Laminated molding and laminated molding method

The new additive manufacturing method separates molten pools into iron-based and oxygen-based phases during solidification, addressing the challenge of producing multi-phase structures without molds, enabling efficient production of laminated products with controlled phase thickness.

JP2024137455APending Publication Date: 2024-10-07KK TOYOTA CHUO KENKYUSHO +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023048982
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing additive manufacturing methods, particularly directed energy deposition (DED) and powder bed fusion (PBF), struggle to produce shaped objects with specific multi-phase structures, such as soft magnetic objects made of isotropic crystal grains, without the need for special molds or large machine tools.

Method used

A new additive manufacturing method that separates a molten pool into an iron-based liquid phase and an oxygen-based liquid phase during solidification, allowing for the formation of a multi-phase structure with an oxygen-based solid phase on an iron-based solid phase, enabling control over the thickness of the oxygen-based solid phase.

Benefits of technology

Enables efficient production of laminated products with controlled multi-phase structures, suitable for applications like soft magnetic members, by leveraging the difference in specific gravity and liquidus temperatures of the separated phases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137455000001_ABST
    Figure 2024137455000001_ABST
Patent Text Reader

Abstract

To provide a laminated molding method capable of efficiently obtaining a laminate molding in which an oxygen base solid phase is formed on an iron base solid phase.SOLUTION: In a laminated molding method, a molten pool formed by dissolving raw material powders on a substrate by irradiation with a high energy beam is solidified to obtain a molded product. The molten pool includes a separated iron base liquid phase and an oxygen base liquid phase. The molded product has an oxygen base solid phase formed on an iron base solid phase. The laminate molding method is performed by, for example, a directional energy deposition method. The oxygen base solid phase is an oxide layer containing, for example, Fe2SiO4, and may further contain Cr2FeO4. Elements liable to form oxides (Mn, Al, Mg, Ti, Zr) are included in the oxygen base solid phase, and Ni, Mo, and the like are included in the iron base solid phase.SELECTED DRAWING: Figure 2B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an additive manufacturing method and the like. [Background technology]

[0002] Unlike conventional subtractive processes (cutting, grinding, shearing, etc.) and molding processes (casting, forging, pressing, etc.), additive manufacturing (AM) is attracting attention as it produces desired objects without requiring dedicated molds or large machine tools. Additive manufacturing (AM) involves repeated layering, which produces objects (laminated objects) that were difficult to produce using conventional manufacturing methods.

[0003] Additive processing is broadly classified into seven types (ASTM standard): Directed Energy Deposition (DED), Powder Bed Fusion (PBF), Binder Jetting, Material Jetting, Material Extrusion, VAT Photopolymerization, and Sheet Lamination.

[0004] Of these, DED and PBF can produce practical objects made of metal or ceramic. Both DED and PBF have in common the fact that they irradiate a high-energy beam (a heat source such as a laser or electron beam) and melt and solidify (bond) raw material powder (including mixed powders) to produce a molded object. DED is easier to reduce the amount of raw material powder used and to expand the degree of freedom in molding than PBF. Many proposals have been made regarding this type of additive manufacturing, and for example, there are related descriptions in the following literature. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Kanamaru et al., Proceedings of the 2021 Autumn Meeting of the Japan Society of Precision Engineering, (2021) p. 326. Summary of the Invention [Problem to be solved by the invention]

[0006] Non-Patent Document 1 describes FeSi and FeCoV objects fabricated by DED, but does not disclose specific component compositions and only covers soft magnetic objects made of isotropic crystal grains.

[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide a new additive manufacturing method and the like. [Means for solving the problem]

[0008] As a result of intensive research, the inventors have succeeded in obtaining an additive manufacturing object by separating the molten pool into liquid phases and solidifying the molten pool while maintaining that state. By expanding on this result, the inventors have completed the present invention, which will be described below.

[0009] Additive manufacturing method (1) The present invention is an additive manufacturing method in which a raw material powder is melted on a substrate by irradiating it with a high-energy beam, and the resulting molten pool is solidified to obtain a molded object. The molten pool contains separated iron-based liquid phase and oxygen-based liquid phase, and the molded object has an oxygen-based solid phase formed on an iron-based solid phase.

[0010] (2) According to the additive manufacturing method (also simply referred to as the "modeling method") of the present invention, it is possible to efficiently manufacture an additively manufactured object (also simply referred to as the "modeled object") having a multi-phase structure in which an oxygen-based solid phase is formed on an iron-based solid phase. For example, even by simply scanning a high-energy beam along one line, it is possible to obtain an additively manufactured object in which an oxygen-based solid phase is formed on an iron-based solid phase. Furthermore, according to the modeling method of the present invention, it is also possible to control the thickness of the oxygen-based solid phase (such as an oxide layer) formed on the surface side of the modeled object.

[0011] The reason why such objects are obtained is thought to be as follows: The molten pool formed by melting the raw material powder on the substrate is separated into an iron-based liquid phase and an oxygen-based liquid phase. At this time, the difference in specific gravity (density) makes it easy for the oxygen-based liquid phase to move (float) above the iron-based liquid phase.

[0012] In addition, the separated liquid phases have different liquidus and solidus temperatures and do not solidify at the same time. Therefore, as the temperature of the molten pool decreases, the low-density oxygen-based liquid phase moves onto the high-density iron-based liquid phase, and solidification proceeds in that state. In this way, a molded object is obtained in which the low-density oxygen-based solid phase is formed on the high-density iron-based solid phase.

[0013] "Layered objects" The present invention can also be understood as an additive manufacturing method. For example, the present invention may be an additive manufacturing method having an oxygen-based solid phase formed on an iron-based solid phase. Such an additive manufacturing method can be obtained by the additive manufacturing method described above.

[0014] Powder for additive manufacturing The present invention can also be understood as a raw material powder (powder for additive manufacturing) to be used for additive manufacturing to obtain the above-mentioned additive manufactured product. The powder for additive manufacturing (referred to as "raw material powder" as appropriate) may be a single type of alloy powder or a mixed powder consisting of multiple types of powders.

[0015] The component composition or blended composition of the raw material powder does not necessarily have to be the same as the overall composition of the molded object (for example, the combined composition of the iron-based solid phase and the oxygen-based solid phase). Not only the component elements of the raw material powder but also small amounts of the component elements of the main body dissolve into the molten pool, and the molten pool solidifies after the component elements of both sides are mixed together. For this reason, the overall composition of the molded object does not necessarily match the overall composition of the raw material powder. The overall composition of the raw material powder may be adjusted in advance, taking such a viewpoint into consideration.

[0016] "others" (1) In this specification, "X group" and the like mean that the X element is contained in an atomic ratio (at% / simply referred to as "%) of the whole object at 50% or more, more than 50%, 55% or more, 60% or more, or 65%. The object may be in a liquid or solid phase, and may be, for example, an alloy, a compound, a composite material, and the like. Compounds include oxides, ceramics, intermetallic compounds, and the like.

[0017] The iron-based liquid phase solidifies to an iron-based solid phase, and the oxygen-based liquid phase solidifies to an oxygen-based solid phase. The respective component compositions of the corresponding liquid and solid phases are essentially substantially the same, but may vary somewhat after solidification.

[0018] (2) The "main body" may be any material, shape, manufacturing process, processing stage, etc., as long as it is a base that can melt the raw material powder and form a molten pool. The main body may be, for example, an iron base material. The iron base material may be pure iron, an iron alloy (carbon steel, alloy steel, castings, etc.), a composite material with dispersed particles in an iron-based matrix, etc. The main body may be, for example, a plate, a block, a component of a desired shape, etc. The main body may be, for example, a raw material, an intermediate material, a final product, etc. The main body may be, for example, an additive manufacturing product, a melt-cast material (wrought material, castings, etc.), a sintered material, etc.

[0019] When the main body is an additively manufactured article, the iron-based solid phase and the oxygen-based solid phase and the main body may be formed consecutively by the same method, or may be formed separately by different methods.

[0020] (3) The "high energy beam" may be any of a laser beam, an electron beam, a plasma arc, etc., so long as it is a heat source that melts the powder. The additive manufacturing method is performed, for example, by directed energy deposition (DED) or powder bed fusion (PBF). With DED, an iron-based solid phase or an oxygen-based solid phase can be efficiently formed at a desired location (e.g., locally). For convenience, this specification will be described by taking up L-DED (LMD), which uses a laser beam, a typical heat source.

[0021] The trajectory and number of times of scanning of the high energy beam are not important. As used herein, the additive manufacturing may be a single line scan or a single layer stack in the same region, as long as an oxygen-based solid phase is formed on an iron-based solid phase. Of course, multiple layers may be used.

[0022] (4) Unless otherwise specified, "x to y" in this specification includes a lower limit value x and an upper limit value y. Any numerical value included in the various numerical values ​​or numerical ranges described in this specification may be used as a new lower limit value or upper limit value to create a new range such as "a to b". In addition, "x to y μm" in this specification means x μm to y μm. The same applies to other units. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a schematic diagram showing additive manufacturing by LMD. [Figure 2A] 1 shows a photograph of the appearance of the molded object of Sample 1 and a digital microscope image of its cross section. [Figure 2B] The following are SEM and EDX images of the cross section (near the interface). [Figure 3A] Photographs showing the appearance of the modeling layer surfaces of Samples 1 to 3. [Figure 3B] These are SEM images of their cross sections (near the interface). [Figure 4] These are digital microscope images of the cross sections (near the interface) of Sample 2 and Sample 4. [Figure 5A] 1 is a phase diagram (an example) obtained by thermodynamic calculation. [Figure 5B] 1 is a temperature-phase fraction diagram (an example) obtained by thermodynamic calculation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] One or more components selected arbitrarily from the present specification may be added to the components of the present invention. The contents described in this specification may be appropriately applied to any of an additive manufacturing object, an additive manufacturing method, and a powder for additive manufacturing.

[0025] Oxygen-based phase The oxygen-based liquid phase or the oxygen-based solid phase (collectively referred to as the "oxygen-based phase") may contain, for example, Fe and Si. In the oxygen-based phase, for example, Fe2SiO4 (fayalite) may be produced. The electrical resistivity (10 7 The linear expansion coefficient of Fe2SiO4 (approximately 10×10 -6 / K) is the linear expansion coefficient of the iron base material (approximately 14×10 -6 / K).

[0026] The oxygen-based phase may contain one or more of Cr, Al, Mn, Mg, Ca, Ti, etc. Such metal elements are easily incorporated into the oxygen-based phase and form oxides. For example, Cr appears in the oxygen-based phase as Cr2FeO4. Cr2FeO4 has a larger linear expansion coefficient (approximately 12×10) than Fe2SiO4. -6 / K, at 500K) and a higher electrical resistivity than FeO (10 1 The metal element may be supplied from the raw material powder or from the main body side.

[0027] The composition of the oxygen-based phase may contain, for example, 15-35% or 20-30% Fe and 5-20% or 8-15% Si, with the whole being 100%. In the case where Cr is contained, for example, 1-15% or 3-10% Cr may be contained. Unless otherwise specified, the composition of the composition in this specification is an atomic ratio (at%) and is simply indicated by "%" or a numerical value.

[0028] Depending on the amount of Fe supplied, FeO, Fe, etc., other than Fe2SiO4, may appear in the oxygen-based phase. However, Ni, Mo, etc. are hardly contained in the oxygen-based phase. For example, if the entire oxygen-based phase is taken as 100%, the content of Ni and Mo is less than 0.1% and less than 0.05%, respectively.

[0029] Iron Phase The iron-based solid phase or iron-based liquid phase (both are collectively referred to as the "iron-based phase") may contain modifier elements and unavoidable elements (including impurities) other than Fe. Such elements include Si, Mn, Al, Mg, Ti, Zr, O, C, etc. The contents of these elements, assuming the entire iron-based phase to be 100%, are, for example, less than 3%, 2% or less, or 1% or less for Si, Mn, Al, Mg, Ti, Zr, etc.; for example, less than 5%, 3% or less, or 1% or less for O; and less than 2%, 1.5% or less, or 1% or less for C.

[0030] The entire iron-based phase, taken as 100%, may contain, for example, 1 to 40%, 5 to 30%, or 10 to 20% Ni and / or 1 to 20%, 5 to 15%, or 7 to 13% Mo. Ni and Mo contribute to solution strengthening of the iron-based solid phase, improvement of corrosion resistance, control of linear expansion coefficient, etc.

[0031] As an example, the composition of the iron-based phase may be, taking the whole as 100%, e.g., Si: less than 3%, O: less than 5%, C: less than 2%, Mn: less than 3%, Al: less than 3%, Mg: less than 3%, Ti: less than 3%, Zr: less than 3%, Ni: 0-40%, Mo: 0-20%, and the balance: Fe.

[0032] 《Raw material powder》 The raw material powder used in additive manufacturing can be of any type, manufacturing process, or form (shape, size) as long as it becomes a substantially uniform liquid phase in the irradiation area (molten pool) of the high-energy beam. For example, it can be a single type of alloy powder, a mixed powder or granulated powder made of multiple types of powders, or an atomized powder or pulverized powder.

[0033] The particle size of the raw material powder may be adjusted or selected as appropriate. For example, the particle size of the raw material powder is 5 to 150 μm or 20 to 105 μm. The particle size in this specification is, for example, specified by a sieving method in which a sieve of a predetermined mesh size is used for classification. A powder with a particle size of "x to y" is composed of particles that do not pass through a sieve with a sieve opening of x (μm) but pass through a sieve with a sieve opening of y (μm). "Less than y" is composed of particles that pass through a sieve with a sieve opening of y (μm).

[0034] The overall composition of the raw material powder is adjusted so that a molten pool separated into two liquid phases is formed on the substrate. For example, the raw material powder may contain, in addition to O, 30-99%, 50-95%, or 60-85% Fe, 0.1-20%, 0.5-15%, or 2-12% Si, with the entire raw material powder being taken as 100%. It may also contain 0.1-25%, 0.5-15%, or 2-10% Cr, 1-40%, 2-25%, or 3-15% Ni, and 1-20%, 2-15%, or 3-12% Mo. Cr, Ni, Mo, etc. may be contained in only one type or in multiple types.

[0035] The raw material powder may further contain one or more of Al, Mn, Mg, Ca, Ti, etc. in a total amount of 1 to 30%, 3 to 25%, or 7 to 20%.

[0036] Two separate oxygen-based and iron-based phases are likely to be generated when the atomic ratio (Fe / Si) of Fe to Si contained in the entire raw material powder is, for example, 2.5 to 60, 3 to 50, 3.5 to 45, 4 to 40, or 5 to 35. When Cr is contained, (Fe+Cr) / Si may be, for example, 3 to 65, 3.5 to 55, 4 to 50, 5 to 45, or 6 to 40.

[0037] "Layered objects" (1) The form (shape, size), purpose, etc. of the molded object are not important. The thickness, range, arrangement, etc. of the oxygen-based solid phase and the iron-based solid phase are appropriately adjusted and selected. The number of layers during additive manufacturing is also not important. The thickness of the oxygen-based solid phase (e.g., oxide layer) is, for example, 0.5 to 100 μm, 1 to 50 μm, or 10 to 20 μm.

[0038] The oxygen-based solid phase can be, for example, an electrical insulating layer or a corrosion-resistant layer. Its electrical resistivity is, for example, 1 to 10 7 Ωcm or 10 1 ~10 6 The high electrical resistivity oxygen-based solid phase can act as a highly corrosion-resistant layer to prevent the formation of a local battery on the main body (iron substrate).

[0039] (2) The object is, for example, a soft magnetic member (yoke, core, etc.) used in an alternating magnetic field. Specifically, it is all or part of a rotor or stator of an electric motor (including a generator), an iron core for a transformer, etc. The oxygen-based solid phase (layer) formed in such an object can contribute to the formation of an efficient magnetic circuit, the improvement of the efficiency of electromagnetic equipment, the reduction of iron loss, etc. EXAMPLES

[0040] Various samples (layer-by-layer manufactured objects) were manufactured by forming layers on a main body using LMD (L-DED), and their structures were evaluated. The present invention will be described in more detail based on these specific examples.

[0041] <Sample Preparation> (1) Raw material powder Pure Fe powder, pure Cr powder (-63μm), and oxide powder (SiO2 powder: (D50) 100μm, FeO powder: (D50) 30μm) were prepared. The particle size of each powder was adjusted (classified) to 45-300μm.

[0042] Each powder was weighed and mixed to the desired composition (balance: O) shown below to prepare a mixed powder, which was then used for additive manufacturing. The overall composition of the raw powder was set in consideration of the theoretical composition of Fe2SiO4 (28.6Fe-14.3Si-O:Fe / Si=2). Sample 1: 29.7Fe-8.5Si-15Cr-O (Fe / Si=3.5) Sample 2: 46.2Fe-6.5Si-11.5Cr-O (Fe / Si=7.1) Sample 3: 79.6Fe-2.5Si-4.4Cr-O (Fe / Si=31.8) Sample 4: 35Fe-10Si-O (Fe / Si=3.5) Unless otherwise specified, the chemical compositions (component compositions) shown in this example are atomic ratios (at%) relative to the entire target (powder, iron base material, composite material, modeling layer (oxide layer), etc.) and are simply indicated by "%" or numerical values.

[0043] (2) Additive Manufacturing The raw powder (mixed powder) placed in the powder feeder (powder box) of the LMD device (laser processing test machine manufactured by Enshu Co., Ltd.) was supplied to the powder nozzle by carrier gas (Ar).

[0044] Using this LMD device, a modeling layer (12 mm x 15 mm x t 0.4 mm) was formed on the outermost surface of a main body (SS400 steel plate (JIS) / 15 x 15 x t 5 mm) in an air atmosphere at room temperature. This process is shown in schematic form in Figure 1. The chemical composition of SS400 (iron substrate) is, for example, P≦0.05 mass%, S≦0.05 mass%, C: 0.15-0.2 mass%, and the remainder: Fe.

[0045] The irradiation conditions for the fiber laser (YLS-4000 manufactured by IPG Corporation / laser wavelength: 1070 nm) were: output: 800 W, beam diameter (spot diameter): 2.5 mm, scanning speed: 800-1600 mm / min. Powder supply amount: 0.06 g / s, scanning pitch (x direction): 0.75-1.5 mm, carrier gas (Ar) flow rate: 10 L / min. The number of stacked modeling layers was one (or one line). Samples 1-4 were produced in this way.

[0046] "observation" (1) Cross section As shown in Fig. 2A, the cross section of the molded product of Sample 1 was observed with a digital microscope (manufactured by Keyence Corporation). As is clear from Fig. 2A, the molded layer was not peeled off from the main body and was formed in close contact with the main body.

[0047] (2) Modeling layer For sample 1, the cross section near the interface between the modeling layer and the main body was observed using a scanning electron microscope (SEM). In addition, the elements that make up the interface were analyzed using an energy dispersive X-ray analyzer (EDX) attached to the SEM. The SEM image and EDX image (element mapping image) obtained in this way are shown together in Figure 2B.

[0048] As is clear from FIG. 2B, the modeling layer had a thin oxide layer (oxygen-based solid phase) formed on the iron base layer (iron-based solid phase).

[0049] It was also found that the iron base layer contains almost no O, Si, or Cr, and is formed almost integrally with the remelted and solidified base material.

[0050] For Samples 1 to 3, the appearance of the modeling layer surface is shown in FIG. 3A, and a digital microscope image of the cross section near the interface is shown in FIG. 3B.

[0051] As is clear from Figure 3A, the modeling layers of Samples 2 and 3 were formed in close contact with the main body without peeling off, similar to Sample 1. As is clear from Figure 3B, the thickness of the oxide layer (oxygen-based solid phase) could be controlled by adjusting the composition of the raw material powder. For example, the oxide layer became thinner as the Fe content of the raw material powder increased or the Si content decreased (as Fe / Si increased).

[0052] The same can be seen from Figure 4, which shows digital microscope images of cross sections near the interface of the modeling layer surface for Sample 2 and Sample 4. As is clear from Figure 4, it was also found that a fairly thin oxide layer is formed on the raised iron base layer due to an increase in Fe, a decrease in Si, the inclusion of Cr, etc. In this way, it was confirmed that the thickness (maximum length) of the oxygen-based solid phase (oxide layer) can be controlled to, for example, 1 to 1000 μm, 5 to 500 μm, or 10 to 100 μm.

[0053] 《Consideration》 (1) Two liquid phase separation Thermodynamic calculations (equilibrium state) were performed using thermodynamic analysis software (Thermo-Calc 2021b / Oxide system database TCOX11) for each iron alloy (raw powder) with the overall composition shown in Table 1. The overall composition shown in Table 1 was assumed to be a mixture of a base powder consisting of 32.9Fe-9.4Si-6Cr-O and additive powders in a ratio of (1-X):X (atomic ratio: 0≦X<1).

[0054] Table 2 shows the phases formed when the iron alloy of each sample reached 1700°C. In each case, the appearance of two liquid phases was confirmed. The first liquid phase was an iron-based liquid phase with Fe as the main component, and the second liquid phase was an oxygen-based liquid phase with O as the main component. The ratio of the first and second liquid phases was shown as a molar fraction. The liquid phase composition was shown for each liquid phase as the atomic ratio of the elements contained in the whole (the whole is 1).

[0055] As is clear from a comparison between Tables 1 and 2, an increase in Fe or a decrease in Si contained in the raw material powder increased the first liquid phase (iron-based liquid phase) and decreased the second liquid phase (oxygen-based liquid phase).

[0056] Even when the molar fraction of the first and second liquid phases changed, Si, O, and Cr were contained in the second liquid phase and were hardly contained in the first liquid phase. Conversely, Ni and Mo were almost entirely contained in the first liquid phase and were not contained in the second liquid phase. In this way, elements other than Fe had a high affinity for one of the liquid phases. This is also thought to affect the separation of the two liquid phases in the molten pool.

[0057] (2) Phase diagram According to the above thermodynamic calculation, (32.9Fe-9.4Si-6Cr-O) (1-X) +100Fe X The phase equilibrium diagram obtained for (0≦X<1) is shown in FIG. 5A. Sample 22 (addition coefficient X=0.5) shown in Table 1 is illustrated in FIG. 5A.

[0058] As is clear from Figure 5A, in the wide range of Fe: 30-98%, Liquid 1: first liquid phase (iron-based liquid phase) and Liquid 2: second liquid phase (oxygen-based liquid phase) appear stably. When these solidify, Liquid 1 eventually becomes αFe (iron-based solid phase) and Liquid 2 becomes Cr2FeO4+Fe2SiO4 (oxygen-based solid phase).

[0059] (3) Temperature-phase fraction diagram The temperature-equilibrium phase fraction diagram for 66.5Fe-4.7Si-3Cr-O (sample 22) obtained from the above-mentioned thermodynamic calculation is shown in Figure 5B. As is clear from Figure 5B, at temperatures above 1700°C, a two-liquid phase separation state was obtained: Liquid 1: first liquid phase (iron-based liquid phase) and Liquid 2: second liquid phase (oxygen-based liquid phase), and it was found that Liquid 2 was above Liquid 1 due to the difference in specific gravity.

[0060] By cooling from this two-liquid phase separation state, Liquid 1 became almost entirely solid (δFe) at approximately 1530°C or less, and as the temperature decreased, it underwent a solid-liquid phase transformation in the order δFe → σFe → αFe. Meanwhile, Liquid 2 gradually crystallized Cr2FeO4 at approximately 1630°C or less, entering a solid-liquid coexistence state, and the remainder of Liquid 2 became Fe2SiO4 at approximately 1200°C.

[0061] From the above, it was confirmed that as the cooling process progresses from a two-liquid phase separation state, a two-solid-phase laminated object is obtained in which an oxygen-based solid phase is formed on an iron-based solid phase.

[0062] [Table 1]

[0063] [Table 2]

Claims

1. A layered manufacturing method for obtaining a molded object by melting a raw material powder on a substrate by irradiating the substrate with a high-energy beam and solidifying the resulting molten pool, comprising the steps of: the molten pool includes a separate iron-based liquid phase and an oxygen-based liquid phase; The object has an oxygen-based solid phase formed on an iron-based solid phase.

2. The additive manufacturing method according to claim 1 , wherein the oxygen-based solid phase contains at least Fe and Si.

3. The oxygen-based solid phase is Fe 2 SiO 4 The additive manufacturing method according to claim 2 ,

4. The additive manufacturing method according to claim 2 , wherein the oxygen-based solid phase contains at least one of Cr, Al, Mn, Mg, Ca, and Ti.

5. The additive manufacturing method according to claim 2 , wherein the oxygen-based solid phase contains less than 0.1 at % of both Ni and Mo, with the entire solid phase being taken as 100 at % (simply referred to as "%").

6. The raw material powder contains Fe, Si, and O, The additive manufacturing method according to claim 1 , wherein the iron-based solid phase has a Si content of less than 3% and an O content of less than 5%, with the entire iron-based solid phase being taken as 100 at % (simply referred to as "%").

7. The additive manufacturing method according to claim 6 , wherein the iron-based solid phase contains less than 3% of any of Mn, Al, Mg, Ti and Zr.

8. The additive manufacturing method according to claim 6 , wherein the iron-based solid phase has a C content of less than 2%.

9. The additive manufacturing method according to claim 6, wherein the iron-based solid phase contains 0.1 to 40% Ni and / or 0.1 to 20% Mo.

10. The additive manufacturing method according to claim 1 , which is performed by directed energy deposition.

11. The layered manufacturing method according to any one of claims 1 to 10, wherein the raw material powder contains 30 to 99 at % Fe relative to the entire powder.

12. An additive manufacturing object having an oxygen-based solid phase formed on an iron-based solid phase.

13. The oxygen-based solid phase is Fe 2 SiO 4 The additive manufacturing object according to claim 12 .

14. The oxygen-based solid phase further comprises Cr 2 FeO 4 The additive manufacturing method according to claim 13 .

15. The layered object according to claim 12 , wherein the iron-based solid phase satisfies the following composition, with the whole of the iron-based solid phase being 100 at % (simply referred to as "%"): Si: less than 3%, O: less than 5%, C: less than 2%, Mn: less than 3%, Al: less than 3%, Mg: less than 3%, Ti: less than 3%, Zr: less than 3%