Gas barrier film, laminated film, and packaging bag
An aluminum-free gas barrier film with a liquid crystal polymer base layer and polyester resin auxiliary layer addresses waste and tear strength issues, offering superior gas barrier and tear resistance.
Patent Information
- Application Number
- JP2023048747
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional laminated films using aluminum-deposited polyester films generate waste with increased CO2 emissions during manufacturing and disposal, and liquid crystal polymers lack sufficient tear strength when used alone.
A gas barrier film composed of a base layer made of a liquid crystal polymer with a melting point of 230°C or less and an auxiliary layer containing a polyester resin polycondensate with 1-5 mol% diethylene glycol, providing excellent gas barrier properties and tear strength.
The film achieves aluminum-free gas barrier properties with improved tear strength, reducing waste and facilitating easy disposal, while maintaining high adhesive strength and processability.
Smart Images

Figure 2024137282000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas barrier film, a laminate film, and a packaging bag. [Background technology]
[0002] Conventionally, packaging bags made of a laminated film in which multiple layers are laminated on the inner surface of a base layer made of film, paper, etc., have been widely used as packaging bags for containing contents such as food, medicine, etc. Generally, the laminated film used in such packaging bags has a gas barrier property that blocks the intrusion of gases that deteriorate the contents, such as water vapor and oxygen, in order to suppress deterioration and spoilage of the contents and to maintain their functions and properties.
[0003] For example, Patent Document 1 discloses a packaging bag made by laminating a base layer / first adhesive layer / gas barrier layer / second adhesive layer / sealant layer in this order in a laminated film, with the sealant layer facing the inner surface, and then sealing to form a sealed portion. It also discloses that the gas barrier layer is a polyester film vapor-deposited with aluminum or an inorganic oxide, which provides excellent gas barrier properties and allows the quality of the fragrance to be maintained for a long time. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-5013 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in conventional laminated films, the gas barrier layer is often an aluminum-deposited polyester film or aluminum foil, and such aluminum-containing laminated films generate a large amount of CO2 during the manufacturing and disposal processes, and have the problem that they are difficult to separate and collect when disposed of. To address this problem, it is conceivable to use a liquid crystal polymer, which has excellent gas barrier properties, as the gas barrier layer, but the liquid crystal polymer has the disadvantage that it lacks tear strength when processed into a film by itself.
[0006] In view of the above, an object of one aspect of the present invention is to provide an aluminum-free gas barrier film having excellent gas barrier properties and tear strength. [Means for solving the problem]
[0007] A gas barrier film according to one embodiment of the present invention has a base layer and an auxiliary layer laminated on one side of the base layer, the base layer being made of a liquid crystal polymer having a melting point of 230°C or lower, and the auxiliary layer containing a polyester resin which is a polycondensate of a polyvalent carboxylic acid component and a polyhydric alcohol component containing 1 mol % to 5 mol % of a diethylene glycol component. Effect of the Invention
[0008] According to one aspect of the present invention, it is possible to provide an aluminum-free gas barrier film having excellent gas barrier properties and tear strength. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic diagram showing a cross section of a gas barrier film according to one embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a cross section of a laminated film according to one embodiment. [Diagram 3] 1 is a schematic diagram of a packaging bag according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In this specification, unless otherwise specified, the numerical range indicated by "to" means that the numerical range includes the numerical range before and after the range as the lower and upper limits.
[0011] (Gas barrier film) 1 is a schematic diagram showing a cross section of a gas barrier film 1 according to one embodiment. The gas barrier film 1 of this embodiment has a base layer 2 and an auxiliary layer 3 laminated on one surface of the base layer 2.
[0012] The base layer 2 is made of a liquid crystal polymer (A) having a melting point of 230° C. or less, and the auxiliary layer 3 contains a polyester resin (B), which is a polycondensate of a polycarboxylic acid component and a polyhydric alcohol component containing 1 mol % to 5 mol % of a diethylene glycol component. With this configuration, the gas barrier film 1 can block the intrusion of gas from the outside and can exhibit excellent gas barrier properties. In addition, the polyhydric alcohol component containing 1 mol % to 5 mol % of a diethylene glycol component can improve the flexibility of the polyester resin (B), so the gas barrier film 1 has excellent tear strength. In addition, the gas barrier film 1 has good processability because of its excellent tear strength. In this specification, the gas barrier property is a property that blocks gas, and includes water vapor barrier property that blocks water vapor and oxygen barrier property that blocks oxygen. In addition, the polyhydric alcohol component containing 1 mol % to 5 mol % of a diethylene glycol component can improve the flexibility of the polyester resin (B), thereby increasing the adhesive strength between the base layer 2 and the auxiliary layer 3, particularly in the width direction, and the gas barrier film 1 can prevent the auxiliary layer 3 from peeling off from the base layer 2.
[0013] The gas barrier film 1 of this embodiment is aluminum-free (does not contain aluminum), and therefore the amount of CO2 generated during the manufacturing and disposal processes can be reduced. Furthermore, when it is disposed of, the gas barrier film 1 can be disposed of as plastic waste, and therefore can be easily separated and collected. Furthermore, since the gas barrier film 1 of this embodiment is aluminum-free, it can be used in a production line that uses a metal detector to detect metallic foreign objects and the like.
[0014] The melting point of the liquid crystal polymer (A) constituting the base layer 2 is preferably 220° C. or lower. When the liquid crystal polymer (A) has a melting point of 220° C. or lower, the temperature during molding can be relatively low, and the polyester resin (B) of the auxiliary layer 3 can be prevented from changing due to thermal decomposition or the like. As a result, the gas barrier film 1 can exhibit superior tear strength.
[0015] Examples of monomers constituting the liquid crystal polymer (A) include one or more selected from terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, hydroquinone, resorcinol, 2,6-dihydroxynaphthalene, 4,4'-biphenol, p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4-aminobenzoic acid, 4-aminophenol, 1,4-phenylenediamine, and the like.
[0016] The liquid crystal polymer (A) preferably contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as monomer components constituting the liquid crystal polymer (A). When the liquid crystal polymer (A) contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as monomer components, the gas barrier film 1 can exhibit more excellent gas barrier properties and has excellent tear strength. From the viewpoint of improving the gas barrier properties, the liquid crystal polymer (A) more preferably contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as main monomer components. Here, the main component means that the liquid crystal polymer (A) contains 50 mol % or more of the monomer components constituting the liquid crystal polymer (A).
[0017] The liquid crystal polymer (A) preferably further contains a terephthalic acid component and a hydroquinone component as monomer components constituting the liquid crystal polymer (A), which allows the gas barrier film 1 to exhibit even better gas barrier properties and has excellent tear strength.
[0018] The monomer component constituting the liquid crystal polymer (A) is preferably an aromatic compound, which allows the gas barrier film 1 to exhibit superior gas barrier properties and also has superior tear strength.
[0019] Examples of the liquid crystal polymer (A) include VECTORA (registered trademark) and ZENITE (registered trademark) manufactured by Celanese, LAPEROS (registered trademark) manufactured by Polyplastics, XYDAR (registered trademark) manufactured by ENEOS, Sumikasuper LCP (registered trademark) manufactured by Sumitomo Chemical, and UENO LCP (registered trademark) manufactured by Ueno Pharmaceutical Co., Ltd.
[0020] Examples of the polyvalent carboxylic acid component constituting the polyester resin (B) contained in the auxiliary layer 3 include one or more selected from terephthalic acid, isophthalic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, adipic acid, sebacic acid, etc.
[0021] Examples of the polyhydric alcohol component constituting the polyester resin (B) other than diethylene glycol include one or more selected from ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexamethylenediol, cyclopentane dimethanol, cyclohexane dimethanol, neopentyl glycol, 2,2-diethyl-1,3-propanediol, 2,2-dipropyl-1,3-propanediol, 2-propyl-2-methyl-1,3-propanediol, 2-propyl-2-ethyl-1,3-propanediol, 2-isopropyl-2-methyl-1,3-propanediol, 2-isopropyl-2-ethyl-1,3-propanediol, 2-butyl-2-methyl-1,3-propanediol, and 2-butyl-2-ethyl-1,3-propanediol. The polyester resin (B) is non-liquid crystal and is different from the liquid crystal polymer (A).
[0022] The polyester resin (B) is preferably a modified polyethylene terephthalate composed of a dicarboxylic acid component composed of terephthalic acid, and a diol component containing an ethylene glycol component and a 1,4-butanediol component. This allows the gas barrier film 1 to exhibit excellent gas barrier properties and has better tear strength. In addition, the adhesive strength between the base layer 2 and the auxiliary layer 3, particularly in the width direction, can be further increased, and peeling of the auxiliary layer 3 from the base layer 2 can be further suppressed.
[0023] The glass transition temperature of the polyester resin (B) is preferably -10°C to 40°C, and more preferably 10°C to 30°C. When the glass transition temperature of the polyester resin (B) is -10°C to 40°C, the flexibility of the polyester resin (B) can be further improved, and the gas barrier film 1 has better tear strength. In addition, the adhesive strength between the base layer 2 and the auxiliary layer 3, particularly in the width direction, can be further increased, and the gas barrier film 1 can further suppress peeling of the auxiliary layer 3 from the base layer 2.
[0024] When the thickness of the base layer 2 is A and the thickness of the auxiliary layer 3 is B, B / A is preferably 0.1 to 0.4, and more preferably 0.2 to 0.3. When B / A is 0.1 to 0.4, the gas barrier film 1 can exhibit superior gas barrier properties and also has superior tear strength.
[0025] The thickness of the base layer 2 is not particularly limited, and may be 70 μm to 90 μm, and the thickness of the auxiliary layer 3 may be 10 μm to 30 μm, relative to a total thickness of 100 μm. When the base layer 2 has a thickness of 70 μm to 90 μm and the auxiliary layer 3 has a thickness of 10 μm to 30 μm, the gas barrier film 1 can exhibit better gas barrier properties and has better tear strength. Furthermore, the gas barrier film 1 can be suitably used particularly for packaging bags.
[0026] The gas barrier film 1 is preferably formed into a film shape by co-extrusion. The gas barrier film 1 can be formed into a film by co-extrusion, in which the material constituting the base layer 2 and the material constituting the auxiliary layer 3 are melt-extruded simultaneously. This can increase the adhesive strength between the base layer 2 and the auxiliary layer 3 compared to laminating the base layer 2 and the auxiliary layer 3 by a lamination method. In addition, since the liquid crystal polymer (A) constituting the base layer 2 has a melting point of 230°C or less, the heating temperature during co-extrusion can be relatively low, and the polyester resin (B) constituting the auxiliary layer 3 can be prevented from changing due to thermal decomposition or the like. Therefore, the gas barrier film 1 can exhibit excellent tear strength. Even when the long gas barrier film 1 is continuously molded and the long molded film is wound after molding, the gas barrier film 1 can be prevented from tearing because of its excellent tear strength.
[0027] The tear strength in the machine direction of the gas barrier film 1 is preferably 0.80 N / 100 μm or more. Here, the tear strength refers to a value measured in accordance with JIS K 7128-1. When the tear strength in the machine direction of the gas barrier film 1 is 0.80 N / 100 μm or more, even when a long gas barrier film 1 is continuously molded and the long molded film is wound up after molding, the gas barrier film 1 has superior tear strength and can be more prevented from tearing.
[0028] The adhesive strength between the base layer 2 and the auxiliary layer 3 in the machine direction and the width direction is preferably 2.0 N or more. The adhesive strength can be measured by a ring method. When the adhesive strength between the base layer 2 and the auxiliary layer 3 in the machine direction and the width direction is 2.0 N or more, the gas barrier film 1 can further suppress peeling of the auxiliary layer 3 from the base layer 2.
[0029] The adhesive strength between the base layer 2 and the auxiliary layer 3 in the width direction is preferably greater than the adhesive strength in the machine direction. In general, when a long laminate film is continuously molded and the long molded body of the film is wound along the machine direction after molding, the base layer and the auxiliary layer are likely to peel off at the ends in the width direction due to the application of a bending load. In the gas barrier film 1 of this embodiment, the adhesive strength between the base layer 2 and the auxiliary layer 3 in the width direction is greater than the adhesive strength in the machine direction, so that the auxiliary layer 3 can be prevented from peeling off from the base layer 2 even when the long molded body of the gas barrier film 1 is wound along the machine direction after molding.
[0030] (Laminated film) FIG. 2 is a schematic diagram showing a cross section of a laminated film according to an embodiment. As shown in FIG. 2, the laminated film 5 of this embodiment has the gas barrier film 1 of this embodiment and a sealant layer 4 laminated on the surface of the auxiliary layer 3 of the gas barrier film 1. The sealant layer 4 contains one or more of a polyethylene resin, a polypropylene resin, a polyester resin, and a cyclic olefin resin. The sealant layer 4 is one of the outermost surfaces of the laminated film 5. Here, the sealant layer 4 is a layer used for heat sealing, and is a layer disposed in the innermost layer in contact with the contents when the laminated film 5 is used as a packaging material. The auxiliary layer 3 and the sealant layer 4 may be bonded via an adhesive layer or an anchor agent layer, but are preferably bonded directly. The sealant layer 4 is preferably a resin film having excellent heat resistance, mechanical properties, and printability.
[0031] When the laminate film 5 is used as a packaging material, the gas barrier film 1 is located outside the sealant layer 4 that contacts the contents, so that the intrusion of gas from the outside can be blocked, and the laminate film 5 of this embodiment can exhibit excellent gas barrier properties. Furthermore, the laminate film 5 has excellent tear strength due to the presence of the gas barrier film 1. And, because the laminate film 5 has excellent tear strength, it has good processability.
[0032] The sealant layer 4 preferably contains isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid. The isophthalic acid-modified polyethylene terephthalate is a copolymer of linear polyester resins obtained by condensation polymerization of a dicarboxylic acid component and a diol component, in which the dicarboxylic acid component is mainly composed of terephthalic acid and further contains isophthalic acid, and the diol component is mainly composed of ethylene glycol. Here, the main component means the component with the highest content. Since the sealant layer 4 is isophthalic acid-modified polyethylene terephthalate, the laminated film 5 of this embodiment can exhibit even better gas barrier properties. Furthermore, since the sealant layer 4 is a polyester-based resin, the adhesion to the auxiliary layer 3 containing the polyester resin (B) can be improved.
[0033] The copolymerization ratio of the isophthalic acid component in the dicarboxylic acid component constituting the isophthalic acid modified polyethylene terephthalate is preferably 3 mol% to 30 mol%, and more preferably 5 mol% to 25 mol%. Here, the copolymerization ratio of the isophthalic acid component in the dicarboxylic acid component is the ratio (mol percentage) of the isophthalic acid component to the dicarboxylic acid component. When the copolymerization ratio of the isophthalic acid component in the dicarboxylic acid component is 3 mol% or more, the laminated film 5 of the present embodiment can exhibit better gas barrier properties and tear strength. In addition, when the copolymerization ratio of the isophthalic acid component in the dicarboxylic acid component is 30 mol% or less, it is possible to provide a laminated film 5 having heat resistance capable of withstanding heat when heat sealing the laminated films 5 together or the laminated film 5 to another film, or heat resistance capable of withstanding heat of the contents when high-temperature contents are filled in a packaging bag or the like formed from the laminated film 5.
[0034] The thickness of the sealant layer 4 depends on the application of the packaging material and is not particularly limited, but may be, for example, 10 μm to 50 μm.
[0035] The sealant layer 4 may contain additives as components other than the resin. The additives are not particularly limited, but examples thereof include antioxidants, lubricants, antiblocking agents, stabilizers, UV absorbers, flame retardants, antistatic agents, colorants, etc.
[0036] The laminated film 5 may have another layer provided on the opposite side of the sealant layer 4 with respect to the base layer 2, and the other layer preferably contains a resin other than the liquid crystal polymer. The other layer may include, for example, an intermediate layer, an adhesive layer, an anchoring agent layer, etc. As the intermediate layer, one or more layers may be appropriately selected from a reinforcing layer, a gas barrier layer, a light-shielding layer, a printing layer, etc.
[0037] The method for producing the laminated film 5 is not particularly limited, and examples thereof include an extrusion lamination method, a dry lamination method, a coextrusion method, or a combination of these. In addition, the strength and heat deformation resistance of the film can be improved by uniaxially or biaxially stretching the formed film before lamination.
[0038] (packaging bag) Fig. 3 is a schematic diagram of a packaging bag 10 according to one embodiment. The packaging bag 10 is formed using the laminated film 5 of this embodiment. As shown in Fig. 3, the packaging bag 10 has a bag-shaped body 11 formed from the laminated film 5 and a mouth 12 joined to at least one location on the periphery of the body 11. The shape of the body 11 is not particularly limited, and examples include a three-sided bag, a four-sided bag, a seamed bag, a gusset bag, and a standing pouch. The body 11 may be a large packaging bag, such as an inner bag for a bag-in-box.
[0039] The material constituting the mouth portion 12 can be suitably used as long as it can be bonded to the sealant layer 4 of the laminated film 5 constituting the packaging bag 10 to ensure hermeticity, but it is preferably a resin that can be heat-sealed to the sealant layer 4 of the laminated film 5. This allows the mouth portion 12 and the laminated film 5 to be bonded by heat sealing. For this reason, the material constituting the mouth portion 12 is preferably polyethylene terephthalate (PET), and more preferably isophthalic acid-modified PET. This allows the mouth portion 12 to be easily heat-sealed to the sealant layer 4 of the laminated film 5, and also improves the gas barrier properties of the packaging bag 10.
[0040] When heat sealing the laminated film 5 and the mouth portion 12, the laminated film 5 may be overlapped with the sealant layer 4 on the inside, and the mouth portion 12 may be inserted between the overlapped sealant layers 4 and heat sealed. Alternatively, a flange portion or a boat-shaped fusion base may be provided at one end of the mouth portion 12, and this flange portion or fusion base may be heat sealed to the periphery of a hole provided in the laminated film 5 or the inner surface of the opening of a packaging bag. EXAMPLES
[0041] The present invention will be specifically described below with reference to examples, although the present invention is not limited to these examples.
[0042] Example 1 As a liquid crystal polymer, UENO LCP (registered trademark) A-8100 (manufactured by Ueno Pharmaceutical Co., Ltd., density ρ = 1.40 g / cm 3 , melting point Tm = 220 °C), and polyester resin PRIT30 (manufactured by Bell Polyester Products, Inc., density ρ = 1.24 g / cm 3 A gas barrier film of Example 1 was produced by laminating a 80 μm-thick base layer made of a liquid crystal polymer and a 20 μm-thick auxiliary layer made of a polyester resin by a co-extrusion method using a liquid crystal polymer having a melting point Tm of 188° C., a glass transition temperature Tg of 30° C., and an intrinsic viscosity IV of 0.75 dl / g.
[0043] The liquid crystal polymer (UENO LCP (registered trademark) A-8100) used in Example 1 contains, as monomer components, a p-hydroxybenzoic acid component, a 6-hydroxy-2-naphthoic acid component, a terephthalic acid component, and a hydroquinone component. The polyester resin (PRIT30) is composed of a dicarboxylic acid component consisting of a terephthalic acid component, and a diol component containing 2 mol% of a diethylene glycol component (including an ethylene glycol component and a 1,4-butanediol component).
[0044] Comparative Example 1 As a liquid crystal polymer, UENO LCP (registered trademark) A-8100 (manufactured by Ueno Pharmaceutical Co., Ltd., density ρ = 1.40 g / cm 3 A gas barrier film of Comparative Example 1 consisting of only a 100 μm-thick base layer was produced by extrusion molding using a T-die extruder. Comparative Example 2 As a polyester resin, isophthalic acid modified polyethylene terephthalate (copolymerization ratio of isophthalic acid component: 12 mol%, density ρ = 1.34 g / cm 3 A gas barrier film of Comparative Example 2 was produced in the same manner as in Example 1, except that a liquid crystal polymer having a thickness of 80 μm and an auxiliary layer having a thickness of 20 μm and made of a polyester resin were laminated together. The gas barrier film of Comparative Example 2 was produced in the same manner as in Example 1, except that a liquid crystal polymer having a thickness of 80 μm and an auxiliary layer having a thickness of 20 μm and made of a polyester resin were used. Comparative Example 3 As a polyester resin, neopentyl glycol modified polyethylene terephthalate (product name "Bellpet (registered trademark) E-03", manufactured by Bell Polyester Products, Inc., density ρ = 1.29 g / cm 3 A gas barrier film of Comparative Example 3 was produced in the same manner as in Example 1, except that a liquid crystal polymer having an intrinsic viscosity of IV=0.83 dl / g and a modification rate of 16 mol%) was used, in which a base layer having a thickness of 80 μm and a polyester resin auxiliary layer having a thickness of 20 μm were laminated. Comparative Example 4 As a polyester resin, modified polyethylene terephthalate (diol components: 1,4-cyclohexanedimethanol, ethylene glycol, 1,4-butanediol) (product name "OKY100", density ρ = 1.08 g / cm 3 A gas barrier film of Comparative Example 4 was produced in the same manner as in Example 1, except that a liquid crystal polymer having a thickness of 80 μm and an auxiliary layer having a thickness of 20 μm and made of a polyester resin were laminated together. The gas barrier film of Comparative Example 4 was produced in the same manner as in Example 1, except that a liquid crystal polymer having a thickness of 80 μm and an auxiliary layer having a thickness of 20 μm and made of a polyester resin were used.
[0045] Next, the obtained films were evaluated as follows: For the gas barrier film of Comparative Example 1, evaluation was performed on properties other than adhesive strength since no auxiliary layer was provided.
[0046] (tear strength) In accordance with JIS K 7128-1, a trouser tear method was used to measure the tear strength in the machine direction by making a 75 mm long slit in the center of a sample cut to 150 mm x 50 mm, with a chuck width of 50 mm and a pulling speed of 200 mm / min.
[0047] (Adhesive strength) The adhesive strength of a sample cut to 25.4 mm x 200 mm was measured by the ring method, with the auxiliary layer clamped between grippers at a peel distance of 30 mm and a peel speed of 5 mm / min. An adhesive strength of 2.0 N or more in the machine direction (MD) and an adhesive strength of 2.0 N or more in the cross direction (TD) were evaluated as pass, and an adhesive strength of less than 2.0 N in the machine direction (MD) and less than 2.0 N in the cross direction (TD) were evaluated as fail.
[0048] (Oxygen gas permeability, water vapor permeability) The oxygen gas permeability and water vapor permeability of the prepared film were measured in accordance with JIS K 7126-2 and JIS K 7129-2.
[0049] The evaluation results are shown in Table 1.
[0050] [Table 1]
[0051] As shown in Table 1, the gas barrier film of Example 1 had the same oxygen permeability and water vapor permeability as the gas barrier film of Comparative Example 1 made of a liquid crystal polymer alone, and it was confirmed that the gas barrier film of Example 1 had excellent gas barrier properties. In addition, it was confirmed that the gas barrier film of Example 1 had excellent tear strength compared to Comparative Examples 1 to 4. Furthermore, it was confirmed that the gas barrier film of Example 1 had adhesive strength that met the pass criteria in both the machine direction and the width direction. Although adhesive strength in the width direction tends to be small in general films, it was confirmed that the gas barrier film of Example 1 had adhesive strength in the width direction that was greater than that in the machine direction, and was particularly excellent in adhesive strength in the width direction. Note that the gas barrier films of Comparative Examples 2 to 4 did not meet the pass criteria in adhesive strength and were problematic in practical use, so oxygen gas permeability and water vapor permeability were not measured.
[0052] Furthermore, using each of the raw materials of Example 1 and isophthalic acid modified PET as the raw material for the sealant layer, a three-layer laminate film was produced by co-extrusion molding, in which a 80 μm thick base layer made of liquid crystal polymer, a 20 μm thick auxiliary layer made of polyester resin, and a 50 μm thick sealant layer made of isophthalic acid modified PET were laminated in this order. A three-pack sealed bag was then produced at a heat seal temperature of 170°C, a seal pressure of 0.2 MPa, and a seal time of 1 sec, and it was confirmed that the packaging bag could be produced without any problems.
[0053] (Embodiments of the present invention) The present invention includes the following aspects. <Aspect 1> A base layer and an auxiliary layer laminated on one surface of the base layer, The substrate layer is made of a liquid crystal polymer having a melting point of 230° C. or less, The auxiliary layer contains a polyester resin, The polyester resin is a gas barrier film which is a polycondensation product of a polycarboxylic acid component and a polyhydric alcohol component containing 1 mol % to 5 mol % of a diethylene glycol component. <Aspect 2> The gas barrier film according to aspect 1, wherein the polyester resin has a glass transition temperature of -10°C to 40°C. <Aspect 3> 3. The gas barrier film according to embodiment 1 or 2, wherein the liquid crystal polymer contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as monomer components constituting the liquid crystal polymer. <Aspect 4> A gas barrier film according to any one of aspects 1 to 3, in which B / A is 0.1 to 0.4, where A is the thickness of the base layer and B is the thickness of the auxiliary layer. <Aspect 5> The gas barrier film according to aspect 4, wherein the auxiliary layer has a thickness of 10 μm to 30 μm. <Aspect 6> 6. The gas barrier film according to any one of aspects 1 to 5, wherein the tear strength in the machine direction is 0.80 N / 100 μm or more. <Aspect 7> A gas barrier film according to any one of aspects 1 to 6, wherein the adhesive strength between the base layer and the auxiliary layer in the machine direction and the width direction is 2.0 N or more. <Aspect 8> A gas barrier film according to any one of aspects 1 to 7, wherein the adhesive strength between the base layer and the auxiliary layer in the width direction is greater than the adhesive strength in the machine direction. <Aspect 9> 9. The gas barrier film according to any one of aspects 1 to 8, wherein the base layer and the auxiliary layer are formed into a film by coextrusion molding. <Aspect 10> A gas barrier film according to any one of aspects 1 to 9; a sealant layer laminated on a surface of the auxiliary layer, The sealant layer is a laminated film containing at least one of a polyethylene resin, a polypropylene resin, a polyester resin, and a cyclic olefin resin. <Aspect 11> 11. The laminate film according to claim 10, wherein the sealant layer contains isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid. <Aspect 12> a layer provided on the opposite side of the sealant layer with respect to the gas barrier film; 12. The laminate film according to aspect 10 or 11, wherein the other layer contains a resin other than the liquid crystal polymer. <Aspect 13> A packaging bag formed using the laminate film according to any one of aspects 10 to 12. [Explanation of symbols]
[0054] 1 Gas barrier film 2 Base material layer 3 Auxiliary layer 4 Sealant Layer 5. Laminated Film 10 packaging bags 11. Torso 12 Mouth
Claims
1. A base layer and an auxiliary layer laminated on one surface of the base layer, The substrate layer is made of a liquid crystal polymer having a melting point of 230° C. or less, The auxiliary layer contains a polyester resin, The polyester resin is a polycondensation product of a polycarboxylic acid component and a polyhydric alcohol component containing 1 mol % to 5 mol % of a diethylene glycol component.
2. 2. The gas barrier film according to claim 1, wherein the glass transition temperature of the polyester resin is from -10°C to 40°C.
3. 3. The gas barrier film according to claim 2, wherein the liquid crystal polymer contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as monomer components constituting the liquid crystal polymer.
4. 4. The gas barrier film according to claim 3, wherein the thickness of the base layer is A and the thickness of the auxiliary layer is B, and B / A is 0.1 to 0.
4.
5. 5. The gas barrier film according to claim 4, wherein the thickness of the auxiliary layer is from 10 μm to 30 μm.
6. 6. The gas barrier film according to claim 5, wherein the tear strength in the machine direction is 0.80 N / 100 μm or more.
7. 7. The gas barrier film according to claim 6, wherein the adhesive strength between the base layer and the auxiliary layer in the machine direction and the width direction is 2.0 N or more.
8. The gas barrier film according to claim 7 , wherein the adhesive strength between the base layer and the auxiliary layer in the width direction is greater than the adhesive strength in the machine direction.
9. The gas barrier film according to claim 8 , wherein the base layer and the auxiliary layer are formed into a film by coextrusion molding.
10. The gas barrier film according to any one of claims 1 to 9, a sealant layer laminated on a surface of the auxiliary layer, The sealant layer is a laminated film containing at least one of a polyethylene resin, a polypropylene resin, a polyester resin, and a cyclic olefin resin.
11. The laminated film according to claim 10 , wherein the sealant layer comprises an isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid.
12. a layer provided on the opposite side of the sealant layer with respect to the gas barrier film; The laminate film according to claim 11 , wherein the other layer contains a resin other than a liquid crystal polymer.
13. A packaging bag formed using the laminated film according to claim 10.