Admixture and cement composition

A cement admixture with controlled particle size distributions and mass loss rates addresses the mixing time and strength issues in high-strength concrete, improving workability and durability.

JP2024137206AActive Publication Date: 2024-10-07DENKA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023048637
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

Existing cement admixtures containing pozzolanic substances like silica fume and fly ash prolong mixing times, affecting the workability and strength development of high-strength concrete, leading to issues such as pipe clogging during pump transfer.

Method used

A cement admixture with specific particle size distributions and mass loss rates, comprising silica fume and other pozzolanic materials, is developed to enhance dispersion and reduce mixing time, ensuring strength development.

Benefits of technology

The admixture shortens mixing time and improves strength by optimizing particle size differences and mass loss rates, enhancing the workability and durability of high-strength concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137206000002
    Figure 2024137206000002
  • Figure 2024137206000001
    Figure 2024137206000001
Patent Text Reader

Abstract

To provide an admixture that can shorten a kneading time and obtain a strength enhancing effect when used for concrete.SOLUTION: An admixture includes a pozzolan material, where, in a volume frequency particle size distribution measured by the laser diffraction scattering method, a difference (Bmax-Amax) between a particle diameter Amax indicating a maximum value of volume frequency at 3-20 μm and a particle diameter Bmax being larger than the particle diameter Amax and indicating a maximum value of volume frequency in the particle diameter range RB of 8-150 μm is 130 μm or smaller, and a mass diminution rate after standing for three hours in a thermostat at 105°C is 1 mass% or smaller.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to admixtures and cement compositions. [Background technology]

[0002] In recent years, not only in Japan but also in Asian countries such as Vietnam and China, the development of social infrastructure has progressed rapidly along with economic development. This has led to a need for the development and stable supply of civil engineering and construction materials that meet local needs.

[0003] In this situation, there is a demand for improved performance in cement concrete, and in particular, there is an increasing need for high-strength concrete in connection with the need to improve the durability and extend the life of high-rise buildings and concrete structures.

[0004] Pozzolanic substances such as silica fume and fly ash are often used as admixtures for high-strength concrete. Admixtures containing pozzolanic substances are effective in increasing the strength and durability of concrete, but the mixing time required to obtain the required fluidity may be longer than that required for normal cement compositions, resulting in a longer construction time for high-strength concrete. Furthermore, if the concrete is not mixed sufficiently, the workability of the concrete may be adversely affected, for example, blockage of piping may easily occur when pumping the concrete into forms or the like.

[0005] Patent Document 1 discloses that the time required for mixing mortar can be shortened by using a cement admixture made by blending blast furnace slag powder of a specific particle size with anhydrous gypsum or with anhydrous gypsum and silica fume. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 6211758 Summary of the Invention [Problem to be solved by the invention]

[0007] However, since Patent Document 1 does not provide a specific evaluation of strength, it is unclear whether the cement admixture is suitable for high-strength concrete.

[0008] In view of the above, an object of the present invention is to provide an admixture that can shorten the mixing time and has a strength-enhancing effect when used in concrete. [Means for solving the problem]

[0009] As a result of intensive research aimed at solving the above problems, the present inventors have come up with the following invention and found that the above problems can be solved.

[0010] [1] Particle size A that contains pozzolanic substances and shows the maximum volume frequency in the range of 3 to 20 μm in the volume frequency particle size distribution measured by the laser diffraction scattering method. max and particle size A max The particle size B, which shows the maximum volume frequency in the particle size range of 8 to 150 μm, is max Difference with (B max -A max ) is 130 μm or less, and the mass loss rate after being left in an incubator at 105°C for 3 hours is 1% or less by mass. [2] Particle size B max and particle size A max The difference between max -A max The admixture according to [1], wherein the particle size is 30 to 100 μm. [3] The pozzolanic material comprises a first pozzolanic material which is silica fume, and a particle size B max The admixture according to [1] or [2], wherein the average particle size of the silica fume is attributed to the admixture. [4] The pozzolanic material further comprises one or more second pozzolanic materials selected from blast furnace slag, fly ash, and metakaolin, and the second pozzolanic material has a particle size A max [3] The admixture according to [3], wherein the average particle size of the second pozzolanic material is attributable to the average particle size of the second pozzolanic material. [5] The admixture according to any one of [1] to [4], further comprising gypsum. [6] A cement composition comprising the admixture according to any one of [1] to [5] and cement. Effect of the Invention

[0011] According to the present invention, it is possible to provide an admixture which can shorten the mixing time and has a strength enhancing effect when used in concrete. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a diagram showing an example of a volume frequency particle size distribution measured by a laser diffraction scattering method in the admixture according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, one embodiment of the present invention (hereinafter, may be referred to as "this embodiment") will be described. In this specification, "parts" and "%" are based on mass unless otherwise specified.

[0014] The admixture according to this embodiment contains a pozzolanic substance, which can increase the strength of the concrete. In addition, the admixture has a particle size A that shows the maximum volume frequency in the range of 3 to 20 μm in the volume frequency particle size distribution measured by the laser diffraction scattering method. max and particle size A max The particle size B, which shows the maximum volume frequency in the particle size range of 8 to 150 μm, is max Difference with (B max -A max (hereinafter referred to as the "maximum difference") is 130 μm or less.

[0015] To explain the above in more detail, in this embodiment, as shown in FIG. 1, for example, a particle size A showing a maximum value (for example, a peak) of the volume frequency in a volume frequency particle size distribution measured by a laser diffraction scattering method is maxParticle size B is in the range of 3 to 20 μm and shows the maximum volume frequency (e.g., peak). max is particle size A max These are in the particle size range of 8 to 150 μm. max -A max ) is 130 μm or less.

[0016] The inventors have discovered that by having the above-mentioned maximum value difference, the admixture is in a state in which it is easily dispersed into each particle when subjected to stirring force by mixing, and this makes it possible to shorten the mixing time.

[0017] The maximum difference is preferably 130 μm or less, and more preferably 110 or less. max and particle size B max If the particle size A is the same, the distribution will be unimodal. max Particle size B max It is preferable that the difference between the maximum values ​​is larger and has a clear bimodal distribution. That is, the difference between the maximum values ​​is preferably 10 μm or more, and more preferably 40 μm or more.

[0018] In particular, from the viewpoint of improving the packing property (closest packing property) of the admixture, the maximum value difference is preferably 30 to 100 μm, and more preferably 40 to 90 μm.

[0019] In order to set the maximum difference within the desired range, for example, the time for mixing and grinding the pozzolanic substance may be adjusted. If the mixing and grinding time is long, B max becomes smaller and the maximum difference becomes smaller. Particle size A max , particle size B max The volume frequency can be measured by the method described in the Examples.

[0020] In addition, the admixture according to this embodiment has a mass loss rate of 1% by mass or less after being left in an incubator at 105° C. for 3 hours. This mass loss rate is related to the dispersion of particles, and by having the mass loss rate be 1% by mass or less, it is possible to shorten the mixing time and impart a strength enhancing effect. The mass loss rate is preferably 0.95% or less, and more preferably 0.8% or less, with the lower limit being practically about 0.2% by mass.

[0021] In order to keep the mass loss rate after leaving it in a 105°C incubator for 3 hours within the desired range, for example, granulated silica fume with a low moisture content described below may be used, or some or all of the various materials may be appropriately heated. The mass loss rate can be measured by the method described in the Examples.

[0022] The pozzolanic material preferably includes a first pozzolanic material which is silica fume, and has a particle size B max is preferably due to the average particle size of the silica fume. Particle size B max The particle size is preferably in the range of 30 to 130 μm, and more preferably in the range of 60 to 110 μm. In this specification, the average particle size refers to the volume-based average particle size (D50) measured by a laser diffraction scattering method.

[0023] The silica fume (hereinafter referred to as SF) is not particularly limited, but is a by-product that occurs when, for example, silicon alloys such as metallic silicon and ferrosilicon are produced in an electric furnace, where SiO2 is vaporized by the heat of an arc and solidifies in the process of cooling in the flue. It is spherical, fine particles with a diameter of 1 μm or less, and its main component is amorphous, highly reactive SiO2.

[0024] Silica fume is classified into two types: powdered silica fume that is not granulated, and granulated silica fume that is obtained by granulating powdered silica fume. Powdered silica fume refers to silica fume described in JIS A 6207, and has a bulk density of 0.4 to 0.8 g / cm. 3 That's about it. Granulated silica fume is silica fume that is made by granulating powdered silica fume, and has a volume-based average particle size of 150 to 350 μm and a density of 2.20 to 2.30 g / cm, as measured by a laser diffraction / scattering particle size distribution analyzer. 3 , BET specific surface area is 15-25m 2 / g.

[0025] Powdered silica fume has excellent dispersibility but is prone to agglomeration during use. On the other hand, granulated silica fume does not agglomerate during use, but may have poor dispersibility. These are trade-offs, but in this embodiment, it is preferable to use at least granulated silica fume. When granulated silica fume is mixed with other materials and mixed and crushed, the agglomeration of the granulated silica fume is broken down and the maximum value difference (B max -A max ) is 130 μm, making it easier to shorten the mixing time.

[0026] The content of silica fume in the admixture is preferably 30 to 80 mass %, and more preferably 35 to 70 mass %.

[0027] It is also preferred that the pozzolanic substance further contains one or more second pozzolanic substances selected from blast furnace slag, fly ash, and metakaolin, and the particle size A max is preferably due to the average particle size of the second pozzolanic material. Particle size A max The particle size is preferably in the range of 5 to 18 μm, and more preferably in the range of 8 to 15 μm.

[0028] Blast furnace slag is molten slag discharged from a blast furnace during the steel manufacturing process, which is rapidly cooled with water or other liquids to turn it into a glassy substance, and is then crushed into powder. Granulated blast furnace slag has latent hydraulic properties and hardens when stimulated by alkali. Other materials such as molten slag made from city waste or sewage sludge, dephosphorized slag, and slowly cooled slag can also be used. The Blaine specific surface area of ​​blast furnace slag (JIS R 5201:2015) is 2500 cm 2 / g or more is preferable, and 3000 to 4500 cm 2 / g is more preferred.

[0029] Fly ash is coal ash generated during coal combustion in coal-fired power plants, and is collected by a dust collector. In the present invention, fly ash classified into types I to IV as specified in JIS A 6201 is preferred, and type II is particularly preferred. The Blaine specific surface area of ​​fly ash is 2500 cm 2 / g or more is preferable, and 3000 to 4500 cm 2 / g is more preferred.

[0030] Metakaolin is a mineral that has been heat-treated at around 600°C to remove the water contained within the crystal lattice in the form of OH. It is an amorphous aluminosilicate when viewed by X-rays and has pozzolanic activity. The Blaine specific surface area of ​​metakaolin is 6000 to 18,000 cm 2 / g, and 10,000 to 15,000 cm 2 It is more preferable that the molecular weight is / g.

[0031] The content of the one or more second pozzolanic substances selected from blast furnace slag, fly ash, and metakaolin in the admixture is preferably 10 to 70 mass %, more preferably 15 to 60 mass %.

[0032] The mass ratio of the second pozzolanic substance to the first pozzolanic substance (second pozzolanic substance / first pozzolanic substance) is preferably 0.7-5, and more preferably 1-4, from the viewpoints of strength development and fluidity.

[0033] The admixture according to this embodiment preferably further contains gypsum. Gypsum is a general term for anhydrous gypsum, semi-gypsum, and dihydrate gypsum, and any of them can be used. These can also be used alone or in combination of two or more. Among them, it is preferable to select anhydrous gypsum from the viewpoint of strength development.

[0034] The particle size of the gypsum is not particularly limited, but is usually 3,000 to 8,000 cm in terms of Blaine specific surface area. 2 / g is preferred, and 4,000 to 7,000 cm 2 / g is more preferable. 2 / g or more, sufficient strength is obtained and abnormal expansion does not occur over the long term. 2 Even if it exceeds / g, no further improvement in effect can be expected. The content of gypsum in the admixture is preferably 0 to 40 mass %, and more preferably 5 to 35 mass %.

[0035] The admixture according to this embodiment is obtained by mixing and grinding the raw materials of the pozzolanic substance described above. For example, when granulated silica fume and the second pozzolanic substance are used as the raw materials, it is preferable to mix and grind them using a ball mill. Since granulated silica fume usually has a larger particle size than the second pozzolanic substance, the granulated silica fume is pulverized further by extending the grinding time using the ball mill. Therefore, the maximum difference (B max -A max ) is 130 μm or less and can be adjusted to the desired range. In addition, the mass reduction rate can be set within a desired range by heat treating at least a portion of the mixture before or after the mixing and grinding.

[0036] [Cement composition] The cement composition according to this embodiment contains the admixture of the present invention and cement. Examples of cement include various types of Portland cement, such as ordinary, early strength, extra early strength, low heat, and moderate heat, various types of blended cement, and filler cement mixed with limestone powder.

[0037] The particle size of the cement composition of the present embodiment is not particularly limited since it depends on the purpose and application of the composition. Generally, the particle size is 2,500 to 8,000 cm in terms of Blaine specific surface area. 2 / g is preferable, and 3,000 to 6,000 cm 2 / g is more preferable. 2 / g or more, sufficient strength expression is obtained, and 2 / g or less can improve workability.

[0038] The cement composition may further contain an aggregate, which is not particularly limited and may be any of fine aggregates and coarse aggregates used in the manufacture of ordinary mortar or concrete. In addition, various admixtures may be contained. When the cement composition of the present embodiment contains fine aggregate, it becomes mortar, and when it contains fine aggregate and coarse aggregate, it becomes concrete.

[0039] The cement composition of the present embodiment may be prepared by mixing the respective materials at the time of application, or may be prepared by mixing a part or all of the materials in advance. The method of mixing the respective materials and water is not particularly limited, and the respective materials may be mixed at the time of application, or may be mixed a part or all of the materials in advance. In addition, the remaining materials may be mixed after a part of the materials is mixed with water.

[0040] As the mixing device, any existing device can be used, for example, a tilting mixer, an omni mixer, a Henschel mixer, a V-type mixer, a Nauta mixer, or the like. EXAMPLES

[0041] Granulated silica fume particles and at least one of ground granulated blast furnace slag, powdered fly ash, powdered metakaolin, and gypsum were loaded into a vibration pot mill (manufactured by Chuo Kakoki Co., Ltd.), ground and mixed under the conditions described below, and appropriately heated at 105°C to produce an admixture having the composition shown in the table below. In addition, the above heat treatment was not carried out for Experiment No. 6.

[0042] <Conditions for grinding and mixing process> An appropriate amount of DEG (diethylene glycol) was dropped onto the raw material filled in the vibration pot mill as a grinding aid, and the particle size A in Table 1 was obtained. max and particle size B max The mixing and grinding time was adjusted so that

[0043] <Materials used in admixtures> · Finely ground blast furnace slag: Ground and classified blast furnace slag, average particle size 10μm Silica fume granulated particles: Commercially available product, average particle size 209 μm, BET specific surface area 18.5 m 2 / g Fly ash powder: JIS fly ash type II, density 2.35g / cm 3 , 4600cm 2 / g Metakaolin powder: Commercially available product, density 2.6g / cm 3 , Blaine specific surface area 12,000cm 2 / g Gypsum: Natural anhydrous gypsum crushed product, Blaine specific surface area 5,000 cm 2 / g

[0044] <Physical properties of admixtures> Volume frequency particle size distribution measurement For each of the prepared admixtures, a laser diffraction / scattering device (product name: Laser diffraction / scattering particle size distribution measuring device LA-960, manufactured by HORIBA) was used to measure the particle size A, which shows the maximum volume frequency in the range of 3 to 20 μm. max Particle size B, which shows the maximum volume frequency in the particle size range of 8 to 150 μm max The maximum difference (B max -A max The results are shown in the table below.

[0045] - Mass loss rate measurement The mass loss rate of each of the prepared admixtures was determined after leaving them in a constant temperature dryer (product name: DVS401, manufactured by YAMATO) at 105°C for 3 hours. The results are shown in the table below.

[0046] The mortars using the admixtures of the above-mentioned examples were evaluated as follows. The results are shown in the table below. The materials used and the mix ratio of the mortars are as follows.

[0047] <Materials and mixes used in mortar> (Materials used) Mixing water: Tap water Cement: Ordinary Portland cement, commercially available, density 3.15g / cm 3 Fine aggregate: Commercially available, density 2.64g / cm 3 , coarse grain ratio 2.27 Admixtures: Commercially available products, polycarboxylic acid-based high-performance water reducers, polyoxyalkylene-based defoamers

[0048] (Composition) ·Water:205kg / m 3 Cement: 927kg / m 3 Admixture in each example: 360kg / m 3 ·Fine aggregate: 905kg / m 3 High-performance water reducing agent 32.2kg / m 3 Defoamer: 6.4kg / m 3

[0049] <Mixing time> The mortar was mixed using a forced twin-axis mixer. The mixing time was recorded by recording the mixer load value every minute, and mixing was completed when it remained constant for 3 consecutive minutes. The kneading time is preferably 25 minutes or less, and more preferably 10 to 20 minutes.

[0050] <Compressive strength> The measurements were made in accordance with JSGE-G 505 "Method of testing compressive strength of mortar or cement paste using cylindrical specimens," specifically, using the following "Sample preparation method and curing method." The material age was set to 3 days after the steam curing.

[0051] (Sample preparation method and curing method) Mortar was prepared using a forced biaxial concrete mixer with a nominal capacity of 55 L, and then left in an environment of 20°C and 80% RH until the material was aged for one day. After demolding at one day, the material was heated to 85°C at a rate of 20°C / h or less, held for 24 hours, and then cooled to 20°C at a rate of 20°C / h or less.

[0052] [Table 1] [Industrial Applicability]

[0053] The admixture of the present invention can be suitably used in the fields of civil engineering and construction, particularly for lightweight, thin-walled concrete members that require ultra-high strength and self-leveling.

Claims

1. Contains pozzolanic substances, Particle size A showing the maximum volume frequency in the range of 3 to 20 μm in the volume frequency particle size distribution measured by the laser diffraction scattering method max and particle size A max The particle size B, which shows the maximum volume frequency in the particle size range of 8 to 150 μm, is max Difference with (B max -A max ) is 130 μm or less, An admixture whose mass loss rate after being left in an incubator at 105°C for 3 hours is 1% by mass or less.

2. Particle size B max and particle size A max The difference between max -A max 2. The admixture according to claim 1, wherein the particle size is 30 to 100 μm.

3. The pozzolanic material comprises a first pozzolanic material which is silica fume, and a particle size B max The admixture according to claim 1, characterized in that the average particle size of the silica fume is attributable to

4. The pozzolanic material further comprises one or more second pozzolanic materials selected from blast furnace slag, fly ash, and metakaolin, and the particle size A max 4. The admixture of claim 3, wherein:

5. The admixture according to claim 3 or 4, further comprising gypsum.

6. A cement composition comprising the admixture according to any one of claims 1 to 5 and cement.

Citation Information

Patent Citations

  • Hydraulic material

    JP1993254899A

  • Method for manufacturing cement-based building material containing amorphous silica

    JP2008246856A

  • Preparation of hydraulic compound using silicon sludge from silicon wafer manufacturing process

    KR101276297B1

  • Pozzolan admixture

    WO2014073634A1

  • Fluororesin composition

    JP1987011758A