit time, and the variation over time of the laser marking agent concentration of the molten material in the extruder can be suppressed. Therefore, it is possible to suppress the variation in the laser marking agent concentration of the molded product, and it is possible to reduce the printing unevenness that may occur when laser marking is performed on the molded product. For example, when the molded product is a roll-shaped film manufactured through a process of extruding a film-shaped molten material, it is possible to suppress the variation in the laser marking agent concentration in the length direction of the film. Therefore, when laser marking is performed on a film cut from a roll, it is possible to reduce the printing unevenness that may occur for each film. On the other hand, when the molded product is a container manufactured by blow molding a parison including a layer extruded by an extruder, it is possible to reduce printing unevenness that may occur in each container. The repose angle of the pellet is preferably 28 degrees or more, more preferably 30 degrees or more, and even more preferably 32 degrees or more. On the other hand, the repose angle of the pellet is preferably 43 degrees or less, and more preferably 42 degrees or less.

[0028] The shape of the pellets may be, for example, a cylindrical shape such as a right circular cylinder or an elliptical cylinder, or an ellipsoid. When the pellets have such a shape, the height of the pellets may be, for example, 1.0 mm or more, 1.3 mm or more, or 1.5 mm or more. On the other hand, the height of the pellets may be, for example, 10.0 mm or less, 7.0 mm or less, or 5.0 mm or less.

[0029] The weight of each pellet is preferably 8 mg or more and 20 mg or less. The weight of each pellet may be, for example, 9 mg or more, or 10 mg or more. On the other hand, the weight of each pellet may be, for example, 18 mg or less, 17 mg or less, or 16 mg or less.

[0030] The bulk density of the pellets is, for example, 0.30 g / cm 3 or more, and may be 0.40 g / cm 3 or more, and may be 0.45 g / cm 3 or more, 0.50 g / cm 3 or more, and may be 0.52 g / cm 3 or more, and may be 0.54 g / cm 3 On the other hand, the bulk density of the pellets may be, for example, 0.60 g / cm 3 or less, 0.57 g / cm 3 It may be less than 0.55 g / cm 3 It may be the following.

[0031] The true specific gravity of a pellet is, for example, 0.94 g / cm 3 or more, 1.00 g / cm 3 or more, and may be 1.02 g / cm 3 or more, 1.03 g / cm 3 On the other hand, the true specific gravity of the pellets is, for example, 1.20 g / cm 3 or less, 1.15 g / cm 3 or less, 1.12 g / cm 3 or less, 1.10 g / cm 3 It may be the following.

[0032] <2. Manufacturing method of molded products> The manufacturing method of the molded product of this embodiment includes at least a step of mixing the above-mentioned pellets (i.e., pellets containing a polyolefin and a laser marking agent and having an angle of repose of 25 degrees or more and 45 degrees or less; hereinafter sometimes referred to as "first pellets") and second pellets (hereinafter sometimes referred to as "mixing step"); a step of supplying the mixed pellets prepared in the step of mixing at least the first pellets and the second pellets from a hopper to an extruder (hereinafter sometimes referred to as "supply step"); and a step of melting and extruding the mixed pellets in the extruder (hereinafter sometimes referred to as "extrusion step").

[0033] Examples of the molded article produced by the manufacturing method of this embodiment include containers and films. The molded article can also include a parison.

[0034] Examples of the containers include containers for food and beverages, medicines, quasi-drugs, cosmetics, dentifrices, paints, and adhesives. Examples of the food and beverages include mayonnaise, ketchup, wasabi paste, mustard paste, and pizza sauce. Among these, containers for food and beverages are preferred, and containers for sauces such as mayonnaise and ketchup are preferred.

[0035] On the other hand, the film can be used as, for example, a label, a container lid. The film can also be used to manufacture labels, container lids, bags, laminated tubes, etc. The label can be, for example, a bottle label. The bag can be, for example, a bag made by heat sealing, such as a vertical pillow bag, a horizontal pillow bag, or a gusset bag. The bag can also be, for example, a bag made by melt-cut sealing.

[0036] The manufacturing method of the container and the manufacturing method of the film will be described below.

[0037] <2.1. Container manufacturing method> The manufacturing method for a container of this embodiment includes at least a step of mixing first pellets (i.e., pellets containing a polyolefin and a laser marking agent and having an angle of repose of 25 degrees or more and 45 degrees or less) and second pellets (i.e., a mixing step), a step of supplying the mixed pellets prepared in the step of mixing at least the first pellets and the second pellets from a hopper to an extruder (i.e., a supply step), a step of melting and extruding the mixed pellets in the extruder (i.e., an extrusion step), and a step of blow molding a parison including the layer extruded by the extruder (hereinafter sometimes referred to as the "blow molding step").

[0038] <2.1.1.Mixing process> In the mixing step, the first pellets and the second pellets are mixed. The mixing can be performed, for example, by a mixer provided upstream of a hopper. In this case, after mixing, the mixed pellets are transferred from the mixer to the hopper. A feeder may be provided between the mixer and the hopper. Alternatively, the mixing may be performed in the hopper.

[0039] The second pellets preferably contain a polyolefin. The description of the polyolefin of the second pellets is omitted because it overlaps with the above description (i.e., the description of the polyolefin of the first pellets). Therefore, the description of the polyolefin of the first pellets can also be used as the description of the polyolefin of the second pellets.

[0040] When the polyolefin of the first pellets contains polyethylene, it is preferable that the polyolefin of the second pellets also contains polyethylene. For example, when the polyolefin of the first pellets contains low density polyethylene, it is preferable that the polyolefin of the second pellets also contains low density polyethylene. When the polyolefin of the first pellets contains linear low density polyethylene, it is preferable that the polyolefin of the second pellets also contains linear low density polyethylene. On the other hand, when the polyolefin of the first pellets contains polypropylene, it is preferable that the polyolefin of the second pellets also contains polypropylene.

[0041] Although the second pellet may or may not contain a laser marking agent, it is preferred that the second pellet does not contain a laser marking agent, since the first pellet contains a laser marking agent and therefore there is no need for the second pellet to contain a laser marking agent.

[0042] The angle of repose of the second pellets is preferably 15 degrees or more and 55 degrees or less. When the angle is 15 degrees or more and 55 degrees or less, it is possible to prevent the ease of the second pellets dropping from the hopper from deviating excessively from that of the first pellets (i.e., the ease of dropping), and therefore, the variation over time in the amount of the first pellets fed per unit time can be further suppressed. As a result, it is possible to further reduce unevenness in printing that may occur when laser marking is performed on a molded product, i.e., a container. The angle of repose of the second pellets is more preferably 20 degrees or more, even more preferably 25 degrees or more, even more preferably 28 degrees or more, even more preferably 30 degrees or more, and even more preferably 32 degrees or more. On the other hand, the angle of repose of the second pellets is more preferably 43 degrees or less, even more preferably 41 degrees or less, and even more preferably 40 degrees or less.

[0043] The description of the shape, weight (specifically, the weight per second pellet) and bulk specific gravity of the second pellets will be omitted because they overlap with the above description (i.e., the description of these for the first pellets). Therefore, the description of the shape, weight and bulk specific gravity of the first pellets can also be treated as the description of these for the second pellets.

[0044] The difference between the angle of repose of the first pellet and the angle of repose of the second pellet is preferably 10 degrees or less in absolute value, more preferably 9 degrees or less, even more preferably 8 degrees or less, even more preferably 7 degrees or less, and even more preferably 6 degrees or less. When it is 10 degrees or less, it is possible to prevent the ease of the first pellets dropping from the hopper from deviating excessively from that of the second pellets (i.e., the ease of dropping), and therefore, it is possible to further suppress the variation over time in the amount of the first pellets supplied per unit time. As a result, it is possible to further reduce the unevenness of printing that may occur when laser printing is performed on a molded product, i.e., a container. This difference may be 5 degrees or less in absolute value, this difference may be 4 degrees or less in absolute value, this difference may be 3 degrees or less in absolute value, and this difference may be 2 degrees or less in absolute value.

[0045] In the mixing step, other pellets (e.g., a third pellet) may be further mixed with the first pellet and the second pellet. The description of the other pellets is omitted because it overlaps with the description of the second pellet. Therefore, the description of the second pellet can also be treated as the description of the other pellets.

[0046] The difference between the maximum and minimum angles of repose of the individual pellets mixed in the mixing step (i.e., the first pellets, the second pellets, and other pellets mixed as necessary) is preferably 10 degrees or less, more preferably 9 degrees or less, even more preferably 8 degrees or less, even more preferably 7 degrees or less, and even more preferably 6 degrees or less. If it is 10 degrees or less, it is possible to further suppress the variation over time in the amount of the first pellets fed per unit time, so that it is possible to further reduce uneven printing that may occur when laser printing is performed on the container. This difference may be 5 degrees or less in absolute value, and this difference may be 4 degrees or less in absolute value.

[0047] In the total mass 100% of the pellets mixed in the mixing step (i.e., the first pellets, the second pellets, and other pellets mixed as necessary), the amount of the first pellets is preferably 1.0% by mass or more, more preferably 1.5% by mass or more. The amount of the first pellets may be 3.0% by mass or more, or may be 5.0% by mass or more. Meanwhile, in the total mass 100% of the pellets mixed in the mixing step, the amount of the first pellets is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.

[0048] In the total mass 100% of the pellets mixed in the mixing step (i.e., the first pellets, the second pellets, and other pellets mixed as necessary), the amount of the second pellets is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and even more preferably 60% by mass or more. Meanwhile, in the total mass 100% of the pellets mixed in the mixing step, the amount of the second pellets is preferably 99.0% by mass or less, more preferably 98.5% by mass or less, and even more preferably 97.0% by mass or less.

[0049] <2.1.2. Supply process> In the feeding step, the mixed pellets are fed from a hopper to the extruder. The hopper can be provided above the feed port of the extruder. The hopper is funnel-shaped. The hopper may be provided with a device for promoting the discharge of the mixed pellets, such as a vibrator, an air knocker, or a screw.

[0050] The inclination angle of the hopper may be, for example, 40 degrees or more, 45 degrees or more, or 50 degrees or more. On the other hand, the inclination angle of the hopper may be, for example, 75 degrees or less, or 70 degrees or less. The inclination angle of the hopper is the angle formed by a pair of opposing inner surfaces of the hopper. For example, when the hopper has a taper, i.e., a conical portion, the inclination angle of the hopper is the angle formed by a pair of opposing inner surfaces of the hopper in a cross-sectional view when the hopper is assumed to be cut along a plane perpendicular to the diameter of the conical portion and located at the center of the diameter. Note that when the inclination angle varies depending on the measurement point, the "inclination angle of the hopper" is expressed as the minimum value.

[0051] <2.1.3. Extrusion process> In the extrusion process, the mixed pellets are melted and extruded in an extruder to form a parison.

[0052] The extruder includes a screw and a cylinder surrounding the screw. In other words, the extruder includes a cylinder and a screw in the cylinder. The extruder can melt the mixed pellets by the rotating screw and extrude them at a fixed amount. Examples of the extruder include a single screw extruder and a twin screw extruder.

[0053] The extruder is fitted with a die. The die may be attached to the cylinder via a head (i.e., extruder head), or the die may include the head.

[0054] In the extrusion process, specifically, the mixed pellets are melted in an extruder, and the melt of the mixed pellets is laminated with the melt from another extruder as necessary, and then the melt, i.e., the parison, is extruded from a die. These melts can be laminated in the head or the die. The number of the other extruders may be one or more.

[0055] Examples of the resin supplied to the other extruder include polyamide, ethylene-vinyl alcohol copolymer (i.e., EVOH), and polyolefin. The resin supplied to the other extruder may be in the form of pellets. An example of polyamide is polymetaxylylene adipamide (MXD6). The explanation of polyolefin is omitted because it overlaps with the explanation above (i.e., the explanation of the polyolefin of the first pellets). Therefore, the explanation of the polyolefin of the first pellets can also be used as the explanation of the polyolefin supplied to the other extruder.

[0056] <2.1.4. Blow molding process> In the blow molding process, a parison is blown. For example, compressed gas (e.g., compressed air) is blown into the parison, and the parison is pressed against the inner surface of a mold. This produces a hollow molded product, specifically a container. The blow molding may be, for example, direct blow molding (i.e., extrusion blow molding) or injection blow molding.

[0057] The parison includes a layer (hereinafter, sometimes referred to as a "laser marking layer") formed using the mixed pellets as a raw material. The laser marking layer includes a polyolefin and a laser marking agent. The laser marking layer may further include various additives. Examples of additives include waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducers, heat stabilizers, coloring pigments, coloring inhibitors, ultraviolet absorbers, and lubricants.

[0058] The parison may consist of only the laser marking layer, i.e., it may be a single layer, or it may include multiple layers.

[0059] When the parison includes multiple layers, the parison may further include a layer including an ethylene-vinyl alcohol copolymer (i.e., EVOH). When the parison includes a layer including an ethylene-vinyl alcohol copolymer, the gas barrier properties of the container can be improved. The parison may include a layer including a polyolefin (e.g., a polyolefin having a functional group) between the layer including an ethylene-vinyl alcohol copolymer and the laser marking layer.

[0060] When the parison contains multiple layers, the following layer configurations can be mentioned, for example: In the following, the layer containing polyethylene is sometimes called the "polyethylene layer", the layer containing ethylene-vinyl alcohol copolymer is sometimes called the "EVOH layer", and the layer containing adhesive resin (e.g., polyolefin having functional groups) is sometimes called the "adhesive resin layer". Polyethylene layer / Laser marking layer / Adhesive resin layer / EVOH layer / Adhesive resin layer / Polyethylene layer Polyethylene layer / EVOH layer / adhesive resin layer / laser marking layer / adhesive resin layer / EVOH layer / polyethylene layer

[0061] A container can be obtained by the above procedure. The container may be subjected to some processing, if necessary.

[0062] <2.2. Film manufacturing method> The method for producing the film of this embodiment includes at least a step of mixing first pellets (i.e., pellets containing a polyolefin and a laser marking agent and having an angle of repose of 25 degrees or more and 45 degrees or less) and second pellets (i.e., a mixing step), a step of supplying the mixed pellets prepared in the step of mixing at least the first pellets and the second pellets from a hopper to an extruder (i.e., a supply step), a step of melting and extruding the mixed pellets in the extruder (i.e., an extrusion step), and a step of solidifying the film-like molten material containing the layer extruded by the extruder with a chill roll.

[0063] <2.2.1. Mixing process and supply process> The description of the mixing step and the supplying step in the film manufacturing method of this embodiment will be omitted because it overlaps with the above description (i.e., the description of the mixing step and the supplying step in the container manufacturing method). Therefore, the description of the mixing step and the supplying step in the container manufacturing method can also be treated as the description of the mixing step and the supplying step in the film manufacturing method.

[0064] <2.2.2. Extrusion process> In the extrusion process, the mixed pellets are melted in an extruder, and the melt is extruded in the form of a film from a die.

[0065] The extruder includes a screw and a cylinder surrounding the screw. In other words, the extruder includes a cylinder and a screw in the cylinder. The extruder can melt the mixed pellets by the rotating screw and extrude them at a fixed amount. Examples of the extruder include a single screw extruder and a twin screw extruder.

[0066] The extruder is fitted with a die. The die may be attached to the cylinder via a head (i.e., extruder head), or the die may include the head.

[0067] In the extrusion process, specifically, the mixed pellets are melted in an extruder, and the melt of the mixed pellets is laminated with the melt from another extruder as necessary, and then the film-like melt is extruded from a die. These melts can be laminated in a feed block or a die. The number of the other extruders may be one or more.

[0068] The explanation of the resins supplied to the other extruders is omitted because it overlaps with the above explanation (i.e., the explanation of the resins in the container manufacturing method). Therefore, the explanation of the resins in the container manufacturing method can also be treated as the explanation of the resins in the film manufacturing method.

[0069] <2.2.3. Other processes> The film-like molten material is solidified by a chill roll. This allows the film-like molten material to be rapidly cooled and solidified, resulting in a substantially unoriented film (hereinafter sometimes referred to as "unstretched film"). The surface temperature of the chill roll is preferably 40°C or lower.

[0070] Next, the unstretched film can be stretched. For example, it can be biaxially stretched. The biaxial stretching may be simultaneous biaxial stretching or sequential biaxial stretching. Of these, sequential biaxial stretching is preferred. In sequential biaxial stretching, it is preferred to stretch the unstretched film in the longitudinal direction, i.e., MD, and then stretch the sheet after MD stretching in the transverse direction, i.e., TD.

[0071] The method for stretching the unstretched film in the longitudinal direction may be, for example, a method of stretching in multiple stages between a plurality of rolls, or a method of stretching by heating with an infrared heater, etc. Among these, the former is preferred.

[0072] When stretching in the longitudinal direction, it is preferable to preheat the unstretched film so that its temperature is 100° C. to 180° C. If the temperature is 100° C. or higher, breakage that may occur when the unstretched film is stretched in the longitudinal direction can be suppressed.

[0073] The stretching ratio when stretching the preheated unstretched film in the longitudinal direction, i.e., the MD stretching ratio, is preferably 1.1 times or more, more preferably 1.5 times or more, and even more preferably 2.0 times or more. If it is 1.1 times or more, it is possible to impart molecular orientation to the film in the longitudinal direction, and therefore the mechanical strength can be improved. The MD stretching ratio is preferably 10 times or less, more preferably 9.5 times or less, and even more preferably 9.0 times or less. If it is 10 times or less, it is possible to suppress breakage that may occur during TD stretching.

[0074] At least one surface of the film stretched in the longitudinal direction may be subjected to a surface treatment such as a corona treatment or a plasma treatment, if necessary. At least one surface of the film stretched in the longitudinal direction may be coated with a resin dispersion or a resin solution, if necessary.

[0075] The film stretched in the longitudinal direction is introduced into a tenter device, both ends of the film are held with clips, the film is heated with hot air, and then the distance between the clips, i.e., the gap, is increased while the film is transported in the longitudinal direction, thereby stretching the film in the width direction.

[0076] The preheating temperature when the film is stretched in the width direction is preferably 110° C. or more and 170° C. or less. The temperature when the film is stretched in the width direction, i.e., the TD stretching temperature, is preferably 120° C. or more and 180° C. or less.

[0077] The stretching ratio when stretching the film in the transverse direction, i.e., the TD stretching ratio, is preferably 1.5 times or more, more preferably 2.0 times or more, and is preferably 20 times or less, more preferably 15 times or less.

[0078] The film stretched in the width direction, i.e., the biaxially stretched film, can be guided to a zone for heat treatment (hereinafter, sometimes referred to as the "heat treatment zone"). Before being guided to the heat treatment zone, the biaxially stretched film may be guided to a zone where active heating is not performed (hereinafter, sometimes referred to as the "intermediate zone"). In other words, the biaxially stretched film may be guided to the intermediate zone before being guided to the heat treatment zone.

[0079] In the heat treatment zone, the film is preferably heated to 130°C or higher and 190°C or lower. Heat treatment promotes crystallization of the film, which makes it easier to reduce the heat shrinkage rate. The heating temperature is preferably 135°C or higher. On the other hand, the heating temperature is preferably 185°C or lower, and more preferably 180°C or lower.

[0080] During the heat treatment, the distance between the clips of the tenter may be reduced, thereby reducing the thermal shrinkage rate in the width direction.

[0081] The film that has passed through the heat treatment zone can be guided to a cooling zone, where the film is preferably cooled with cooling air at 10° C. to 30° C. for 2 to 20 seconds.

[0082] Both ends of the film can be cut and removed as necessary while winding. Slit processing can be performed as necessary before winding. A roll-shaped film can be obtained by this procedure. Printing can be performed at any time, and the gas barrier layer can be formed at any time. Examples of raw materials for the gas barrier layer include metals such as silicon, aluminum, tin, zinc, iron, and manganese, and inorganic compounds containing one or more of these metals. Examples of inorganic compounds include oxides, nitrides, carbides, and fluorides.

[0083] <2.2.4.Film> The film includes a layer (i.e., a laser marking layer) formed using the mixed pellets as a raw material. The laser marking layer includes a polyolefin and a laser marking agent. The laser marking layer may further include various additives. Examples of the additives include waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducing agents, heat stabilizers, coloring pigments, coloring inhibitors, ultraviolet absorbing agents, and lubricants.

[0084] The thickness of the laser marking layer is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thicker the thickness, the darker the mark formed by the laser, i.e., the laser marking, can be. On the other hand, the thickness of the laser marking layer is preferably 100 μm or less, more preferably 95 μm or less, and even more preferably 90 μm or less. The thinner the thickness, the more the haze of the film tends to be reduced.

[0085] The film may consist of only the laser marking layer, that is, it may be a single layer.

[0086] On the other hand, the film may include a laser marking layer and other layers. That is, the film may include a plurality of layers. For example, the film may include a first layer, a second layer, and a third layer. The first layer, the second layer, and the third layer are arranged in this order in the thickness direction of the film. Here, at least one of the first layer, the second layer, and the third layer may be a laser marking layer. Note that other layers may exist between the first layer and the second layer, or between the second layer and the third layer.

[0087] When the film includes a first layer, a second layer, and a third layer, and the second layer is a laser marking layer, it is preferable that the first layer includes a polyolefin. The description of the polyolefin of the first layer is omitted because it overlaps with the above description (i.e., the description of the polyolefin of the first pellet). Therefore, the description of the polyolefin of the first pellet can also be treated as the description of the polyolefin of the first layer. In addition, when the polyolefin of the laser marking layer includes polyethylene, it is preferable that the first layer also includes polyethylene. For example, when the laser marking layer includes low density polyethylene, it is preferable that the first layer includes at least one of low density polyethylene and high density polyethylene. When the laser marking layer includes linear low density polyethylene, it is preferable that the first layer also includes linear low density polyethylene. On the other hand, when the laser marking layer includes polypropylene, it is preferable that the first layer also includes polypropylene.

[0088] The first layer preferably further contains a lubricant. Examples of the lubricant include particles such as silica and talc. Examples of the lubricant include fatty acid amides, alkyl sulfonates, stearic acids, and erucic acid amides. The first layer may contain various additives.

[0089] When the film includes a first layer, a second layer, and a third layer, and the second layer is a laser marking layer, the third layer preferably includes a polyolefin. The description of the polyolefin of the third layer is omitted because it overlaps with the above description (i.e., the description of the polyolefin of the first pellet). Therefore, the description of the polyolefin of the first pellet can also be treated as the description of the polyolefin of the third layer. In addition, when the polyolefin of the laser marking layer includes polyethylene, it is preferable that the third layer also includes polyethylene. For example, when the laser marking layer includes low density polyethylene, it is preferable that the third layer includes at least one of low density polyethylene and high density polyethylene. When the laser marking layer includes linear low density polyethylene, it is preferable that the third layer also includes linear low density polyethylene. On the other hand, when the laser marking layer includes polypropylene, it is preferable that the third layer also includes polypropylene.

[0090] The third layer preferably further contains a lubricant. Examples of the lubricant include particles such as silica and talc. Examples of the lubricant include fatty acid amides, alkyl sulfonates, stearic acids, and erucic acid amides. The third layer may contain various additives.

[0091] The film may be subjected to a corona treatment, a coating treatment, a flame treatment, or the like.

[0092] The thickness of the film is preferably 8 μm or more, more preferably 13 μm or more, and even more preferably 18 μm or more. The thickness of the film may be, for example, 20 μm or more, or 30 μm or more. On the other hand, the thickness of the film is preferably 200 μm or less, more preferably 195 μm or less, and even more preferably 190 μm or less. The thinner the thickness, the more cost can be reduced. The thickness of the film may be, for example, 150 μm or less, 100 μm or less, 80 μm or less, or 60 μm or less.

[0093] When the film is in a roll form, the length of the film may be, for example, 500 m or more, 1000 m or more, 5000 m or more, or 10000 m or more.

[0094] In the length direction of the film, the fluctuation range of the content of the main metal element of the laser marking agent (hereinafter sometimes referred to as "main metal element of the laser marking agent") is preferably 0.10 mass% or less, more preferably 0.09 mass% or less, even more preferably 0.08 mass% or less, and even more preferably 0.07 mass% or less. Here, "main metal element of the laser marking agent" means the metal element with the highest content among the metal elements contained in the laser marking agent. The main metal element of the laser marking agent preferably accounts for 50 mass% or more when the content of all metal elements in the laser marking agent is 100 mass%. Note that the main metal element of the laser marking agent may account for 50 mass% or more when the content of all metal elements in the film is 100 mass%. Examples of the main metal element of the laser marking agent include Sn (tin), Bi (bismuth), Ti (titanium), Nd (neodymium), Gd (gadolinium), Sb (antimony), Al (aluminum), and Mo (molybdenum). For example, the main metal element of IRIOTEC (registered trademark) 8825 (Merck Performance Materials, main component antimony-doped tin / mica) used in the examples described later is Sn, i.e., tin. On the other hand, the main metal element of TOMATEC COLOR42-920A (TOMATEC Corporation, main component Bi2O3) is Bi, i.e., bismuth. The fluctuation range of the content of the main metal element of the laser marking agent is the absolute value of the difference between the average value when the content of the main metal element of the laser marking agent is measured at 50 m intervals in the length direction of the film and the value farthest from the average value. This fluctuation range can be obtained by the method described in the examples. If the fluctuation range is 0.10% by mass or less, it is possible to reduce printing unevenness that may occur when laser printing is performed. The fluctuation range may be, for example, 0.001% by mass or more, 0.003% by mass or more, 0.005% by mass or more, 0.01% by mass or more, or 0.02% by mass or more.

[0095] Laser marking L along the length of the film *The variation in value is preferably 2.5 or less, more preferably 2.0 or less, even more preferably 1.7 or less, and even more preferably 1.5 or less. * The variation in value is determined by laser marking at 50m intervals along the length of the film, and then * value (i.e., L of the laser-irradiated part) * The variation is the difference between the maximum and minimum values ​​when the measured value (value) is measured. This variation can be obtained by the method described in the Examples. EXAMPLES

[0096] The present invention will be described in more detail below with reference to examples and comparative examples. In the following, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0097] <1. Raw materials> The following raw materials were used: <1.1. Polyolefin> Sumitomo Noblen® FS2011DG3 (polypropylene manufactured by Sumitomo Chemical Co., Ltd.) Novatec PP FL203D (polypropylene made by Japan Polypropylene Corporation) Sumikathen (registered trademark) FV405 (linear low-density polyethylene manufactured by Sumitomo Chemical Co., Ltd.) Harmolex NC564A (linear low-density polyethylene manufactured by Japan Polyethylene Co., Ltd.) Sumikathene (registered trademark) FV407 (linear low-density polyethylene manufactured by Sumitomo Chemical Co., Ltd.) Hi-Zex (HZ) 2300L (high density polyethylene manufactured by Prime Polymer Co., Ltd.)

[0098] The size, true specific gravity, bulk specific gravity, weight (specifically, weight per grain), and angle of repose were measured for these. The measurement methods are described below. The results are shown in Table 1. [Table 1] In Table 1, "-" indicates that the item was not measured or evaluated.

[0099] <1.2. Laser marking agent> IRIOTEC® 8825 (Merck Performance Materials, main component antimony-doped tin / mica) TOMATEC COLOR42-920A (TOMATEC Corporation, main component Bi2O3)

[0100] <2. Preparation of master batch pellets> <2.1. Preparation of pellets B, J, L, and M> FS2011DG3 and IRIOTEC (registered trademark) 8825 were mixed (dry blended) in a mass ratio of 80:20, fed into a twin-screw extruder, and melted and mixed at 250°C. A cylindrical strand was discharged from a strand die, cooled with water, and cut with a strand cutter to obtain pellet B. Pellets J, L, and M were obtained in the same manner as for pellet B, except that the raw materials were mixed as described in Table 2.

[0101] <2.2. Preparation of pellets E and K> FV405 and IRIOTEC (registered trademark) 8825 were mixed (dry blended) in a mass ratio of 90:10, fed into a twin-screw extruder, and melted and mixed at 250°C. Cylindrical strands were discharged from a strand die, cooled with water, and cut with a strand cutter to obtain pellets E. Pellet K was obtained in the same manner as pellet E, except that the raw materials were mixed as described in Table 2.

[0102] <2.3. Preparation of Pellet F> FV405 and silica were mixed so that the silica content was 20,000 ppm, and then charged into a twin-screw extruder and melted and mixed at 250° C. A cylindrical strand was discharged from a strand die, cooled with water, and cut with a strand cutter to obtain pellets F.

[0103] <2.4. Measurement results of masterbatch pellets> The size, true specific gravity, bulk specific gravity, weight (specifically, weight per pellet), and angle of repose of the master batch pellets were measured. The measurement methods will be described later. The results are shown in Table 2. [Table 2] In addition, "-" in the row of laser marking agent means that no laser marking agent was added. In the row of lubricant, "-" also means that no lubricant was added. The shape, size, true specific gravity, bulk specific gravity, and weight per pellet of pellet F have not been measured.

[0104] 3. Preparation of film <3.1. Preparation of film in Example 1> Pellet B and pellet C were mixed in a mass ratio of 1.5:98.5, and then fed from a hopper (inclined at 60 degrees) into a single screw extruder, melted at 250°C, and extruded from a T-die into a film-like melt. The film-like melt was cooled and solidified on a chill roll set at a surface temperature of 30°C. An unstretched film was thus obtained. The unstretched film was introduced into a longitudinal stretching machine in which a plurality of roll groups were arranged in series, and was preheated on a preheating roll until the film temperature reached 125°C, and then stretched 4.5 times. The film after longitudinal stretching was introduced into a transverse stretching machine (i.e., a tenter) and preheated for 5 seconds until the surface temperature reached 160°C, and then stretched 9 times in the width direction (transverse direction). The film was then introduced into a heat treatment zone and heat-treated at 163°C for 5 seconds. At this time, a 7% relaxation treatment was performed in the width direction. The film that had passed through the heat treatment zone was cooled with cooling air at 30°C for 5 seconds, and then both edges of the film were cut and removed, and a film with a width of 400 mm and a thickness of 40 μm was wound into a roll. This resulted in a film with a length of 500 m.

[0105] 3.2. Preparation of films in Examples 3 and 4 and Comparative Examples 2 and 3 A film was obtained in the same manner as in Example 1, except that the pellets were mixed as described in Table 3.

[0106] <3.3. Preparation of film in Comparative Example 1> As shown in Table 3, a film was obtained in the same manner as in Example 1, except that only pellet C was used as the pellet.

[0107] <3.4. Preparation of film in Example 2> To obtain the raw material for forming the core layer, pellets D, E, and G were mixed in a mass ratio of 30:3:67. On the other hand, to obtain the raw material for forming the skin layer, pellets F, H, and I were mixed in a mass ratio of 10:80:10. The raw material for forming the skin layer (i.e., a mixture of pellets F, H, and I) was fed to the first and third extruders and melted at 250°C. The raw material for forming the core layer (i.e., a mixture of pellets D, E, and G) was fed from a hopper (inclined at 60°C) to the second extruder and melted at 250°C. The melt from each extruder was guided to a feed block, laminated to form a skin layer / core layer / skin layer, and then a film-like melt was extruded from a T-die. At this time, the discharge ratio was adjusted so that the thickness ratio of the skin layer / core layer / skin layer was 15 / 70 / 15. The film-like melt was cooled and solidified on a chill roll set at a surface temperature of 30°C. Both edges of the film that had passed through the chill roll, i.e., the unstretched laminated film, were cut and removed, and a film 400 mm wide and 30 μm thick was wound into a roll, thereby obtaining a film 500 m long.

[0108] <4.Measurement method> <4.1.Size> Using a caliper, various lengths of the pellets were measured. Specifically, when the pellets were elliptical cylindrical, dimensions 1, 2, and 3 were measured according to Figure 1. On the other hand, when the pellets were ellipsoidal, dimensions 1, 2, and 3 were measured according to Figure 2. This measurement was performed for 10 pellets, and the average value was calculated.

[0109] <4.2. Weight per grain> The weight (g) of one pellet was measured using a weighing scale. This measurement was repeated for 10 pellets, and the average value was calculated.

[0110] <4.3.True specific gravity> After determining the volume of each grain, the true specific gravity (g / mm 3 When the pellets were cylindrical, the volume per pellet was calculated using the following formula. Volume = Height x Major axis x Minor axis x 3.14 That is, according to Figure 1, Volume = dimension 1 x dimension 2 x dimension 3 x 3.14 On the other hand, when the pellets are ellipsoidal as shown in FIG. 2, the volume per pellet was calculated using the following formula. Volume = dimension 1 x dimension 2 x dimension 3 x 4 / 3 x 3.14

[0111] <4.4. Bulk density> The pellets were placed in a metal cup until it was level, and the weight of the pellets in the cup was measured. This procedure was repeated twice, and the average value was calculated. The average value (i.e., the average weight of the pellets in the cup) was divided by the volume of the cup to obtain the bulk density (g / mm 3 The volume of the cup was determined by filling the cup with water, transferring the water to a measuring cylinder, and then measuring the volume of the water.

[0112] <4.5.Angle of repose> A metal cylindrical container stand with a diameter of 50 mm and a polyethylene funnel with an opening of 10 mm were prepared. With the funnel's opening (i.e., the 10 mm opening) positioned at a height of 50 mm from the center of the top surface of the stand (i.e., the plane with a diameter of 50 mm), the pellets in the funnel were dropped. This was continued until the periphery of the stand was overflowing with pellets. The angle of repose, i.e., the angle between the slope of the pellets piled up on the stand and the top surface of the stand (i.e., the horizontal plane), was measured with a protractor.

[0113] <4.6. Fluctuation range of main metal element content in laser marking agents> A 500m long film was sampled at 50m intervals. Specifically, samples were cut out from the 50m, 100m, 150m, 200m, 250m, 300m, 350m, 400m, and 450m positions of the 500m long film. For each sample, the content of the main metal element in the laser marking agent was measured, the average value (i.e., the average value of the content of the main metal element) was calculated, and the absolute value of the difference from the value farthest from the average value (maximum or minimum value) was calculated as the fluctuation range (i.e., the fluctuation range of the content of the main metal element in the laser marking agent). The content of the main metal element was calculated by the following method.

[0114] After weighing 50 mg of the sample into a 100 mL quartz Erlenmeyer flask, 3 mL of concentrated sulfuric acid was added, and the solution was gradually heated on a hot plate to perform wet carbonization until the solution turned black. Then, 30% hydrogen peroxide water was added to the solution until the solution became colorless and transparent, and the solution was further heated on a hot plate. After confirming that the color of the solution did not change due to this heating, the solution was allowed to cool to room temperature. The solution after cooling, that is, the decomposition solution after cooling, was placed in a 50 mL digital tube, and the volume was adjusted to 50 mL using 10 mL of 6N hydrochloric acid and ultrapure water. This resulted in a pretreatment solution. The pretreatment solution was measured using a high-frequency inductively coupled plasma emission spectrometer (SPECTROBLUE, manufactured by Hitachi High-Tech Science Corporation) to quantify the amount of metal elements, specifically the amount of major metal elements. When the sample contained IRIOTEC (registered trademark) 8825, Sn was quantified as the major metal element. On the other hand, when the sample contained TOMATEC COLOR42-920A, Bi was quantified as the major metal element. The content of the major metal element in the sample is A (ppm = mg / kg), the concentration of the major metal element in the pretreatment solution is B (mg / L), and the concentration of the major metal element in the blank test solution used as a measurement blank (i.e., 10 mL of 6N hydrochloric acid with ultrapure water to a constant volume of 50 mL) is C (mg / L). The amount of the major metal element in 50 mg of sample was calculated as follows. A = (BC) x 50 / 50

[0115] <4.7. Laser marking L * Variation in values> A 500m long film was sampled at 50m intervals. Specifically, samples were cut out from the 50m, 100m, 150m, 200m, 250m, 300m, 350m, 400m, and 450m positions of the 500m long film. Each sample was laser-printed, and the L of the laser marking was * value (i.e., L of the laser-irradiated part) * The L * The L value was measured twice for each sample. * The average value of the values ​​was calculated. The difference between the maximum and minimum values ​​of these average values ​​was used as the laser marking L. * It was calculated as the variation in value.

[0116] <4.7.1. Laser marking> Each sample was irradiated with a 355 nm ultraviolet (UV) laser marker (MD-U1000, Keyence Corporation) under the conditions of laser power 40%, scan speed 1000 mm / sec, pulse frequency 40 kHz, and spot variable -20, thereby printing "ABC123." The size of the characters was 0.8 cm ± 0.2 cm in height and 0.6 cm ± 0.2 cm in width per character (for example, "B").

[0117] <4.7.2.L * Value> Laser-printed L * value (i.e., L of the laser-irradiated part) * The L value was measured using a spectrophotometer (ZE-6000, manufactured by Nippon Denshoku Co., Ltd.) by the reflection method. Specifically, the measurements were performed using the following procedure. First, a 3 cm square sample was cut out so that all of the letters "B" from the printed "ABC123" would fit inside. Next, the sample was placed in the opening of a 6 mm diameter sample stage (the opening where the measurement light hits is approximately 1 cm in diameter) so that the letter "B" would fit inside. Then, using a 6 mm diameter viewing hole, * The values ​​were measured.

[0118] <5. Film evaluation results> [Table 3] The angle of repose of each pellet is indicated after its name. For Example 2, the thickness ratio of the three layers, ie, skin layer / core layer / skin layer, is 15 / 70 / 15.

[0119] Regarding the pellets containing the laser marking agent (i.e., pellets B, J, L, M, E, and K), the laser marking L was significantly larger when pellets B with a repose angle of 42 degrees, pellets J with a repose angle of 32 degrees, pellets E with a repose angle of 41 degrees, and pellets K with a repose angle of 36 degrees were used, compared to when pellets L with a repose angle of 55 degrees and pellets M with a repose angle of 23 degrees were used. * The variation in the values ​​was small. The range of variation in the amount of laser marking agent was also small. [Industrial Applicability]

[0120] INDUSTRIAL APPLICABILITY The present invention can provide pellets, molded articles (for example, films and containers), and methods for producing molded articles, and is therefore industrially applicable.

Claims

1. A polyolefin; a laser marking agent; The angle of repose is 25 degrees or more and 45 degrees or less. pellet.

2. The pellet according to claim 1 , wherein the content of the laser marking agent is from 1% by mass to 50% by mass.

3. 2. The pellet according to claim 1, wherein the weight of each pellet is 8 mg or more and 20 mg or less.

4. The pellets according to claim 1, which are used to manufacture a container.

5. A step of mixing at least the pellet according to any one of claims 1 to 4 and a second pellet; feeding the mixed pellets prepared in the step of mixing at least the pellets and the second pellets from a hopper to an extruder; and melting and extruding the mixed pellets in the extruder. Manufacturing method of molded products.

6. The method of claim 5 further comprising the step of blow molding a parison comprising the layer extruded by the extruder.

7. The method for producing a molded product according to claim 5 , wherein in the step of melting and extruding the mixed pellets in the extruder, a film-like melt is extruded.

8. The method for producing a molded article according to claim 5, wherein a difference between an angle of repose of the pellet and an angle of repose of the second pellet is 10 degrees or less in absolute value.

9. A polyolefin; A film comprising a laser marking agent, the fluctuation range of the content of the main metal element in the laser marking agent in the longitudinal direction of the film is 0.10 mass% or less, and the fluctuation range is the absolute value of the difference between the average value when the content of the main metal element is measured at 50 m intervals in the longitudinal direction of the film and the value farthest from the average value; film.

Citation Information

Patent Citations

  • Crystal nucleator for polyolefin resins, method for producing crystal nucleator for polyolefin resins, and method for improving fluidity of crystal nucleator for polyolefin resins

    WO2018052010A1

  • Laser-printable film and packaging in which same is used

    WO2021125135A1

  • Resin raw material composition for molding use, resin raw material composition for microporous membranes, and methods respective for producing those products

    WO2022138963A1

  • Manufacture of semiconductor device

    JP1987060265A

  • Small pouch packaging with date display and method for manufacturing the small pouch packaging.