Resin composition and method for producing the same
A resin composition with a specific block copolymer and modified ethylene/α-olefin copolymer addresses the flexibility and adhesive property issues of conventional hot melt adhesives, providing excellent performance across varying temperatures.
Patent Information
- Application Number
- JP2023048572
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional hot melt adhesives experience a significant decrease in flexibility and adhesive properties at low temperatures, leading to reduced performance across a wide range of temperature conditions.
A resin composition comprising a specific block copolymer, a modified ethylene/α-olefin copolymer, and an adhesive resin, which are formulated to maintain excellent adhesive properties from low to high temperatures through a combination of amorphous ethylene/α-olefin skeletons, vinyl aromatic moieties, and compatibility with polymer blocks.
The resin composition ensures flexibility and strong adhesion across a wide temperature range, maintaining effective adhesive properties from low to high temperatures, enhancing the versatility and performance of molded articles.
Smart Images

Figure 2024137161000001 
Figure 2024137161000002 
Figure 2024137161000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and a method for producing the same. [Background technology]
[0002] Conventionally, thermoplastic resins have been used by being molded by various molding methods into various members, films, sheets, fiber adhesives, foams, crosslinked bodies, etc. In order to adapt thermoplastic resins to a wide variety of applications, it is important to design materials suited to each application. For example, in hot melt adhesive applications, it has been reported that a hot melt adhesive exhibiting good fluidity and heat resistance can be obtained by combining an amorphous poly-α-olefin with a crystalline α-olefin elastomer (e.g., Patent Document 1). In addition, for example, it has been reported that a hot melt adhesive that exhibits good adhesion under low temperature conditions can be obtained by combining a styrene-based block copolymer, a specific tackifier resin, and a specific polymer (for example, Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-196839 A [Patent Document 2] JP 2006-241444 A Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional hot melt adhesives have a problem in that their flexibility is significantly reduced under low temperature conditions, resulting in reduced adhesiveness. However, with conventional hot melt adhesives, improving the adhesiveness under low temperature conditions often results in a decrease in adhesiveness under high temperature conditions, leaving room for improvement. An object of one embodiment of the present invention is to provide a resin composition having excellent adhesiveness under a wide range of temperature conditions from low to high, a molded article containing the composition, and a method for producing the resin composition. [Means for solving the problem]
[0005] Means for Solving the Problems The present inventors have conducted intensive research aimed at solving the above problems and have found that a resin composition having excellent adhesiveness over a wide range of temperature conditions, from low to high, can be obtained by using a specific block copolymer (A), a specific modified ethylene-α-olefin copolymer (B), and an adhesive resin (C). The present invention relates to, for example, the following <1> ~ <14> Regarding.
[0006] <1> A block copolymer (A) which is a hydrogenated product of a block copolymer containing a polymer block (X) mainly composed of a vinyl aromatic compound and a polymer block (Y) mainly composed of a conjugated diene compound; A modified ethylene-α-olefin copolymer (B) that satisfies the following requirements (b-1) to (b-4); A resin composition comprising: Requirement (b-1): The content of structural units derived from ethylene is in the range of 15 to 85 mol % (provided that the total content of structural units derived from ethylene and the content of structural units derived from α-olefins is 100 mol %); Requirement (b-2): The weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 1,000 to 100,000; Requirement (b-3): A modified copolymer having a substituent derived from a vinyl aromatic compound, in which the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 1 to 70 mass%; Requirement (b-4): The Brookfield viscosity at 100°C is in the range of 1 to 10,000 mPa·s. <2> In the above requirement (b-1), the content of structural units derived from ethylene is in the range of 40 to 60 mol % (wherein the total content of structural units derived from ethylene and the content of structural units derived from α-olefins is 100 mol %), In the above-mentioned requirement (b-2), the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 2,000 to 30,000, and in the above-mentioned requirement (b-3), the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 5 to 30 mass%. <1> The resin composition according to claim 1. <3> The block copolymer (A) satisfies the following requirement (a-1): <1> or <2> The resin composition according to claim 1 ; Requirement (a-1): MFR (230°C, 5 kg) is in the range of 0.1 to 1,000 g / 10 min. <4> When the content of the block copolymer (A) is taken as 100 parts by mass, the content of the copolymer (B) is in the range of 10 to 150 parts by mass, and the content of the adhesive resin (C) is in the range of 10 to 300 parts by mass. <1> ~ <3> 10. The resin composition according to claim 9 . <5> <1> ~ <4> 13. A pressure-sensitive adhesive comprising the resin composition according to any one of claims 1 to 12. <6> <1> ~ <4> A hot melt adhesive comprising the resin composition according to any one of the above. <7> <1> ~ <4> A heat sealing material comprising the resin composition according to any one of the above items. <8> <1> ~ <4> A primer comprising the resin composition according to any one of the above items. <9> a block copolymer (A) which is a hydrogenated product of a block copolymer containing a polymer block (X) mainly made of a vinyl aromatic compound and a polymer block (Y) mainly made of a conjugated diene compound; A modified ethylene-α-olefin copolymer (B) that satisfies the following requirements (b-1) to (b-4); a pressure-sensitive adhesive resin (C); Requirement (b-1): The content of structural units derived from ethylene is in the range of 15 to 85 mol % (provided that the total content of structural units derived from ethylene and the content of structural units derived from α-olefins is 100 mol %); Requirement (b-2): The weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 1,000 to 100,000; Requirement (b-3): A modified copolymer having a substituent derived from a vinyl aromatic compound, in which the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 1 to 70 mass%; Requirement (b-4): The Brookfield viscosity at 100°C is in the range of 1 to 10,000 mPa·s. <10> The modified ethylene-α-olefin copolymer (B) is a modified product of an unmodified ethylene-α-olefin copolymer (B′) produced by the following method (α): <9> A method for producing the resin composition according to the present invention; Method (α): A bridged metallocene compound (P-1) represented by the following formula (1), and A method comprising a step of solution polymerizing ethylene and an α-olefin in the presence of a catalyst system containing at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P-1) to form an ion pair.
[0007] [ka]
[0008] [In formula [1], R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure; R 6 and R 11 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 7 and R 10 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 6 and R 7 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 6 , R 7 , R 10 and R 11 is not a hydrogen atom at the same time, Y is a carbon atom or a silicon atom; R 13 and R 14 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be bonded to each other to form a ring structure, M is Ti, Zr or Hf; Q is independently a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating to a lone pair of electrons; j is an integer from 1 to 4.
[0009] <11> In the above formula 1, R 13 and R 14 At least one of the groups is an aryl group; <10> A method for producing the resin composition according to claim 1. <12> In the above formula 1, R 13 and R 14 are both aryl groups, and R 2 and R 3 one of the above is a saturated hydrocarbon group having 4 carbon atoms; <10> A method for producing the resin composition according to claim 1. <13> The block copolymer (A) satisfies the following requirement (a-1), and in the requirement (b-1), the content of structural units derived from ethylene is in the range of 40 to 60 mol %, in the requirement (b-2), the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 2,000 to 30,000, and in the requirement (b-3), the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 5 to 30 mass %. <9> ~ <12> A method for producing a resin composition according to any one of the above items; Requirement (a-1): MFR (230°C, 5 kg) is in the range of 0.1 to 1,000 g / 10 min. <14> When the content of the block copolymer (A) is taken as 100 parts by mass, the content of the copolymer (B) is in the range of 10 to 150 parts by mass, and the content of the adhesive resin (C) is in the range of 30 to 300 parts by mass. <9> ~ <13> 13. A method for producing the resin composition according to claim 12. Effect of the Invention
[0010] According to one embodiment of the present invention, there are provided a resin composition having excellent adhesiveness under a wide range of temperature conditions from low to high, a molded article containing the composition, and a method for producing the resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be specifically described below. In this specification, when a numerical range is indicated by "-", for example, "M to N", it means "M or more and N or less" unless otherwise specified. In this specification, when an olefin constituting a certain polymer is represented by M, the expression "structural unit derived from M" is sometimes used, which means a "structural unit corresponding to M", that is, a structural unit having a pair of bonds formed by opening a π bond constituting a double bond of M. In this specification, the term "(meth)acrylic" is used as a concept encompassing acrylic, methacrylic, and both acrylic and methacrylic. In this specification, the terms "aromatic" and "aromatic ring" are used as a concept encompassing not only a benzene ring, but also condensed polycyclic aromatics such as naphthalene, anthracene, and triphenylene, heteroaromatics such as furan, thiophene, pyrrole, imidazole, oxazole, thiazole, and pyridine, ionic aromatics such as cyclopentadienyl anion, and various compounds exhibiting aromaticity, such as azulene and porphyrin, and rings exhibiting aromaticity. In this specification, the term "mainly composed of" means that the polymer block contains structural units derived from a vinyl aromatic compound or a conjugated diene compound in an amount of 50% by mass or more, preferably 60% by mass or more, and more preferably 80% by mass or more. For example, a polymer block mainly composed of a vinyl aromatic compound means that the polymer block contains structural units derived from a vinyl aromatic compound in an amount of preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more, based on the total mass of the polymer block. As used herein, a combination of two or more preferred embodiments is a more preferred embodiment. In this specification, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, the amount refers to the total amount of multiple substances present in the composition, unless otherwise specified. The present invention will now be described in further detail.
[0012] [Resin composition] The resin composition of the present invention contains the block copolymer (A) shown below, the modified ethylene-α-olefin copolymer (B) shown below, and the adhesive resin (C). The resin composition has the above-mentioned structure, and thus has excellent adhesiveness under a wide range of temperature conditions from low to high. The reason for this is not clear, but the following mechanism is presumed. The ethylene-α-olefin skeleton of the modified ethylene-α-olefin copolymer (B) is amorphous and has a low glass transition point, and therefore has fluidity even in the low temperature range. Therefore, when it is contained in a composition together with the block copolymer (A), it is possible to lower the glass transition point, and the composition can be kept flexible even under lower temperature conditions. Due to this effect, it is believed that the resin composition of the present invention has excellent adhesiveness even at lower temperatures. The vinyl aromatic moiety contained in the modified ethylene-α-olefin copolymer (B) exhibits high compatibility (miscibility) with the polymer block (X) of the block copolymer (A) described below. The polymer block (X) is a physical crosslinking point in the block copolymer (A) and is a moiety that contributes to ensuring strength. The compatibility of this polymer block (X) with the vinyl aromatic moiety of the modified ethylene-α-olefin copolymer (B) reinforces the polymer block (X) and makes it possible to firmly maintain the physical crosslinking points up to higher temperature ranges. Due to this effect, it is believed that the resin composition of the present invention has excellent adhesion up to higher temperatures. The adhesive resin (C) contributes to improving the adhesiveness at room temperature. Therefore, it is believed that the inclusion of the block copolymer (A), the modified ethylene-α-olefin copolymer (B), and the adhesive resin (C) provides excellent adhesiveness over a wide range of temperature conditions, from low to high. The wide temperature range referred to here is a range having a temperature range of preferably 30° C. or more, more preferably 40° C. or more, and even more preferably 50° C. or more.
[0013] <Block copolymer (A)> The block copolymer (A) is a hydrogenated product of a block copolymer containing a polymer block (X) mainly made of a vinyl aromatic compound and a polymer block (Y) mainly made of a conjugated diene compound (hereinafter also referred to as an "X / Y block copolymer").
[0014] <<Polymer block (X)>> The polymer block (X) is mainly composed of a vinyl aromatic compound. Specific examples of the vinyl aromatic compound constituting the polymer block (X) include, for example, styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 1,3-dimethylstyrene, 4-tert-butylstyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 4-propylstyrene, 4-isopropylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, monochlorostyrene, dichlorostyrene, methoxystyrene, vinylanthracene, etc., among which styrene is the most preferred. These vinyl aromatic compounds may be one type or two or more types. The resin composition preferably contains a polymer block mainly composed of a vinyl aromatic compound, which tends to have good affinity with various materials such as non-polar resins, polar resins, and metals. Good affinity between the resin composition and non-polar resins, polar resins, and metals is useful because it can be applied to a wide range of resins and metals when used as an adhesive material such as a hot melt adhesive or a heat seal material.
[0015] <<Polymer block (Y)>> The polymer block (Y) is mainly composed of a conjugated diene compound. The conjugated diene compound constituting the polymer block (Y) is preferably a conjugated diene having 4 to 20 carbon atoms. Specific examples of the conjugated diene having 4 to 20 carbon atoms include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene, and among these, butadiene and isoprene are most preferred. These conjugated diene compounds may be of one type or two or more types.
[0016] The X / Y block copolymer may be either linear or branched with two or more branches, and its structure is not particularly limited, but an XYX type triblock structure is particularly preferred.
[0017] Specific examples of the X / Y block copolymer include a styrene-butadiene-styrene block copolymer, a styrene-isoprene-styrene block copolymer, and a styrene-butadiene / isoprene-styrene block copolymer. For example, a styrene-butadiene-styrene block copolymer means a block copolymer having a structure of polystyrene block-polybutadiene block-polystyrene block.
[0018] The method for producing the X / Y block copolymer is not particularly limited, and examples thereof include a method for producing the X / Y block copolymer by sequentially polymerizing a vinyl aromatic compound and a conjugated diene compound in an inert solvent using a known method such as ionic polymerization, e.g., anionic polymerization or cationic polymerization, radical polymerization, or coordination polymerization.
[0019] Since the copolymer (A) contains a hydrogenated product of the X / Y block copolymer, the number of aliphatic double bonds in the X / Y block copolymer is reduced, and the heat resistance and weather resistance of the resulting molded article are improved, and the compatibility with the modified ethylene-α-olefin copolymer (B) is also improved.
[0020] The hydrogenated X / Y block copolymer is preferably one in which 90% to 100% of the aliphatic double bonds in the X / Y block copolymer are hydrogenated and 10% or less of the aromatic double bonds are hydrogenated, and more preferably one in which 99% to 100% of the aliphatic double bonds are hydrogenated and 5% or less of the aromatic double bonds are hydrogenated. In such a hydrogenated X / Y block copolymer, the polymer block (Y) in which the aliphatic double bonds are hydrogenated is substantially a block of polyolefin structure.
[0021] Examples of the hydrogenated X / Y block copolymer include a styrene-(ethylene / butene)-styrene copolymer, a styrene-(ethylene / propylene)-styrene copolymer, and a styrene-(ethylene / ethylene / propylene)-styrene copolymer. In particular, the hydrogenated product of the X / Y block copolymer is preferably a hydrogenated product of a block copolymer containing a polymer block mainly composed of styrene and a copolymer block mainly composed of butadiene and isoprene.
[0022] The method for hydrogenating the X / Y block copolymer is not particularly limited, and any known method can be used. For example, the hydrogenated product of the X / Y block copolymer can be obtained by reacting the X / Y block copolymer in the presence of a hydrogenation catalyst and hydrogen under appropriate temperature and pressure conditions.
[0023] The X / Y block copolymer used as the block copolymer (A) may be one type alone or two or more types in combination, for example, two or more types of X / Y block copolymers having different properties such as molecular weight and styrene content may be used.
[0024] The block copolymer (A) preferably satisfies the following requirement (a-1).
[0025] <Requirement (a-1)> The requirement (a-1) is that the MFR (230° C., 5 kg) of the block copolymer (A) is in the range of 0.1 to 1,000 g / 10 min. The MFR (230° C., 5 kg) is 0.1 to 1,000 g / 10 min, preferably 0.5 to 800 g / 10 min, more preferably 0.5 to 500 g / 10 min, and further preferably 1 to 100 g / 10 min. When the MFR (230°C 5 kg) is 0.1 g / 10 min or more, the adhesiveness of the resin composition is good, while when it is 1,000 g / 10 min or less, the fluidity is excellent and the kneading and coating properties are good.
[0026] The weight average molecular weight (Mw) of the X / Y block copolymer (block copolymer (A)) in terms of polystyrene measured by GPC is preferably 20,000 to 500,000, more preferably 20,000 to 300,000, and further preferably 30,000 to 200,000. When the weight average molecular weight of the X / Y block copolymer is 20,000 or more, the adhesiveness of the resin composition is good, while when it is 500,000 or less, the flowability is excellent and the kneading property and coating property are good.
[0027] The ratio of polymer block (X) and polymer block (Y) in the X / Y block copolymer (block copolymer (A)) depends on the number average molecular weight of the X / Y block copolymer, the number average molecular weight of the polymer block (X) and the polymer block (Y), etc., but generally, based on the total mass of the X / Y block copolymer, the ratio of polymer block (X) is preferably 5 to 80 mass% and the ratio of polymer block (Y) is preferably 20 to 95 mass%, more preferably polymer block (X) is 5 to 65 mass% and polymer block (Y) is 35 to 95 mass%, and further preferably polymer block (X) is 10 to 40 mass% and polymer block (Y) is 60 to 90 mass%. When the ratios of polymer blocks (X) and (Y) are within the above ranges, the adhesiveness of the resin composition is good. In the X / Y block copolymer, the ratio of the polymer blocks (X) and (Y) affects the hardness and flexibility of the X / Y block copolymer. If the adhesive is too hard, the adhesion to the substrate decreases and the interface peels easily, while if it is too soft, the strength of the adhesive layer decreases and it is prone to cohesive failure under small stress. Therefore, in order to more easily obtain maximum adhesion, it is preferable to use an X / Y block copolymer that has been adjusted to the optimal hardness and flexibility by each blend.
[0028] The block copolymer (A) may be modified to the extent that the object of the present invention is not impaired. As the modification method, various known methods can be used, for example, oxidation modification, halogenation modification such as chlorosulfonation, chlorination, bromination, etc., graft modification or terminal modification with a vinyl compound having an oxygen-containing group such as an acid, an acid anhydride, an ester, an alcohol, an epoxy, an ether, etc., a vinyl compound having a nitrogen-containing group such as an isocyanate, an amide, etc., or a vinyl compound having a silicon-containing group such as vinyl silane, etc.
[0029] Specific examples of vinyl compounds used for graft modification or terminal modification include unsaturated epoxy monomers such as unsaturated glycidyl ethers and unsaturated glycidyl esters (e.g., glycidyl methacrylate), trimethoxyvinylsilane, dimethylmethoxyvinylsilane, dimethoxymethylvinylsilane, triethoxyvinylsilane, trimethylvinylsilane, diethylmethylvinylsilane, diacetoxyethylvinylsilane, diethoxymethylvinylsilane, ethoxydimethylvinylsilane, triacetoxyvinylsilane, tris(2-methoxyethoxy)vinylsilane, triphenyl Vinyl silane, monovinyl silanes such as triphenoxyvinyl silane, polyvinyl silanes such as diphenyldivinyl silane and allyloxydimethylvinyl silane, unsaturated carboxylic acid ester-based silane compounds such as methacryloxypropyltrimethoxysilane, methacryloxypropyltriethoxysilane and acryloxypropyltrimethoxysilane, vinyl compounds having silicon-containing groups such as styryl-based silane compounds such as styryltrimethoxysilane, acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acid. TM(endo-cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid), and derivatives of the above unsaturated carboxylic acids, such as acid halide compounds, amide compounds, imide compounds, acid anhydrides, and ester compounds. Specific examples of the derivatives of the above unsaturated carboxylic acids include malenyl chloride, maleimide, maleic anhydride, citraconic anhydride, monomethyl maleate, dimethyl maleate, and glycidyl maleate. Among these, unsaturated dicarboxylic acids and their acid anhydrides are more preferred, and in particular maleic acid, nadic acid, TM and acid anhydrides thereof are particularly preferably used. When a modified block copolymer is used as the block copolymer (A), it is preferable because the affinity with non-polar resins, polar resins, metals, and inorganic materials such as carbon and silica can be adjusted.
[0030] The X / Y block copolymer used as the block copolymer (A) may be a commercially available product, such as "Septon (registered trademark)" and "Hybler (registered trademark)" manufactured by Kuraray Co., Ltd., "Tuftec (registered trademark)" manufactured by Asahi Kasei Corporation, "Dynaron (registered trademark)" manufactured by JSR Corporation, and "G Series" manufactured by Kraton Polymers.
[0031] <Modified ethylene-α-olefin copolymer (B)> The resin composition according to the present invention contains a modified ethylene-α-olefin copolymer (B) (hereinafter sometimes abbreviated as "modified copolymer (B)") that satisfies the following requirements (b-1) to (b-4).
[0032] <<Requirements (b-1)>> The requirement (b-1) is that the content of structural units derived from ethylene in the modified ethylene-α-olefin copolymer (B) (hereinafter sometimes abbreviated as "ethylene content") is in the range of 15 to 85 mol % (provided that the total of the content of structural units derived from ethylene and the content of structural units derived from α-olefin is 100 mol %). The ethylene content is 15 to 85 mol%, preferably 20 to 80 mol%, more preferably 30 to 70 mol%, and further preferably 40 to 60 mol%. When the ethylene content is 15 to 85 mol%, the compatibility with the block copolymer (A) and the flexibility of the resin composition are excellent, and the adhesive strength at low temperatures is also excellent.
[0033] The ethylene content of the modified ethylene-α-olefin copolymer (B) is: 13 The measurement can be performed by C-NMR, and peaks can be identified and quantified, for example, according to the method described below and the method described in "Polymer Analysis Handbook" (published by Asakura Publishing, pp. 163-170).
[0034] The α-olefin constituting the modified ethylene-α-olefin copolymer (B) includes α-olefins having 3 or more carbon atoms, and typical examples include α-olefins having 3 to 20 carbon atoms such as propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene. These α-olefins may be used alone or in combination of two or more.
[0035] Among these α-olefins, α-olefins having 3 to 10 carbon atoms are preferred, propylene and 1-butene are more preferred, and propylene is even more preferred, from the viewpoints that crystallinity can be effectively reduced, a liquid copolymer can be obtained, and a resin composition and a molded article having the desired effects can be easily obtained.
[0036] The ethylene and α-olefin having 3 or more carbon atoms may be, for example, a monomer derived from a fossil fuel or a monomer derived from biomass, and these monomers may be used alone or in combination of two or more. In other words, the modified ethylene-α-olefin copolymer (B) may be composed only of monomers derived from a fossil fuel, or may be composed only of monomers derived from biomass, or may use a combination of monomers derived from a fossil fuel and monomers derived from biomass.
[0037] The modified ethylene-α-olefin copolymer (B) may be polymerized in the presence of at least one monomer selected from the group consisting of polar group-containing monomers, vinyl aromatic compounds, and cyclic olefins (hereinafter also referred to as "other monomers") in the reaction system. The content of the other monomers is, for example, preferably 20 parts by mass or less, more preferably 10 parts by mass or less, per 100 parts by mass of the total of ethylene and α-olefin having 3 or more carbon atoms.
[0038] Examples of polar group-containing monomers include α,β-unsaturated carboxylic acids such as acrylic acid, methacrylic acid, fumaric acid, and maleic anhydride, and metal salts thereof such as sodium salts, α,β-unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, methyl methacrylate, and ethyl methacrylate, vinyl esters such as vinyl acetate and vinyl propionate, and unsaturated glycidyls such as glycidyl acrylate and glycidyl methacrylate.
[0039] Examples of vinyl aromatic compounds include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, methoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, p-chlorostyrene, divinylbenzene, α-methylstyrene, and allylbenzene.
[0040] Examples of the cyclic olefin include cyclic olefins having 3 to 30 carbon atoms, preferably 3 to 20 carbon atoms, such as cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, 5-ethylidene-2-norbornene, 5-vinyl-2-norbornene, and tetracyclododecene.
[0041] <<Requirements (b-2)>> The requirement (b-2) is that the modified ethylene-α-olefin copolymer (B) has a weight average molecular weight (Mw) in the range of 1,000 to 100,000 as determined by gel permeation chromatography (GPC). The measurement conditions for gel permeation chromatography (GPC) include the measurement conditions employed in the examples described below. The Mw of the modified ethylene / α-olefin copolymer (B) is from 1,000 to 100,000, preferably from 1,500 to 80,000, more preferably from 2,000 to 50,000, and even more preferably from 2,000 to 30,000.
[0042] When the weight average molecular weight (Mw) of the modified ethylene / α-olefin copolymer (B) is within the above range, it is possible to obtain a resin composition that has excellent adhesiveness under a wide range of temperature conditions from low to high temperatures.
[0043] <<Requirements (b-3)>> The requirement (b-3) is that the modified ethylene-α-olefin copolymer (B) is a modified copolymer having a substituent derived from a vinyl aromatic compound, and the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 1 to 70 mass%. The grafting position of the above substituent is not particularly limited.
[0044] Examples of vinyl aromatic compounds include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, methoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, p-chlorostyrene, divinylbenzene, α-methylstyrene, vinylnaphthalene, vinylbiphenyl, vinylanthracene, vinyltriphenylene, vinylthiophene, and vinylpyridine. Among these, styrene is preferred from the viewpoint of availability and compatibility. These vinyl aromatic compounds may be used alone or in combination of two or more. The grafting position of the vinyl aromatic compound is not particularly limited.
[0045] The content of the portion derived from the vinyl aromatic compound in the modified ethylene-α-olefin copolymer (B) is 1 to 70 mass%, preferably 2 to 50 mass%, and more preferably 3 to 30 mass%. When the content of the portion derived from the vinyl aromatic compound is within the above range, a good balance is achieved between the amorphousness and softening effect of the portion derived from the ethylene-α-olefin copolymer and the reinforcing effect of the portion derived from the grafted vinyl aromatic compound, so that a resin composition having excellent adhesiveness over a wide range of temperature conditions from low to high temperatures can be obtained. The content of the portion derived from the vinyl aromatic compound can be determined by various known methods, and a method suitable for each compound having a carbon-carbon unsaturated bond is known. For example, 1 It can be calculated from the area ratio of the peaks attributable to aromatic protons observed on the low magnetic field side by H-NMR to the peaks attributable to ethylene-α-olefin copolymers and methyl-methylene-methine derived from the vinyl groups of vinyl aromatics observed on the high magnetic field side.
[0046] The modified ethylene-α-olefin copolymer (B) may be modified by allowing one or more compounds having a carbon-carbon unsaturated bond (i.e., an ethylenically unsaturated bond) other than the vinyl aromatic compound to coexist in the reaction system. When the total of the vinyl aromatic compound and the compound other than the vinyl aromatic compound having a carbon-carbon unsaturated bond is taken as 100 mass%, the content of the compound other than the vinyl aromatic compound having a carbon-carbon unsaturated bond is preferably in the range of 0 to 20 mass%, more preferably 0 to 10 mass%.
[0047] Examples of compounds having carbon-carbon unsaturated bonds other than vinyl aromatic compounds include compounds having acid or acid-derived groups such as acid, acid anhydride, ester, amide, and imide, compounds having oxygen-containing groups such as alcohol, epoxy, and ether, compounds having nitrogen-containing groups such as amine, nitrile, and isocyanate, compounds having sulfur-containing groups such as sulfide, sulfoxide, sulfone, and sulfonamide, and compounds having silicon-containing groups such as vinyl silane. Among these, compounds having acid or acid-derived groups and compounds having oxygen-containing groups are preferred, and unsaturated carboxylic acids and their derivatives and compounds having alcoholic hydroxyl groups are more preferred. The grafting position of compounds having carbon-carbon unsaturated bonds other than vinyl aromatic compounds is not particularly limited.
[0048] Examples of unsaturated carboxylic acids include (meth)acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acid (endo cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid).
[0049] The derivatives of the unsaturated carboxylic acids include acid anhydrides, esters, amides and imides of the unsaturated carboxylic acids.
[0050] Examples of esters of unsaturated carboxylic acids include esters and half esters such as methyl (meth)acrylate, ethyl (meth)acrylate, monoethyl maleate, diethyl maleate, monomethyl fumarate, dimethyl fumarate, monomethyl itaconic acid, and diethyl itaconic acid.
[0051] Examples of the amide of an unsaturated carboxylic acid include (meth)acrylamide, maleic acid monoamide, maleic acid diamide, maleic acid-N-monoethylamide, maleic acid-N,N-diethylamide, maleic acid-N-monobutylamide, maleic acid-N,N-dibutylamide, fumaric acid monoamide, fumaric acid diamide, fumaric acid-N-monobutylamide, and fumaric acid-N,N-dibutylamide. Examples of imides of unsaturated carboxylic acids include maleimide, N-butylmaleimide, and N-phenylmaleimide.
[0052] Among the unsaturated carboxylic acids and derivatives thereof, unsaturated dicarboxylic acids and derivatives thereof are more preferred, and maleic acid and maleic anhydride are particularly preferred because they are less likely to produce by-products such as homopolymers in the reaction for producing the modified ethylene-α-olefin copolymer (B).
[0053] Examples of compounds having an alcoholic hydroxy group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, glycerin mono(meth)acrylate, pentaerythritol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, allyl alcohol, 2-methyl-3-buten-1-ol, 2-methyl-3-buten-2-ol, 3-methyl-3-buten-1-ol, 10-undecen-1-ol, 1-octen-3-ol, 2-methanol norbornene, and 2-butene-1,4-diol. Examples of suitable acrylic acid esters include aryl ether, hydroxystyrene, hydroxymethyl vinyl ether, hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxymethyl propenyl ether, hydroxyethyl propenyl ether, hydroxypropyl propenyl ether, hydroxybutyl propenyl ether, hydroxymethyl butenyl ether, hydroxyethyl butenyl ether, hydroxypropyl butenyl ether, hydroxybutyl butenyl ether, N-methylol acrylamide, 2-(meth)acryloyloxyethyl acetyl phosphate, glycerin monoallyl ether, and allyloxyethanol.
[0054] The modified ethylene-α-olefin copolymer (B) preferably satisfies the requirement (b-1), that the content of structural units derived from ethylene is in the range of 40 to 60 mol % (the total content of structural units derived from ethylene and the content of structural units derived from α-olefin is 100 mol %), the requirement (b-2), that the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 2,000 to 30,000, and the requirement (b-3), that the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 5 to 30 mass %.
[0055] <<Requirements (b-4)>> The requirement (b-4) is that the modified ethylene / α-olefin copolymer (B) has a Brookfield viscosity at 100° C. in the range of 1 to 10,000 mPa·s. The Brookfield viscosity of the modified ethylene / α-olefin copolymer (B) at 100° C. is 1 to 10,000 mPa·s, preferably 5 to 5,000 mPa·s, more preferably 10 to 1,000 mPa·s, even more preferably 15 to 500 mPa·s, and particularly preferably 15 to 250 mPa·s. When the Brookfield viscosity at 100° C. is within the above range, a resin composition can be obtained that has an excellent balance between the softening effect and the viscosity-lowering effect, and that has an excellent balance between the kneadability when producing the resin composition and the coatability when using the resin composition as a pressure-sensitive adhesive.
[0056] The content of the modified ethylene-α-olefin copolymer (B) in the resin composition of the present invention is preferably in the range of 10 to 150 parts by mass, more preferably 10 to 100 parts by mass, per 100 parts by mass of the block copolymer (A). When the content of the modified ethylene-α-olefin copolymer (B) is in the above range, a resin composition having excellent adhesiveness over a wide range of temperature conditions from low to high temperatures can be obtained.
[0057] The modified ethylene-α-olefin copolymer (B) is an unmodified ethylene-α-olefin copolymer (B') satisfying the requirement (b-1) preferably modified with the vinyl aromatic compound to give a modified ethylene-α-olefin copolymer (B), or more preferably graft-modified with the vinyl aromatic compound.
[0058] <<Unmodified ethylene-α-olefin copolymer (B′)>> The method for producing the unmodified ethylene-α-olefin copolymer (B') is not particularly limited, but includes a method using a vanadium catalyst consisting of a vanadium compound and an organoaluminum compound, as described in JP-B-2-1163 and JP-B-2-7998. In addition, as a method for producing a copolymer with high polymerization activity, a method using a catalyst system consisting of a metallocene compound such as zirconocene and an organoaluminum oxy compound (aluminoxane), as described in JP-A-61-221207, JP-B-7-121969, and Japanese Patent No. 2796376, may be used, which is more preferable because it can reduce the chlorine content of the resulting copolymer and the 2,1-insertion of α-olefin. In the method using a vanadium catalyst, a larger amount of chlorine compound is used as a cocatalyst compared to the method using a metallocene catalyst, so there is a possibility that a trace amount of chlorine remains in the resulting unmodified ethylene-α-olefin copolymer (B').
[0059] In addition, the reduction in the 2,1-insertion of α-olefins makes it possible to further reduce the ethylene chains in the copolymer molecules, and suppresses the intramolecular crystallinity of ethylene, so that the unmodified ethylene-α-olefin copolymer (B') becomes an amorphous copolymer with good fluidity. The amount of 2,1-insertion of α-olefins can be reduced according to the method described in JP-A-7-145212. 13 It is determined by C-NMR measurement and analysis, and is preferably less than 1%, further preferably 0 to 0.5%, and even more preferably 0 to 0.1%. It is particularly preferable that no peak is observed in the range of 15.0 to 17.5 ppm.
[0060] From the viewpoint of obtaining an unmodified ethylene-α-olefin copolymer (B') having a good balance of performance in terms of molecular weight control, molecular weight distribution, amorphousness, etc., the following production method is particularly preferred.
[0061] The method for producing the unmodified ethylene-α-olefin copolymer (B') preferably comprises a step of copolymerizing ethylene and an α-olefin having 3 to 20 carbon atoms in the presence of an olefin polymerization catalyst containing a bridged metallocene compound (P) represented by the following formula [I], and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair.
[0062] [ka]
[0063] [Bridged metallocene compound (P)] The bridged metallocene compound (P) is represented by the above formula [I]. 1 ~R 14 , Q, n and j are explained below.
[0064] (Y, M, R 1 ~R 14 , Q, n and j) Y is a Group 14 atom, examples of which include a carbon atom, a silicon atom, a germanium atom and a tin atom, and is preferably a carbon atom or a silicon atom, and more preferably a carbon atom.
[0065] M is a titanium atom, a zirconium atom or a hafnium atom, and is preferably a zirconium atom. R 1 ~R 12 are atoms or substituents selected from the group consisting of hydrogen atoms, hydrocarbon groups having 1 to 20 carbon atoms, silicon-containing groups, nitrogen-containing groups, oxygen-containing groups, halogen atoms and halogen-containing groups, and may be the same or different. 1 From R 12 Adjacent substituents up to may be bonded to each other to form a ring, or may not be bonded to each other.
[0066] Here, examples of the hydrocarbon group having 1 to 20 carbon atoms include an alkyl group having 1 to 20 carbon atoms, a cyclic saturated hydrocarbon group having 3 to 20 carbon atoms, a linear unsaturated hydrocarbon group having 2 to 20 carbon atoms, a cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms, an alkylene group having 1 to 20 carbon atoms, and an arylene group having 6 to 20 carbon atoms.
[0067] Examples of the alkyl group having 1 to 20 carbon atoms include linear saturated hydrocarbon groups such as methyl, ethyl, n-propyl, allyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decanyl, and branched saturated hydrocarbon groups such as isopropyl, isobutyl, s-butyl, t-butyl, t-amyl, neopentyl, 3-methylpentyl, 1,1-diethylpropyl, 1,1-dimethylbutyl, 1-methyl-1-propylbutyl, 1,1-propylbutyl, 1,1-dimethyl-2-methylpropyl, 1-methyl-1-isopropyl-2-methylpropyl, and cyclopropylmethyl. The number of carbon atoms in the alkyl group is preferably 1 to 6.
[0068] Examples of cyclic saturated hydrocarbon groups having 3 to 20 carbon atoms include cyclic saturated hydrocarbon groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, norbornenyl, 1-adamantyl, and 2-adamantyl, and groups in which hydrogen atoms of cyclic saturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 17 carbon atoms such as 3-methylcyclopentyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 4-cyclohexylcyclohexyl, and 4-phenylcyclohexyl. The number of carbon atoms in the cyclic saturated hydrocarbon group is preferably 5 to 11.
[0069] Examples of the linear unsaturated hydrocarbon group having 2 to 20 carbon atoms include alkenyl groups such as ethenyl group (vinyl group), 1-propenyl group, 2-propenyl group (allyl group), 1-methylethenyl group (isopropenyl group), etc., and alkynyl groups such as ethynyl group, 1-propynyl group, 2-propynyl group (propargyl group), etc. The number of carbon atoms in the linear unsaturated hydrocarbon group is preferably 2 to 4.
[0070] Examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms include cyclic unsaturated hydrocarbon groups such as cyclopentadienyl, norbornyl, phenyl, naphthyl, indenyl, azulenyl, phenanthryl, and anthracenyl, groups in which hydrogen atoms of cyclic unsaturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 15 carbon atoms such as 3-methylphenyl (m-tolyl), 4-methylphenyl (p-tolyl), 4-ethylphenyl, 4-t-butylphenyl, 4-cyclohexylphenyl, biphenylyl, 3,4-dimethylphenyl, 3,5-dimethylphenyl, and 2,4,6-trimethylphenyl (mesityl), groups in which hydrogen atoms of linear hydrocarbon groups or branched saturated hydrocarbon groups are replaced with cyclic saturated hydrocarbon groups or cyclic unsaturated hydrocarbon groups having 3 to 19 carbon atoms such as benzyl and cumyl. The number of carbon atoms of the cyclic unsaturated hydrocarbon group is preferably 6 to 10.
[0071] Examples of the alkylene group having 1 to 20 carbon atoms include a methylene group, an ethylene group, a dimethylmethylene group (an isopropylidene group), an ethylmethylene group, a methylethylene group, an n-propylene group, etc. The number of carbon atoms in the alkylene group is preferably 1 to 6.
[0072] Examples of the arylene group having 6 to 20 carbon atoms include an o-phenylene group, an m-phenylene group, a p-phenylene group, a 4,4'-biphenylylene group, etc. The number of carbon atoms in the arylene group is preferably 6 to 12.
[0073] Examples of the silicon-containing group include alkylsilyl groups such as trimethylsilyl group, triethylsilyl group, t-butyldimethylsilyl group, and triisopropylsilyl group, which are groups in which carbon atoms in a hydrocarbon group having 1 to 20 carbon atoms are replaced with silicon atoms, arylsilyl groups such as dimethylphenylsilyl group, methyldiphenylsilyl group, and t-butyldiphenylsilyl group, pentamethyldisilanyl group, and trimethylsilylmethyl group, etc. The number of carbon atoms in the alkylsilyl group is preferably 1 to 10, and the number of carbon atoms in the arylsilyl group is preferably 6 to 18.
[0074] Examples of the nitrogen-containing group include an amino group, a group in which the =CH- structural unit in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms or silicon-containing group is replaced with a nitrogen atom, a group in which the -CH2- structural unit is replaced with a nitrogen atom to which a hydrocarbon group having 1 to 20 carbon atoms is bonded, or a group in which the -CH3 structural unit is replaced with a nitrogen atom to which a hydrocarbon group having 1 to 20 carbon atoms is bonded or a nitrile group, such as a dimethylamino group, a diethylamino group, an N-morpholinyl group, a dimethylaminomethyl group, a cyano group, a pyrrolidinyl group, a piperidinyl group, a pyridinyl group, an N-morpholinyl group, and a nitro group. As the nitrogen-containing group, a dimethylamino group and an N-morpholinyl group are preferred.
[0075] Examples of the oxygen-containing group include a hydroxyl group, a group in which the -CH2- structural unit in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group or nitrogen-containing group is replaced with an oxygen atom or a carbonyl group, or a group in which the -CH3 structural unit is replaced with an oxygen atom bonded to a hydrocarbon group having 1 to 20 carbon atoms, such as a methoxy group, ethoxy group, t-butoxy group, phenoxy group, trimethylsiloxy group, methoxyethoxy group, hydroxymethyl group, methoxymethyl group, ethoxymethyl group, t-butoxymethyl group, 1-hydroxyethyl group, 1-methyl ... Examples of the oxygen-containing group include 1-methoxyethyl group, 1-ethoxyethyl group, 2-hydroxyethyl group, 2-methoxyethyl group, 2-ethoxyethyl group, n-2-oxabutylene group, n-2-oxapentylene group, n-3-oxapentylene group, aldehyde group, acetyl group, propionyl group, benzoyl group, trimethylsilylcarbonyl group, carbamoyl group, methylaminocarbonyl group, carboxy group, methoxycarbonyl group, carboxymethyl group, ethoxycarboxymethyl group, carbamoylmethyl group, furanyl group, and pyranyl group. As the oxygen-containing group, a methoxy group is preferable.
[0076] Examples of halogen atoms include group 17 elements such as fluorine, chlorine, bromine, and iodine. can be. Examples of the halogen-containing group include a trifluoromethyl group, a tribromomethyl group, a pentafluoroethyl group, a pentafluorophenyl group, and the like, which are groups in which a hydrogen atom in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group, nitrogen-containing group, or oxygen-containing group is substituted with a halogen atom.
[0077] Q may be the same or different and selected in combination from a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an anionic ligand, and a neutral ligand capable of coordinating with a lone electron pair. Details of the halogen atom and the hydrocarbon group having 1 to 20 carbon atoms are as described above. When Q is a halogen atom, it is preferably a chlorine atom. When Q is a hydrocarbon group having 1 to 20 carbon atoms, the hydrocarbon group preferably has 1 to 7 carbon atoms.
[0078] Examples of the anionic ligand include alkoxy groups such as methoxy, t-butoxy, and phenoxy groups, carboxylate groups such as acetate and benzoate, and sulfonate groups such as mesylate and tosylate.
[0079] Examples of neutral ligands capable of coordinating with lone electron pairs include organic phosphorus compounds such as trimethylphosphine, triethylphosphine, triphenylphosphine, and diphenylmethylphosphine, and ether compounds such as tetrahydrofuran, diethyl ether, dioxane, and 1,2-dimethoxyethane. j is an integer of 1 to 4, and is preferably 2. n is an integer of 1 to 4, preferably 1 or 2, and more preferably 1.
[0080] R 13 and R 14 are atoms or substituents selected from the group consisting of hydrogen atoms, hydrocarbon groups having 1 to 20 carbon atoms, aryl groups, substituted aryl groups, silicon-containing groups, nitrogen-containing groups, oxygen-containing groups, halogen atoms and halogen-containing groups, and may be the same or different. 13 and R 14 may be bonded to each other to form a ring, or may not be bonded to each other.
[0081] Details of the hydrocarbon group having 1 to 20 carbon atoms, the silicon-containing group, the nitrogen-containing group, the oxygen-containing group, the halogen atom and the halogen-containing group are as described above. Examples of the aryl group include, but are not limited to, the above-mentioned examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms, and are exemplified by substituents derived from aromatic compounds, such as phenyl, 1-naphthyl, 2-naphthyl, anthracenyl, phenanthrenyl, tetracenyl, chrysenyl, pyrenyl, indenyl, azulenyl, pyrrolyl, pyridyl, furanyl, and thiophenyl groups. The aryl group is preferably a phenyl group or a 2-naphthyl group.
[0082] Examples of the aromatic compounds include aromatic hydrocarbons and heterocyclic aromatic compounds such as benzene, naphthalene, anthracene, phenanthrene, tetracene, chrysene, pyrene, indene, azulene, pyrrole, pyridine, furan, and thiophene.
[0083] The substituted aryl group partially overlaps with the examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms described above, but examples include groups in which one or more hydrogen atoms of the aryl group are substituted with at least one substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, an aryl group, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a halogen atom, and a halogen-containing group. Specific examples include a 3-methylphenyl group (m-tolyl group), a 4-methylphenyl group (p-tolyl group), a 3-ethylphenyl group, a 4-ethylphenyl group, a 3,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a biphenylyl group, a 4-(trimethylsilyl)phenyl group, a 4-aryl ... Examples of such an aminophenyl group include a 4-(dimethylamino)phenyl group, a 4-(diethylamino)phenyl group, a 4-morpholinylphenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-phenoxyphenyl group, a 3,4-dimethoxyphenyl group, a 3,5-dimethoxyphenyl group, a 3-methyl-4-methoxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3-(trifluoromethyl)phenyl group, a 4-(trifluoromethyl)phenyl group, a 3-chlorophenyl group, a 4-chlorophenyl group, a 3-fluorophenyl group, a 4-fluorophenyl group, a 5-methylnaphthyl group, and a 2-(6-methyl)pyridyl group.
[0084] Among them, R 13 and R 14 A bridged metallocene compound (P) in which at least one of the two is independently an aryl group is preferred, and a bridged metallocene compound (P) in which both are independently an aryl group is more preferred.
[0085] In particular, R 13 and R 14The bridged metallocene compound (P) in which both are independently aryl groups has high polymerization activity for copolymerization of ethylene and α-olefin, and the use of this bridged metallocene compound (P) selectively terminates polymerization by introduction of hydrogen into the molecular end, resulting in fewer unsaturated bonds in the unmodified ethylene-α-olefin copolymer (B'). Therefore, by simply carrying out a simpler hydrogen addition operation or even without carrying out a hydrogen addition operation, an unmodified ethylene-α-olefin copolymer (B') having a high degree of saturation and excellent heat resistance can be obtained, which is also excellent in terms of cost. In addition, the unmodified ethylene-α-olefin copolymer (B') obtained from the compound (P) has a controlled molecular weight distribution due to its high random copolymerizability.
[0086] In the bridged metallocene compound (P) represented by the above formula [I], n is preferably 1. Such a bridged metallocene compound (hereinafter also referred to as "bridged metallocene compound (P-1)") is represented by the following formula (1).
[0087] [ka]
[0088] In formula 1, Y, M, and R 1 ~R 14 The definitions of Y, M, R, Q, and j are as follows: 1 ~R 14 , Q, n and j have the same meanings, and the preferred embodiments are also the same.
[0089] The bridged metallocene compound (P-1) has a simplified production process and reduced production costs compared to the compound in the above formula [I] where n is an integer of 2 to 4. Thus, the use of this bridged metallocene compound (P-1) has the advantage of reducing the production costs of the ethylene-α-olefin copolymer (B'). From the above viewpoints, the modified ethylene / α-olefin copolymer (B) is preferably a modified product of an unmodified ethylene / α-olefin copolymer (B') obtained by the following method (α). Method (α): A bridged metallocene compound (P-1) represented by the above formula (1), and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) which reacts with the bridged metallocene compound (P-1) to form an ion pair; 1. A process comprising the step of solution polymerizing ethylene and an α-olefin in the presence of a catalyst system comprising:
[0090] In the bridged metallocene compound (P) represented by the above general formula [I] and the bridged metallocene compound (P-1) represented by the above (formula 1), M is more preferably a zirconium atom. When ethylene and one or more monomers selected from α-olefins having 3 to 20 carbon atoms are copolymerized in the presence of an olefin polymerization catalyst containing the above bridged metallocene compound in which M is a zirconium atom, the polymerization activity is higher than when M is a titanium atom or a hafnium atom, and the production cost of the unmodified ethylene-α-olefin copolymer (B') can be advantageously reduced.
[0091] In one embodiment of the present invention, in the above formula (1), R 13 and R 14 At least one of R is preferably an aryl group. 13 and R 14 are both aryl groups, and R 2 and R 3 It is more preferable that either one of the above is a saturated hydrocarbon group having 4 carbon atoms.
[0092] Examples of such bridged metallocene compounds (P) include [Dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5-3,6-di-t-butylfluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -2-methyl-4-t-butylcyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5-3,6-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene{η 5 -(2-methyl-4-i-propylcyclopentadienyl)}(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [diphenylsilylene(η 5-cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Ethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5-(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5-(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5-Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5-(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5-(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5-(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](2,7-diphenyl-3,6-di-tert-butylfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, and the like.
[0093] Further examples of the bridged metallocene compound (P) include compounds in which the zirconium atom of the above-mentioned bridged metallocene compound (P) is replaced with a hafnium atom or a titanium atom, and compounds in which the chloro ligand is replaced with a methyl group. In addition, η 5 -Tetramethyloctahydrodibenzofluorenyl is 4,4,7,7-tetramethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group, η 5 -Octamethyloctahydrodibenzofluorenyl is 1,1,4,4,7,7,10,10-octamethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group, respectively. The bridged metallocene compound (P) may be used alone or in combination of two or more kinds.
[0094] [Compound (Q)] The compound (Q) is at least one compound selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair.
[0095] As the organometallic compound (Q-1), specifically, the following organometallic compounds (Q-1a), (Q-1b), and (Q-1c) of Groups 1 and 2 and Groups 12 and 13 of the periodic table are used.
[0096] (Q-1a) General formula R a m Al(OR b ) n H p X q An organoaluminum compound represented by the formula: (In the formula, R a and R bmay be the same as or different from each other, and represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; X represents a halogen atom; m is a number such that 0 < m ≦ 3, n is a number such that 0 ≦ n < 3, p is a number such that 0 ≦ p < 3, q is a number such that 0 ≦ q < 3, and m + n + p + q = 3)
[0097] Examples of such compounds include tri-n-alkylaluminums such as trimethylaluminum, triethylaluminum, tri-n-butylaluminum, tri-n-hexylaluminum, and tri-n-octylaluminum, tri-branched alkylaluminums such as triisopropylaluminum, triisobutylaluminum, tri-sec-butylaluminum, tri-t-butylaluminum, tri-2-methylbutylaluminum, tri-3-methylhexylaluminum, and tri-2-ethylhexylaluminum, tricycloalkylaluminums such as tricyclohexylaluminum and tricyclooctylaluminum, triarylaluminums such as triphenylaluminum and tri(4-methylphenyl)aluminum, dialkylaluminum hydrides such as diisopropylaluminum hydride and diisobutylaluminum hydride, General formula (i-C4H9) x Al y (C5H 10 ) z (wherein x, y, and z are positive numbers and z ≦ 2x.) Alkenylaluminums such as isoprenylaluminum represented by the formula, alkylaluminum alkoxides such as isobutylaluminum methoxide and isobutylaluminum ethoxide, dialkylaluminum alkoxides such as dimethylaluminum methoxide, diethylaluminum ethoxide, and dibutylaluminum butoxide, alkylaluminum sesquialkoxides such as ethylaluminum sesquiethoxide and butylaluminum sesquibutoxide, General formula R a 2.5 Al(ORb ) 0.5 Partially alkoxylated alkylaluminum having an average composition represented by the following formula: Alkyl aluminum aryloxides such as diethyl aluminum phenoxide and diethyl aluminum (2,6-di-t-butyl-4-methylphenoxide); Dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, dibutylaluminum chloride, diethylaluminum bromide, and diisobutylaluminum chloride; Alkyl aluminum sesquihalides such as ethyl aluminum sesquichloride, butyl aluminum sesquichloride, and ethyl aluminum sesquibromide; partially halogenated alkylaluminums, such as alkylaluminum dihalides, such as ethylaluminum dichloride; dialkylaluminum hydrides such as diethylaluminum hydride and dibutylaluminum hydride; Alkyl aluminum dihydrides such as ethyl aluminum dihydride, propyl aluminum dihydride and other partially hydrogenated alkyl aluminums; Partially alkoxylated and halogenated alkylaluminums such as ethylaluminum ethoxychloride, butylaluminum butoxychloride, and ethylaluminum ethoxybromide In addition, the above general formula R a m Al(OR b ) n H p X q Compounds similar to the compound represented by the formula (1) can also be used, such as organoaluminum compounds in which two or more aluminum compounds are bonded via nitrogen atoms. Specific examples of such compounds include (C2H5)2AlN(C2H5)Al(C2H5)2.
[0098] (Q-1b) General formula M 2 AlR a4, a complex alkylation product of a metal of Group 1 of the periodic table and aluminum. (Wherein, M 2 indicates Li, Na or K, and R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms.
[0099] Such compounds include LiAl(C2H5)4, LiAl(C7H 15 ) 4 can be given as an example.
[0100] (Q-1c) General formula R a R b M 3 A dialkyl compound of a metal of Group 2 or 12 of the periodic table represented by the formula: a and R b may be the same or different and each represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; M 3 is Mg, Zn or Cd.)
[0101] As the organoaluminum oxy compound (Q-2), a conventionally known aluminoxane can be used as it is.Specific examples include a compound represented by the following general formula [III] and a compound represented by the following general formula [IV].
[0102] [ka]
[0103] In formulas [III] and [IV], R each independently represents a hydrocarbon group having 1 to 10 carbon atoms, and n represents an integer of 2 or more.
[0104] In particular, methylaluminoxanes in which R is a methyl group and n is at least 3, preferably at least 10, are used. There is no problem if these aluminoxanes contain a small amount of an organoaluminum compound.
[0105] In the present invention, when copolymerization of ethylene with an α-olefin having 3 or more carbon atoms is carried out at high temperature, benzene-insoluble organoaluminum oxy compounds as exemplified in JP-A-2-78687 can also be used. In addition, organoaluminum oxy compounds described in JP-A-2-167305, and aluminoxanes having two or more alkyl groups described in JP-A-2-24701 and JP-A-3-103407 can also be suitably used. The "benzene-insoluble organoaluminum oxy compounds" that may be used in the present invention are compounds that are insoluble or poorly soluble in benzene, and that have an Al component that dissolves in benzene at 60°C in terms of Al atoms of usually 10% or less, preferably 5% or less, and particularly preferably 2% or less.
[0106] Further, the organoaluminum oxy compound (Q-2) may also include modified methylaluminoxanes as represented by the following general formula [V].
[0107] [ka]
[0108] In formula [V], R represents a hydrocarbon group having 1 to 10 carbon atoms, and m and n each independently represent an integer of 2 or more.
[0109] Methylaluminoxane, an example of an organoaluminum oxy compound (Q-2), is commonly used as an activator in olefin polymerization because it is readily available and has high polymerization activity. However, methylaluminoxane is difficult to dissolve in saturated hydrocarbons, and has been used as a solution in aromatic hydrocarbons such as toluene or benzene, which are environmentally undesirable. For this reason, a flexible body of methylaluminoxane represented by formula [IV] has been developed and used in recent years as an aluminoxane dissolved in saturated hydrocarbons. This modified methylaluminoxane represented by formula [V] is prepared using trimethylaluminum and alkylaluminum other than trimethylaluminum, for example, trimethylaluminum and triisobutylaluminum, as shown in, for example, U.S. Pat. No. 4,960,878 and U.S. Pat. No. 5,041,584. Aluminoxanes in which Rx is an isobutyl group are commercially available in the form of saturated hydrocarbon solutions under the trade names MMAO and TMAO (see Tosoh Finechem Corporation, Tosoh Research&Technology Review, Vol 47, 55 (2003)).
[0110] Further, the organoaluminum oxy compound (Q-2) may also include a boron-containing organoaluminum oxy compound represented by the following general formula [VI].
[0111] [ka]
[0112] In formula [VI], R c R represents a hydrocarbon group having 1 to 10 carbon atoms. d may be the same or different and represent a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.
[0113] Examples of the compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair (hereinafter, sometimes abbreviated as "ionized ionic compound" or simply "ionic compound") include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-T-1-501950, JP-T-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and U.S. Pat. No. 5,321,106. Further examples include heteropoly compounds and isopoly compounds.
[0114] The ionizing ionic compound preferably used in the present invention is a boron compound represented by the following general formula [VII].
[0115] [ka]
[0116] In formula [VII], R e+ As for H + , carbenium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptyltrienyl cation, ferrocenium cation having a transition metal, etc. f ~R i may be the same or different and are substituents selected from a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a halogen atom and a halogen-containing group, and are preferably substituted aryl groups.
[0117] Specific examples of the carbenium cation include tri-substituted carbenium cations such as triphenylcarbenium cation, tris(4-methylphenyl)carbenium cation, and tris(3,5-dimethylphenyl)carbenium cation.
[0118] Specific examples of the ammonium cation include trialkyl-substituted ammonium cations such as trimethylammonium cation, triethylammonium cation, tri(n-propyl)ammonium cation, triisopropylammonium cation, tri(n-butyl)ammonium cation, and triisobutylammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as diisopropylammonium cation and dicyclohexylammonium cation.
[0119] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tris(4-methylphenyl)phosphonium cation, and tris(3,5-dimethylphenyl)phosphonium cation.
[0120] R e+ Of the above specific examples, preferred are carbenium cations and ammonium cations, with triphenylcarbenium cation, N,N-dimethylanilinium cation and N,N-diethylanilinium cation being particularly preferred.
[0121] Among the ionized ionic compounds preferably used in the present invention, examples of compounds containing a carbenium cation include triphenylcarbenium tetraphenylborate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis{3,5-di-(trifluoromethyl)phenyl}borate, tris(4-methylphenyl)carbenium tetrakis(pentafluorophenyl)borate, and tris(3,5-dimethylphenyl)carbenium tetrakis(pentafluorophenyl)borate.
[0122] Among the ionizing ionic compounds preferably used in the present invention, compounds containing a trialkyl-substituted ammonium cation include triethylammonium tetraphenylborate, tripropylammonium tetraphenylborate, tri(n-butyl)ammonium tetraphenylborate, trimethylammonium tetrakis(4-methylphenyl)borate, trimethylammonium tetrakis(2-methylphenyl)borate, tri(n-butyl)ammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(2,4-dimethylphenyl)borate, tri(n-butyl)ammonium tetrakis(3,5-dimethylphenyl)borate, tri(n-butyl)ammonium tetrakis{4-(trifluoromethyl)phenyl}borate, tri Examples of the borate include (n-butyl)ammonium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, tri(n-butyl)ammonium tetrakis(2-methylphenyl)borate, dioctadecylmethylammonium tetraphenylborate, dioctadecylmethylammonium tetrakis(4-methylphenyl)borate, dioctadecylmethylammonium tetrakis(4-methylphenyl)borate, dioctadecylmethylammonium tetrakis(pentafluorophenyl)borate, dioctadecylmethylammonium tetrakis(2,4-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis(3,5-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis{4-(trifluoromethyl)phenyl}borate, dioctadecylmethylammonium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, and dioctadecylmethylammonium.
[0123] Among the ionizing ionic compounds preferably used in the present invention, examples of compounds containing an N,N-dialkylanilinium cation include N,N-dimethylanilinium tetraphenylborate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, N,N-diethylanilinium tetraphenylborate, N,N-diethylanilinium tetrakis(pentafluorophenyl)borate, N,N-diethylanilinium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, N,N-2,4,6-pentamethylanilinium tetraphenylborate, and N,N-2,4,6-pentamethylanilinium tetrakis(pentafluorophenyl)borate.
[0124] Among the ionizing ionic compounds preferably used in the present invention, examples of compounds containing a dialkylammonium cation include di-n-propylammonium tetrakis(pentafluorophenyl)borate and dicyclohexylammonium tetraphenylborate.
[0125] In addition, the ionic compounds exemplified in JP-A-2004-51676 can also be used without any restrictions. The above ionic compounds (Q-3) may be used alone or in combination of two or more.
[0126] Examples of the catalyst system include the following [1] to [4]. [1] Bridged metallocene compound (P) and compound (Q-2) [2] Includes bridged metallocene compound (P), compound (Q-1) and compound (Q-2) [3] Bridged metallocene compound (P), compound (Q-1) and compound (Q-3) are included. [4] Includes bridged metallocene compound (P), compound (Q-2) and compound (Q-3)
[0127] The bridged metallocene compound (P) and the compounds (Q-1) to (Q-3) may be introduced into the reaction system in any order.
[0128] [Carrier (R)] In the method for producing a resin composition of the present invention, a support (R) may be used as a constituent component of the olefin polymerization catalyst, if necessary.
[0129] The carrier (R) that may be used in the present invention is an inorganic or organic compound, which is a granular or particulate solid. Among these, the inorganic compound is preferably a porous oxide, an inorganic chloride, a clay, a clay mineral, or an ion-exchangeable layered compound.
[0130] As the porous oxide, specifically, SiO2, Al2O3, MgO, ZrO, TiO2, B2O3, CaO, ZnO, BaO, ThO2, etc., or a composite or mixture containing these, such as natural or synthetic zeolite, SiO2-MgO, SiO2-Al2O3, SiO2-TiO2, SiO2-V2O5, SiO2-Cr2O3, SiO2-TiO2-MgO, etc. can be used. Among these, those containing SiO2 and / or Al2O3 as the main component are preferred. Although the properties of such porous oxides vary depending on the type and manufacturing method, the carrier preferably used in the present invention has a particle size of 0.5 to 300 μm, preferably 1.0 to 200 μm, and a specific surface area of 50 to 1000 m. 2 / g, preferably 100 to 700m 2 / g and the pore volume is 0.3-3.0 cm 3 The carrier is calcined at 100 to 1000° C., preferably 150 to 700° C., as required, before use.
[0131] Examples of inorganic chlorides that can be used include MgCl2, MgBr2, MnCl2, and MnBr2. The inorganic chlorides can be used as they are, or can be used after being pulverized by a ball mill or a vibration mill. In addition, the inorganic chlorides can be dissolved in a solvent such as alcohol, and then precipitated into fine particles using a precipitating agent.
[0132] Clay is usually composed of clay minerals as the main component. In addition, an ion-exchangeable layered compound is a compound having a crystal structure in which the constituent faces are stacked in parallel with each other with weak bonding force due to ionic bonds, etc., and the ions contained therein are exchangeable. Most clay minerals are ion-exchangeable layered compounds. In addition, these clays, clay minerals, and ion-exchangeable layered compounds are not limited to natural products, and artificial synthetic products can also be used. In addition, examples of clays, clay minerals, and ion-exchangeable layered compounds include clays, clay minerals, and ionic crystalline compounds having layered crystal structures such as hexagonal close packing type, antimony type, CdCl2 type, and CdI2 type. Examples of such clays and clay minerals include kaolin, bentonite, kibushi clay, gairome clay, allophane, hisingerite, pyrophyllite, ummo group, montmorillonite group, vermiculite, ryokudeite group, palygorskite, kaolinite, nacrite, dickite, and halloysite, and examples of ion-exchangeable layered compounds include α-Zr(HAsO4)2·H2O, α-Zr(HPO4)2, α-Zr(KPO4)2·3H2O, α-Ti(HPO4)2, α-Ti(HAsO4)2·H2O, α-Sn(HPO4)2·H2O, γ-Zr(HPO4)2, γ-Ti(HPO4)2, and γ-Ti(NH4PO4)2·H2O, and other crystalline acid salts of polyvalent metals. It is also preferable to subject the clay and clay minerals used in the present invention to chemical treatment. The chemical treatment may be any of surface treatments that remove impurities adhering to the surface, treatments that affect the crystal structure of the clay, etc. Specific examples of the chemical treatment include acid treatment, alkali treatment, salt treatment, and organic matter treatment.
[0133] The ion-exchangeable layered compound may be a layered compound in which the space between layers is expanded by utilizing the ion exchangeability and exchanging the exchangeable ions between layers with other large bulky ions. Such bulky ions play a role of supporting the layered structure and are usually called pillars. The introduction of another substance (guest compound) between layers of a layered compound in this way is called intercalation. Examples of guest compounds include cationic inorganic compounds such as TiCl4 and ZrCl4, metal alkoxides such as Ti(OR)4, Zr(OR)4, PO(OR)3, and B(OR)3 (R is a hydrocarbon group, etc.), [Al 13 O4(OH) 24 ] 7+ , [Zr4(OH) 14 ] 2+ , [Fe3O(OCOCH3)6] + Metal hydroxide ions such as these can be used. These compounds can be used alone or in combination of two or more. When these compounds are intercalated, polymers obtained by hydrolysis and polycondensation of metal alkoxides such as Si(OR)4, Al(OR)3, Ge(OR)4 (R is a hydrocarbon group, etc.), colloidal inorganic compounds such as SiO2, etc. can also be coexisted. Examples of pillars include oxides produced by intercalating the above metal hydroxide ions between layers and then dehydrating them with heat.
[0134] Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, pectolite, taeniolite and synthetic mica are particularly preferred. The organic compound as the carrier (R) may be a granular or fine particle solid having a particle size in the range of 0.5 to 300 μm. Specifically, it may be a (co)polymer produced mainly from an α-olefin having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, or 4-methyl-1-pentene, or a (co)polymer produced mainly from vinylcyclohexane or styrene, or a modified product thereof.
[0135] The method of use and order of addition of each component of the polymerization catalyst may be selected arbitrarily, and at least two of the components in the catalyst may be contacted in advance. The bridged metallocene compound (P) (hereinafter also referred to as "component (P)") is usually 1 x 10 -9 ~1×10 -1 Molar, preferably 1 x 10 -8 ~1×10 -2 It is used in molar amounts.
[0136] The organometallic compound (Q-1) (hereinafter also referred to as "component (b-1)") is used in an amount such that the molar ratio of component (Q-1) to the transition metal atom (M) in component (P) [(Q-1) / M] is generally 0.01 to 50,000, preferably 0.05 to 10,000.
[0137] The organoaluminum oxy compound (Q-2) (hereinafter also referred to as "component (Q-2)") is used in an amount such that the molar ratio [(Q-2) / M] of the aluminum atom in component (Q-2) to the transition metal atom (M) in component (P) is generally 10 to 5,000, preferably 20 to 2,000.
[0138] The ionic compound (Q-3) (hereinafter also referred to as "component (Q-3)") is used in an amount such that the molar ratio of component (Q-3) to the transition metal atom (M) in component (P) [(Q-3) / M] is generally 1 to 10,000, preferably 1 to 5,000.
[0139] The polymerization temperature is usually -50°C to 300°C, preferably 30 to 250°C, more preferably 100°C to 250°C, and further preferably 130°C to 200°C. In the polymerization temperature range, as the temperature increases, the solution viscosity during polymerization decreases and the heat of polymerization is easily removed. The polymerization pressure is usually normal pressure to 10 MPa gauge pressure (MPa-G), and preferably normal pressure to 8 MPa-G.
[0140] The polymerization reaction can be carried out in any of batch, semi-continuous and continuous systems. Furthermore, the polymerization can be carried out continuously in two or more polymerization vessels with different reaction conditions. The molecular weight of the resulting copolymer can be adjusted by changing the hydrogen concentration in the polymerization system or the polymerization temperature. It can also be adjusted by the amount of component (Q) used. When hydrogen is added, the amount is appropriately about 0.001 to 5,000 NL per kg of the resulting copolymer.
[0141] The polymerization solvent used in the liquid phase polymerization method is usually an inert hydrocarbon solvent, preferably a saturated hydrocarbon having a boiling point of 50°C to 200°C under normal pressure. Specific examples of the polymerization solvent include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, and alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane, and particularly preferably hexane, heptane, octane, decane, and cyclohexane. The α-olefin itself, which is the object of polymerization, can also be used as the polymerization solvent. Incidentally, aromatic hydrocarbons such as benzene, toluene, and xylene, and halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane can also be used as the polymerization solvent, but from the viewpoint of reducing the burden on the environment and minimizing the impact on human health, the use of these is not preferred.
[0142] The kinetic viscosity of unmodified ethylene-α-olefin copolymer (B') at 100°C depends on the molecular weight of the polymer. That is, the higher the molecular weight, the higher the viscosity, and the lower the molecular weight, the lower the viscosity. Therefore, the kinetic viscosity at 100°C can be adjusted by adjusting the molecular weight as described above. Furthermore, by removing low molecular weight components from the obtained polymer by a conventionally known method such as reduced pressure distillation, the molecular weight distribution (Mw / Mn) of the obtained polymer can be adjusted. Furthermore, the obtained polymer may be subjected to hydrogenation (hereinafter also referred to as "hydrogenation") by a conventionally known method. If the double bonds of the obtained polymer are reduced by hydrogenation, the oxidation stability and heat resistance are improved.
[0143] The resulting unmodified ethylene-α-olefin copolymer (B′) may be used alone or in combination of two or more types having different molecular weights or different monomer compositions.
[0144] The modified ethylene-α-olefin copolymer (B) is a modified copolymer having a substituent derived from a vinyl aromatic compound as required by requirement (b-3), and can be produced by modifying the unmodified ethylene-α-olefin copolymer (B') described above. Specifically, the unmodified ethylene-α-olefin copolymer (B') can be produced by modifying the unmodified ethylene-α-olefin copolymer by various conventionally known methods described in JP-A-61-126120 and JP-A-2593264, or by the following methods (1) and (2), for example. (1) A method in which an unmodified ethylene-α-olefin copolymer (B') is charged into an extruder, batch reactor, etc., and modified by adding a compound having a carbon-carbon double bond, such as a vinyl aromatic compound, to be reacted therewith. (2) A method in which an unmodified ethylene-α-olefin copolymer (B') is dissolved in a solvent and modified by adding a compound having a carbon-carbon unsaturated bond (a compound having an ethylenically unsaturated bond), such as a vinyl aromatic compound.
[0145] In any of the above methods, in order to efficiently graft a compound having a carbon-carbon unsaturated bond (ethylenically unsaturated bond), such as a vinyl aromatic compound, it is preferable to carry out the graft copolymerization in the presence of one or more radical initiators, etc.
[0146] Examples of the radical initiator include organic peroxides and azo compounds. Examples of the organic peroxide include benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,4-bis(tert-butylperoxyisopropyl)benzene, and the like. Examples of the azo compound include azobisisobutyronitrile, dimethylazoisobutyrate, and the like. Among these, dialkyl peroxides such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 1,4-bis(tert-butylperoxyisopropyl)benzene are particularly preferably used.
[0147] The amount of the radical initiator used is usually 0.001 to 15 parts by mass, preferably 0.01 to 15 parts by mass, and more preferably 0.05 to 15 parts by mass, based on 100 parts by mass of the unmodified ethylene / α-olefin copolymer (B′).
[0148] The reaction temperature in the modification reaction is usually 20 to 350°C, and preferably 60 to 300°C.
[0149] The modified ethylene-α-olefin copolymer (B) produced by the above method may be further modified by a second modification, for example, the method described in JP-A-2008-508402 etc. In addition to the above, the modified ethylene-α-olefin copolymer (B) may be modified by reacting it with a reactive gas or liquid.
[0150] The reactive gas or liquid includes air, oxygen, ozone, chlorine, bromine, sulfur dioxide, sulfuryl chloride, etc., and one or more of these can be used. Among these, oxidation reactions using air and / or oxygen, chlorination using chlorine, and chlorosulfonation reactions using sulfuryl chloride, chlorine and sulfur dioxide, chlorine and sulfuryl chloride, and chlorine, sulfur dioxide and sulfuryl chloride are preferred. The gas used in this method may be diluted to any concentration with an inert gas such as nitrogen, argon, or carbon dioxide.
[0151] When modification is performed by an oxidation reaction using air and / or oxygen, the reaction may be carried out in the presence of one or more selected from a metal or metal salt, an inorganic acid, an organic acid, and the like, in addition to the radical initiator, in order to promote the reaction. Examples of the metals or metal salts include manganese acetate, cobalt acetate, manganese chloride, nickel oxide, copper, etc., examples of the inorganic acids include hydrochloric acid and nitric acid, and examples of the organic acids include formic acid, acetic acid, oxalic acid, malonic acid, maleic acid, tartaric acid, malic acid, adipic acid, citric acid, etc.
[0152] The reaction temperature for reacting with the reactive gas or liquid is usually 20 to 350° C., preferably 60 to 300° C., and the reaction pressure is preferably normal pressure to 5 MPa.
[0153] <Adhesive resin (C)> The resin composition according to the present invention contains an adhesive resin (C). The adhesive resin (C) adjusts the viscosity of the resin composition when melted and plays a role in improving hot tackiness and wettability. Therefore, it is usually a substance with good fluidity when melted, and an oligomer having a molecular weight of several hundred to several tens of thousands and a softening point of about 60 to 160°C is generally used. In the present invention, any resin known as a tackifier can be used as the adhesive resin (C).
[0154] Examples of the adhesive resin (C) include aliphatic hydrogenated tackifiers, rosin, modified rosin or ester compounds thereof, aliphatic petroleum resins, alicyclic petroleum resins, aromatic petroleum resins, copolymerized petroleum resins of aliphatic and aromatic components, low molecular weight styrene resins, isoprene resins, alkylphenol resins, terpene resins, hydrogenated terpene resins, coumarone-indene resins, etc. Alternatively, as disclosed in JP-A-2005-194488, it may be one obtained by copolymerizing multiple monomers selected from terpene monomers, chroman monomers, styrene monomers, or phenol monomers. The adhesive resin (C) may be used alone or in combination of two or more kinds.
[0155] In the resin composition of the present invention, the molecules of the modified ethylene-α-olefin copolymer (B) are entangled with the molecular chains of the block copolymer (A), thereby interacting with the block copolymer (A) and uniformly softening the block copolymer (A). This makes it easier for the adhesive resin (C) to exhibit good dispersibility, and as a result, makes it easier to obtain a resin composition excellent in hot tack property, wettability, and adhesion, making the composition useful.
[0156] The content of the adhesive resin (C) in the resin composition of the present invention is preferably 10 to 300 parts by mass, more preferably 20 to 250 parts by mass, and even more preferably 30 to 200 parts by mass, based on 100 parts by mass of the block copolymer (A). When the content of the adhesive resin (C) is within the above range, a resin composition having excellent adhesiveness under a wide range of temperature conditions from low to high temperatures can be obtained.
[0157] [Optional ingredients] The resin composition of the present invention may contain optional components such as various known compounding agents, depending on the desired performance, etc., within the scope of not impairing the object of the present invention. Examples of optional components include resin components other than the block copolymer (A) and the modified ethylene-α-olefin copolymer (B), softeners and plasticizers, tackifiers other than the adhesive resin (C), antioxidants, ultraviolet absorbers, flame retardants, fillers, silane coupling agents, lubricants, crosslinking agents, crosslinking assistants, antioxidants, processing assistants, antistatic agents, various dyes, representative examples of which are disperse dyes and acid dyes, inorganic and organic pigments, foaming agents, defoamers, antibacterial agents, etc.
[0158] Examples of the resin component other than the block copolymer (A) include polyolefin resins, polyvinyl chloride resins, polyamide resins, polyester resins, styrene-based resins, polyurethane resins, polyacetal resins, acrylic resins, polycarbonate resins, polyphenylene ether resins, polyphenylene sulfide resins, fluorine-based resins, polyimide resins, and polyether ketone resins.
[0159] Examples of polyolefin resins include low density polyethylene, medium density polyethylene, high density polyethylene, linear low density polyethylene, polypropylene, polybutene, poly(4-methyl-1-pentene), cyclic olefin polymers, ethylene-propylene copolymers, ethylene-butene copolymers, ethylene-octene copolymers, propylene-ethylene copolymers, propylene-butene copolymers, propylene-ethylene-butene copolymers, propylene-4-methyl-1-pentene copolymers, and ethylene-cyclic olefin copolymers.
[0160] Examples of polyvinyl chloride resins include vinyl chloride homopolymers, and copolymers of vinyl chloride with vinylidene chloride, acrylic esters, acrylonitrile, propylene, ethylene, and the like.
[0161] Examples of polyamide resins include nylon 6, nylon 11, nylon 12, nylon 46, nylon 66, nylon M XD6, fully aromatic polyamides, and semi-aromatic polyamides.
[0162] Examples of polyester resins include polyethylene terephthalate and polybutylene terephthalate.
[0163] Examples of styrene resins include polystyrene, acrylonitrile-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, and other styrene polymers and their hydrogenated products. The styrene polymers and their hydrogenated products may be either random copolymers or block copolymers.
[0164] Examples of polyurethane resins include those synthesized from an isocyanate such as m-xylylene diisocyanate (XDI), 4,4'-methylenebis(cyclohexyl isocyanate) (HMDI) or isophorone diisocyanate (IPDI) and a polyester-based or polyether-based diol.
[0165] Examples of polyacetal resins include polyacetal homopolymers and copolymers of formaldehyde and trioxane.
[0166] Examples of acrylic resins include those having structural units derived from unsaturated monomers such as acrylic acid, methyl acrylate, ethyl acrylate, butyl acrylate, sodium acrylate, ammonium acrylate, 2-hydroxyethyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, sodium methacrylate, ammonium methacrylate, 2-hydroxyethyl methacrylate, glycidyl methacrylate, acrylamide, methacrylamide, etc. Also, the above-listed unsaturated monomers may be copolymerized with other unsaturated monomers such as styrene, vinyl acetate, vinyl chloride, vinylidene chloride, divinylbenzene, etc.
[0167] An example of the polycarbonate resin is bisphenol A type aromatic polycarbonate.
[0168] Examples of the polyphenylene ether resin include polyphenylene ether and modified polyphenylene ether.
[0169] Examples of fluorine-based resins include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkylvinyl ether copolymer (PFA), and tetrafluoroethylene-ethylene copolymer (ETFE).
[0170] Examples of polyimide resins include those obtained from combinations of pyromellitic anhydride and diaminodiphenyl ether, bismaleimide and diaminodiphenylmethane, and the like.
[0171] Examples of the polyether ketone resin include polyether ketone, polyether ether ketone, polyether ketone ketone, and polyether ether ketone ketone.
[0172] Examples of the softener and plasticizer include petroleum-based softeners such as process oil, lubricating oil, paraffin, liquid paraffin, petroleum asphalt, and vaseline; coal tar-based softeners such as coal tar and coal tar pitch; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, and coconut oil; tall oil; sap; waxes such as beeswax, carnauba wax, and lanolin; fatty acids and fatty acid salts such as ricinoleic acid, palmitic acid, barium stearate, calcium stearate, and zinc laurate; and synthetic resins such as petroleum resin and coumarone-indene resin. The softener and plasticizer are preferably compounds other than the modified ethylene-α-olefin copolymer (B). These softeners may be used alone or in combination of two or more. Among them, petroleum-based softeners are preferred, process oils are more preferred, and paraffin-based process oils are particularly preferred.
[0173] Examples of the antioxidant include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenyl)propionate, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,4-bis(octylthiomethyl)-o-cresol, 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2,4-di-t-amyl-6-[1-(3,5-di-t-amyl-2-hydroxyphenyl)ethyl] Examples of the antioxidant include phenol-based antioxidants such as phenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)]acrylate, and tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane; sulfur-based antioxidants such as dilauryl thiodipropionate, lauryl stearyl thiodipropionate, and pentaerythritol tetrakis(3-lauryl thiopropionate); phosphorus-based antioxidants such as tris(nonylphenyl)phosphite and tris(2,4-di-t-butylphenyl)phosphite; and lactone-based antioxidants. Further examples of the antioxidant include primary antioxidants such as naphthylamines, p-phenylenediamines, quinolines, phenols, hindered phenols and hindered amines, and secondary antioxidants such as phosphites, thioethers and hydroxylamines. Among these, the phenol-based antioxidants are preferred as the antioxidant.
[0174] Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-t-butylphenyl)benzotriazole, and 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole; benzophenone-based ultraviolet absorbers such as 2-hydroxy-4-methoxybenzophenone; salicylic acid ester-based ultraviolet absorbers; cyanoacrylate-based ultraviolet absorbers; and hindered amine-based light stabilizers.
[0175] Examples of flame retardants include organic phosphorus-containing compounds, inorganic phosphorus-containing compounds, organic halogen-containing compounds, inorganic halogen-containing compounds, organic phosphorus-halogen-containing compounds, inorganic phosphorus-halogen-containing compounds, antimony oxide, titanium oxide, metal hydroxides, and hydrated inorganic crystalline compounds.
[0176] Examples of the filler include carbon black, graphite, carbon black that has been surface-treated with a silane coupling agent or the like, oxide-based fillers such as finely powdered silicic acid, silica, alumina, magnesium oxide, barium oxide, calcium oxide, and titanium oxide, hydroxide-based fillers such as aluminum hydroxide and magnesium hydroxide, sedimentary rock-based fillers such as diatomaceous earth and limestone, clay mineral-based fillers such as kaolinite and montmorillonite, magnetic fillers such as ferrite, iron, and cobalt, conductive fillers such as silver, gold, copper, and alloys, light calcium carbonate, heavy calcium carbonate, talc, and clay. Examples of carbon black include SAF, ISAF, HAF, EPC, XCF, FEF, GPF, HMF, SRF, FT, and MT. The silica is not particularly limited, and examples thereof include dry process silica (anhydrous silicic acid) and wet process silica (hydrated silicic acid).
[0177] Examples of silane coupling agents include trimethoxyvinylsilane and γ-glycidylsilane. propyltrimethoxysilane and the like.
[0178] Examples of lubricants include higher fatty acids such as ricinoleic acid, stearic acid, palmitic acid, and lauric acid; higher fatty acid salts such as barium stearate, zinc stearate, and calcium stearate; and higher fatty acid esters such as ricinoleic acid esters, stearic acid esters, palmitic acid esters, and lauric acid esters.
[0179] As the crosslinking agent, organic peroxides, sulfur and sulfur compounds can be used, of which sulfur is preferred. Examples of organic peroxides include dialkyl peroxides such as dicumyl peroxide, di-t-butyl peroxide, di-t-butylperoxy-3,3,5-trimethylcyclohexane, t-butylcumyl peroxide, di-t-amyl peroxide, t-butyl hydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxine)hexyne-3, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,5-dimethyl-2,5-mono(t-butylperoxy)-hexane, and α,α'-bis(t-butylperoxy-m-isopropyl)benzene; and peroxy esters such as t-butyl peroxy acetate, t-butyl peroxy isobutyrate, t-butyl peroxy pivalate, t-butyl peroxy maleic acid, t-butyl peroxy neodecanoate, t-butyl peroxy benzoate, and di-t-butyl peroxy phthalate. Ketone peroxides such as dicyclohexanone peroxide, and mixtures of these Examples include: Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, surface-treated sulfur, and insoluble sulfur. Specific examples of sulfur compounds include sulfur chloride, sulfur dichloride, polymeric polysulfides, and sulfur compounds that release active sulfur to crosslink at crosslinking (vulcanization) temperatures, such as morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, dipentamethylenethiuram tetrasulfide, and selenium dimethyldithiocarbamate.
[0180] [Method of producing resin composition] The method for producing a resin composition of the present invention includes a step of mixing a block copolymer (A), a modified ethylene-α-olefin copolymer (B) satisfying the above requirements (b-1) to (b-4), and an adhesive resin (C). The method for producing a resin composition of the present invention may also include a step of melt-kneading and / or mixing optional components, in addition to the above components, as necessary, by a conventionally known method. In this case, each component may be melt-kneaded and / or mixed at once, or all or a part of the components may be mixed in advance without melting, and then heated to melt-knead and / or mix. For example, a plastomill, a Henschel mixer, a V-blender, a ribbon blender, a tumbler blender, a kneader, a kneader-ruder, a pressure kneader, a Brabender type kneader, a disperser, a single screw extruder, a twin screw extruder, a plastomill, a Banbury mixer, etc. can be used for melt kneading and / or mixing. The inside of these devices may be depressurized as necessary. The melt kneaded and / or mixed resin composition can be filled into a release box, a pail can, a drum can, etc., cooled and solidified, and stored.
[0181] If desired, a crosslinking agent such as an organic peroxide, a crosslinking assistant, etc. may be added, or these necessary components may be mixed at the same time and melt-kneaded and mixed to cause partial crosslinking to the extent that does not impair the effects of the present invention. It is also possible to add a crosslinking agent such as an organic peroxide, a crosslinking assistant, etc. to form a crosslinked body. By forming a partial crosslink or a crosslinked body, the rubber elasticity at high temperatures can be improved. Suitable examples of the crosslinking agent include organic peroxides, such as 2,5-dimethyl-2,5-di(t-butylperoxy)-hexane; 2,5-dimethyl-2,5-di(benzoylperoxy)-hexane; t-butylperoxybenzoate; dicumyl peroxide; t-butylcumyl peroxide; diisopropylbenzohydroperoxide; 1,3-bis-(t-butylperoxyisopropyl)-benzene; benzoyl peroxide; 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane, and useful examples of the crosslinking assistant include divinylbenzene, trimethylolpropane triacrylate, ethylene dimethacrylate, diallyl phthalate, quinone dioxime, phenylene bismaleimide, polyethylene glycol dimethacrylate, and unsaturated silane compounds. These organic peroxides and crosslinking assistants can be used in an amount of 0.1 to 5 parts by mass when the total amount of the block copolymer (A) and the modified ethylene-α-olefin copolymer (B) is taken as 100 parts by mass, to adjust the degree of crosslinking. Two or more of these organic peroxides and crosslinking assistants can be used in combination as necessary. When an unsaturated silane compound is used as the crosslinking assistant, the crosslinking can be promoted by contacting the compound with moisture in the presence of a silanol condensation catalyst.
[0182] The resin composition of the present invention can be used for various applications without limitation. Specifically, the resin composition can be used for adhesives, hot melt adhesives, heat seal materials, primers, sealants, electric wires, wires, cables, wire harnesses, linings, hoses, tubes, pipes, bottles, separators, molding materials, mandrels, belts, shock absorbing pads, protectors, protective equipment such as helmets and guards, various grip members such as golf clubs, tennis rackets, bats, and tools, mouth guards, various balls such as baseballs, tennis balls, and golf balls, vibration-damping pallets, shock absorbing dampers, insulators, shock absorbing materials for footwear, shock absorbing foams, toothbrushes, flooring materials, electric power tool members, agricultural equipment members, heat dissipation materials, transparent substrates, soundproofing materials, cushioning materials, gaskets, caps, medicine stoppers, packing materials, cap liners, and shoes. Examples of such materials include shoe and sandal components such as soles, shoe bottom soles, shoe midsoles, inner soles, and soles; leather, nonwoven fabrics, fibers, cloth materials; films and sheets used for various purposes such as packaging, optics, release, heat transfer, conductivity, dust prevention, transfer, protection, and shock absorption; bumpers, door trims, rear package trims, seat back garnishes, instrument panels, interior materials, exterior materials; masterbatches such as pellets, powders, and pastes containing fillers, pigments, oils, fibers, and the like; various molded products such as extrusion molded products, injection molded products, hollow molded products, foam molded products, and crosslinked molded products; building materials, automobile components, home appliance components, industrial components, clothing components, daily necessities components, kitchenware components, and sporting goods components.
[0183] [Adhesives, hot melt adhesives, heat seal materials, primers] The resin composition of the present invention can be appropriately molded by a conventionally known method and used as a pressure-sensitive adhesive, a hot melt adhesive, a heat seal material, a primer, etc. The resin composition of the present invention has excellent adhesiveness under a wide range of temperature conditions from low to high temperatures, and is therefore suitably used as a pressure-sensitive adhesive, a hot melt adhesive, a heat seal material, or a primer. EXAMPLES
[0184] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The raw material components used in the examples and comparative examples are as follows.
[0185] [Block copolymer (A) and unhydrogenated block copolymer (A')] In the following Examples and Comparative Examples, the following commercially available products were used as the block copolymer (A). A-1: Polystyrene-poly(ethylene / butene)-polystyrene block copolymer (SEBS), Kraton G1657 manufactured by Kraton Polymers (styrene content: 13% by mass, MFR (230°C, 5 kg): 22 g / 10 min, Mw = 110,000) A'-1: Polystyrene-polyisoprene-polystyrene block copolymer (SIS), SIS5403P (styrene content: 15% by mass) manufactured by ENEOS Materials Co., Ltd.
[0186] [Modified ethylene-α-olefin copolymer (B)] The physical properties of the modified ethylene / α-olefin copolymer (B) and the unmodified ethylene / α-olefin copolymer (B′) were measured as follows.
[0187] <Kinematic viscosity at 100℃> The kinetic viscosity at 100° C. (100° C. kinetic viscosity) was measured and calculated according to the method described in JIS K2283.
[0188] <Weight average molecular weight (Mw), Mw / Mn> The molecular weights (Mw) and Mw / Mn of the modified ethylene-α-olefin copolymer (B) and unmodified ethylene-α-olefin copolymer (B′) were determined by the following high-speed GPC measurement apparatus. High-speed GPC measurement device: Tosoh Corporation HLC8320GPC Mobile phase: THF (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., stabilizer-free, liquid chromatography grade) Column: Two TSKgel Super MultiporeHZ-M columns (Tosoh Corporation) connected in series Sample concentration: 5mg / mL Mobile phase flow rate: 0.35mL / min Measurement temperature: 40℃ Standard sample for calibration curve: PStQuick MP-M manufactured by Tosoh Corporation
[0189] <Ethylene content (mol%)> The ethylene content of the modified ethylene-α-olefin copolymer (B) and the unmodified ethylene-α-olefin copolymer (B′) was measured using a JEOL ECP500 nuclear magnetic resonance spectrometer with a mixed solvent of orthodichlorobenzene / heavy benzene (80 / 20% by volume), a sample concentration of 55 mg / 0.6 mL, a measurement temperature of 120°C, and observation nuclei of 13 The measurements were performed using C (125 MHz), a sequence of single pulse proton decoupling, a pulse width of 4.7 μs (45° pulse), a repetition time of 5.5 seconds, an accumulation count of 10,000 or more, and a chemical shift reference value of 27.50 ppm.
[0190] The ethylene contents of the modified ethylene-α-olefin copolymer (B) and the unmodified ethylene-α-olefin copolymer (B′) were measured as described above. 13 The values were calculated from C-NMR spectra based on the reports of "Polymer Analysis Handbook" (published by Asakura Publishing, pp. 163-170), GJ Ray (Macromolecules, 10, 773 (1977)), JC Randal (Macromolecules, 15, 353 (1982)), and K. Kimura (Polymer, 25, 4418 (1984)).
[0191] <Content of parts derived from styrene> The content of styrene-derived moieties (hereinafter referred to as "styrene content (modification amount)") is 1 It was determined by the following formula using the H-NMR area ratio. Content of styrene-derived moieties (mass%) = 100 × (B × 104 ÷ 5) ÷ [(AB × 3 / 5) × 14 ÷ 2 + (B × 104 ÷ 5)] (A=area ratio of 0.3 to 4 ppm, B=area ratio of 6 to 8 ppm)
[0192] <Brookfield viscosity at 150℃> The Brookfield viscosity at 150°C of the modified ethylene·α-olefin copolymer (B) was measured and calculated according to the method described in JIS K7117-1, 2.
[0193] [Preparation of modified ethylene / α-olefin copolymer (B) and unmodified ethylene / α-olefin copolymer (B′)] The methods for producing the modified ethylene / α-olefin copolymer (B) and the unmodified ethylene / α-olefin copolymer (B') used in the examples and comparative examples are described below.
[0194] [Production Example 1] Preparation of ethylene-propylene copolymer (B'-1) In a 2-liter continuous polymerization reactor equipped with an agitator and thoroughly purifying the atmosphere with nitrogen, 1 liter of dehydrated and purified hexane was placed, and ethylaluminum sesquichloride (Al(C2H5) 1.5 ·Cl 1.5) in hexane at a rate of 500mL / h for 1 hour, and then a hexane solution of VO(OC2H5)Cl2 adjusted to 16mmol / L as a catalyst at a rate of 500mL / h and hexane at a rate of 500mL / h were continuously fed. Meanwhile, the polymerization solution was continuously extracted from the top of the reactor so that the polymerization solution in the reactor was always 1L. Next, ethylene gas was fed at a rate of 18L / h, propylene gas at a rate of 18L / h, and hydrogen gas at a rate of 120L / h using a bubbling tube. The copolymerization reaction was carried out at 35°C by circulating a coolant through a jacket attached to the outside of the reactor. As a result, a polymerization solution containing an ethylene-propylene copolymer was obtained. The obtained polymerization solution was washed three times with 500mL of 0.2mol / L hydrochloric acid per 1L of the polymerization solution, and then three times with 500mL of distilled water per 1L of the polymerization solution, dried over magnesium sulfate, and the solvent was distilled off under reduced pressure. The resulting viscous liquid was dried under reduced pressure at 130°C for 24 hours to obtain ethylene-propylene copolymer (B'-1). The ethylene content of the obtained ethylene-propylene copolymer (B′-1) was 1820, the weight average molecular weight (Mw) was 1820, and the kinetic viscosity at 100°C was 20 mm 2 / s.
[0195] [Production Example 2] Preparation of ethylene-propylene copolymer (B'-2) 910 mL of heptane and 45 g of propylene were charged into a 2 L stainless steel autoclave that had been thoroughly purged with nitrogen, and the temperature inside the system was raised to 130°C. Then, 2.24 MPa of hydrogen and 0.09 MPa of ethylene were fed to adjust the total pressure to 3 MPaG. Next, 0.4 mmol of triisobutylaluminum, [diphenylmethylene (η 5 -3-n-butylcyclopentadienyl)(η 50.0006mmol of N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate was added with nitrogen and polymerization was started by changing the stirring speed to 400 rpm. Then, the total pressure was kept at 3MPaG by continuously supplying only ethylene, and polymerization was carried out at 130°C for 5 minutes. After the polymerization was stopped by adding a small amount of ethanol to the system, unreacted ethylene, propylene, and hydrogen were purged. The obtained polymerization solution was washed three times with 1000mL of 0.2mol / L hydrochloric acid and then three times with 1000mL of distilled water, dried over magnesium sulfate, and the solvent was removed under reduced pressure to obtain a crude ethylene-propylene copolymer.
[0196] A 1L stainless steel autoclave was charged with 100mL of a hexane solution of 0.5% Pd / alumina catalyst and 500mL of a 30% hexane solution of the crude ethylene-propylene copolymer. The autoclave was then sealed and purged with nitrogen. The temperature was then raised to 140°C while stirring, and the system was purged with hydrogen. The pressure was then raised to 1.5MPa with hydrogen and the hydrogenation reaction was carried out for 15 minutes. The reaction solution was filtered to remove the hydrogenation catalyst, the solvent was removed under reduced pressure, and the mixture was dried at 80°C under reduced pressure for 24 hours to obtain ethylene-propylene copolymer (B'-2). The copolymer (B'-2) had an ethylene content of 51.9 mol%, Mw of 2,700, Mw / Mn of 1.5, and a kinetic viscosity at 100°C of 40 mm 2 / s.
[0197] [Production Example 3] Production of styrene-modified ethylene-propylene copolymer (B-1) 324g of unmodified ethylene-α-olefin copolymer (B'-1) was placed in a 1L glass autoclave, and the atmosphere was replaced with nitrogen. Next, the temperature was raised to 160°C with stirring, and 86g of styrene and 14.5g of di-tert-butyl peroxide were fed over 4 hours, and the reaction was allowed to proceed for 1 hour after the completion of the feeding. Next, the pressure was reduced for 1 hour while gradually passing nitrogen through using a vacuum pump to remove impurities (unreacted styrene and decomposition products of di-tert-butyl peroxide). The above operations yielded styrene-modified ethylene-propylene copolymer (B-1). The styrene content (modification amount) of this styrene-modified ethylene-propylene copolymer (B-1) was 21 mass%, Mw was 4,700, Mw / Mn was 2.2, and the Brookfield viscosity at 100°C was 62 mPa·s.
[0198] [Production Example 4] Production of styrene-modified ethylene-propylene copolymer (B-2) 327g of unmodified ethylene-α-olefin copolymer (B'-2) was placed in a 1L glass autoclave, and the atmosphere was replaced with nitrogen. Next, the temperature was raised to 160°C with stirring, and 87g of styrene and 14.7g of di-tert-butyl peroxide were fed over 4 hours, and the reaction was allowed to proceed for 1 hour after the completion of the feeding. Next, the pressure was reduced for 1 hour while gradually passing nitrogen through using a vacuum pump to remove impurities (unreacted styrene and decomposition products of di-tert-butyl peroxide). The above operations yielded styrene-modified ethylene-propylene copolymer (B-2). The styrene content (modification amount) of this styrene-modified ethylene-propylene copolymer (B-2) was 20 mass%, Mw was 8,800, Mw / Mn was 3.1, and the Brookfield viscosity at 100°C was 170 mPa·s.
[0199] [Production Example 5] Production of styrene-modified ethylene-propylene copolymer (B-3) 362g of unmodified ethylene-α-olefin copolymer (B'-1) was placed in a 1L glass autoclave, and the atmosphere was replaced with nitrogen. Next, the temperature was raised to 160°C with stirring, and 45g of styrene and 7.6g of di-tert-butyl peroxide were fed over 2 hours, and the reaction was allowed to proceed for 1 hour after the completion of the feeding. Next, the pressure was reduced for 1 hour while gradually passing nitrogen through using a vacuum pump to remove impurities (unreacted styrene and decomposition products of di-tert-butyl peroxide). The above operations yielded styrene-modified ethylene-propylene copolymer (B-3). The styrene content (modification amount) of this styrene-modified ethylene-propylene copolymer (B-3) was 11 mass%, Mw was 3,000, Mw / Mn was 1.8, and the Brookfield viscosity at 100°C was 24 mPa·s.
[0200] [Adhesive resin (C)] In the following Examples and Comparative Examples, the following commercially available products were used as the adhesive resin (C). C-1: C5C9 petroleum resin, Eastman Chemical Company, Regalite C6100
[0201] [Optional ingredients] The following commercially available antioxidants were used: D-1: Phenolic antioxidant, manufactured by BASF Japan, Irganox 1010
[0202] [Mineral oil] In the following comparative examples, the following commercially available mineral oils were used. Z-1: Paraffin-based mineral oil, Idemitsu Kosan Co., Ltd., Diana Process Oil PW-90 Z-2: Paraffin-based mineral oil, Idemitsu Kosan Co., Ltd., Diana Process Oil PW-380
[0203] [Styrene modified ethylene propylene rubber] In the comparative examples below, the styrene-modified ethylene-propylene rubber used was modified rubber (Z-3) produced by the following method. 100 parts by mass of ethylene-propylene copolymer rubber (Esprene E-120, Sumitomo Chemical Co., Ltd.), 40 parts by mass of styrene, 500 parts by mass of water, 1.5 parts by mass of benzoyl peroxide, 3 parts by mass of calcium phosphate, and 3 parts by mass of polyethylene glycol were charged into a polymerization vessel, and the inside of the vessel was thoroughly replaced with nitrogen while stirring. Polymerization was then carried out at 90°C for 1 hour, and then at 110°C for 1 hour. The polystyrene in the obtained graft copolymer was extracted with methyl ethyl ketone, and it was confirmed that approximately 20% by mass of styrene was grafted to the copolymer. The Brookfield viscosity at 100°C could not be measured because it was too high a viscosity.
[0204] [Examples 1 to 3 and Comparative Examples 1 to 6] The block copolymer (A-1), the unhydrogenated block copolymer (A'-1), the modified ethylene-α-olefin copolymers (B-1) to (B-3), the unmodified ethylene-α-olefin copolymers (B'-1) and (B'-2), and the adhesive resin (C-1), as well as the optional components, the mineral oils (Z-1) and (Z-2), and the styrene-modified ethylene-propylene rubber (Z-3), were melt-mixed in a separable glass flask equipped with a stirrer to prepare a resin composition (mixing conditions: 180°C, 60 minutes, 150 rpm).
[0205] <Melting and mixing> The melt mixability of the resin compositions obtained above was evaluated according to the following criteria. -Evaluation criteria- A: The entire composition was melt-mixed, and a homogeneous resin composition was obtained. B: Some of the components of the composition separated, and only a non-uniform resin composition was obtained.
[0206] <Adhesiveness> The resin compositions of Examples 1 to 3 and Comparative Examples 1 to 4, which were obtained as homogeneous resin compositions, were applied between two adherend PP (polypropylene) films and pressed using a heat sealer to prepare laminated samples having a structure of adherend PP film / adhesive layer / adherend PP film. The heat sealing conditions were 180°C and 1 MPa. The obtained laminated samples were subjected to a T-peel test (crosshead speed: 300 mm / min, width of laminated sample: 25 mm) at each temperature condition of 0°C, 25°C, and 50°C, and the average peel strength at this time was measured. The average peel strength was evaluated according to the following evaluation criteria. When the evaluation criteria are "A" and "B", it can be said that the adhesiveness is excellent. When the evaluation results of the average peel strength at each temperature condition of 0°C, 25°C, and 50°C are all "A" and "B", it can be said that the adhesiveness is excellent under a wide range of temperature conditions from low temperature to high temperature. -Evaluation criteria- A: The average peel strength is 5N / cm or more. B: The average peel strength is 2 N / cm or more and less than 5 N / cm. C: The average peel strength is less than 2 N / cm.
[0207] [Table 1]
[0208] It is clear that the adhesives containing the resin compositions of Examples 1 to 3 have superior adhesive properties over a wide range of temperature conditions from low to high temperatures, as compared to the adhesives containing the resin compositions of Comparative Examples 1 to 4.
Claims
1. a block copolymer (A) which is a hydrogenated product of a block copolymer containing a polymer block (X) mainly made of a vinyl aromatic compound and a polymer block (Y) mainly made of a conjugated diene compound; A modified ethylene / α-olefin copolymer (B) that satisfies the following requirements (b-1) to (b-4); A resin composition comprising: Requirement (b-1): The content of structural units derived from ethylene is in the range of 15 to 85 mol % (the total of the content of structural units derived from ethylene and the content of structural units derived from α-olefins is 100 mol %); Requirement (b-2): the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 1,000 to 100,000; Requirement (b-3): A modified copolymer having a substituent derived from a vinyl aromatic compound, and the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 1 to 70 mass%; Requirement (b-4): The Brookfield viscosity at 100° C. is in the range of 1 to 10,000 mPa·s.
2. In the above requirement (b-1), the content of structural units derived from ethylene is in the range of 40 to 60 mol % (wherein the total content of structural units derived from ethylene and the content of structural units derived from α-olefins is 100 mol %), In the requirement (b-2), the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 2,000 to 30,000, and in the requirement (b-3), the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 5 to 30 mass%. The resin composition according to claim 1.
3. The resin composition according to claim 1, wherein the block copolymer (A) satisfies the following requirement (a-1): Requirement (a-1): MFR (230° C., 5 kg) is in the range of 0.1 to 1,000 g / 10 min.
4. The content of the block copolymer (A) is 100 parts by mass, the content of the copolymer (B) is in the range of 10 to 150 parts by mass, and the content of the adhesive resin (C) is in the range of 10 to 300 parts by mass. The resin composition according to claim 1.
5. A pressure-sensitive adhesive comprising the resin composition according to any one of claims 1 to 4.
6. A hot melt adhesive comprising the resin composition according to any one of claims 1 to 4.
7. A heat seal material comprising the resin composition according to any one of claims 1 to 4.
8. A primer comprising the resin composition according to any one of claims 1 to 4.
9. a block copolymer (A) which is a hydrogenated product of a block copolymer containing a polymer block (X) mainly made of a vinyl aromatic compound and a polymer block (Y) mainly made of a conjugated diene compound; A modified ethylene / α-olefin copolymer (B) that satisfies the following requirements (b-1) to (b-4); a pressure-sensitive adhesive resin (C); Requirement (b-1): The content of structural units derived from ethylene is in the range of 15 to 85 mol % (the total of the content of structural units derived from ethylene and the content of structural units derived from α-olefins is 100 mol %); Requirement (b-2): the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 1,000 to 100,000; Requirement (b-3): A modified copolymer having a substituent derived from a vinyl aromatic compound, and the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 1 to 70 mass%; Requirement (b-4): The Brookfield viscosity at 100° C. is in the range of 1 to 10,000 mPa·s.
10. The method for producing a resin composition according to claim 9, wherein the modified ethylene / α-olefin copolymer (B) is a modified product of an unmodified ethylene / α-olefin copolymer (B') produced by the following method (α): Method (α): A bridged metallocene compound (P-1) represented by the following formula (1), and A method comprising a step of solution polymerizing ethylene and an α-olefin in the presence of a catalyst system containing at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P-1) to form an ion pair. [Formula 1] [In formula [1], R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure; R 6 and R 11 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 7 and R 10 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 6 and R 7 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 6 , R 7 , R 10 and R 11 is not a hydrogen atom at the same time, Y is a carbon atom or a silicon atom; R 13 and R 14 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be bonded to each other to form a ring structure, M is Ti, Zr or Hf; Q is independently a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating to a lone pair of electrons; j is an integer from 1 to 4.
11. In the formula 1, R 13 and R 14 The method for producing a resin composition according to claim 10 , wherein at least one of the above is an aryl group.
12. In the formula 1, R 13 and R 14 are both aryl groups, and R 2 and R 3 The method for producing a resin composition according to claim 10, wherein either one of the above is a saturated hydrocarbon group having 4 carbon atoms.
13. The method for producing a resin composition according to claim 9, wherein the block copolymer (A) satisfies the following requirement (a-1), and the requirement (b-1) is that the content of structural units derived from ethylene is in the range of 40 to 60 mol%, the requirement (b-2) is that the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 2,000 to 30,000, and the requirement (b-3) is that the content of the portion derived from the vinyl aromatic compound in the modified copolymer is in the range of 5 to 30 mass%: Requirement (a-1): MFR (230° C., 5 kg) is in the range of 0.1 to 1,000 g / 10 min.
14. The method for producing a resin composition according to claim 9, wherein the content of the block copolymer (A) is 100 parts by mass, the content of the copolymer (B) is in the range of 10 to 150 parts by mass, and the content of the adhesive resin (C) is in the range of 30 to 300 parts by mass.
Citation Information
Patent Citations
Hot melt hardenable pressure-sensitive adhesive
JP2006241444A
Thermoplastic resin composition and use thereof
JP2020196839A