Method for producing active energy ray-curable ink composition

By omitting polymerization inhibitors in the production process, the ink composition effectively prevents precipitate formation, ensuring stable storage and ejection performance of active energy ray-curable inks.

JP2024137395APending Publication Date: 2024-10-07MAXELL LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023048904
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing active energy ray-curable ink compositions containing pigments and pigment derivatives suffer from precipitate formation during long-term storage, leading to reduced ejectability and stability issues, particularly in inkjet printers.

Method used

A method for producing an active energy ray-curable ink composition by mixing pigments, pigment derivatives, and polymerizable compounds without the use of polymerization inhibitors, ensuring proper adsorption and dispersion of components, thereby preventing precipitate formation and enhancing storage stability.

Benefits of technology

The method results in an ink composition with excellent storage stability and ejection properties, maintaining dispersibility and preventing pigment derivative precipitation even after prolonged storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137395000001
    Figure 2024137395000001
  • Figure 2024137395000002
    Figure 2024137395000002
  • Figure 2024137395000003
    Figure 2024137395000003
Patent Text Reader

Abstract

To provide a method for producing an ink composition that does not generate deposit even when an active energy ray-curable ink composition is stored for a long time, and produces an ink composition excellent in storage stability.SOLUTION: A method for producing an active energy ray-curable ink composition containing a polymerization inhibitor, comprises the steps of: mixing and stirring a pigment, a pigment dispersant, a pigment derivative, and a polymerizable compound to prepare a mixture; dispersing the mixture with a dispersion medium to prepare a pigment dispersion; and mixing and stirring the pigment dispersion, the polymerizable compound, and a polymerization initiator to prepare an ink composition. In the step of preparing the mixture, the composition does not contain a polymerization inhibitor.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an active energy ray-curable ink composition. [Background technology]

[0002] The active energy ray-curable ink composition is an ink composition that contains a polymerizable compound and a polymerization initiator, and is cured by irradiation with active energy rays. The ink composition is used as an ink in a printing device such as an inkjet printer, and is used in a printing method in which the ink composition is ejected onto a recording medium and cured by irradiation with active energy rays.

[0003] On the other hand, when an active energy ray-curable ink composition is stored for a certain period of time after production, depending on the surrounding environment, the polymerizable compound contained in the ink composition may gradually react, even without irradiation with active energy rays, causing changes in the ink composition. For this reason, for example, a polymerization inhibitor may be added as a method for suppressing changes in viscosity or gelation of the ink composition.

[0004] Patent Document 1 discloses a method for producing an active energy ray-curable ink composition, in which, when producing an active energy ray-curable ink composition containing a pigment, a pigment, a pigment dispersant, and a portion of a radical polymerizable compound and a hindered amine-based polymerization inhibitor are mixed and stirred to prepare a mixture, the mixture is dispersed in a dispersion medium to prepare a pigment dispersion, and the pigment dispersion, the remainder of the radical polymerizable compound and the hindered amine-based polymerization inhibitor, and a photopolymerization initiator are mixed and stirred to produce the ink composition. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-189586 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the method described in Patent Document 1, in an ink composition that contains a pigment derivative in addition to a pigment, a precipitate derived from the pigment derivative is generated when the ink composition is stored for a long period of time, and there is a problem that the ejection properties from the inkjet head of an inkjet printer are particularly deteriorated.

[0007] Therefore, an object of the present invention is to provide a method for producing an actinic energy ray-curable ink composition containing a pigment and a pigment derivative, which does not produce precipitates even when the ink composition is stored for a long period of time and has excellent storage stability. [Means for solving the problem]

[0008] The present inventors have discovered that in an actinic ray-curable ink composition containing a pigment and a pigment derivative, precipitation originating from the pigment derivative can be suppressed by controlling the process of adding a polymerization inhibitor, thereby achieving the above-mentioned object.

[0009] That is, the present invention provides the following preferred embodiments. [1] A method for producing an active energy ray-curable ink composition containing a polymerization inhibitor, the method comprising the steps of: mixing and stirring a pigment, a pigment dispersant, a pigment derivative, and a polymerizable compound to prepare a mixture; dispersing the mixture in a dispersion medium to prepare a pigment dispersion; and mixing and stirring the pigment dispersion, the polymerizable compound, and a polymerization initiator to prepare the ink composition, wherein the polymerization inhibitor is not further contained in the step of preparing the mixture. [2] The method for producing an active energy ray-curable ink composition according to [1], wherein the polymerization inhibitor is at least one selected from the group consisting of hindered amine polymerization inhibitors and phenol polymerization inhibitors. [3] The method for producing an active energy ray-curable ink composition according to [2], wherein the polymerization inhibitor is a hindered amine-based polymerization inhibitor. [4] The method for producing an active energy ray-curable ink composition according to [3], wherein the polymerization inhibitor is a hindered amine-based polymerization inhibitor having an N-hydroxy-2,2,6,6-tetramethylpiperidinyl group. [5] The method for producing an active energy ray-curable ink composition according to [1], wherein the pigment is a cyan or black pigment. [6] The method for producing an active energy ray-curable ink composition according to [1], wherein the pigment derivative is a phthalocyanine derivative. [7] The method for producing an active energy ray-curable ink composition according to [1], wherein the blending amount of the pigment derivative is 1 to 15 mass % based on the blending amount of the pigment. [8] The method for producing an active energy ray-curable ink composition according to [1], wherein the blending amount of the pigment derivative is 1 to 20 mass % based on the blending amount of the pigment dispersant. [9] The method for producing an active energy ray-curable ink composition according to [1], further comprising a step of adding the polymerization inhibitor to the pigment dispersion liquid.

[10] The method for producing an active energy ray-curable ink composition according to [1], further comprising the step of adding the polymerization inhibitor in the step of preparing the ink composition.

[11] The method according to [1], wherein the ink composition is an ink-jet ink composition. Effect of the Invention

[0010] According to the production method of the present invention, it is possible to provide a production method for producing an active energy ray-curable ink composition containing a pigment and a pigment derivative, which does not produce precipitates even when the ink composition is stored for a long period of time, has excellent storage stability, and is excellent in ejection properties from an inkjet head. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The method for producing an active energy ray-curable ink composition of the present invention includes a step of mixing and stirring a pigment, a pigment dispersant, a pigment derivative, and a polymerizable compound to prepare a mixture, a step of preparing a pigment dispersion by dispersing the mixture in a dispersion medium, and a step of mixing and stirring the pigment dispersion, the polymerizable compound, and a polymerization initiator to adjust an ink composition, and is characterized in that the step of preparing the mixture further does not contain a polymerization inhibitor.

[0012] In the manufacturing method of the present invention, by not adding a polymerization inhibitor when preparing a mixture containing a pigment derivative, the pigment, pigment derivative, and pigment dispersant can be in an appropriate state for mutual adsorption, and by adsorbing the pigment and the pigment derivative and fully exerting the interaction with the pigment dispersant, the dispersibility of these components in the ink composition is improved. Although the reason is unclear, it is presumed that if a polymerization inhibitor is present when preparing the mixture, the adsorption of the pigment and the pigment derivative is inhibited, resulting in excess pigment derivative, which aggregates during long-term storage of the ink composition and becomes a precipitate that reduces the ejection performance of the inkjet head. In other words, by not adding a polymerization inhibitor when preparing the mixture, the amount of pigment derivative that is not adsorbed to the pigment is reduced, and the precipitation of the pigment derivative in the ink composition is suppressed, resulting in an ink composition with excellent storage stability.

[0013] The production method of the present invention will now be described in detail.

[0014] The active energy ray-curable ink composition produced by the production method of this embodiment contains a pigment, a pigment derivative, a pigment dispersant, a polymerizable compound, and a polymerization initiator. From the viewpoint of storage stability, the ink composition further contains a polymerization inhibitor.

[0015] In the production of the actinic energy ray-curable ink composition of the present embodiment, first, a mixing and stirring step is performed in which the pigment, the pigment derivative, the pigment dispersant, and a portion of the polymerizable compound are mixed and stirred to prepare a mixture. By such a mixing and stirring step, the surface of the pigment can be wetted with the polymerizable compound in advance, and even in a mixture with a high pigment concentration, the pigment can be highly dispersed in the dispersion step. Note that in the step of preparing the mixture, the mixture does not contain a polymerization inhibitor.

[0016] As the pigment, it is preferable to use either an inorganic pigment or an organic pigment, or both, from the viewpoint of weather resistance.

[0017] Specific examples of inorganic pigments include titanium oxide, zinc oxide, tripon, iron oxide, aluminum oxide, silicon dioxide, kaolinite, montmorillonite, talc, barium sulfate, calcium carbonate, silica, alumina, cadmium red, red iron oxide, molybdenum red, chrome vermilion, molybdate orange, yellow lead, chrome yellow, cadmium yellow, yellow iron oxide, titanium yellow, chromium oxide, pyridian, cobalt green, titanium cobalt green, cobalt chrome green, ultramarine blue, Prussian blue, cobalt blue, cerulean blue, manganese violet, cobalt violet, and mica.

[0018] Specific examples of organic pigments include azo, azomethine, polyazo, phthalocyanine, quinacridone, anthraquinone, indigo, thioindigo, quinophthalone, benzimidazolone, and isoindoline organic pigments. Carbon black made of acidic, neutral, or basic carbon may also be used. Hollow particles of crosslinked acrylic resin may also be used as the organic pigment.

[0019] Specific examples of pigments having a cyan color include CI Pigment Blue 1, CI Pigment Blue 2, CI Pigment Blue 3, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 16, CI Pigment Blue 22, and CI Pigment Blue 60. Among these, in terms of weather resistance, coloring power, etc., either or both of CI Pigment Blue 15:3 and CI Pigment Blue 15:4 are preferred.

[0020] Specific examples of pigments having a magenta color include CI Pigment Red 5, CI Pigment Red 7, CI Pigment Red 12, CI Pigment Red 48 (Ca), CI Pigment Red 48 (Mn), CI Pigment Red 57 (Ca), CI Pigment Red 57:1, CI Pigment Red 112, CI Pigment Red 122, CI Pigment Red 123, CI Pigment Red 168, CI Pigment Red 184, CI Pigment Red 202, CI Pigment Red 209, CI Pigment Red 254, and CI Pigment Violet 19. Among these, at least one selected from the group consisting of CI Pigment Red 122, CI Pigment Red 202, CI Pigment Red 209, CI Pigment Red 254, and CI Pigment Violet 19 is preferred from the standpoint of weather resistance, coloring power, and the like.

[0021] Specific examples of pigments having a yellow color include CI Pigment Yellow 1, CI Pigment Yellow 2, CI Pigment Yellow 3, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14C, CI Pigment Yellow 16, CI Pigment Yellow 17, CI Pigment Yellow 73, CI Pigment Yellow 74, CI Pigment Yellow 75, CI Pigment Yellow 83, CI Pigment Yellow 93, CI Pigment Yellow 95, CI Pigment Yellow 97, CI Pigment Yellow 98, CI Pigment Yellow 109, Examples of pigments include CI Pigment Yellow 110, CI Pigment Yellow 114, CI Pigment Yellow 120, CI Pigment Yellow 128, CI Pigment Yellow 129, CI Pigment Yellow 130, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 147, CI Pigment Yellow 150, CI Pigment Yellow 151, CI Pigment Yellow 154, CI Pigment Yellow 155, CI Pigment Yellow 180, CI Pigment Yellow 185, CI Pigment Yellow 213, and CI Pigment Yellow 214. Among these, from the viewpoint of weather resistance and the like, at least one selected from the group consisting of CI Pigment Yellow 74, CI Pigment Yellow 83, CI Pigment Yellow 109, CI Pigment Yellow 110, CI Pigment Yellow 120, CI Pigment Yellow 128, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 150, CI Pigment Yellow 151, CI Pigment Yellow 154, CI Pigment Yellow 155, CI Pigment Yellow 213, and CI Pigment Yellow 214 is preferred.

[0022] Specific examples of black pigments include HCF, MCF, RCF, LFF, and SCF manufactured by Mitsubishi Chemical Corporation, Monarch and Regal manufactured by Cabot Corporation, Color Black, Special Black, and Printex manufactured by Degussa-Huls Co., Ltd., Toka Black manufactured by Tokai Carbon Co., Ltd., and Raven manufactured by Columbia Chemical Co., Ltd. Among these, at least one selected from the group consisting of HCF#2650, HCF#2600, HCF#2350, HCF#2300, MCF#1000, MCF#980, MCF#970, MCF#960, MCF88, LFFMA7, MA8, MA11, MA77, and MA100 manufactured by Mitsubishi Chemical Corporation, and Printex 95, Printex 85, Printex 75, Printex 55, and Printex 45 manufactured by Degussa-Huls Co., Ltd. is preferred.

[0023] The amount of the pigment in the ink composition is 0.1 to 7% by mass, and preferably 1 to 5% by mass, based on the total amount of the ink composition, and the amount of the pigment in the pigment dispersion is 5 to 30% by mass, and preferably 10 to 20% by mass, based on the total amount of the pigment dispersion.

[0024] The mixture contains a pigment derivative in order to improve the dispersibility of the pigment in the ink composition. By mixing the pigment and the pigment derivative in advance before the dispersion step, the pigment and the pigment derivative are chemically adsorbed, and an adsorption site for the pigment with the pigment dispersant described below can be provided to the pigment in a pseudo manner. Examples of such pigment derivatives include compounds in which functional groups such as hydroxyl groups, carboxyl groups, sulfone groups, amino groups, and carboamino groups are introduced onto the surface of a pigment or a compound similar to a pigment skeleton, and specific examples thereof include pigment derivatives having a dialkylaminoalkyl group and pigment derivatives having a dialkylaminoalkylsulfonic acid amide group.

[0025] In addition, examples of the pigment derivatives having functional groups introduced therein include phthalocyanine derivatives and condensed polycyclic derivatives such as quinacridone derivatives or anthraquinone derivatives. These pigment derivatives having functional groups introduced therein are organic pigments or derivatives having a structure similar to that of organic pigments, and can improve the dispersibility of organic pigments in particular. When an ink composition containing a phthalocyanine derivative, which is a pigment derivative, is stored for a long period of time, the phthalocyanine derivative is likely to precipitate, but according to the manufacturing method of the present invention, such precipitation of the pigment derivative can be suppressed. Phthalocyanine derivatives are often used from the viewpoint of improving the dispersibility of the pigment in an ink composition containing a pigment having a black or cyan color.

[0026] Examples of commercially available pigment derivatives include EFKA-745 manufactured by EFKA Corporation, and Solsperse 5000, Solsperse 5000S, Solsperse 12000, and Solsperse 22000 manufactured by Lubrizol Corporation.

[0027] The amount of the pigment derivative is 1% by mass or more, preferably 2% by mass or more, based on the amount of the pigment. Also, the amount is 15% by mass or less, preferably 12% by mass or less, based on the amount of the pigment. When the amount is within the above upper and lower limits, the pigment can be sufficiently dispersed, the dispersion stability is improved, and precipitation of excess pigment derivative can be suppressed.

[0028] The amount of the pigment derivative is 1% by mass or more, preferably 3% by mass or more, based on the amount of the pigment dispersant, and 20% by mass or less, preferably 15% by mass or less, based on the amount of the pigment dispersant. Within the above upper and lower limits, the pigment can be sufficiently dispersed, the solubility of the pigment derivative in the ink is improved, and precipitation of excess pigment derivative can be suppressed.

[0029] The mixture contains a pigment dispersant to improve the dispersibility of the pigment in the ink composition. By mixing the pigment and the pigment dispersant in advance before the dispersion step, the surface of the pigment can be appropriately wetted with the pigment dispersant. Specific examples of such pigment dispersants include ionic or nonionic surfactants and anionic, cationic or nonionic polymer compounds. Among these, polymer compounds containing cationic or anionic groups are preferred from the viewpoint of dispersion stability. Examples of pigment dispersants available on the market include SOLSPERSE manufactured by Lubrizol Corporation, DISPERBYK manufactured by BYK-Chemie, and EFKA manufactured by EFKA Additives. The amount of pigment dispersant in the mixture depends on the amount of pigment, but is usually preferably 0.05 to 15% by mass with respect to the total amount of the mixture.

[0030] The pigment dispersant is present in an amount of 50% by mass or more, preferably 70% by mass or more, based on the amount of the pigment, and is present in an amount of 90% by mass or less, preferably 80% by mass or less, based on the amount of the pigment. When the amount is within the above upper and lower limits, the pigment can be sufficiently dispersed, and the dispersion stability is improved.

[0031] The mixture contains a part of the polymerizable compound in the final composition of the ink composition. In the mixing and stirring step, by using only a part of the polymerizable compound in the final composition of the ink composition, rather than the entire amount, it is possible to prepare a pigment dispersion having a high pigment concentration.

[0032] As the polymerizable compound, a monofunctional monomer having one ethylenic double bond in the molecule, or a polyfunctional monomer, oligomer, or prepolymer having a plurality of ethylenic double bonds in the molecule, which has the property of being cured by energy rays, can be used. When a monofunctional monomer and a polyfunctional monomer are used in combination as the polymerizable compound in the final ink composition, a polymerizable compound containing a monofunctional monomer or a polyfunctional monomer as a main component can be used in the mixing and stirring process. As the polymerizable functional group of the polymerizable compound, a (meth)acrylic group, a (meth)acryloyl group, or a vinyl ether group is preferable. As the polymerizable compound used in the present embodiment, a radical polymerizable compound in which polymerization proceeds by a radical polymerization reaction is preferable.

[0033] Specific examples of monofunctional monomers having one ethylenic double bond in the molecule include amyl (meth)acrylate, isoamyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isomyristyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, tridecyl (meth)acrylate, 2-ethylhexyl-diglycol (meth)acrylate, 2-(meth)acryloyloxyethylhexahydrophthalic acid, neopentyl glycol (meth)acrylic acid benzoate, butoxyethyl (meth)acrylate, ethoxy-diethylene glycol (meth)acrylate, methoxy-triethylene glycol (meth)acrylate, methoxy -polyethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxy-polyethylene glycol (meth)acrylate, nonylphenol ethylene oxide adduct (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-succinic acid, 2-(meth)acryloyloxyethyl-phthalic acid, 2-(meth)acryloyloxyethyl-2-hydroxyethyl-phthalic acid, etc. These may be used alone or in combination. The above monomers may also be substituted with functional groups such as phosphorus and fluorine. Among these, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and tridecyl (meth)acrylate are particularly preferred because they have low viscosity.

[0034] Specific examples of polyfunctional monomers having two ethylenic double bonds in the molecule include 1,3-butylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol diacrylate, cyclohexanedimethanol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and vinyl ether group-containing (meth)acrylic acid esters; 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, 2-(vinyloxyisopropoxy)propyl (meth)acrylate, and 2-(vinyloxyisopropoxy)isopropyl (meth)acrylate. These may be used alone or in combination.

[0035] Specific examples of polyfunctional monomers having three ethylenic double bonds in the molecule include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, glyceryl tri(meth)acrylate, and ethylene oxide-modified, propylene oxide-modified, and caprolactone-modified versions of these. These may be used alone or in combination.

[0036] Specific examples of polyfunctional monomers having four ethylenic double bonds in the molecule include ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, and ethylene oxide-modified, propylene oxide-modified, and caprolactone-modified versions of these. These may be used alone or in combination.

[0037] Specific examples of polyfunctional monomers having five ethylenic double bonds in the molecule include dipentaerythritol hydroxypenta(meth)acrylate, and ethylene oxide-modified, propylene oxide-modified, and caprolactone-modified versions thereof. These may be used alone or in combination.

[0038] Specific examples of polyfunctional monomers having six ethylenic double bonds in the molecule include dipentaerythritol hexa(meth)acrylate, and ethylene oxide-modified, propylene oxide-modified, and caprolactone-modified versions thereof. These may be used alone or in combination.

[0039] The mixture may contain an oligomer or prepolymer as a polymerizable compound. The oligomer or prepolymer preferably has a urethane group, an epoxy group, or an ester group, and more preferably has a urethane group. Examples of such oligomers include urethane (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, and polyester (meth)acrylate oligomers.

[0040] In this specification, "oligomer" or "prepolymer" refers to a polymer having a weight average molecular weight (Mw) of 500 to 10,000. The weight average molecular weight (Mw) of the oligomer is preferably 800 or more, and more preferably more than 1,000. The weight average molecular weight (Mw) refers to the weight average molecular weight in terms of polystyrene measured by GPC (gel permeation chromatography).

[0041] Specific examples of such oligomers or prepolymers include Ebecryl 230, Ebecryl 244, Ebecryl 245, Ebecryl 270, Ebecryl 280 / 15IB, Ebecryl 284, Ebecryl 285, Ebecryl 4830, Ebecryl 4835, Ebecryl 4858, Ebecryl 4883, Ebecryl 8402, Ebecryl 8803, Ebecryl 8800, Ebecryl 254, Ebecryl 26 ...70, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270, Ebecryl 270 l294 / 35HD, Ebecryl1259, Ebecryl1264, Ebecryl4866, Ebecryl9260, Ebecryl8210, Ebecryl1290, Ebecryl1290K, Ebecryl5129, Ebecryl2000, Ebecr yl2001, Ebecryl2002, Ebecryl2100, KRM7222, KRM7735, KRM4842, KRM210, KRM215, KRM4827, KRM4849, KRM6700, KRM6700-20T, KRM204, KRM205, KRM660 2, KRM220, KRM4450, KRM770, IRR567, IPR81, IPR84, IPR83, IPR80, IPR657, IPR800, IPR805, IPR808, IPR810, IPR812, IPR1657, IPR1810, IRR302, IPR4 50, IPR670, IPR830, IPR835, IPR870, IPR1830, IPR1870, IPR2870, IRR267, IPR813, IRR483, IPR811, IPR436, IPR438, IPR446, IPR505, IPR524, IPR525, IPR554W, IPR584, IPR586, IPR745, IPR767, IPR1701, IPR1755, IPR740 / 40TP, IPR600, IPR601, IPR604, IPR605, IPR607, IPR608, IPR609, IPR600 / 25TO , IPR616, IPR645, IPR648, IPR860, IPR1606, IPR1608, IPR1629, IPR1940, IPR2958, IPR2959, IPR3200, IPR3201, IPR3404, IPR3411, IPR3412, IPR3415,IPR3500, IPR3502, IPR3600, IPR3603, IPR3604, IPR3605, IPR3608, IPR3700, IPR3700-20H, IPR3700-20T, IPR3700-25R, IPR3701, IPR3701-20T, IPR3703, IPR3702, RDX63182, RDX6040, IRR419; CN104, CN120, CN124, CN136, CN151, CN2270, CN2271E, CN435, CN454, CN970, CN971, CN972, CN9782, CN981, CN9893, CN991 by Sartomer; Laromer by BASF EA81, Laromer LR8713, Laromer LR8765, Laromer LR8986, Laromer PE56F, Laromer PE44F, Laromer LR8800, Laromer PE46T, Laromer LR8907, Laromer PO43F, Laromer PO77F, Laromer PE55F, Laromer LR8967, Laromer LR8981, Laromer LR8982, Laromer LR8992, Laromer LR9004, Laromer LR8956, Laromer LR8985, Laromer LR8987, Laromer UP35D, Laromer UA19T, Laromer LR9005, Laromer PO83F, Laromer PO33F, Laromer PO84F, Laromer PO94F, Laromer LR8863, Laromer LR8869, Laromer LR8889, Laromer LR8997, Laromer LR8996, Laromer LR9013, Laromer LR9019, Laromer PO9026V, Laromer PE9027V; Photomer 3005, Photomer 3015, Photomer 3016, Photomer 3072, Photomer 3982, 3215, Photomer 5010, Photomer 5429, Photomer 5430, Photomer 5432, Photomer 5662, Photomer 5806, Photomer 5930, Photomer 6008, Photomer 6010, Photomer 6019, Photomer 6184, Photomer 6210, Photomer 6217,Photomer 6230, Photomer 6891, Photomer 6892, Photomer 6893-20R, Photomer 6363, Photomer 6572, Photomer 3660; Art Resin UN-9000HP, Art Resin UN-9000PEP, Art Resin UN-9200A, Art Resin UN-7600, Art Resin UN-5200, Art Resin UN-1003, Art Resin UN-1255, Art Resin UN-3320HA, Art Resin UN-3320HB, Art Resin U made by Negami Chemical Industries. N-3320HC, Art Resin UN-3320HS, Art Resin UN-901T, Art Resin UN-1200TPK, Art Resin UN-6060PTM, Art Resin UN-6060P; Nippon Gosei Kagaku Shiko UV-6630B, Shiko UV -7000B, Shiko UV-7510B, Shiko UV-7461TE, Shiko UV-3000B, Shiko UV-3200B, Shiko UV-3210EA, Shiko UV-3310B, Shiko UV-3500BA, Shiko UV-3520TL, Shiko UV-3700B, Shiko U V-6100B, Shiko UV-6640B, Shiko UV-1400B, Shiko UV-1700B, Shiko UV-6300B, Shiko UV-7550B, Shiko UV-7605B, Shiko UV-7610B, Shiko UV-7620EA, Shiko UV-7630B, Shiko UV -7640B, Shiko UV-2000B, Shiko UV-2010B, Shiko UV-2250EA, Shiko UV-2750B; Nippon Kayaku Co., Ltd. Kayarad R-280, Kayarad R-146, Kayarad R131, Kayarad R-205, Kayarad EX2320 , Kayarad R190, Kayarad R130, Kayarad R-300, Kayarad C-0011, Kayarad TCR-1234, Kayarad ZFR-1122, Kayarad UX-2201, Kayarad UX-2301, Kayarad UX3204, Kayarad UX-3301, Kayarad UX-4101, Kayarad UX-6101, Kayarad UX-7101, Kayarad MAX-5101, Kayarad MAX-5100, Kayarad MAX-3510, Kayarad UX-4101, etc.

[0042] The blending amount of the polymerizable compound in the mixture is not particularly limited as long as the blending amount of the pigment can be ensured, but is preferably 40 to 90 mass %, more preferably 40 to 70 mass %, based on the total amount of the mixture.

[0043] The ink composition preferably contains a hindered amine-based or phenol-based polymerization inhibitor. By containing a hindered amine-based or phenol-based polymerization inhibitor in the ink composition, the ink composition is less likely to increase in viscosity or gel. Furthermore, by using a hindered amine-based or phenol-based polymerization inhibitor in a process after the preparation of the pigment dispersion, the pigment dispersion is less likely to increase in viscosity or gel even if the prepared pigment dispersion is stored for a certain period of time. Furthermore, when the pigment dispersion after storage is diluted to produce an ink composition, it is possible to obtain an ink composition in which fine particles of pigment are dispersed without becoming highly viscous.

[0044] The above-mentioned hindered amine polymerization inhibitor includes a compound having a piperidine skeleton, and preferably has a hindered amine polymerization inhibitor having a 2,2,6,6-tetramethylpiperidinyl group.Specific examples of such hindered amine polymerization inhibitor include 2,2,6,6-tetramethylpiperidine-N-oxyl, 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine-N-oxyl, ester of 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl, bis(1-oxyl-2,2,6,6-tetramethylpiperidin-4-yl)sebacate, decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl)ester, etc.These may be used alone or in combination. Among these, 2,2,6,6-tetramethylpiperidine-N-oxyl, 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl, and bis(1-oxyl-2,2,6,6-tetramethylpiperidin-4-yl) sebacate having N-hydroxy-2,2,6,6-tetramethylpiperidinyl group are preferred. Hindered amine-based polymerization inhibitors having 2,2,6,6-tetramethylpiperidinyl group that are available on the market include H-TEMPO (manufactured by Evonik Degussa Japan), IRGASTAB UV-10 (manufactured by BASF), TINUVIN 111 FDL (manufactured by BASF), TINUVIN 144 (manufactured by BASF), TINUVIN 292 (manufactured by BASF), and TINUVIN 123 (manufactured by BASF).

[0045] The phenol-based polymerization inhibitor means a polymerization inhibitor having a phenolic hydroxyl group as a basic skeleton, such as 2,6-di-tert-butyl-4-methylphenol, 2,6-di-tert-butyl-4-ethylphenol, mono-, di- or tri-(α-methylbenzyl)phenol, 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), 4,4'-thio ... Methyl-6-tert-butylphenol), 2,5-di-tert-butylhydroquinone, 2,5-di-tert-amylhydroquinone, triethylene glycol-bis-[3-(3-t-butyl-5-methyl-4 hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythritol=tetrakis[3-(3' ,5'-di-tert-butyl-4'-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 3,5-di-t-butyl-4-hydroxy-benzylphosphonate-diethyl ester, 13,5-trimethyl-2,4,6-tris(3,5-di-t- butyl-4-hydroxybenzyl)benzene, bis(3,5-di-t-butyl-4-hydroxybenzylphosphonic acid ethyl)calcium, tris-(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 2,4-2,4-bis[(octylthio)methyl]o-cresol, N,N'-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyl]hydrazine, tris(2,4-di-t-butylphenyl)phosphite, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)-benzotriazole, methyl-3-[3-t-butyl-5 -(2H-benzotriazol-2-yl)-4-hydroxyphenyl]propionate-polyethylene glycol (molecular weight about 300) condensate, hydroxyphenylbenzotriazole derivatives, 2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butylmalonic acid bis(1,2,2,6,6-pentamethyl-4-piperidyl), 2,4-di-t-butylphenyl-3,5-di-t-butyl-4-hydroxybenzoate, 4-methoxyphenol, 2,6-di-t-butyl-p-cresol, 1,4-dihydroxybenzene, etc. Among them, 1,4-dihydroxybenzene, 4-methoxyphenol, and 2,6-di-t-butyl-p-cresol are preferred, and 4-methoxyphenol and 2,6-di-t-butyl-p-cresol are more preferred. The phenol-based polymerization inhibitor may be used alone or in combination of two or more. In addition, commercially available products may be used as the phenol-based polymerization inhibitor, and examples thereof include p-methoxyphenol (manufactured by Wako Pure Chemical Industries, Ltd.), (hydroquinone monomethyl ether (manufactured by Tokyo Chemical Industry Co., Ltd.), and butylhydroxytoluene (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0046] In the present embodiment, the mixture is substantially free of hindered amine-based or phenol-based polymerization inhibitors. Here, "substantially free" means that the pigment, the pigment derivative, the pigment dispersant, and a part of the polymerizable compound are mixed and stirred to prepare a mixture, and the intentionally added polymerization inhibitor is excluded. Depending on the polymerizable compound used, a small amount of polymerization inhibitor, for example, about several ppm, may be present in the polymerizable compound. However, since it is unavoidably contained at the time of obtaining the material, in the present embodiment, such a case is not included in the intentionally added polymerization inhibitor. By not including a hindered amine-based or phenol-based polymerization inhibitor in the mixture, the pigment derivative in the mixture is easily adsorbed to the pigment, and precipitation due to the pigment derivative after long-term storage of the ink composition can be suppressed.

[0047] The amount of the hindered amine or phenol polymerization inhibitor in the pigment dispersion depends on the type and amount of the polymerizable compound, but it may not be included in the pigment dispersion. When the hindered amine or phenol polymerization inhibitor is included in the pigment dispersion, the amount is preferably 0.01 to 3 mass%, more preferably 0.05 to 2 mass%, based on the total amount of the pigment dispersion. If the amount of the hindered amine or phenol polymerization inhibitor is 0.01 mass% or more, radicals generated during the dispersion process or storage of the pigment dispersion can be sufficiently captured, and an increase in viscosity and gelation of the pigment dispersion can be further suppressed. On the other hand, if the amount of the hindered amine polymerization inhibitor is 3 mass% or less, the decrease in the polymerization reaction during energy ray irradiation can be suppressed, and an ink composition with excellent curability can be obtained.

[0048] The amount of the hindered amine or phenolic polymerization inhibitor in the ink composition is 0.01% by mass or more, preferably 0.1% by mass or more, and more preferably 0.2% by mass or more, based on the total amount of the ink composition. Also, the amount is 1% by mass or less, preferably 0.7% by mass or less, and more preferably 0.5% by mass or less, based on the total amount of the ink composition. If the amount is within the above lower limit, an increase in viscosity or gelation of the ink composition can be suppressed, and if the amount is within the above upper limit, a decrease in the polymerization reaction upon irradiation with energy rays can be suppressed, and an ink composition with excellent curability can be obtained.

[0049] The pigment dispersion or ink composition may contain, as a polymerization inhibitor other than the above hindered amine-based or phenol-based polymerization inhibitor, for example, another polymerization inhibitor such as a phosphorus-based antioxidant. The amount of these other polymerization inhibitors is not particularly limited, but is preferably 0.01 to 3 mass% based on the total amount of the pigment dispersion, and is preferably 0.01 to 1 mass% based on the total amount of the ink composition.

[0050] In preparing the mixture, a conventionally known mixer / stirrer can be used, specifically, for example, a disperser, a kneader, a planetary mixer, etc.

[0051] Next, in order to refine the pigment in the mixture prepared as described above, a dispersion step is performed in which the mixture is dispersed using a dispersion device filled with dispersion media. By dispersing a mixture with a high pigment concentration using a dispersion device filled with dispersion media, the pigment can be refined, and a pigment dispersion liquid in which the pigment is dispersed with a small particle size can be prepared. As the dispersion device, a conventionally known media-type dispersion device can be used. Specifically, for example, a paint conditioner, an attritor, a ball mill, a pin mill, a sand mill, a dyno mill, etc. can be mentioned. As the dispersion media, a conventionally known dispersion media such as glass beads, ceramic beads, and metal beads (including those whose surfaces are coated with resin) can be used. Among these, beads made of ceramics such as alumina, zirconia, and titania are preferred. The particle size of the dispersion media is preferably 0.05 to 2.0 mm, more preferably 0.3 to 1.6 mm.

[0052] A polymerization inhibitor may be added to the pigment dispersion liquid prepared in the step of preparing the pigment dispersion liquid. The amount of the polymerization inhibitor may be the total amount based on the total amount of the polymerization inhibitor added to the ink composition, and when a part of the polymerization inhibitor is added, the amount is preferably 10 to 90% by mass, more preferably 30 to 60% by mass, based on the total amount of the polymerization inhibitor added to the ink composition.

[0053] The dispersion time varies depending on the type and composition of the pigment and polymerizable compound, but is preferably 10 to 120 minutes. In addition, in order to prevent the pigment dispersion from becoming too hot during dispersion, it is preferable to prepare the pigment dispersion while cooling the dispersing device.

[0054] The viscosity of the pigment dispersion immediately after the dispersion step is preferably 15 to 100 mP·s at 25° C. In addition, the average dispersed particle size of the pigment immediately after the dispersion step is preferably 20 to 200 nm.

[0055] Next, a dilution step is carried out to prepare an ink composition by mixing and stirring the pigment dispersion liquid with a high pigment concentration prepared as described above, the remainder of the polymerizable compound used in the preparation of the mixture, other polymerizable compounds contained in the final ink composition such as monofunctional monomers, polyfunctional monomers, and oligomers, and a polymerization initiator. By such a dilution step, the pigment concentration in the ink composition can be reduced, and a low-viscosity ink composition suitable for the inkjet recording method can be obtained. In the dilution step for preparing the ink composition, a polymerization inhibitor may be further added.

[0056] The polymerizable compound used in the dilution step can be any of the above-mentioned polymerizable compounds. Among these, it is preferable to use a polymerizable compound containing a monofunctional monomer or a polyfunctional monomer as a main component. The total blend amount of the polymerizable compounds in the final composition of the ink composition is not particularly limited as long as the blend amount of the pigment can be ensured, but is preferably 60 to 95 mass % with respect to the total amount of the ink composition.

[0057] Examples of the polymerization initiator include acylphosphine oxides, α-aminoalkylphenones, thioxanthones, aryl alkyl ketones, oxime ketones, acyl phosphonates, S-phenyl thiobenzoates, titanocenes, aromatic ketones, benzils, quinone derivatives, and ketocoumarins. Among these, at least one polymerization initiator selected from the group consisting of acylphosphine oxides, α-aminoalkylphenones, and thioxanthones, which can initiate polymerization with low energy when used together with the polymerizable compound, is preferred, and acylphosphine oxides or a mixture of α-aminoalkylphenones and thioxanthones is more preferred. The polymerization initiator is preferably a photopolymerization initiator, and more preferably a photoradical polymerization initiator.

[0058] Specific examples of acylphosphine oxides include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,3,5,6-tetramethylbenzoyldiphenylphosphine oxide, 2,6-dimethylbenzoyldiphenylphosphine oxide, 4-methylbenzoyldiphenylphosphine oxide, 4-ethylbenzoyldiphenylphosphine oxide, 4-isopropylbenzoyldiphenylphosphine oxide, 1-methylcyclohexanoylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2,4,6-trimethylbenzoylphenylphosphinic acid isopropyl ester, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, etc. These may be used alone or in combination. Commercially available acylphosphine oxides include Omnirad TPO manufactured by BASF.

[0059] Specific examples of α-aminoalkylphenones include 2-methyl-1[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1, and 2-methyl-1-[4-(methoxythio)-phenyl]-2-morpholinopropan-2-one. These may be used alone or in combination. Commercially available α-aminoalkylphenones include IRGACURE 369 and IRGACURE 907 manufactured by IGM Resins BV.

[0060] Specific examples of thioxanthones include thioxanthone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, and 1-chloro-4-propoxythioxanthone. These may be used alone or in combination. Commercially available thioxanthones include KAYACURE DETX-S manufactured by Nippon Kayaku Co., Ltd. and Chivacure ITX manufactured by Double Bond Chemical Co., Ltd.

[0061] The amount of the polymerization initiator in the final composition of the ink composition depends on the type and amount of the polymerizable compound, but is preferably 2 to 15% by mass in total with respect to the total amount of the ink composition. If the amount of the polymerization initiator is 2% by mass or more, an ink composition having excellent curability and adhesion can be obtained even with low-energy irradiation. On the other hand, if the amount of the polymerization initiator is 15% by mass or less, the remaining unreacted components can be suppressed.

[0062] In the dilution step, the above-mentioned hindered amine-based or phenol-based polymerization inhibitor may be added. By adding a hindered amine-based or phenol-based polymerization inhibitor in the dilution step, the storage stability of the ink composition can be further improved.

[0063] In the dilution step, additives such as a surface conditioner, a surfactant, a leveling agent, an antifoaming agent, a pH adjuster, a bactericide, a preservative, a deodorizer, a charge control agent, a wetting agent, a fragrance, a chain transfer agent, and a sensitizer may be further added as necessary for the purpose of improving other properties.

[0064] The mixer used in the dilution step may be the same as the mixer used in the mixing step.

[0065] The average particle size of the pigment in the ink composition produced as described above is preferably 20 to 200 nm, more preferably 50 to 160 nm. In the pigment dispersion of the present embodiment, the pigment is highly dispersed and has excellent dispersion stability even at a high pigment concentration, so that an ink composition in which fine particles of the pigment as described above are dispersed can be obtained. If the average particle size of the dispersion is less than 20 nm, the particles are too fine, and the weather resistance of the printed matter tends to decrease. On the other hand, if the average particle size of the dispersion is more than 200 nm, the fineness of the printed matter tends to decrease.

[0066] Furthermore, the pigment dispersion of the present embodiment shows little increase in viscosity even when dispersion is performed with high dispersion energy, and an ink composition having a low viscosity of about 4 to 23 mPa·s at 25° C. can be obtained by producing the ink composition. The ink composition of the present embodiment has low viscosity even without heating, and further has good pigment dispersion stability, with little increase in viscosity or gelation during storage or use, and good storage stability without problems such as pigment settling. Therefore, even if the ink composition does not actually contain a diluting solvent such as an organic solvent, stable ejection can be obtained at room temperature without heating the ink in the inkjet recording method.

[0067] As described above, the ink composition of the present embodiment does not need to contain a dilution solvent, but when an industrial product is used, for example, the ink composition may inevitably contain a dilution solvent. The amount of such unavoidably mixed dilution solvent is usually 3 mass % or less relative to the total amount of the ink composition, and it is preferable that the ink composition is substantially free of dilution solvent.

[0068] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" means "parts by mass." EXAMPLES

[0069] The components of the inks used in the examples and comparative examples are shown in the following Table 1. The compositions shown in Tables 2 and 3 are the same as the abbreviations shown in Table 1.

[0070] [Table 1]

[0071] <Preparation of pigment dispersion> The pigment, pigment derivative, pigment dispersant, polymerizable compound, and polymerization inhibitor were weighed out in the amounts shown in Table 2 and mixed and stirred in a plastic bottle to prepare a mixture. 100 parts of zirconia beads (diameter: 0.3 mm) were added to this mixture and dispersed for 2 hours using a paint conditioner (manufactured by Toyo Seiki Co., Ltd.). After dispersion, the contents were suction filtered using a glass filter (manufactured by Kiriyama Seisakusho Co., Ltd.) to prepare a pigment dispersion.

[0072] [Table 2]

[0073] <Ink manufacturing> Next, each pigment dispersion immediately after preparation as described above was used to dilute the ink so that the final composition was the ink composition shown in Table 3 below, and each ink was produced. The ink composition shown in Table 3 is the ink composition when diluted with 10 parts of the pigment dispersion A-4 described in Table 2. In other examples and comparative examples, 10 parts of each pigment dispersion was used in the same manner, and the components other than the pigment, pigment derivative, and pigment dispersant were prepared so as to have the composition shown in Table 3. In Examples 2 and 4, the pigment dispersion immediately after preparation was used to which a polymerization inhibitor had been added in advance, and ink was produced. The ink using BT-617-D as the pigment corresponds to a cyan ink, and the ink using #1000 as the pigment corresponds to a black ink.

[0074] [Table 3]

[0075] Immediately after production, each of the inks produced as described above was evaluated for the viscosity of the ink, the average dispersed particle size of the pigment in the ink, and the precipitation of the pigment derivative in the ink as described below. In addition, the storage stability of each of the produced inks was evaluated as follows.

[0076] [Ink Viscosity] The viscosity of the ink immediately after production was measured using a TV25 type viscometer (manufactured by Toki Sangyo Co., Ltd.) under conditions of 25° C. and a cone rotation speed of 20 rpm.

[0077] [Average dispersed particle size of pigment in ink] The average dispersed particle size of the pigment in the ink immediately after production was measured using a particle size distribution measuring device FPER-1000 (manufactured by Otsuka Electronics Co., Ltd.).

[0078] [Precipitation of pigment derivatives in ink] A slide was prepared using the ink immediately after production, and the presence or absence of precipitation was observed using an optical microscope at 500x magnification with transmitted light, and evaluated according to the following criteria. ○: No precipitate △: Precipitates confirmed in 1 out of 10 fields of view ×: Precipitates confirmed in 2 or more of 10 fields of view

[0079] [Storage stability of ink] The ink immediately after production was stored at 60°C for 30 days, and the viscosity of the ink after storage was measured in the same manner as above. The ink was observed for viscosity change and the presence or absence of gelation, and the storage stability was evaluated according to the following criteria. ○: Viscosity increase of less than 5% △: Viscosity increase of 5 or more, less than 10% ×: Viscosity increase of 10% or more In addition, the average dispersed particle diameter of the pigment in the ink after storage in the same manner was measured, and the storage stability was evaluated according to the following criteria. ○: Less than 10% increase in average dispersed particle size ×: Increase in average dispersed particle size of 10% or more

[0080] [Precipitation of pigment derivatives in ink] The ink immediately after production was stored at 10°C for 30 days. After storage, a specimen was prepared using the ink and observed for the presence or absence of precipitation using an optical microscope at 500x magnification using transmitted light. The storage stability was evaluated according to the following criteria. ○: No precipitate △: Precipitates confirmed in 1 out of 10 fields of view ×: Precipitates confirmed in 2 or more of 10 fields of view

[0081] The evaluation results are shown in Tables 4 and 5.

[0082] [Table 4]

[0083] [Table 5]

[0084] Referring to Tables 4 and 5, it was confirmed that the ink composition produced by the production method of the present invention had small changes in ink viscosity before and after storage, and small changes in the average dispersed particle size of the pigment in the ink, and that precipitation of the pigment derivative was suppressed both initially and after storage, thereby demonstrating excellent storage stability.

Claims

1. A method for producing an active energy ray-curable ink composition containing a polymerization inhibitor, comprising the steps of: A step of mixing and stirring a pigment, a pigment dispersant, a pigment derivative, and a polymerizable compound to prepare a mixture; preparing a pigment dispersion by dispersing the mixture in a dispersion medium; preparing the ink composition by mixing and stirring the pigment dispersion, the polymerizable compound, and a polymerization initiator; The method for producing an active energy ray-curable ink composition, wherein the mixture is prepared without further containing a polymerization inhibitor.

2. The method for producing an active energy ray-curable ink composition according to claim 1 , wherein the polymerization inhibitor is at least one selected from the group consisting of hindered amine-based polymerization inhibitors and phenol-based polymerization inhibitors.

3. The method for producing an active energy ray-curable ink composition according to claim 2 , wherein the polymerization inhibitor is a hindered amine-based polymerization inhibitor.

4. The method for producing an active energy ray-curable ink composition according to claim 3, wherein the polymerization inhibitor is a hindered amine-based polymerization inhibitor having an N-hydroxy-2,2,6,6-tetramethylpiperidinyl group.

5. The method for producing an active energy ray-curable ink composition according to claim 1 , wherein the pigment is a cyan or black pigment.

6. The method for producing an active energy ray-curable ink composition according to claim 1 , wherein the pigment derivative is a phthalocyanine derivative.

7. The method for producing an active energy ray-curable ink composition according to claim 1, wherein the blending amount of the pigment derivative is 1 to 15 mass % with respect to the blending amount of the pigment.

8. The method for producing an active energy ray-curable ink composition according to claim 1, wherein the blending amount of the pigment derivative is 1 to 20 mass % with respect to the blending amount of the pigment dispersant.

9. The method for producing an active energy ray-curable ink composition according to claim 1 , further comprising the step of adding the polymerization inhibitor to the pigment dispersion liquid.

10. The method for producing an active energy ray-curable ink composition according to claim 1 , further comprising the step of adding the polymerization inhibitor in the step of preparing the ink composition.

11. The method according to claim 1 , wherein the ink composition is an ink-jet ink composition.

Citation Information

Patent Citations

  • Ink composition, inkjet recording method and printed matter

    JP2010070665A

  • Active ray-curable inkjet ink and inkjet image forming method

    JP2017128665A

  • Inkjet ink composition and image formation method

    WO2018131400A1

  • Liquid composition for inkjet and inkjet recording method

    WO2018159236A1

  • Method for producing energy ray-curable inkjet ink composition, and energy ray-curable inkjet ink composition

    JP2010189586A