Ferrite-austenite duplex stainless steel plate
A ferritic-austenitic duplex stainless steel sheet with controlled oxide film and grain size addresses the challenge of balancing strength, corrosion resistance, and etched surface quality, supporting precise etching in electronic and precision machinery components.
Patent Information
- Application Number
- JP2023048350
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Existing stainless steel materials struggle to balance high strength, excellent corrosion resistance, and smooth etched surface finish while maintaining flatness before and after etching, especially in components exposed to corrosive environments, and there is a need for materials that support downsizing and weight reduction without compromising rigidity.
A ferritic-austenitic duplex stainless steel sheet with a specific chemical composition and controlled oxide film formation through strain relief heat treatment in a reducing atmosphere, ensuring a minimum Mn concentration and thickness in the oxide film, along with a fine average grain size and controlled metallographic structure.
The solution provides a stainless steel sheet with enhanced corrosion resistance, high strength, and excellent etched surface smoothness and flatness, suitable for precision machinery and electronic equipment, enabling effective etching processes without warping.
Smart Images

Figure 2024137013000001 
Figure 2024137013000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic-austenitic duplex stainless steel sheet, and in particular to a ferritic-austenitic duplex stainless steel sheet with excellent corrosion resistance suitable as a component material for electronic devices and precision machines. [Background technology]
[0002] Parts used in electronic devices and precision instruments may be exposed to corrosive environments, in which case the material used must be corrosion resistant. There is also a demand for parts to be made smaller and lighter, and the corresponding materials need to be thinner while still being stronger to maintain the rigidity required for the parts.
[0003] In addition, when manufacturing the above-mentioned parts, a method of partially thinning the plate thickness by etching is often used as one of the means for obtaining a predetermined shape with high precision. Therefore, the material of the above-mentioned parts is required to have small shape change and no plate warping after etching, that is, excellent flatness before and after etching and smoothness of the etched surface.
[0004] Sheet warpage refers to the deformation of the entire steel sheet after partial etching (herein referred to as "half etching") of the steel sheet surface. The warpage of the steel sheet after half etching is caused by the residual stress of the steel sheet. Therefore, the warpage can be reduced by carrying out a heat treatment for the purpose of relieving the stress after temper rolling, that is, a so-called stress relief heat treatment.
[0005] Furthermore, the material for the above-mentioned parts is often austenitic stainless steel, which has an excellent balance between strength and elongation among stainless steels that generally have excellent corrosion resistance, and whose strength has been increased by temper rolling, etc. In particular, metastable austenitic stainless steels such as SUS301 and SUS304 are used, which combine high strength associated with deformation-induced martensitic transformation with excellent workability due to the TRIP effect, and which are relatively easy to obtain high strength among the above-mentioned austenitic stainless steels.
[0006] The austenitic stainless steel sheet, the strength of which has been increased by temper rolling or the like, is further subjected to shape correction using a tension leveler, distortion relief heat treatment for the purpose of reducing residual stress, and the like. This is to make the steel sheet shaped and flat in response to the precision machining of the above-mentioned parts. In addition, when small pieces corresponding to parts are taken out from a material manufactured from a relatively large steel sheet or steel strip by pressing, etching, or the like, or when the thickness of a part of the small pieces is reduced by further etching, as described above, deformation due to residual stress occurs. Furthermore, the more excellent the smoothness of the processed surface, particularly the etched surface (hereinafter also referred to as the etched surface), the more precise parts with higher dimensional accuracy can be manufactured from the material.
[0007] Patent Document 1 discloses a stainless steel sheet for photoetching in which the average crystal grain size is refined so as to obtain a smooth etched surface, and which is further subjected to a distortion relief heat treatment.
[0008] Patent Document 2 discloses a method for manufacturing an austenitic stainless steel sheet in which cold rolling conditions and straightening conditions using a tension leveler are adjusted, and further a tension equivalent to 0.2% yield strength or less of the cold-rolled material is applied to perform a strain relief heat treatment. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2005-320587 A [Patent Document 2] JP 2001-226718 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, since strain relief heat treatment is a heat treatment carried out in a temperature range where sensitization of stainless steel is likely to occur, it is necessary to select a material that is less likely to cause sensitization for the steel plate to be subjected to strain relief heat treatment. In such cases, there is a possibility that the strength cannot be ensured. As described above, it has been difficult to obtain a stainless steel sheet that has the required excellent corrosion resistance while also having high strength suitable for small size and weight reduction, excellent smoothness of the etched surface, and flatness before and after etching.
[0011] The present invention aims to provide a ferritic-austenitic duplex stainless steel sheet having excellent corrosion resistance, high strength, smoothness of the etched surface, and excellent flatness before and after etching. [Means for solving the problem]
[0012] In order to solve the above problems, the inventors have conducted extensive research into the use of surface oxide films in duplex stainless steels having a specific chemical composition and the stress relief heat treatment for this purpose. As a result, they have found that by subjecting duplex stainless steels having specific components to stress relief heat treatment in a reducing atmosphere, an oxide film containing a specific concentration of Mn or more is formed, and when the thickness of the oxide film is greater than or equal to a specific value, the corrosion resistance is improved. They have also found that a fine average crystal grain size can be maintained even after stress relief heat treatment, and that high strength, excellent smoothness of the etched surface, and flatness after etching can be secured. The present invention has been completed by clarifying the characteristics of the chemical composition and metal structure of the steel sheet that can achieve these effects.
[0013] The present invention has been made based on the above findings and further studies, and the gist of the present invention, which has the object of solving the above problems, is as follows.
[0014] [1] A base steel plate; and an oxide film formed on the base steel sheet, The chemical composition of the base steel sheet is, in mass%, C: 0.08% or less, Si: 0.2-1.0%, Mn: 0.8-3.0%, Cr: 20.0-28.0%, Ni: 2.0-6.0%, Mo: 1.0-3.0%, N: 0.10-0.30%, Cu: 0-2.0%, Nb: 0-0.50%, Ti: 0 to 0.50%, V: 0 to 0.50%, W: 0 to 0.50%, Co: 0-0.50%, B: 0 to 0.0050%, Sn: 0-0.50%, Al: 0-0.50%, Mg: 0 to 0.010%, Ca: 0 to 0.0100%, Ta: 0 to 0.050%, Ga: 0 to 0.050%, Zr: 0 to 0.50%, and Rare earth elements: 0~0.010% with the remainder being Fe and impurities, The average crystal grain size is 2.0 μm or less, Vickers hardness is 400HV or more. The thickness of the oxide film is 15 nm or more, A ferritic-austenitic duplex stainless steel sheet, characterized in that the Mn concentration in the oxide film is 1.5% or more. [2] The ferritic-austenitic duplex stainless steel sheet according to [1] above, characterized in that in the metal structure, the ferritic phase ratio is 20 to 80%. [3] A ferritic-austenitic duplex stainless steel sheet according to [1] or [2] above, characterized in that the radius of curvature after half-etching is 150 mm or more. [4] A ferritic-austenitic duplex stainless steel sheet according to [1] or [2] above, characterized in that it is used for parts of electronic devices or precision instruments. [5] A ferritic-austenitic duplex stainless steel sheet according to the above [3], characterized in that it is used for parts of electronic devices or precision instruments. Effect of the Invention
[0015] According to the present invention, it is possible to provide a ferritic-austenitic duplex stainless steel sheet which has excellent corrosion resistance, high strength, excellent smoothness of the etched surface, and excellent flatness before and after etching. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, a ferritic-austenitic duplex stainless steel sheet according to an embodiment of the present invention (hereinafter, also referred to as "duplex stainless steel sheet", "stainless steel sheet" or "steel sheet") will be described in detail.
[0017] 1. Ferritic-austenitic duplex stainless steel plate The ferritic-austenitic duplex stainless steel sheet according to this embodiment comprises a base steel sheet and an oxide coating formed on the base steel sheet.
[0018] (chemical composition) First, the chemical composition of the base steel sheet of the duplex stainless steel sheet according to this embodiment will be described in detail. The austenite phase (γ phase) constituting the duplex stainless steel sheet according to this embodiment is composed of a stable γ phase that does not exhibit deformation-induced transformation. In other words, the chemical composition of the duplex stainless steel sheet according to this embodiment is a component system that does not exhibit deformation-induced transformation. The specific chemical composition will be described below. Note that, unless otherwise noted, % for element content in this specification means mass %.
[0019] C: 0.08% or less Carbon (C) is an element that acts as a stabilizing element for the austenite phase. If the C content exceeds 0.08%, coarse Cr carbonitrides are generated, which may reduce corrosion resistance. Therefore, the C content is set to 0.08% or less, preferably 0.06% or less, and more preferably 0.04% or less. There is no particular lower limit for the C content. However, if the C content is reduced too much, the manufacturing cost increases. From this viewpoint, the C content is preferably 0.005% or more.
[0020] Silicon: 0.2 to 1.0% Silicon (Si) is an element that acts as a stabilizing element for the ferrite phase. Si is also an effective element for generating an oxide film on the surface of the steel sheet. If the Si content is less than 0.2%, the thickness of the oxide film cannot be ensured, and there is a risk that corrosion resistance cannot be ensured. Therefore, the Si content is set to 0.2% or more. It is preferably 0.3% or more, and more preferably 0.4% or more. On the other hand, if the Si content exceeds 1.0%, cracking during manufacturing is promoted. Also, excessive inclusion of Si is a factor that inhibits the workability of parts. Therefore, the Si content is set to 1.0% or less. It is preferably 0.9% or less, and more preferably 0.6% or less.
[0021] Mn: 0.8-3.0% Mn is an element that acts as a stabilizing element for the austenite phase. Mn is also an effective element for the formation of an oxide film during stress relief heat treatment, and is presumed to contribute to improving corrosion resistance. If the Mn content is less than 0.8%, the thickness of the oxide film and the Mn concentration in the oxide film will be insufficient, and there is a possibility that corrosion resistance cannot be ensured. Therefore, the Mn content is set to 0.8% or more. It is preferably set to 1.0% or more, and more preferably set to 1.2% or more. On the other hand, if the Mn content exceeds 5.0%, it will lead to an increase in manufacturing costs. Therefore, the Mn content is set to 5.0% or less. It is preferably set to 4.0% or less, and more preferably set to 3.0% or less.
[0022] Cr: 20.0~28.0% Chromium (Cr) is an element that acts on the phase ratio as a stabilizing element of the ferrite phase. In addition, Si is also an element that is effective in generating an oxide film on the surface of the steel sheet. In addition, Cr also acts as an element that improves corrosion resistance. If the Cr content is less than 20.0%, the corrosion resistance may be insufficient. Therefore, the Cr content is set to 20.0% or more. It is preferably 22.0% or more, and more preferably 23.0% or more. On the other hand, if the Cr content exceeds 28.0%, it may lead to a decrease in workability and an increase in manufacturing costs. Therefore, the Cr content is set to 28.0% or less. It is preferably 26.0% or less, and more preferably 25.0% or less.
[0023] Ni: 2.0~6.0% Nickel (Ni) is an element that acts as a stabilizing element for the austenite phase. Ni is also an element that improves corrosion resistance. If the Ni content is less than 1.0%, the corrosion resistance after stress relief heat treatment may be insufficient. Therefore, the Ni content is set to 1.0% or more. It is preferably 1.2% or more, and more preferably 1.5% or more. On the other hand, if the Ni content exceeds 6.0%, it may lead to an increase in alloy costs and an impairment of manufacturability. Therefore, the Ni content is set to 6.0% or less. It is preferably 5.8% or less, and more preferably 5.5% or less.
[0024] Mo: 1.0-3.0% Molybdenum (Mo) is an element that acts as a stabilizing element for the ferrite phase. It is also an element that effectively acts on corrosion resistance. If the Mo content is less than 1.0%, the corrosion resistance may be insufficient. Therefore, the Mo content is set to 1.0% or more. It is preferably 1.1% or more, and more preferably 1.2% or more. On the other hand, if the Mo content exceeds 3.0%, there is a risk of causing a decrease in workability and an increase in manufacturing costs. Therefore, the Mo content is set to 3.0% or less. It is preferably 2.6% or less, and more preferably 2.0% or less.
[0025] N: 0.10~0.30% Nitrogen (N), like C, is an element that acts as a stabilizing element for the austenite phase. It is also an element that effectively acts on corrosion resistance. If the N content is less than 0.10%, corrosion resistance may not be ensured. Therefore, the N content is set to 0.10% or more. It is preferably 0.12% or more, and more preferably 0.14% or more. On the other hand, if the N content exceeds 0.30%, coarse Cr carbonitrides may be generated, which may reduce corrosion resistance. Therefore, the N content is set to 0.30% or less. It is preferably 0.28% or less, and more preferably 0.20% or less.
[0026] The above is the basic chemical composition of the ferritic-austenitic stainless steel sheet of this embodiment, with the remainder being iron (Fe) and impurities. Furthermore, the ferritic-austenitic stainless steel sheet of this embodiment may optionally contain one or more of Cu, Nb, Ti, V, W, Co, B, and Sn in order to further improve workability, corrosion resistance, and hot workability. The lower limit of these elements is 0% or more, and preferably more than 0%.
[0027] Cu:2.0% or less Copper (Cu) is an austenite stabilizing element, and also has the effect of improving corrosion resistance by suppressing the precipitation of nitrides. Therefore, the Cu content may be 0.10% or more. However, if the Cu content exceeds 2.0%, it may increase the raw material cost and deteriorate the hot workability. Therefore, the Cu content is preferably 2.0% or less, and more preferably 1.8% or less.
[0028] Nb: 0.50% or less Niobium (Nb) forms nitrides (NbN) and carbides (NbC) and has the effect of improving workability. Therefore, the Nb content may be 0.01% or more. However, if the Nb content exceeds 0.50%, there is a risk of reducing ductility, so the Nb content is preferably 0.50% or less. The Nb content is more preferably 0.30% or less, and even more preferably 0.20% or less.
[0029] Ti: 0.50% or less Titanium (Ti), like Nb, forms nitrides (TiN) and carbides (TiC) and has the effect of improving workability. Therefore, the Ti content may be 0.01% or more. However, if the Ti content exceeds 0.50%, there is a risk of reducing ductility, so the Ti content is preferably 0.50% or less. The Ti content is more preferably 0.30% or less, and even more preferably 0.20% or less.
[0030] V: 0.50% or less Vanadium (V) forms nitrides and has the effect of improving workability. Therefore, the V content may be 0.01% or more. However, if the V content exceeds 0.50%, there is a risk of reducing ductility and hot workability, so the V content is preferably 0.50% or less, and more preferably 0.40% or less.
[0031] W: 0.50% or less Tungsten (W) is an element that improves corrosion resistance, and in order to exert this effect, the W content is preferably 0.05% or more. However, if the W content exceeds 0.50%, there is a risk of reducing workability, so the W content is preferably 0.50% or less, and more preferably 0.40% or less.
[0032] Co:0.50% or less Cobalt (Co) has the effect of increasing high-temperature strength and improving hot workability. Therefore, the Co content is preferably 0.01% or more. However, if the Co content exceeds 0.50%, there is a risk of reducing toughness, so the Co content is preferably 0.50% or less, and more preferably 0.30% or less.
[0033] B: 0.0050% or less Boron (B) is an element that segregates to grain boundaries and improves hot workability. To achieve this effect, the B content is preferably 0.0002% or more. However, if the B content exceeds 0.0050%, the corrosion resistance may be significantly deteriorated, so the B content is preferably 0.0050% or less, and more preferably 0.0030% or less.
[0034] Sn: 0.50% or less Tin (Sn) is an element that can improve corrosion resistance. To achieve this effect, the Sn content is preferably 0.01% or more, and more preferably 0.03% or more. However, if the Sn content exceeds 0.50%, there is a risk of deteriorating hot workability, so the Sn content is preferably 0.50% or less, and more preferably 0.40% or less.
[0035] Furthermore, the ferritic-austenitic stainless steel sheet of this embodiment may optionally contain one or more of Al, Ca, Mg, Ta, Ga, Zr, and rare earth elements for deoxidization and desulfurization during refining. The lower limit of these elements is 0% or more, preferably more than 0%.
[0036] Al: 0.50% or less Aluminum (Al) may be contained in small amounts for desulfurization and deoxidation. The above effects are exhibited when the Al content is 0.01%, so the Al content is preferably 0.01% or more. However, when the Al content exceeds 0.50%, there is a risk of increasing manufacturing defects and increasing raw material costs, so the Al content is preferably 0.50% or less.
[0037] Mg: 0.010% or less Magnesium (Mg) not only deoxidizes but also has the effect of refining the solidified structure. To achieve these effects, the Mg content is preferably 0.0002% or more. However, if the Mg content exceeds 0.010%, it will increase the cost of the steelmaking process, so the Mg content should be 0.010% or less.
[0038] Ca:0.0100% or less A small amount of calcium (Ca) may be contained for desulfurization and deoxidization. The above effects are exhibited when the Ca content is 0.0001% or more, so the Ca content is preferably 0.0001% or more. However, if the Ca content exceeds 0.0100%, there is a risk of hot work cracking and a decrease in corrosion resistance, so the Ca content is preferably 0.0100% or less, and more preferably 0.0050% or less.
[0039] Ta: 0.050% or less Tantalum (Ta) is an element that improves corrosion resistance by modifying inclusions, and may be contained as necessary. In order to exert this effect, the Ta content is preferably 0.0002% or more. However, if the Ta content exceeds 0.050%, there is a risk of causing a decrease in room temperature ductility and toughness, so the Ta content is preferably 0.050% or less, more preferably 0.030% or less.
[0040] Ga: 0.050% or less Gallium (Ga) is an element that improves corrosion resistance and suppresses hydrogen embrittlement, and may be contained as necessary. In order to exert this effect, the Ga content is preferably 0.0002% or more. However, if the Ga content exceeds 0.050%, there is a risk of causing a decrease in workability, so the Ga content is preferably 0.050% or less, and more preferably 0.030% or less.
[0041] Zr: 0.50% or less Zirconium (Zr) has a similar effect to Nb and Ti, and is also an element that improves oxidation resistance. To achieve these effects, the Zr content is preferably 0.01% or more. However, if the Zr content exceeds 0.50%, it will lead to an increase in raw material costs, so the Zr content is preferably 0.50% or less, and more preferably 0.30% or less.
[0042] Rare earth elements: 0.010% or less Rare earth elements (REM) are elements that improve hot workability. The above effects are achieved when the total content of rare earth elements is 0.0002% or more, so the content of rare earth elements may be 0.0002% or more. However, if the total content of rare earth elements exceeds 0.010%, manufacturability is impaired and costs increase, so the upper limit of rare earth elements is preferably 0.010%. A more preferable content range of rare earth elements is 0.0005 to 0.008%.
[0043] Here, rare earth elements (REM) refer to two elements, scandium (Sc) and yttrium (Y), and 15 elements (lanthanoids) from lanthanum (La) to lutetium (Lu). In this specification, "rare earth elements" refers to one or more elements selected from these rare earth elements, and "content of rare earth elements" refers to the total amount of rare earth elements.
[0044] The stainless steel sheet of this embodiment contains, in addition to the elements described above, Fe and impurities (including unavoidable impurities). However, in addition to the elements described above, other elements can also be contained within a range that does not impair the effects of the present invention.
[0045] In addition, scrap materials are often used in the manufacture of stainless steel sheets. Therefore, various impurity elements are often inevitably mixed into the stainless steel sheets, and it is difficult to determine the content of the impurity elements uniquely. Therefore, the impurities in this embodiment refer to elements contained in an amount that does not impair the effects of the present invention.
[0046] (Metal structure) In the metal structure of the ferritic-austenitic duplex stainless steel sheet of this embodiment, when the ferritic phase ratio is within a predetermined range, the average crystal grain size of the metal structure can be easily refined. The ferritic phase ratio is preferably 20% or more and 80% or less. When the ferritic phase ratio is within this range, the ferritic phase and the austenitic phase inhibit each other's grain growth, and the crystal grains can be further refined. It is more preferably 25% or more and 75% or less, and even more preferably 30% or more and 70% or less. From the viewpoint of the above-mentioned grain growth inhibition effect, the ferritic phase ratio is most preferably 50%.
[0047] <Average grain size> In order to achieve high strength of the steel sheet and obtain excellent smoothness of the etched surface, it is effective to make the average crystal grain size of the metal structure 2.0 μm or less. If the average crystal grain size exceeds 2.0 μm, the etched surface becomes rough, and good smoothness of the etched surface cannot be obtained. The average crystal grain size is preferably 1.5 μm or less, and more preferably 1.0 μm or less. The lower limit of the average crystal grain size is not particularly limited, but may be 0.4 μm or more for practical purposes.
[0048] (Vickers hardness) As a material that can respond to the trend toward smaller and lighter electronic devices and precision machinery, and the associated trend toward thinner materials, it is effective for the steel plate to have a Vickers hardness (hereinafter also simply referred to as "hardness") of 400 HV or more. The hardness is preferably 410 HV or more, and more preferably 420 HV or more. There is no particular upper limit to the hardness, but it is set to 440 HV or less in consideration of the processability during part molding. On the other hand, if the hardness is less than 400 HV, the strength required as a material for the parts cannot be ensured.
[0049] Hardness and strength are considered to be proportional to each other, and a 400HV steel plate can be said to have a 0.2% yield strength of 1200MPa or more. Furthermore, the total elongation (elongation at break) at that time is about 5%.
[0050] (Radius of curvature after half etching) In order to obtain flatness of the steel sheet before and after etching, it is effective that the radius of curvature after half etching is 150 mm or more. The radius of curvature after half etching is preferably 175 mm or more, and more preferably 200 mm or more. The upper limit of the radius of curvature before and after etching is desirably ∞ (infinity), i.e., no warping, and is not particularly limited. However, in addition, the value after half etching may be 400 mm or less in practical use. On the other hand, if the radius of curvature after half etching is less than 150 mm, the flatness before and after etching required for the material of the part cannot be ensured.
[0051] The term "half etching" used here refers to etching one of the rolled surfaces of a steel sheet in the sheet thickness direction until the sheet thickness is reduced to half. Half etching is performed by coating the rolled surface with nail polish and immersing it in an etching solution such as ferric chloride.
[0052] (Oxide film) In order to obtain the necessary corrosion resistance, it is effective that the thickness of the oxide film formed on the base steel sheet is 15 nm or more and the Mn concentration in the oxide film is 1.5% or more. If the thickness of the oxide film is less than 15 nm, the necessary corrosion resistance cannot be ensured. In addition, a dense oxide film is obtained by containing a predetermined amount or more of Mn in the oxide film, and corrosion resistance is ensured. From these viewpoints, the thickness of the oxide film is preferably 17 nm or more, more preferably 20 nm or more. The thicker the oxide film, the better the corrosion resistance, but if it exceeds 200 nm, it may exhibit interference colors and impair the appearance of the steel sheet. It is preferably 150 nm or less. In addition, the Mn concentration in the oxide film is preferably 1.7% or more, more preferably 2.0% or more. The upper limit of the Mn concentration in the oxide film is not particularly limited, but it may be 4.5% or less.
[0053] The thickness of the oxide film can be determined by the following method. X-ray photoelectron spectroscopy (GDS) is used to obtain an element concentration profile in the depth direction of a duplex stainless steel sheet, and the depth position where the oxygen (O) concentration (strength) is half that of the outermost surface of the oxide film is determined. In this embodiment, the distance in the depth direction from the outermost surface of the steel sheet to the position where the O concentration (strength) is half is defined as the "thickness of the oxide film." The thickness of the oxide film is measured by GDS five times from the outermost surface to a depth of 200 nm, and the average of the measurement results is used as the representative value.
[0054] The Mn concentration in the oxide film can be determined by the following method. The concentration profile obtained by GDS is converted to mass concentration (%), and the lowest Mn concentration in the depth range (distance) defined as the thickness of the oxide film above is defined as the "Mn concentration in the oxide film." Concentration measurements using GDS are performed five times up to a depth of 200 nm, and the average of the measurement results is used as the representative value.
[0055] (Thickness) The thickness of the duplex stainless steel plate according to this embodiment is not particularly limited, but may be 3.0 to 0.05 mm. It is preferably 0.08 mm or more. Furthermore, by making the thickness 1.5 mm or less, it becomes easy to refine the metal structure, and the above-mentioned metal structure can be easily ensured. Therefore, the thickness may be 1.0 mm or less. It is preferably 0.5 mm or less.
[0056] 2. Manufacturing method of ferritic-austenitic duplex stainless steel sheet A method for manufacturing the ferritic-austenitic duplex stainless steel sheet of this embodiment will now be described. The ferritic-austenitic duplex stainless steel sheet according to this embodiment can achieve the above-mentioned effects as long as it has the above-mentioned characteristics, regardless of the manufacturing method. However, in order to achieve both corrosion resistance, strength, smoothness of the etched surface, and flatness before and after etching, it is necessary to control the metal structure (particularly the average crystal grain size), oxide film, and hardness as described above. The above-mentioned metal structure, oxide film, and hardness can be achieved by combining the chemical composition of the steel with appropriate manufacturing conditions. A preferred manufacturing method for obtaining the ferritic-austenitic duplex stainless steel sheet of this embodiment will be described below.
[0057] (Manufacturing method) First, a steel slab having the above-mentioned chemical composition, which is produced by continuous casting or ingot casting after melting, is hot-rolled into a steel sheet (hot rolling process). Then, a hot-rolled sheet annealing process, a pickling process, and a cold rolling process are performed to obtain a cold-rolled sheet having a predetermined thickness. The hot-rolled sheet annealing may be performed as necessary, and may be omitted. Each of the above processes may be a general manufacturing method for ferritic-austenitic duplex stainless steel sheet.
[0058] (Finish annealing process) Finish annealing is performed on the cold-rolled steel sheet controlled to a predetermined thickness in the cold rolling process. The finish annealing temperature is 850°C or more and 1050°C or less. If the finish annealing temperature is less than 850°C, the metal structure will be a mixture of recrystallized grains and non-recrystallized grains, resulting in a state in which the hardness between the crystal grains varies. If the hardness varies between the crystal grains, good flatness cannot be obtained after shape correction by a tension leveler. On the other hand, if the finish annealing temperature exceeds 1050°C, the average crystal grain size after the finish annealing will become coarse, and the average crystal grain size after the distortion relief heat treatment will also become coarse. Therefore, the finish annealing temperature is 850°C or more and 1050°C or less. The annealing time (holding time) in the finish annealing process can be set appropriately. Typically, it is 600 seconds or less. It is preferably 400 seconds or less, more preferably 150 seconds or less. From the viewpoint of recrystallization, the lower limit of the annealing time in the final annealing step may be set to 5 seconds or more.
[0059] After the finish annealing process, the steel sheet is cooled to room temperature (around 25°C). The average cooling rate during cooling may be 1°C / sec to 100°C / sec. If the average cooling rate is less than 1°C / sec, grain growth may occur during the cooling process. In addition, taking into consideration productivity and pickling properties, the average cooling rate is preferably 5 to 50°C / sec. Here, the "average cooling rate" is defined as the temperature drop of the steel sheet from the start of cooling (end of holding) to room temperature divided by the time required to cool from the start of cooling to room temperature.
[0060] (Temper rolling process) After the finish annealing process, temper rolling is performed (temper rolling process). Temper rolling is a process for improving the strength of the material (steel plate). The temper rolling in this embodiment may be a common manufacturing method in stainless steel manufacturing, and the temper rolling reduction ratio may be adjusted according to the desired strength. For example, the temper rolling ratio may be 40 to 70%. Note that the austenite phase of the ferritic-austenitic duplex stainless steel in this embodiment is in a stable state, and deformation-induced martensite is not generated during temper rolling.
[0061] (shape correction process) The steel sheet after the temper rolling is repeatedly bent while applying a tension of 0.5 to 3.0% elongation by a tension leveler, thereby performing shape correction (shape correction process). Shape correction by a tension leveler is a process for ensuring flatness of the steel sheet, and is usually controlled by the elongation. The shape correction process in this embodiment can be performed under general conditions in the production of ferritic-austenitic duplex stainless steel sheets, but it is preferable to set the elongation to 0.5 to 3.0%. If the elongation is less than 0.5%, warping after half etching may become large. On the other hand, if the elongation exceeds 3.0, hardening may occur in the production line. From the viewpoint of stable production, the elongation is preferably in the range of 0.5% to 1.5%.
[0062] (Distortion heat treatment process) After shape straightening using a tension leveller, the steel plate is subjected to stress relief heat treatment at a temperature range of 700°C to 800°C (strain relief heat treatment process). Strain relief heat treatment is a process for providing an oxide film on the steel plate, and is also a process for reducing residual stress caused by temper rolling and shape straightening using a tension leveller.
[0063] The strain relief heat treatment of this embodiment is preferably performed in a dew point range of -50°C to -30°C and a temperature range of 700°C to 800°C so as to provide a reducing atmosphere of Cr. By performing the strain relief heat treatment under the above conditions, an oxide film containing a predetermined or higher Mn concentration and having a predetermined or higher thickness can be obtained. More preferably, the conditions of the strain relief heat treatment are a dew point of -45°C to -35°C and a temperature range of the strain relief heat treatment of 725°C to 775°C. If the dew point is less than -50°C, the thickness of the oxide film may not be ensured. On the other hand, if the dew point exceeds -30°C, the oxide film may become thick and may develop color. If the dew point is too high, the thickness of the oxide film may become uneven, and the corrosion resistance may not be ensured locally. If the temperature of the strain relief heat treatment is less than 700°C, the thickness of the oxide film may be insufficient, and the necessary corrosion resistance may not be ensured. If the temperature of the strain relief heat treatment is too low, the removal of residual stress may also be insufficient. On the other hand, if the temperature of the stress relief heat treatment exceeds 800°C, the hardness significantly decreases, and the necessary strength cannot be ensured.
[0064] The treatment time (annealing time) of the strain relief heat treatment is preferably, for example, 15 seconds or more. More preferably, it is 20 seconds or more. The thickness of the oxide film increases as the treatment time of the strain relief heat treatment increases. There is no need to particularly limit the upper limit of the time of the strain relief heat treatment, and the treatment time of the strain relief heat treatment may be adjusted within a range that ensures the required strength and steel sheet appearance. However, assuming production by continuous sheet threading, the industrial upper limit of the treatment time of the strain relief heat treatment is 600 seconds or less. Preferably, it is 300 seconds or less.
[0065] The stress relief heat treatment in this embodiment is preferably performed in a reducing atmosphere of Cr (hereinafter, also referred to as "bright annealing"). For example, the stress relief heat treatment may be performed in a reducing atmosphere of a mixed gas of 25% nitrogen + 75% nitrogen.
[0066] The cooling of the steel sheet after the strain heat treatment step is preferably slow cooling. Specifically, the average cooling rate in the range from after the strain heat treatment to 500°C is preferably 2°C / sec or less, more preferably 1°C / sec or less. More preferably, the cooling temperature is up to 400°C. This allows a predetermined residual stress and oxide film to be obtained.
[0067] The process described above makes it possible to manufacture the ferritic-austenitic duplex stainless steel sheet according to this embodiment. EXAMPLES
[0068] In order to confirm the effects of the present invention in detail, the following experiment was carried out. Note that this example shows one embodiment of the present invention, and the present invention is not limited to the following configuration.
[0069] Steel having the chemical composition shown in Table 1 was melted to obtain an ingot having a thickness of 100 mm. The ingot was then heated to 1230°C, and hot-rolled to obtain a hot-rolled sheet having a thickness of 5.0 mm. The hot-rolled sheet was then annealed (annealing temperature: 1060°C, annealing time: 60 seconds), and cold-rolled with intermediate annealing repeatedly performed to obtain a cold-rolled sheet having a thickness of 0.29 mm. The cold-rolled sheet was heated at the finish annealing temperature in Table 2 for 90 seconds, and then cooled to room temperature at an average cooling rate of 20°C / s to obtain a finish annealed sheet. Furthermore, the finish annealed sheet was subjected to temper rolling at a rolling rate of 60% and shape correction using a tension leveler (TL) with an elongation rate of 1.0%, to obtain a steel sheet having a thickness of 0.10 mm. Then, a strain relief heat treatment was performed at 750°C under the conditions shown in Table 2 to obtain a duplex stainless steel sheet. The atmosphere for the stress relief heat treatment was either bright annealing (a reducing atmosphere of a mixed gas of 25% nitrogen + 75% nitrogen) or air annealing. When air annealing was performed, the steel sheet was pickled after annealing to remove oxide scale from the surface. The resulting duplex stainless steel sheets were subjected to the following various evaluation tests.
[0070] (Method of measuring average crystal grain size) The average crystal grain size was determined as follows: The L-section (plane including the rolling direction and the sheet thickness direction) of the steel sheet prepared by electrolytic polishing was measured by electron backscatter diffraction (EBSD). The measurement area was 100 μm × 300 μmL at the center of the sheet thickness, and the measurement step size was 0.1 μm. Using the analysis software "OIM-Analysis" made by TSL Solutions, plot data with a Confidence Index value of more than 0.1 was extracted from the measured data, and the average grain size was calculated by quadrature. If the crystal orientation difference between adjacent plot data was less than 15°, they were considered to be the same grain, and if the orientation difference was 15° or more, they were treated as different grains. In addition, no distinction was made between the ferrite phase and the austenite phase when calculating the average grain size.
[0071] (Hardness measurement method) The hardness of the steel plate surface was measured using a Vickers hardness tester in accordance with JIS Z 2244:2009. The steel plate surface was measured 10 times with a load of 0.5 kgf, and the average value was calculated and used as the representative value. If the hardness was 400 HV or more, it was deemed to have the necessary strength and passed the test.
[0072] (Method of measuring ferrite phase ratio) The measurement of the ferrite phase ratio was specified as follows: A number of test pieces measuring t×40 mm were cut out from the steel plate, stacked to a total thickness of 2 mm or more, and then measured using a ferrite meter. The measurement was carried out five times, and the average value was taken as the ferrite phase ratio of the steel plate.
[0073] (Method for measuring oxide film thickness and Mn concentration in oxide film) The oxide film thickness was determined as follows: First, the element concentration profile in the depth direction of the obtained duplex stainless steel sheet was obtained by X-ray photoelectron spectroscopy (GDS), and the depth position where the O concentration (strength) was 1 / 2 of the outermost surface of the oxide film was determined. In this example, the distance in the depth direction from the outermost surface of the steel sheet (i.e., the outermost surface of the oxide film) to the position where the O concentration (strength) was 1 / 2 was defined as the "oxide film thickness." The oxide film thickness was measured five times by GDS from the outermost surface to a depth of 200 nm, and the average value of the obtained measurement results was used as the representative value. On the other hand, the Mn concentration in the oxide film was determined as follows. The concentration profile obtained by GDS was converted to mass concentration (%), and the lowest Mn concentration in the depth range (distance) defined as the oxide film thickness above was defined as the "Mn concentration in the oxide film." The concentration measurement by GDS was performed five times up to a depth of 200 nm, and the average of the measurement results was used as the representative value of the Mn concentration in the oxide film.
[0074] (Evaluation test of smoothness of etched surface) One surface of a test piece cut from a steel plate with a thickness of 0.1 mm x 50 mm x 50 mm was etched by spraying an aqueous solution of ferric chloride with a specific gravity of 1.35 heated to 50°C for 4 minutes. The smoothness of the etched surface was measured using a contact surface roughness meter to measure the arithmetic mean roughness Ra along the direction perpendicular to the rolling direction. A Ra of 0.6 μm or less was considered to be acceptable.
[0075] (Evaluation test of flatness before and after etching) A test piece measuring 0.1 mm thick x 12 mm wide x 100 mm wide was cut from the steel plate, which was then half-etched in an aqueous solution of ferric chloride. The radius of curvature of the test piece was measured when the thickness had been reduced by half. If the radius of curvature after half-etching was 150 mm or more, the test piece was deemed to have passed the test, as it had the necessary flatness before and after etching.
[0076] (Corrosion resistance evaluation test) Test pieces were cut out from the obtained duplex stainless steel sheets, and the exposed surface was covered with resin to have a size of 10 mm x 10 mm to prepare electrodes for measurement. The exposed surface was either bright annealed or pickled. A pitting corrosion test was carried out in artificial seawater at 50°C to measure the pitting potential (V´ c100 : Current value is 100μA / cm 2 The pitting potential was measured at a potential sweep rate of 20 mV / min. The test was performed five times, and the average pitting potential was used for evaluation. When the pitting potential was 0.9 V or higher, the specimen was deemed to have excellent corrosion resistance and passed the test. When the anodic current density was 1000 μA / cm at the time when the pitting potential was 0.9 V, the specimen was deemed to have excellent corrosion resistance and passed the test. 2 If the test result was less than 100%, the pitting test was terminated and the result was rated as "passed."
[0077] (Steel sheet appearance evaluation) The appearance of the obtained duplex stainless steel sheet was visually inspected for the presence or absence of coloring (particularly, interference color).
[0078] The results of the various evaluation tests are shown in Table 2. Note that the underlines in Tables 1 and 2 indicate that the results are outside the scope of the present invention, or outside the scope of the preferred manufacturing conditions and properties of the present invention.
[0079] Inventive Examples Nos. 1 to 8 and 16 to 25, in which the chemical composition, hardness, average crystal grain size, radius of curvature after half-etching, thickness of oxide film, and Mn concentration in the oxide film were within the prescribed ranges, satisfied all of the requirements for strength, smoothness of the etched surface, flatness after etching, and corrosion resistance. In addition, in these inventive examples as well as the comparative examples described below, the radius of curvature of the steel sheet before half-etching was nearly ∞ (infinity), and the steel sheet was adjusted to a flat shape without warping.
[0080] No. 9, which had been subjected to stress relief heat treatment by air annealing and then pickling, had a thin oxide film and a low Mn concentration in the oxide film, so its corrosion resistance was insufficient. No. 10, which had a low dew point during stress relief heat treatment, had a thin oxide film and therefore insufficient corrosion resistance.
[0081] No. 11, which is a ferrite-austenite dual phase material outside the chemical composition range of the present invention, had insufficient corrosion resistance due to a low Mn concentration in the oxide film. No. 12, an austenitic stainless steel, had a thin oxide film and a low Mn concentration in the oxide film, so its corrosion resistance was insufficient. In addition, No. 12 had a coarse grain size, so the smoothness of the etched surface was insufficient.
[0082] Nos. 13 and 14, which are ferrite-austenite dual phase and do not fall within the chemical composition range of the present invention, had a thin oxide film and insufficient corrosion resistance.
[0083] No. 15, in which the dew point during stress relief heat treatment was too high, had an oxide film exceeding 100 nm, exhibiting interference colors and deteriorating the appearance of the steel sheet.
[0084] [Table 1]
[0085] [Table 2] [Industrial Applicability]
[0086] The ferritic-austenitic duplex stainless steel sheet of the present invention combines corrosion resistance, high strength, flatness after etching, and smoothness of the etched surface. In other words, by using the ferritic-austenitic duplex stainless steel sheet of the present invention as a component material, it is expected that etching will be performed, for example, and that the miniaturization of components that require corrosion resistance will be achieved.
Claims
1. A base steel plate; and an oxide film formed on the base steel sheet, The chemical composition of the base steel sheet is, in mass%, C: 0.08% or less, Si: 0.2-1.0%, Mn: 0.8 to 3.0%, Cr: 20.0-28.0%, Ni: 2.0 to 6.0%, Mo: 1.0-3.0%, N: 0.10-0.30%, Cu: 0-2.0%, Nb: 0 to 0.50%, Ti: 0 to 0.50%, V: 0 to 0.50%, W: 0 to 0.50%, Co: 0 to 0.50%, B: 0 to 0.0050%, Sn: 0 to 0.50%, Al: 0-0.50%, Mg: 0 to 0.010%, Ca: 0-0.0100%, Ta: 0 to 0.050%, Ga: 0 to 0.050%, Zr: 0 to 0.50%, and Rare earth elements: 0-0.010% with the remainder being Fe and impurities, The average crystal grain size is 2.0 μm or less, Vickers hardness is 400 HV or more, The thickness of the oxide film is 15 nm or more, A ferritic-austenitic duplex stainless steel sheet, characterized in that the Mn concentration in the oxide film is 1.5% or more.
2. 2. The ferritic-austenitic duplex stainless steel sheet according to claim 1, characterized in that in the metal structure, the ferritic phase ratio is 20 to 80%.
3. 3. The ferritic-austenitic duplex stainless steel sheet according to claim 1, wherein the radius of curvature after half etching is 150 mm or more.
4. 3. The ferritic-austenitic duplex stainless steel sheet according to claim 1 or 2, which is used for parts of electronic devices or precision devices.
5. The ferritic-austenitic duplex stainless steel sheet according to claim 3, which is used for parts of electronic devices or precision instruments.
Citation Information
Patent Citations
Production of duplex stainless steel excellent in corrosion resistance and sheet of same
JP1991079742A
Ferritic-austenitic stainless steel sheet having excellent press formability, and method for producing the same
JP2011184792A
Two phase stainless steel for ozone-containing water
JP2016191149A
Dual phase stainless steel plate and dual phase stainless hot-rolled plate, and method for manufacturing dual phase stainless steel plate
WO2022114145A1
Method for producing stainless steel sheet excellent in flatness after etching
JP2001226718A