Cover tape for packing electronic component and electronic component packing body
The cover tape with controlled surface properties and composition addresses blocking and sticking issues by reducing contact area and enhancing surface irregularity, facilitating easy peeling and retrieval of electronic components.
Patent Information
- Application Number
- JP2023048726
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Conventional cover tapes for packaging electronic components suffer from issues of blocking and sticking during transportation due to vibrations, making it difficult to peel off the cover tape and retrieve the components.
A cover tape design with specific surface properties, including a peak density (Spd) of 3×10^5 to 1×10^6 /mm^2 and a root mean square slope (Sdq) of 1.0×10^-2 to 5.0×10^-1, optimized through the use of a base layer, intermediate layer, and sealant layer composed of certain resins and inorganic particles, to reduce contact area and enhance surface irregularity.
The optimized cover tape effectively suppresses blocking and sticking of components, ensuring easy peeling and retrieval even under severe conditions.
Smart Images

Figure 2024137268000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a cover tape for packaging electronic components and an electronic component package. [Background technology]
[0002] Electronic components such as transistors, diodes, capacitors, and piezoelectric resistors are sometimes transported in the form of "electronic component packages" obtained by housing electronic components in recesses of a carrier tape that are formed with recesses capable of housing the electronic components to prevent damage, and then heat-sealing a cover tape to the carrier tape so as to seal the electronic components in the recesses. Electronic component packages are often imported and exported across countries by air or sea. When the packaged electronic component is to be used, the cover tape in the electronic component package is peeled off and the electronic component is taken out of the recess.
[0003] The following patent documents can be cited as prior art relating to cover tapes (cover tapes for packaging electronic components) intended for use in the manner described above. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-171393 A [Patent Document 2] International Publication No. 2012 / 079258 [Patent Document 3] JP 2003-246358 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors, through their investigation into improvements to conventional cover tapes, have found that there is still room for improvement in conventional cover tapes in the following points (i) and (ii). (i) Blocking: The cover tape is usually in a long shape and is wound up before use. At this time, the cover tapes may stick together and become difficult to peel off. (ii) Sticking of components: In electronic component packages obtained by heat sealing a cover tape to a carrier tape, electronic components housed in recesses of the carrier tape may stick to the cover tape due to vibration during transportation, etc. If such sticking occurs, it becomes difficult to properly remove the electronic components when peeling the cover tape from the carrier tape.
[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a cover tape for packaging electronic components, which is suppressed in blocking and in which sticking of components is suppressed. [Means for solving the problem]
[0007] In order to solve the above problems, the present inventors have studied improvements to the cover tape from various perspectives. Through the study, they have found that the state of the surface (exposed surface) of the sealant layer in the cover tape seems to be related to blocking and adhesion of electronic components. Based on this knowledge, the present inventors have completed the invention provided below. And, the above problems have been solved.
[0008] 1. A cover tape for packaging electronic components comprising a base layer and a sealant layer provided on one side of the base layer, a surface of the sealant layer opposite to the base layer is an exposed surface; The peak density Spd of the exposed surface as defined by ISO 25178 is 3×10 5 ~1×10 6 / mm 2 and The root mean square slope Sdq of the exposed surface as defined in ISO 25178 is 1.0×10 ―2 ~5.0×10 ―1 That is the cover tape. 2. 1. The cover tape according to claim 1, The cover tape, wherein the exposed surface has an arithmetic mean height Sa, as defined by ISO 25178, of 0.05 to 0.5 μm. 3. 1. or 2. A cover tape according to claim 1, The cover tape, wherein the sealant layer comprises inorganic particles. 4. A cover tape according to any one of 1. to 3., The cover tape, wherein the sealant layer contains one or both of a styrene-based resin and a (meth)acrylic resin. 5. A cover tape according to any one of 1. to 4., The cover tape, wherein the base layer comprises polyester. 6. A cover tape according to any one of 1. to 5., The cover tape further comprises an intermediate layer between the base layer and the sealant layer. 7. 6. The cover tape according to claim 6, The cover tape, wherein the intermediate layer comprises a polyethylene-based resin. 8. A carrier tape having electronic components housed in recesses and a cover tape according to any one of 1 to 7, An electronic component package in which the sealant layer is adhered to the carrier tape so as to seal the electronic component. Effect of the Invention
[0009] According to the present invention, there is provided a cover tape for packaging electronic components in which blocking is suppressed and sticking of components is suppressed. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram illustrating an example of a layer structure of a cover tape. [Diagram 2]FIG. 2 is a diagram showing an example of a state in which a cover tape is bonded (heat sealed) to a carrier tape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In all drawings, similar components are given similar symbols and descriptions thereof are omitted where appropriate. In order to avoid complexity, (i) when there are multiple identical components in the same drawing, only one of them will be given a symbol, and not all of them, or (ii) especially in Figure 2 and subsequent figures, components similar to those in Figure 1 will not be given a symbol again. All drawings are for illustrative purposes only. The shapes and dimensional ratios of each component in the drawings do not necessarily correspond to the actual objects.
[0012] In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass".
[0013] In this specification, the term "(meth)acrylic" refers to a concept that includes both acrylic and methacrylic. The same applies to similar terms such as "(meth)acrylate."
[0014] <Cover tape for packaging electronic components> FIG. 1 is a schematic diagram showing an example of the layer structure of a cover tape (cover tape 10) for packaging electronic components according to this embodiment. The cover tape 10 comprises a base layer 1 and a sealant layer 3 provided on at least one side of the base layer 1. The surface of the sealant layer 3 opposite to the base layer 1 is an exposed surface (in contact with air). The cover tape 10 preferably includes an intermediate layer 2 between the base layer 1 and the sealant layer 3 .
[0015] The peak density Spd, as defined by ISO 25178, of the exposed surface of sealant layer 3 is 3×10 5 ~1×10 6 / mm 2 , preferably 3.5 x 10 5 ~9×10 5 / mm 2 , and more preferably 3.5×10 5 ~8×10 5 / mm 2 ,be. The root mean square slope Sdq of the exposed surface of the sealant layer 3, as defined by ISO 25178, is 1.0×10 ―2 ~5.0×10 ―1 , preferably 5.0 x 10 ―2 ~5.0×10 ―1 , and more preferably 1.0×10 ―1 ~3.5×10 ―1 It is.
[0016] The reason why blocking and component sticking are suppressed by setting Spd and Sdq within appropriate numerical ranges can be explained as follows. Just to be clear, the following explanation includes speculation, and the present invention is not limited by the following explanation.
[0017] The peak density (Spd) is the density of the peaks per square millimeter on the surface of the object being measured. 2 This represents the number of peaks larger than a given size per pixel. If not specified, the given size is set to 5% of the height of the maximum amplitude of the contour surface. Spd is 3x10 5 / mm 2 The above means that there is a certain density of "protrusions" on the exposed surface of the sealant layer 3. This is thought to reduce the contact area between the electronic component and the sealant layer 3, suppressing adhesion. In addition, when the cover tape 10 is wound, the contact area between the base layer 1 and the sealant layer 3 also becomes small, suppressing blocking. On the other hand, if Spd is too large, problems other than the contact area may occur. For example, the cover tape or electronic component package may be image-inspected with a camera. In this case, if Spd is too large, there is a risk of impeding the image inspection. Therefore, in this embodiment, the upper limit of Spd is set to 1×10 6 / mm 2 It is set as follows.
[0018] The root mean square slope Sdq is an index calculated by taking the root mean square of the slope at all points of a defined area, and represents the average value of the local gradient of a surface. A perfectly flat surface has an Sdq of 0. Although the details are unknown, Sdq is 1.0×10 ―2 ~5.0×10 ―1 It is considered that the surface of the sealant layer 3 having a moderate unevenness or undulations reduces the contact area between the electronic component and the sealant layer 3, thereby suppressing the sticking of the electronic component. ―2 The above fact is believed to mean that there is a moderate gradient on the surface of the sealant layer 3, resulting in fewer flat surfaces. This is believed to reduce the contact area between the base layer 1 and the sealant layer 3 when the cover tape 10 is wound, thereby suppressing blocking. On the other hand, if Sdq is too large, the unevenness or undulations of the sealant layer 3 may mesh with the unevenness or undulations that may exist on the surface of the sealant layer 1, which may cause blocking. Therefore, in this embodiment, the upper limit of Sdq is set to 5.0×10 ―1 is set to.
[0019] Both Spd and Sdq are indices relating to the surface properties of the sealant layer 3. In the cover tape 10, these two indices are both optimized, thereby suppressing blocking and component sticking. As far as the inventors have studied, even if one of Spd and Sdq is optimized, if the other is not optimized, blocking may be more likely to occur and / or component sticking may not be sufficiently suppressed.
[0020] The cover tape 10 can be obtained by using an appropriate material and by an appropriate manufacturing method and manufacturing conditions. For example, by paying sufficient attention to the viscosity of the coating liquid for forming the sealant layer and the conditions for forming the sealant layer, the cover tape 10 having Spd and Sdq within an appropriate numerical range can be manufactured. Specifically, the cover tape 10 having Spd and Sdq within an appropriate numerical range can be manufactured by coating the surface of the intermediate layer 2 with a solvent-containing coating liquid adjusted to an appropriate viscosity, and by paying attention to drying the solvent by using an appropriate device, at an appropriate temperature, and for an appropriate time when drying the solvent to form the sealant layer. The method for producing the cover tape will be described in detail later.
[0021] The cover tape 10 will be described in more detail below.
[0022] [Base material layer] There are no particular limitations on the material that constitutes the base material layer 1. Any film can be used as long as it has the mechanical strength to withstand the external force applied to the cover tape 10 and the heat resistance to withstand the heat during heat sealing.
[0023] Specific examples of materials constituting the base layer 1 include polyester resins, polyamide resins, polyolefin resins, polyacrylate resins, polymethacrylate resins, polyimide resins, polycarbonate resins, ABS resins, etc. Among these, polyester resins and polyolefin resins are preferred as materials constituting the base layer 1, and polyester resins that can improve mechanical strength, particularly polyethylene terephthalate, are preferred.
[0024] The film used to form the base layer 1 may be a stretched film, or a film stretched in a uniaxial or biaxial direction. From the viewpoint of improving the mechanical strength of the cover tape 10, a film stretched in a uniaxial or biaxial direction is preferable.
[0025] The substrate layer 1 may be a single layer or a multilayer. The base layer 1 may contain an antistatic agent from the viewpoint of reducing the amount of static electricity generated when the carrier tape is peeled off. In addition, an antistatic layer may be provided as one layer of the base layer on the surface of the base layer 1 opposite to the surface on which the intermediate layer 2 is provided.
[0026] The thickness of the base layer 1 is, for example, 6 to 35 μm, preferably 7 to 33 μm, and more preferably 8 to 30 μm. Since the base layer 1 is not too thick, the rigidity of the cover tape is not too high. Even if a torsional stress is applied to the carrier tape after sealing, the cover tape 10 follows the deformation of the carrier tape, reducing the possibility of peeling off. Since the thickness of the base material layer 1 is not too thin, it is easy to make the mechanical strength of the cover tape 10 suitable. Furthermore, even when the cover tape 10 is peeled off from the carrier tape at high speed, the possibility that the cover tape 10 will break can be reduced.
[0027] [Middle layer] The intermediate layer 2 is provided mainly for the purpose of improving the cushioning properties of the cover tape 10. By improving the cushioning properties of the cover tape 10, the pressure of the sealing iron during heat sealing can be more easily and firmly transmitted to the cover tape 10. This can further improve the adhesion between the cover tape 10 and the carrier tape.
[0028] The material of the intermediate layer 2 is not particularly limited. Any material capable of imparting cushioning properties to the cover tape 10 can be used without particular limitation. For example, one or more selected from polyacrylic acid derivatives, polyacrylic acid ester derivatives, polyvinyl acetate derivatives, styrene-based resins, olefin-based resins, cyclic olefin resins, and copolymers thereof can be used. Among these, polyolefin-based resins are preferred, and polyethylene-based resins are more preferred. From the viewpoint of cushioning properties, low-density polyethylene (density 880 kg / m3 More than 930kg / m 3 Polyethylene of less than 100 mm is preferred.
[0029] The intermediate layer 2 may be a single layer or a multilayer. The thickness of the intermediate layer 2 is typically 10 to 50 μm, and preferably 15 to 45 μm, from the viewpoint of further improving the adhesion between the cover tape 10 and the carrier tape during heat sealing.
[0030] [Sealant layer] The sealant layer 3 is provided on at least one side of the base layer 1. When the intermediate layer 2 is present, the sealant layer 3 is provided on the side of the intermediate layer 2 opposite to the side in contact with the base layer 1. As already mentioned, the peak density Spd of the exposed surface of the sealant layer 3 as defined by ISO 25178 is 3×10 5 ~1×10 6 / mm 2 The root mean square slope Sdq of the exposed surface of the sealant layer 3, as defined by ISO 25178, is 1.0×10 ―2 ~5.0×10 ―1 It is. The sealant layer 3 comes into contact with the carrier tape when the cover tape 10 is heat-sealed to the carrier tape. The sealant layer 3 softens or melts when heated by the sealing iron, and adheres to the carrier tape.
[0031] The sealant layer 3 preferably contains a thermoplastic resin. Specifically, the sealant layer 3 contains one or more resins selected from (meth)acrylic resins, styrene resins, olefin resins, urethane resins, and ester resins. Among these, (meth)acrylic resins and styrene resins are preferred from the viewpoints of good heat sealability and good dispersion of inorganic particles.
[0032] Specific examples of (meth)acrylic resins include acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and other acrylic acid esters; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, and other methacrylic acid esters; and resins having structural units derived from monomers such as acrylonitrile, methacrylonitrile, and acrylamide. The (meth)acrylic resin may contain structural units derived from one or more monomers among these examples. Of course, the (meth)acrylic resin may or may not further contain structural units derived from monomers other than these examples.
[0033] Specific examples of styrene-based resins include polystyrene, styrene-butadiene copolymer (SB), styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-butadiene-butylene-styrene block copolymer (SBBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-methyl (meth)acrylate copolymer, hydrogenated styrene block copolymer, high impact polystyrene (HIPS), general purpose polystyrene resin (GPPS), etc. Among them, from the viewpoint of balance of various performances, styrene-ethylene-butylene-styrene block copolymer (SEBS) or styrene-butadiene-butylene-styrene block copolymer (SBBS) are preferable.
[0034] The ester resin usually comprises a structural unit derived from an alcohol component and a structural unit derived from a carboxylic acid component. Specific examples of the alcohol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2,2-dimethyl-1,3-propanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, and other chain or branched aliphatic diols, alicyclic diols such as hydrogenated bisphenol A [2,2-bis(4-hydroxycyclohexyl)propane] and hydrogenated bisphenol A with alkylene oxide (average molar addition number of 2 to 12) having 2 to 4 carbon atoms, and trihydric or higher polyhydric alcohols such as glycerin, pentaerythritol, trimethylolpropane, and sorbitol. These alcohol components may be used alone or in combination. Specific examples of the carboxylic acid component include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, adipic acid, sebacic acid, dodecanedioic acid, azelaic acid, dodecylsuccinic acid, dodecenylsuccinic acid, and octenylsuccinic acid, polyvalent carboxylic acids having three or more valences such as trimellitic acid or its anhydride, and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic aromatic dicarboxylic acid. These carboxylic acid components may be used alone or in combination.
[0035] The sealant layer 3 preferably contains inorganic particles. By using inorganic particles, the state of the exposed surface of the sealant layer 3 can be adjusted, and Spd and Sdq can be easily set to desired values, which may further suppress blocking and further suppress sticking of parts. In addition, by using inorganic particles, it may be possible to expect improvement in peelability from the carrier tape.
[0036] Metal element-containing particles can be mentioned as one type of inorganic particles. Metal element-containing particles have relatively high conductivity due to the inclusion of metal, and therefore can function as an antistatic agent. The use of metal element-containing particles reduces damage to electronic components to be packaged due to static electricity.
[0037] Specific examples of the metal element-containing particles include metal oxides such as aluminum oxide, tin oxide, zinc oxide, indium oxide, and titanium oxide, and sulfides such as zinc sulfide, copper sulfide, cadmium sulfide, nickel sulfide, and palladium sulfide. Furthermore, examples of particles having an antistatic function, but not necessarily containing a metal element, include fine carbon particles. From the viewpoints of availability and ease of adjusting the peel strength, metal oxides are preferred as the metal element-containing particles.
[0038] From the viewpoint of electrical conductivity in particular, the metal element-containing particles may be doped with a trace element to enhance electrical conductivity. Examples of the trace element include antimony and indium. Particularly preferred antistatic agents are ITO: tin-doped indium oxide, or ATO: antimony-doped tin oxide.
[0039] The inorganic particles have an average particle size of preferably 1 to 1000 nm, more preferably 3 to 500 nm. By selecting inorganic particles with an appropriate average particle size, it is easy to obtain the effect of improving other performances without excessively impairing the transparency of the sealant layer 3. The average particle size of the inorganic particles can be determined by averaging the circle-equivalent diameters of at least 100 inorganic particles in a microscope image.
[0040] When inorganic particles are used, the amount of inorganic particles varies depending on the intended use of the inorganic particles and the specific gravity of the inorganic particles, but is 40 to 80 mass %, preferably 50 to 70 mass %, of the entire sealant layer 3 (non-volatile components in the coating solution for forming the sealant layer in the cover tape manufacturing method described below). In addition, when inorganic particles are used, the amount of inorganic particles used is preferably 10 to 40 volume %, more preferably 15 to 35 volume %, of the entire sealant layer 3, on a volume basis.
[0041] In the exposed surface of the sealant layer 3, in addition to Spd and Sdq, it is preferable that the arithmetic mean height Sa defined in ISO 25178 is within an appropriate numerical range. When Sa is within an appropriate numerical range, further improvements in various performances can be expected. Specifically, Sa is usually 0.05 to 0.5 μm, preferably 0.1 to 0.4 μm, and more preferably 0.1 to 0.3 μm.
[0042] The thickness (dry film thickness) of the sealant layer 3 is preferably 0.05 to 5 μm, more preferably 0.1 to 3 μm, from the viewpoint of obtaining sufficient heat sealability without excessively impairing other performances.
[0043] [Total thickness] From the viewpoint of a balance between ensuring strength and ease of handling, the total thickness of the cover tape 10 is preferably 30 to 65 μm, and more preferably 35 to 60 μm.
[0044] <Cover tape manufacturing method> As described above, the cover tape 10 can be manufactured by using appropriate materials and through an appropriate manufacturing process. A suitable manufacturing method and the materials used in the manufacturing method will be described in more detail below.
[0045] First, the intermediate layer 2 is formed on at least one surface side of the base layer 1. The base layer 1 is preferably a film formed of an ester-based resin, an olefin-based resin, etc. The intermediate layer 2 can be formed by, for example, an extrusion lamination method or a dry lamination method. In order to prevent peeling between the base layer 1 and the intermediate layer 2, a layer of, for example, an anchor coating agent may be present between the base layer 1 and the intermediate layer 2.
[0046] Next, a coating liquid for forming a sealant layer is applied to the surface of the intermediate layer 2 opposite to the substrate layer 1, and then dried. As a coating method, for example, a gravure coating method can be adopted.
[0047] The sealant layer-forming coating liquid can typically be prepared by thoroughly mixing a resin (preferably a thermoplastic resin such as the above-mentioned (meth)acrylic resin or styrene resin), an organic solvent, and, if necessary, additives such as inorganic particles and antistatic components. From the viewpoint of coatability and obtaining a desired film thickness, the viscosity of the sealant layer-forming coating liquid at 28°C is preferably 2 to 10 mPa·s when measured using a vibration viscometer in accordance with JIS Z 8803. The viscosity can be adjusted by adjusting the amount of solvent, using an appropriate organic solvent, or the like. The organic solvent that can be used in preparing the coating liquid for forming the sealant layer is not particularly limited, but is preferably selected from esters such as ethyl acetate and butyl acetate; ketones such as methyl ethyl ketone, acetone, cyclohexanone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene and xylene; and aliphatic or alicyclic alcohols such as methanol, ethanol, n-propanol, isopropanol, and cyclohexanol.
[0048] In this embodiment, in addition to using a coating liquid with an appropriate viscosity, it is preferable to optimize the drying conditions of the coating liquid applied to the surface of the intermediate layer 2 opposite to the base layer 1, thereby manufacturing a cover tape 10 with Spd and Sdq within appropriate numerical ranges. Specifically, the coating body formed by applying the sealant layer forming coating liquid adjusted to the above-mentioned viscosity onto the intermediate layer is conveyed into a drying furnace with a length of 8 to 12 m and an internal temperature set to 70 to 100° C., while the solvent is dried. At this time, the conveying speed is set to 140 to 200 m / min. Although the details are unclear, it is speculated that since the drying of the solvent is "uneven" and "fluctuation", by appropriately controlling the viscosity of the coating liquid (particularly related to the ease of spreading) as well as the drying speed of the solvent and other drying conditions, unevenness will be generated on the surface of the sealant layer 3, and the exposed surface of the sealant layer 3 after drying will tend to have good surface properties for preventing blocking and sticking of parts. Also, when the coating liquid for forming the sealant layer contains particles (e.g. particles containing metal elements), it is speculated that the values of Spd and Sdq can be adjusted by controlling the viscosity of the coating liquid, which is closely related to the ease of settling of the particles, as well as the drying speed of the solvent, so that the particles are fixed in an appropriately sunk state (or an appropriately floating state) in the final sealant layer 3.
[0049] <Electronic component packaging> An electronic component package can be obtained from the above-described cover tape 10 and a carrier tape having electronic components housed in recesses. This will be described with reference to FIG.
[0050] In FIG. 2, cover tape 10 for packaging electronic components is used as a lid material for band-shaped carrier tape 20 having recessed pockets 21 continuously formed to match the shapes of electronic components. Specifically, the cover tape 10 for packaging electronic components is adhered (usually by heat sealing) to the surface of the carrier tape 20 so as to cover the entire opening of the pocket 21 of the carrier tape 20. Hereinafter, the structure obtained by adhering the cover tape 10 for packaging electronic components and the carrier tape 20 together will be referred to as the electronic component package 100.
[0051] The electronic component packaging body 100 can be produced, for example, by the following procedure. First, electronic components are placed in the pockets 21 of the carrier tape 20 . Next, the cover tape 10 for packaging electronic components is adhered to the surface of the carrier tape 20 by a heat sealing method so as to cover the entire opening of the pocket 21 of the carrier tape 20. At this time, the sealant layer 3 of the cover tape 10 for packaging electronic components is in contact with the carrier tape 20 (that is, the heat sealing is performed so that the "back surface" of the cover tape 10 for packaging electronic components in FIG. 2 becomes the sealant layer 3). The specific method and conditions for heat sealing are not particularly limited as long as the cover tape 10 for packaging electronic components is sufficiently strongly adhered to the carrier tape 20. Typically, a known heat sealing machine is used, and the heat sealing can be performed at a temperature of 100 to 240° C., a load of 0.1 to 10 kgf, and a time of 0.0001 to 1 second.
[0052] In this manner, a structure (electronic component packaging body 100) in which electronic components are hermetically housed is obtained. This structure (electronic component packaging 100) is, for example, wound on a reel and stored until the electronic components are to be used. Alternatively, the reel on which electronic component packaging 100 is wound may be transported to a remote location by sea or air. The reel may be made of metal, paper, plastic, or the like.
[0053] When the electronic components are to be used, the cover tape 10 for packaging electronic components is peeled off from the carrier tape 20, and the housed electronic components are taken out. There are no particular limitations on the electronic components contained in the electronic component packaging 100. Examples include general components used in the manufacture of electric and electronic devices, such as semiconductor chips, transistors, diodes, capacitors, piezoelectric elements, optical elements, LED-related members, connectors, and electrodes.
[0054] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0055] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.
[0056] <Example 1> The cover tape was manufactured according to the following procedure. (1) A biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) having a thickness of 25 μm was prepared as a substrate layer. On one side of the film, a low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was formed into a film having a thickness of 20 μm by extrusion lamination at an extrusion temperature of 300° C. to provide an intermediate layer. In this way, a laminated film was obtained. (2) As non-volatile components, antistatic agent: 60% by mass of antimony-doped tin oxide ("T-1" manufactured by Mitsubishi Materials Corporation, average particle size approximately 20 nm) and poly(meth)acrylic acid derivative: 40% by mass of "A450A" manufactured by DIC Corporation were uniformly dispersed or dissolved in toluene to prepare a coating liquid. The amount of solvent used was adjusted so that the viscosity at 28°C was 6 mPa s. (3) The coating liquid was applied to the surface of the laminated film on which the intermediate layer was formed by gravure coating to obtain a coated body. The temperature of the coating liquid immediately before coating was 28°C. The coated body was then transported into a drying oven with a length of about 10 m, the temperature of which was set at 85°C, to dry the solvent. The transport speed was set at 180 m / min (i.e., the coated body was heated in the drying oven for 10 m / (180 m / min) = 1 / 18 min = about 3.3 seconds while being transported). The amount of the coating solution applied was adjusted so that the dry thickness of the sealant layer was 0.5 μm.
[0057] <Example 2> The cover tape was manufactured according to the following procedure. (1) A biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) having a thickness of 25 μm was prepared as a substrate layer. On one side of the film, a low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was formed into a film having a thickness of 20 μm by extrusion lamination at an extrusion temperature of 300° C. to provide an intermediate layer. In this way, a laminated film was obtained. (2) As non-volatile components, antistatic agent: 60 mass% antimony-doped tin oxide ("T-1" manufactured by Mitsubishi Materials Corporation), poly(meth)acrylic acid derivative: 24 mass% "A450A" manufactured by DIC Corporation, styrene-butadiene copolymer: 16 mass% "Tuftec H1517" manufactured by Asahi Kasei Corporation (styrene content (PS ratio): 43%, MFR (230°C, 2.16 kg): 3 g / 10 min) were uniformly dispersed or dissolved in toluene to prepare a coating liquid. The amount of solvent used was adjusted so that the viscosity at 28°C was 4 mPa s. (3) The coating liquid was applied to the surface of the laminated film on which the intermediate layer was formed by gravure coating to obtain a coated body. The temperature of the coating liquid immediately before coating was 28°C. The coated body was then transported into a drying oven with a length of about 10 m, the temperature of which was set at 85°C, to dry the solvent. The transport speed was set at 180 m / min (i.e., the coated body was heated in the drying oven for 10 m / (180 m / min) = 1 / 18 min = about 3.3 seconds while being transported). The amount of the coating solution applied was adjusted so that the dry thickness of the sealant layer was 0.2 μm.
[0058] <Example 3> The cover tape was manufactured according to the following procedure. (1) A biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) having a thickness of 25 μm was prepared as a substrate layer. On one side of the film, a low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was formed into a film having a thickness of 20 μm by extrusion lamination at an extrusion temperature of 300° C. to provide an intermediate layer. In this way, a laminated film was obtained. (2) As non-volatile components, antistatic agent: 60 mass% antimony-doped tin oxide ("T-1" manufactured by Mitsubishi Materials Corporation), poly(meth)acrylic acid derivative: 24 mass% "A450A" manufactured by DIC Corporation, styrene-butadiene copolymer: 16 mass% "Tuftec H1517" manufactured by Asahi Kasei Corporation (styrene content (PS ratio): 43%, MFR (230°C, 2.16 kg): 3 g / 10 min) were uniformly dispersed or dissolved in toluene to prepare a coating liquid. The amount of solvent used was adjusted so that the viscosity at 28°C was 2.5 mPa s. (3) The coating liquid was applied to the surface of the laminated film on which the intermediate layer was formed by gravure coating to obtain a coated body. The temperature of the coating liquid immediately before coating was 28°C. The coated body was then transported into a drying oven with a length of about 10 m, the temperature of which was set at 85°C, to dry the solvent. The transport speed was set at 180 m / min (i.e., the coated body was heated in the drying oven for 10 m / (180 m / min) = 1 / 18 min = about 3.3 seconds while being transported). The amount of the coating solution applied was adjusted so that the dry thickness of the sealant layer was 0.2 μm.
[0059] <Comparative Example 1> The cover tape was manufactured according to the following procedure. (1) A biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) having a thickness of 25 μm was prepared as a substrate layer. On one side of the film, a low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was formed into a film having a thickness of 20 μm by extrusion lamination at an extrusion temperature of 300° C. to provide an intermediate layer. In this way, a laminated film was obtained. (2) As non-volatile components, antistatic agent: 60 mass% antimony-doped tin oxide ("T-1" manufactured by Mitsubishi Materials Corporation), poly(meth)acrylic acid derivative: 24 mass% "A450A" manufactured by DIC Corporation, styrene-butadiene copolymer: 16 mass% "Tuftec H1517" manufactured by Asahi Kasei Corporation (styrene content (PS ratio): 43%, MFR (230°C, 2.16 kg): 3 g / 10 min) were uniformly dispersed or dissolved in toluene to prepare a coating liquid. The amount of solvent used was adjusted so that the viscosity at 28°C was 1.5 mPa s. (3) The coating liquid was applied to the surface of the laminated film on which the intermediate layer was formed by gravure coating to obtain a coated body. The temperature of the coating liquid immediately before coating was 28°C. The coated body was then transported into a drying oven with a length of about 10 m, the temperature of which was set at 85°C, to dry the solvent. The transport speed was set at 180 m / min (i.e., the coated body was heated in the drying oven for 10 m / (180 m / min) = 1 / 18 min = about 3.3 seconds while being transported). The amount of the coating solution applied was adjusted so that the dry thickness of the sealant layer was 0.2 μm.
[0060] <Comparative Example 2> The cover tape was manufactured according to the following procedure. (1) A biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) having a thickness of 25 μm was prepared as a substrate layer. On one side of the film, a low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was formed into a film having a thickness of 20 μm by extrusion lamination at an extrusion temperature of 300° C. to provide an intermediate layer. In this way, a laminated film was obtained. (2) On the formed intermediate layer, a molten mixture of 90% by mass of ethylene-vinyl acetate copolymer ("Ultrathene 537" manufactured by Tosoh Corporation, vinyl acetate group content: 6% by mass) and 10% by mass of tackifier ("Alcon P-100" manufactured by Arakawa Chemical Industries Co., Ltd.) was extruded onto the surface of the intermediate layer at an extrusion temperature of 280°C by extrusion molding to form a film with a thickness of 10 μm. Immediately after that, the sealant layer surface was roughened by rotating a cooling roll with protrusions having a surface roughness of 5.5 μm from the sealant layer side and a silicone rubber mat roll from the base layer side at a pressure of 0.2 MPa. At this time, the temperature of the cooling roll was set to 20°C.
[0061] <Comparative Example 3> The cover tape was manufactured according to the following procedure. (1) A biaxially oriented polyester film ("E7415" manufactured by Toyobo Co., Ltd.) with a thickness of 25 μm was prepared as a substrate layer. On one side of the substrate, a low-density polyethylene ("Sumikathene L705" manufactured by Sumitomo Chemical Co., Ltd.) was formed into a film with a thickness of 20 μm by extrusion lamination at an extrusion temperature of 300° C. to form an intermediate layer. (2) On the formed intermediate layer, a molten mixture of 90% by mass of ethylene-vinyl acetate copolymer ("Ultrathene 537" manufactured by Tosoh Corporation, vinyl acetate group content: 6% by mass) and 10% by mass of tackifier ("Alcon P-100" manufactured by Arakawa Chemical Industries Co., Ltd.) was extruded onto the surface of the intermediate layer at an extrusion temperature of 280°C by extrusion molding to form a film with a thickness of 10 μm. Immediately after that, the sealant layer surface was roughened by rotating a cooling roll with protrusions having a surface roughness of 7.0 μm from the sealant layer side and a silicone rubber mat roll from the base layer side while sandwiching them at a pressure of 0.2 MPa. At this time, the temperature of the cooling roll was set to 20°C.
[0062] <Measurement of surface characteristics of sealant layer> The following indices of the sealant layer (exposed) of each of the above-mentioned Examples and Comparative Examples were measured using a laser microscope VK-X3000 manufactured by Keyence Corp. The analysis software used was that attached to the device. Arithmetic mean height Sa as defined in ISO 25178 Peak density Spd as defined in ISO 25178 · Root mean square slope Sdq as defined in ISO 25178
[0063] <Rating: Blocking> The cover tape of each of the examples and comparative examples was cut to a width of 5.4 mm and a length of 500 m. The cut cover tape was then wound tightly around a reel. The cover tape wound on the reel was left in a 65°C environment for 24 hours. After leaving it, the reel on which the cover tape was wound was vertically rotated slowly in the opposite direction to the direction in which the cover tape was wound. At this time, the strength of adhesion between the front and back of the cover tape (degree of blocking) was evaluated by checking whether the wound cover tape could be unwound under its own weight, and if it could not be unwound under its own weight, how much force was required to unwind it. Specifically, it was evaluated according to the following criteria. - Cover tape can be unwound by its own weight: Very good The cover tapes are slightly stuck together and cannot be unwound under their own weight, but if you shake the cover tape lightly with your hand, the stuck parts come off and it can be unwound: Good The cover tapes are relatively tightly attached to each other, and even if you shake the cover tape lightly with your hand, it does not come off and cannot be unwound: Bad
[0064] <Evaluation: Parts sticking> The adhesion of parts was evaluated by conducting an adhesion test using metal pieces simulating electronic parts as described below.
[0065] (1) The cover tapes obtained in the examples and comparative examples were cut to an appropriate size and attached to a slide glass so that the surface of the sealant layer was facing upward. A test specimen was prepared by placing 20 metal pieces (length 0.4 mm x width 0.8 mm x thickness 0.4 mm) on the sealant layer. The metal pieces were obtained by cutting nickel with a precision cutting machine. (2) The obtained test piece was left to stand under conditions of 60° C. and 95% RH for 24 hours, and then left to stand at room temperature and humidity for another 24 hours. (3) After the above (2), the test specimen was fixed with double-sided tape on a vortex mixer with the slide glass inverted. Then, the vortex mixer was set to 1,500 rpm and vibration was applied to the test specimen for 20 seconds. (Because there was no dedicated device for applying vibration, a vortex mixer, which is normally used to mix liquids, was used to apply vibration to the test specimen.) (4) After step (3) was completed, the adhesion rate was calculated from the number of metal pieces adhering to the surface of the sealant layer.
[0066] The above measurement results and evaluation results are summarized in the table below.
[0067] [Table 1]
[0068] As shown in the table above, the peak density Spd of the exposed surface of the sealant layer is 3×10 5 ~1×10 6 / mm 2 and the root mean square slope Sdq of the exposed surface of the sealant layer is within 1.0×10 ―2 ~5.0×10 ―1 In the evaluation of the cover tapes of Examples 1 to 3, blocking was suppressed, and sticking of components was also suppressed. In contrast, Spd is 3 × 10 5 Comparative Examples 1 and 2, in which Spd is smaller than 3 × 10 5 is smaller than 5×10 ―1 In Comparative Example 3, in which the thickness was larger than 100 mm, the evaluation result for blocking was poor, and sticking of parts occurred.
[0069] Incidentally, in the above blocking evaluation, the occurrence of blocking was suppressed even under the severe evaluation conditions of leaving the material in an environment of 65°C for 24 hours. Such good results were achieved by focusing on and optimizing the indices Spd and Sdq of the sealant layer. [Explanation of symbols]
[0070] 1 Base material layer 2. Middle Tier 3 Sealant Layer 10 Cover Tape 20 Carrier Tape 21 Pocket 100 Electronic component packaging body
Claims
1. A cover tape for packaging electronic components comprising a base layer and a sealant layer provided on one side of the base layer, a surface of the sealant layer opposite to the base layer is an exposed surface; The exposed surface has a peak density Spd of 3×10 as defined by ISO 25178. 5 ~1×10 6 / mm 2 and The root mean square slope Sdq of the exposed surface defined in ISO 25178 is 1.0×10 ―2 ~5.0 x 10 ―1 That is the cover tape.
2. 2. The cover tape of claim 1, The cover tape has an arithmetic mean height Sa of 0.05 to 0.5 μm as defined in ISO 25178 on the exposed surface.
3. 3. The cover tape according to claim 1 or 2, The cover tape, wherein the sealant layer comprises inorganic particles.
4. 3. The cover tape according to claim 1 or 2, The cover tape, wherein the sealant layer comprises one or both of a styrene-based resin and a (meth)acrylic resin.
5. 3. The cover tape according to claim 1 or 2, The cover tape, wherein the base layer comprises polyester.
6. 3. The cover tape according to claim 1 or 2, The cover tape further comprises an intermediate layer between the base layer and the sealant layer.
7. 7. The cover tape according to claim 6, The cover tape, wherein the intermediate layer comprises a polyethylene-based resin.
8. A carrier tape having electronic components housed in recesses and the cover tape according to claim 1 or 2, An electronic component package in which the sealant layer is adhered to the carrier tape so as to seal the electronic component.
Citation Information
Patent Citations
Powder contact member and surface treatment method of powder contact member
JP2020142831A
Cover tape ane electronic component package
JP2021091437A
Cover tape for taping packaging for electronic parts
JP2003246358A
Electronic component packaging body
JP2017171393A
Heat-sealing film and cover tape for packaging electronic components
WO2012079258A1