Lithium secondary battery

A non-aqueous electrolyte with specific additives and limited ethylene carbonate stabilizes lithium nickel manganese oxide electrodes, addressing structural collapse and metal elution issues, thereby improving battery stability and lifespan under high voltage and temperature conditions.

JP2024137655AActive Publication Date: 2024-10-07SAMSUNG SDI CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023197388
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2023-11-21
Publication Date
2024-10-07
Estimated Expiration
2043-11-21

AI Technical Summary

Technical Problem

Lithium nickel manganese oxide-based positive electrodes suffer from structural collapse and transition metal elution under high voltage and high temperature conditions, leading to gas generation, increased resistance, and reduced battery life.

Method used

A non-aqueous electrolyte solution containing specific additives and a non-aqueous organic solvent with limited ethylene carbonate content is used in combination with a lithium nickel manganese oxide positive electrode to stabilize the electrode structure and reduce metal elution.

Benefits of technology

The solution effectively suppresses structural collapse, reduces gas generation, and enhances battery stability and lifespan under high voltage and temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137655000001_ABST
    Figure 2024137655000001_ABST
Patent Text Reader

Abstract

To provide a lithium secondary battery in which a positive electrode containing lithium nickel manganese oxide is used in combination with an electrolyte solution capable of effectively protecting the positive electrode containing lithium nickel manganese oxide, positive electrode structure collapse is suppressed by reducing transitional metal elution under a high-voltage condition and a high-temperature condition, and accordingly, a high-voltage characteristic and a high-temperature characteristic of the battery are improved.SOLUTION: A lithium secondary battery in one embodiment includes: an electrolyte solution containing a nonaqueous organic solvent, a lithium salt, and an additive; a positive electrode containing a positive electrode active material; and a negative electrode containing a negative electrode active material. The nonaqueous organic solvent contains ethylene carbonate by less than 5 wt% relative to entire weight of the nonaqueous organic solvent. The positive electrode active material contains lithium nickel manganese oxide. The additive contains a compound expressed by Chemical Formula 1. The Chemical Formula 1 is defined in the specification.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This description relates to lithium secondary batteries. [Background technology]

[0002] Lithium secondary batteries are rechargeable and have more than three times the energy density per unit weight compared to conventional lead-acid batteries, nickel-cadmium batteries, nickel-metal hydride batteries, and nickel-zinc batteries, allowing for fast charging. As a result, they have been commercialized for use in laptops, mobile phones, power tools, and electric bicycles, and research and development is being actively conducted to further improve their energy density.

[0003] In particular, as IT devices become increasingly sophisticated, there is a demand for higher-capacity batteries. By expanding the voltage range to achieve higher capacity, the energy density can be increased. However, there is a problem that the electrolyte is oxidized in the high-voltage range, deteriorating the performance of the positive electrode.

[0004] In particular, cobalt-free lithium nickel manganese oxide as a positive electrode active material is a positive electrode active material composed mainly of nickel, manganese, etc., without introducing cobalt into the positive electrode active material composition. Since positive electrodes containing this are economical and can achieve high energy density, it is attracting attention as a next-generation positive electrode active material.

[0005] However, when a positive electrode containing cobalt-free lithium nickel manganese oxide is used in a high voltage environment, the positive electrode structure collapses, causing transition metal elution, which can lead to problems such as gas generation inside the cell and capacity reduction. This transition metal elution phenomenon tends to become more severe in high temperature environments, and the eluted transition metals can precipitate on the surface of the negative electrode, inducing side reactions, which can lead to an increase in battery resistance and a decrease in battery life and output characteristics.

[0006] Thus, when using a positive electrode containing a cobalt-free lithium nickel manganese oxide, an electrolyte that can be used under high voltage and high temperature conditions is required. Summary of the Invention [Problem to be solved by the invention]

[0007] In one embodiment, a positive electrode including a lithium nickel manganese-based oxide is used in combination with an electrolyte that can effectively protect the positive electrode including the lithium nickel manganese-based oxide, thereby reducing the elution of transition metals under high voltage and high temperature conditions, thereby suppressing the collapse of the positive electrode structure, thereby providing a lithium secondary battery with improved high voltage and high temperature characteristics. [Means for solving the problem]

[0008] One embodiment of the present invention includes an electrolyte solution including a non-aqueous organic solvent, a lithium salt, and an additive; a positive electrode including a positive electrode active material; and a negative electrode including a negative electrode active material, The non-aqueous organic solvent contains ethylene carbonate in an amount of less than 5% by weight based on the total weight of the non-aqueous organic solvent; The positive electrode active material includes a lithium nickel manganese oxide, The additive provides a lithium secondary battery, comprising a compound represented by the following Chemical Formula 1: [ka]

[0009] In the above chemical formula 1, X 1 and X 2 are each independently O, S, or CR a R b and X 1 and X 2 At least one of is O; R a , R b , and R 1 ~R 4each independently represents a hydrogen atom, a halogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 3 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 50 carbon atoms, a substituted or unsubstituted alkylaryl group having 7 to 50 carbon atoms, or a substituted or unsubstituted heteroaryl group having 6 to 50 carbon atoms, n is an integer of 1 or 2.

[0010] The non-aqueous organic solvent may consist solely of a chain carbonate.

[0011] The chain carbonate can be represented by the following chemical formula 2. [ka] In the above chemical formula 2, R 5 and R 6 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.

[0012] The non-aqueous organic solvent may be a mixed solvent of at least two of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and ethyl methyl carbonate (EMC).

[0013] The non-aqueous organic solvent may contain ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 0:100 to 50:50.

[0014] The formula 1 can be represented by the following formula 1A or 1B. [ka]

[0015] In the above Chemical Formula 1A and Chemical Formula 1B, R a , R b , R 1 ~R 4 and n is as previously described.

[0016] R of Formula 1 a , R b , and R 1 ~R 4 may each independently be a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.

[0017] In the above formula 1, n may be 1.

[0018] The compound represented by Chemical Formula 1 can be selected from the compounds listed in Group 1 below. [ka]

[0019] The compound represented by Chemical Formula 1 may be included in an amount of 0.05 to 5.0 parts by weight based on 100 parts by weight of the total amount (lithium salt + non-aqueous organic solvent) excluding additives in the electrolyte for lithium secondary batteries.

[0020] The electrolyte may be any of vinylene carbonate (VC), fluoroethylene carbonate (FEC), difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, vinylethylene carbonate (VEC), adiponitrile (AN), succinonitrile (SN), 1,3,6-hexanetricyanide (HTCN), propene sultone (PST), propane sultone (PS), lithium tetrafluoroborate (LiBF 4 ), lithium difluorophosphate (LiPO 2 F 2), and 2-fluorobiphenyl (2-FBP).

[0021] The lithium nickel manganese oxide may include a cobalt-free lithium composite oxide represented by the following Formula 4. [Chemical formula 4] Li a Ni x Mn y M 1 z M 2 w O 2±b X c

[0022] In the above chemical formula 4, 0.5≦a<1.8, 0≦b≦0.1, 0≦c≦0.1, 0≦w<0.1, 0.6≦x<1.0, 0 <y<0.4、0<z<0.1、w+x+y+z=1であり、 M 1 and M. 2 are each independently one or more elements selected from Al, Mg, Ti, Zr, Sr, V, B, W, Mo, Si, Ba, Ca, Ce, Cr, Fe, and Nb, and X is one or more elements selected from S, F, P, and Cl.

[0023] The above formula 4 can be represented by the following formula 4-1. [Chemical formula 4-1] Li a Ni x1 Mn y1 Al z1 M 2 w1 O 2±b X c

[0024] In the above chemical formula 4-1, 0.5≦a<1.8, 0≦b≦0.1, 0≦c≦0.1, 0≦w1<0.1, 0.6≦x1<1.0, 0 <y1<0.4、0<z1<0.1、w1+x1+y1+z1=1であり、 M 2is one or more elements selected from Mg, Ti, Zr, Sr, V, B, W, Mo, Si, Ba, Ca, Ce, Cr, Fe, and Nb, and X is one or more elements selected from S, F, P, and Cl.

[0025] In the above Chemical Formula 4-1, x1 may be 0.6≦x1≦0.79, y1 may be 0.2≦y1≦0.39, and z1 may be 0.01≦z1<0.1.

[0026] The negative electrode active material may include at least one of graphite and a Si composite.

[0027] The upper limit charging voltage of the lithium secondary battery may be 4.35 V or higher. Effect of the Invention

[0028] In one embodiment, a positive electrode containing a lithium nickel manganese oxide is used in combination with an electrolyte capable of effectively protecting the positive electrode containing a lithium nickel manganese oxide, thereby ensuring the phase transition safety of the positive electrode even in a high temperature and high voltage environment, and suppressing decomposition of the electrolyte and side reactions with the electrodes to reduce gas generation and simultaneously suppress an increase in the internal resistance of the battery, thereby realizing a lithium secondary battery with improved battery stability and life characteristics. [Brief description of the drawings]

[0029] [Figure 1] 1 is a schematic diagram showing a lithium secondary battery according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, a lithium secondary battery according to an embodiment of the present invention will be described in detail with reference to the accompanying drawings, which are given by way of example only and are not intended to limit the present invention, which is defined only by the following claims.

[0031] As used herein, unless otherwise defined, "substituted" means that at least one hydrogen atom in a substituent or compound is replaced with deuterium, a halogen group, a hydroxyl group, an amino group, a substituted or unsubstituted amine group having 1 to 30 carbon atoms, a nitro group, a substituted or unsubstituted silyl group having 1 to 40 carbon atoms, an alkyl group having 1 to 30 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, an arylsilyl group having 6 to 30 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a heterocycloalkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, a heteroaryl group having 2 to 30 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a fluoroalkyl group having 1 to 10 carbon atoms, a cyano group, or a combination thereof.

[0032] In one embodiment of the present invention, "substitution" means that at least one hydrogen atom in a substituent or compound is substituted with deuterium, a halogen group, an alkyl group having 1 to 30 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, an arylsilyl group having 6 to 30 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a heterocycloalkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, a heteroaryl group having 2 to 30 carbon atoms, a fluoroalkyl group having 1 to 10 carbon atoms, or a cyano group. In one specific embodiment of the present invention, "substitution" means that at least one hydrogen atom in a substituent or compound is substituted with deuterium, a halogen group, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, a fluoroalkyl group having 1 to 10 carbon atoms, or a cyano group. In one specific embodiment of the present invention, "substitution" means that at least one hydrogen atom in a substituent or compound is substituted with deuterium, a halogen group, an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 18 carbon atoms, a fluoroalkyl group having 1 to 5 carbon atoms, or a cyano group. In addition, in a specific example of the present invention, "substituted" means that at least one hydrogen in a substituent or compound is replaced with deuterium, a cyano group, a halogen group, a methyl group, an ethyl group, a propyl group, a butyl group, a phenyl group, a biphenyl group, a terphenyl group, a trifluoromethyl group, or a naphthyl group.

[0033] Lithium secondary batteries can be classified into lithium ion batteries, lithium ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used, into cylindrical, square, coin, pouch, and other types depending on the shape, and into bulk and thin film types depending on the size. The structure and manufacturing method of these batteries are widely known in the art, so a detailed description will be omitted.

[0034] Here, a cylindrical lithium secondary battery will be described as an example of the lithium secondary battery. Fig. 1 is a schematic diagram showing the structure of a lithium secondary battery according to an embodiment. Referring to Fig. 1, a lithium secondary battery 100 according to an embodiment includes a battery cell including a positive electrode 114, a negative electrode 112 facing the positive electrode 114, a separator 113 disposed between the positive electrode 114 and the negative electrode 112, and an electrolyte (not shown) impregnating the positive electrode 114, the negative electrode 112, and the separator 113, a battery container 120 containing the battery cell, and an encapsulation member 140 sealing the battery container 120.

[0035] The configuration of the lithium secondary battery 100 according to one embodiment of the present invention will now be described in more detail.

[0036] A lithium secondary battery according to one embodiment of the present invention includes an electrolyte, a positive electrode, and a negative electrode.

[0037] The electrolyte solution includes a non-aqueous organic solvent, a lithium salt, and an additive, the non-aqueous organic solvent includes ethylene carbonate in an amount of less than 5 wt % based on the total weight of the non-aqueous organic solvent, and the additive may include a compound represented by the following Chemical Formula 1: [ka]

[0038] In the above chemical formula 1, X 1 and X 2 are each independently O, S, or CR aR b and X 1 and X 2 At least one of is O; R a , R b , and R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 3 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 50 carbon atoms, a substituted or unsubstituted alkylaryl group having 7 to 50 carbon atoms, or a substituted or unsubstituted heteroaryl group having 6 to 50 carbon atoms, n is an integer of 1 or 2.

[0039] The positive electrode may include a positive electrode active material including a lithium nickel manganese-based oxide.

[0040] In the case of positive electrode active materials containing lithium nickel manganese oxide, structural instability is high under high voltage conditions, leading to solvent decomposition and dissolution of transition metals, particularly Ni.

[0041] Such a transition metal elution phenomenon causes degradation and short circuit, which reduces the battery life capacity and causes a sudden increase in resistance.

[0042] However, when the above-mentioned electrolyte is used together, the decrease in the life capacity of the battery and the sudden increase in resistance can be alleviated.

[0043] In particular, by using a positive electrode containing a lithium nickel manganese-based oxide in an electrolyte containing ethylene carbonate in an amount of less than 5 wt % based on the total weight of the non-aqueous organic solvent, it is possible to effectively reduce the elution of transition metals under high voltage and high temperature conditions, thereby suppressing the collapse of the positive electrode structure and improving the high voltage and high temperature characteristics of the battery.

[0044] The non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.

[0045] The non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent.

[0046] Examples of the carbonate-based solvent include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Examples of the ester-based solvent include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanolide, mevalonolactone, caprolactone, etc. Examples of the ether-based solvent include dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. The ketone solvent may be cyclohexanone, etc. The alcohol solvent may be ethyl alcohol, isopropyl alcohol, etc., and the aprotic solvent may be nitriles such as R-CN (R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, sulfolanes, etc.

[0047] The non-aqueous organic solvent may be used alone or in combination of two or more thereof. When two or more are used in combination, the mixing ratio may be appropriately adjusted depending on the desired battery performance, which should be widely understood by those skilled in the art.

[0048] As an example, the non-aqueous organic solvent may contain ethylene carbonate in an amount of less than 5% by weight based on the total weight of the non-aqueous organic solvent.

[0049] When the content of ethylene carbonate is 5 wt% or more based on the total weight of the non-aqueous organic solvent, the activity of Ni increases during high voltage operation, and the oxidation number of Ni tends to be reduced from 4 to 2, and ethylene carbonate, which has low oxidation stability, is oxidized and decomposed, resulting in Ni elution and deposition on the negative electrode.

[0050] As a specific example, the non-aqueous organic solvent may be composed only of a chain carbonate, in which case the resistance increase rate during high temperature storage is significantly reduced, thereby achieving excellent high temperature storage characteristics.

[0051] In this specification, the expression "consisting only of a chain carbonate" means that the organic solvent is not mixed with a cyclic carbonate or the like, and is a single organic solvent or a combination of organic solvents that belong to the range of a chain carbonate.

[0052] In one embodiment, the chain carbonate may be represented by the following Chemical Formula 2: [ka]

[0053] In the above chemical formula 2, R 5 and R 6 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.

[0054] As an example, R 5 and R6 may each independently be a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms. For example, 5 and R 6 may each independently be a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms.

[0055] In one embodiment, R 5 and R 6 may each independently be a substituted or unsubstituted methyl group, a substituted or unsubstituted ethyl group, a substituted or unsubstituted n-propyl group, a substituted or unsubstituted n-butyl group, a substituted or unsubstituted n-pentyl group, a substituted or unsubstituted iso-butyl group, or a substituted or unsubstituted neo-pentyl group.

[0056] For example, the non-aqueous organic solvent according to a specific embodiment may be a mixed solvent of at least two of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and ethyl methyl carbonate (EMC).

[0057] The non-aqueous organic solvent according to a most specific embodiment may be a mixed solvent of dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC).

[0058] The non-aqueous organic solvent may contain ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a weight ratio of 0:100 to 50:50.

[0059] It may be more advantageous in terms of improving battery characteristics if the non-aqueous organic solvent contains dimethyl carbonate (DMC) in an amount of more than 50 wt % based on the total weight of the non-aqueous organic solvent.

[0060] For example, the non-aqueous organic solvent may contain ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 0:100 to 40:60, 0:100 to 30:70, 10:90 to 40:60, or 10:90 to 30:70.

[0061] The non-aqueous organic solvent may further include an aromatic hydrocarbon-based organic solvent in addition to the carbonate-based solvent, and the carbonate-based solvent and the aromatic hydrocarbon-based solvent may be mixed in a volume ratio of 1:1 to 30:1.

[0062] As the aromatic hydrocarbon solvent, an aromatic hydrocarbon compound represented by the following formula 3 can be used. [ka]

[0063] In the above chemical formula 3, R 11 ~R 16 are the same or different and are selected from the group consisting of hydrogen, halogen, an alkyl group having 1 to 10 carbon atoms, a haloalkyl group, and combinations thereof.

[0064] Specific examples of the aromatic hydrocarbon solvent include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorobenzene ... and combinations thereof.

[0065] The lithium salt is a material that is dissolved in a non-aqueous organic solvent and acts as a source of lithium ions in a battery to enable basic operation of a lithium secondary battery and promote the movement of lithium ions between the positive electrode and the negative electrode. A representative example of such a lithium salt is LiPF 6 , LiBF 4 , lithium difluoro(oxalate)borate (LiDFOB), LiPO 2 F 2 , LiSbF 6 , LiAsF 6 , Li(FSO 2 ) 2 N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC 4 F9 SO 3 , LiClO 4 , LiAlO 2 , LiAlCl 4 , LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 ) (wherein x and y are each independently an integer from 1 to 20), LiCl, LiI, and LiB (C 2 O 4 ) 2 (lithium bis(oxalato)borate (LiBOB))

[0066] The lithium salt is preferably used at a concentration within the range of 0.1 M to 2.0 M. If the concentration of the lithium salt is within this range, the electrolyte has appropriate conductivity and viscosity, and therefore can exhibit excellent electrolyte performance, allowing lithium ions to migrate effectively.

[0067] The formula 1 can be represented by the following formula 1A or 1B. [ka]

[0068] In the above Chemical Formula 1A and Chemical Formula 1B, R a , R b , R 1 ~R 4 and n is as previously described.

[0069] As an example, R a , R b , and R 1 ~R 4 may each independently be a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.

[0070] As a specific example, R a , R b , and R 1 ~R 4 may each independently be hydrogen or a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms.

[0071] For example, R a , R b , and R 1 ~R 4 may each independently be hydrogen or a substituted or unsubstituted alkyl group having 1 to 3 carbon atoms.

[0072] For example, n in the above formula 1 may be 1.

[0073] The compound represented by Chemical Formula 1 can be selected from the compounds listed in Group 1 below. [ka]

[0074] The compound represented by Chemical Formula 1 may be included in an amount of 0.05 to 5.0 parts by weight based on 100 parts by weight of the total amount (lithium salt + non-aqueous organic solvent) excluding additives in the electrolyte for lithium secondary batteries.

[0075] For example, the compound represented by Formula 1 may be included in an amount of 0.05 to 3.0 parts by weight based on 100 parts by weight of the total amount (lithium salt + non-aqueous organic solvent) excluding additives in the electrolyte for lithium secondary batteries.

[0076] For example, the compound represented by Chemical Formula 1 may be included in an amount of 0.1 to 3.0 parts by weight, 0.3 to 3.0 parts by weight, 0.5 to 3.0 parts by weight, or 0.5 to 2.0 parts by weight based on 100 parts by weight of the total amount (lithium salt + non-aqueous organic solvent) excluding additives in the electrolyte for lithium secondary batteries.

[0077] When the content of the compound represented by Chemical Formula 1 is within the above range, an increase in resistance at high temperatures can be prevented, thereby realizing a lithium secondary battery having improved life characteristics and output characteristics.

[0078] On the other hand, the electrolyte may be vinylene carbonate (VC), fluoroethylene carbonate (FEC), difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, vinylethylene carbonate (VEC), adiponitrile (AN), succinic acid nitrile (SN), 1,3,6-hexanetricyanide (HTCN), propene sultone (PST), propane sultone (PS), lithium tetrafluoroborate (LiBF 4 ), lithium difluorophosphate (LiPO 2 F 2 ), and 2-fluorobiphenyl (2-FBP).

[0079] By further including the other additives, the life span can be further improved or gas generated from the positive and negative electrodes during high temperature storage can be effectively controlled.

[0080] The other additives may be included in an amount of 0.2 to 20 parts by weight, specifically 0.2 to 15 parts by weight, for example 0.2 to 10 parts by weight, based on 100 parts by weight of the total (lithium salt + non-aqueous organic solvent) excluding the additives in the electrolyte for lithium secondary batteries.

[0081] When the content of the other additives is within the above range, the increase in film resistance can be minimized to improve the battery performance.

[0082] The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material.

[0083] The positive electrode active material may include a lithium nickel manganese oxide.

[0084] For example, the lithium nickel manganese-based oxide may include at least one of cobalt-free lithium composite oxides represented by the following Formula 4: [Chemical formula 4] Li a Ni x Mn y M 1 z M 2 w O 2±b X c

[0085] In the above chemical formula 4, 0.5≦a<1.8, 0≦b≦0.1, 0≦c≦0.1, 0≦w<0.1, 0.6≦x<1.0, 0 <y<0.4、0<z<0.1、w+x+y+z=1であり、 M 1 and M. 2 are each independently one or more elements selected from Al, Mg, Ti, Zr, Sr, V, B, W, Mo, Si, Ba, Ca, Ce, Cr, Fe, and Nb, and X is one or more elements selected from S, F, P, and Cl.

[0086] In this specification, the cobalt-free lithium composite oxide as the positive electrode active material means a positive electrode active material composed mainly of nickel, manganese, etc., which does not contain cobalt in the composition of the positive electrode active material.

[0087] Of course, the lithium composite oxide may have a coating layer on its surface, or may be mixed with a compound forming the coating layer. The coating layer may contain at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compounds forming the coating layer may be amorphous or crystalline. The coating elements contained in the coating layer may be Mg, Al, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating layer forming step may use any coating method as long as it can coat the positive electrode active material in a manner that does not adversely affect the physical properties of the positive electrode active material (e.g., spray coating, immersion method, etc.), and detailed explanations of this will be omitted since it is well understood by those skilled in the art.

[0088] For example, Formula 4 can be represented by Formula 4-1 below. [Chemical formula 4-1] Li a Ni x1 Mn y1 Al z1 M 2 w1 O 2±b X c

[0089] In the above chemical formula 4-1, 0.5≦a<1.8, 0≦b≦0.1, 0≦c≦0.1, 0≦w1<0.1, 0.6≦x1<1.0, 0 <y1<0.4、0<z1<0.1、w1+x1+y1+z1=1であり、 M 2 is one or more elements selected from Mg, Ti, Zr, Sr, V, B, W, Mo, Si, Ba, Ca, Ce, Cr, Fe, and Nb, and X is one or more elements selected from S, F, P, and Cl.

[0090] In one embodiment, in the formula 4-1, 0.6≦x1≦0.9, 0.1≦y1<0.4, and 0 <z1<0.1であってもよく、0.6≦x1≦0.8、0.2≦y1<0.4、および0<z1<0.1であってもよい。

[0091] For example, in the above chemical formula 4-1, x1 may be 0.6≦x1≦0.79, y1 may be 0.2≦y1≦0.39, and z1 may be 0.01≦z1<0.1.

[0092] The content of the positive electrode active material may be 90% by weight to 98% by weight based on the total weight of the positive electrode active material layer.

[0093] In an embodiment of the present invention, the positive electrode active material layer may include a binder, and the content of the binder may be 1 wt % to 5 wt % based on the total weight of the positive electrode active material layer.

[0094] The binder serves to adhere the positive electrode active material particles to each other and to the current collector well. Representative examples of the binder include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, nylon, etc.

[0095] The positive electrode current collector may be made of Al, but is not limited thereto.

[0096] The negative electrode includes a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector and including a negative electrode active material.

[0097] The negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and undoping lithium, or a transition metal oxide.

[0098] As the material capable of reversibly intercalating / deintercalating lithium ions, any of the carbon-based negative electrode active materials generally used in lithium secondary batteries can be used. Representative examples thereof include crystalline carbon, amorphous carbon, or both of them. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite. Examples of the amorphous carbon include soft carbon, hard carbon, mesophase pitch carbide, fired coke, and the like.

[0099] As the alloy of lithium metal, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn can be used.

[0100] As the material capable of doping and undoping lithium, Si, Si-C composite, SiO x (0 < x ≦ 2), Si-Q alloy (where Q is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element excluding Si, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof), Sn, SnOy (0 < y ≦ 2), Sn-R 11 (where R 11 is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element excluding Sn, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof), and the like can be mentioned. Also, at least one of these and SiO 2 can be mixed and used.

[0101] the elements Q and R 11 Examples of these include Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0102] Examples of the transition metal oxide include vanadium oxide, lithium vanadium oxide, or lithium titanium oxide.

[0103] In a specific embodiment, the negative electrode active material can include at least one of graphite and a Si composite.

[0104] The Si composite includes a core containing Si-based particles and an amorphous carbon coating layer. For example, the Si-based particles can include one or more of silicon particles, Si-C composites, SiO x (0 < x ≦ 2), and Si alloys.

[0105] As an example, the core containing the Si-based particles contains voids at the center, the radius of the center corresponds to 30% to 50% of the radius of the negative electrode active material, the average particle size of the Si composite is 5 μm to 20 μm, and the average particle size of the Si-based particles may be 10 nm to 200 nm.

[0106] In this specification, the average particle size may be the particle size (D50) at 50% as the volume ratio in the cumulative size-distribution curve.

[0107] When the average particle size of the Si-based particles is within the above range, volume expansion generated during charge and discharge can be suppressed, and disconnection of the conductive path due to particle crushing during charge and discharge can be prevented.

[0108] The core containing the Si-based particles additionally contains amorphous carbon, and in this case, the central portion does not contain amorphous carbon, and amorphous carbon is present only in the surface portion of the Si composite.

[0109] In this case, the surface portion means the region from the outermost surface of the center portion to the outermost surface of the Si composite.

[0110] Furthermore, the Si-based particles are present substantially uniformly throughout the Si composite, that is, at a substantially uniform concentration in the center and surface portions.

[0111] The amorphous carbon may be soft carbon, hard carbon, mesophase pitch charcoal, calcined coke, or a combination thereof.

[0112] For example, the Si-C composite can include silicon particles and crystalline carbon.

[0113] The silicon particles may be included in an amount of 1 to 60 wt % based on the total weight of the Si-C composite, for example, 3 to 60 wt %.

[0114] The crystalline carbon may be, for example, graphite, and in particular may be natural graphite, artificial graphite, or a combination thereof.

[0115] The average particle size of the crystalline carbon may be 5 μm to 30 μm.

[0116] When the negative electrode active material contains both graphite and a Si complex, the graphite and the Si complex may be contained in the form of a mixture. In this case, the graphite and the Si complex may be contained in a weight ratio of 99:1 to 50:50.

[0117] More specifically, the graphite and the Si complex may be contained in a weight ratio of 97:3 to 80:20, or 95:5 to 80:20.

[0118] The amorphous carbon precursor may be coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, or a polymer resin such as a phenol resin, a furan resin, or a polyimide resin.

[0119] The negative active material layer may have a negative active material content of 95 wt % to 99 wt % based on the total weight of the negative active material layer.

[0120] In one embodiment of the present invention, the negative electrode active material layer includes a binder and may optionally further include a conductive material. The content of the binder in the negative electrode active material layer may be 1 wt% to 5 wt% based on the total weight of the negative electrode active material layer. When the negative electrode active material layer further includes a conductive material, the negative electrode active material may be 90 wt% to 98 wt%, the binder may be 1 wt% to 5 wt%, and the conductive material may be 1 wt% to 5 wt%.

[0121] The binder serves to adhere the negative active material particles to each other and to the current collector well. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.

[0122] The water-insoluble binder may be polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.

[0123] The water-soluble binder may be a rubber-based binder or a polymeric resin binder. The rubber-based binder may be selected from styrene butadiene rubber, acrylated styrene butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, and combinations thereof. The polymeric resin binder may be selected from polytetrafluoroethylene, ethylene propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0124] When a water-soluble binder is used as the negative electrode binder, a cellulose-based compound capable of imparting viscosity may be further included as a thickener. The cellulose-based compound may be a mixture of one or more of carboxymethylcellulose, hydroxypropylmethylcellulose, methylcellulose, or alkali metal salts thereof. The alkali metal may be Na, K, or Li. The amount of the thickener used may be 0.1 to 3 parts by weight based on 100 parts by weight of the negative electrode active material.

[0125] The conductive material is used to impart conductivity to the electrodes, and any material can be used as long as it does not cause a chemical change in the battery that is constructed and is electronically conductive. Examples of conductive materials that can be used include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers of copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; and mixtures of these.

[0126] The negative electrode current collector may be made of a material selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0127] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multi-layer film of two or more layers of these may be used, and of course, a mixed multi-layer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may be used.

[0128] The upper limit charging voltage of the lithium secondary battery may be equal to or higher than 4.35 V. For example, the upper limit charging voltage of the lithium secondary battery may be 4.35 V to 4.55 V.

[0129] Examples and comparative examples of the present invention will be described below. However, the following examples are merely examples of the present invention, and the present invention is not limited to the following examples. EXAMPLES

[0130] Manufacturing of lithium secondary batteries Example 1 LiNi as the positive electrode active material 0.75 Mn 0.23 Al 0.02 O 2 The positive electrode active material slurry was prepared by mixing the above-mentioned powder, polyvinylidene fluoride as a binder, and acetylene black as a conductive material in a weight ratio of 96:3:1, and dispersing the mixture in N-methylpyrrolidone.

[0131] The positive electrode active material slurry was coated on an aluminum foil having a thickness of 15 μm, dried at 100° C., and pressed to prepare a positive electrode.

[0132] A mixture of artificial graphite and a Si composite in a weight ratio of 93:7 was used as the negative electrode active material, and the negative electrode active material, a styrene butadiene rubber binder, and carboxymethyl cellulose were mixed in a weight ratio of 98:1:1, respectively, and dispersed in distilled water to prepare a negative electrode active material slurry.

[0133] The Si composite used had a core containing artificial graphite and silicon particles, and the surface of the core was coated with coal-based pitch.

[0134] The negative electrode active material slurry was coated on a copper foil having a thickness of 10 μm, dried at 100° C., and pressed to prepare a negative electrode.

[0135] The prepared positive and negative electrodes were assembled with a 10 μm thick polyethylene separator to prepare an electrode assembly, and an electrolyte was injected to prepare a lithium secondary battery.

[0136] The electrolyte composition is as follows: (Electrolyte composition) Lithium salt: LiPF 6 1.5M Non-aqueous organic solvent: ethyl methyl carbonate: dimethyl carbonate (EMC:DMC=20:80 volume ratio) Additive: 0.5 parts by weight of a compound represented by the following formula 1-1 [ka] (Note that in the above electrolyte composition, "parts by weight" refers to the relative weight of the additive to 100 parts by weight of the entire electrolyte (lithium salt + non-aqueous organic solvent) excluding the additive.)

[0137] Example 2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound represented by Formula 1-1 was added in an amount of 1 part by weight.

[0138] Example 3 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a compound represented by the following Formula 1-2 was used instead of the compound represented by Formula 1-1. [ka]

[0139] Example 4 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound represented by Formula 1-2 was added in an amount of 1 part by weight.

[0140] Comparative Example 1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound represented by Formula 1-1 was not added to the electrolyte composition.

[0141] Comparative Example 2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that ethylene carbonate was added in an amount of 20 wt % based on the total weight of the non-aqueous organic solvent in the electrolyte composition.

[0142] Comparative Example 3 A lithium secondary battery was manufactured in the same manner as in Example 3, except that ethylene carbonate was added in an amount of 20 wt % based on the total weight of the non-aqueous organic solvent in the electrolyte composition.

[0143] Comparative Example 4 A lithium secondary battery was manufactured in the same manner as in Example 1, except that 0.5 parts by weight of fluoroethylene carbonate (FEC) was added instead of the compound represented by Formula 1-1 in the electrolyte composition.

[0144] Examples 5 and 6 Lithium secondary batteries were fabricated in the same manner as in Examples 1 and 3, except that the non-aqueous organic solvent was changed to 100% dimethyl carbonate by volume.

[0145] Comparative Examples 5 to 10 The positive electrode active material is LiCoO 2 Except for the above change, lithium secondary batteries were fabricated in the same manner as in Examples 1 to 4 and Comparative Examples 1 and 2.

[0146] Comparative Examples 11 to 16 The positive electrode active material is LiNi 0.5 Co 0.2 Al 0.3 O 2 Except for the above change, lithium secondary batteries were fabricated in the same manner as in Examples 1 to 4 and Comparative Examples 1 and 2.

[0147] Comparative Examples 17 to 22 The positive electrode active material is LiNi 0.8 Co 0.1 Mn 0.1 O 2 Except for the above change, lithium secondary batteries were fabricated in the same manner as in Examples 1 to 4 and Comparative Examples 1 and 2.

[0148] Example 7, Example 8, and Comparative Example 23 Lithium secondary batteries were fabricated in the same manner as in Example 1, except that the mixing ratio of ethyl methyl carbonate and dimethyl carbonate was changed to a volume ratio of 30:70 (Example 7), 40:60 (Example 8), and 70:30 (Comparative Example 23), respectively.

[0149] Example 9, Example 10, Comparative Example 24 Lithium secondary batteries were fabricated in the same manner as in Example 3, except that the mixing ratio of ethyl methyl carbonate and dimethyl carbonate was changed to a volume ratio of 30:70 (Example 9), 40:60 (Example 10), and 70:30 (Comparative Example 24), respectively.

[0150] The compositions are as shown in Table 1 below.

[0151] [Table 1A] [Table 1B]

[0152] Evaluation 1: High temperature storage characteristic evaluation For the lithium secondary batteries manufactured in Examples 1 to 10 and Comparative Examples 1 to 24, the initial DC resistance (DCIR) was measured using ΔV / ΔI (change in voltage / change in current) values, and the maximum energy state inside the battery was set as a fully charged state (SOC 100%), and the batteries were stored in this state at high temperature (60°C) for 30 days, after which the DC resistance was measured. The DCIR increase rate (%) was calculated using the following formula 1, and the results are shown in Tables 2, 3, and 6 below. [Formula 1] DCIR increase rate = {(DCIR after 30 days of high temperature storage) / (Initial DCIR)}*100

[0153] Evaluation 2: High temperature life characteristics evaluation The lithium secondary batteries produced in Examples 1 to 6 and Comparative Examples 1 to 4 were charged and discharged once at 0.2 C to measure the charge and discharge capacity. In addition, the lithium secondary batteries produced in Examples 1 to 6 and Comparative Examples 1 to 4 were charged at an upper charge voltage limit of 4.35 V to 4.45 V, and then discharged at a constant current of 0.2 C to 2.5 V to measure the initial discharge capacity. Again, the discharge capacity was measured while performing 200 charge / discharge cycles at 0.33 C charge (CC / CV, 4.35 V and 4.45 V, 0.025 C cut-off) / 1.0 C discharge (CC, 2.5 V cut-off) at 45° C. The ratio of the discharge capacity to the initial discharge capacity was defined as the capacity recovery rate (%, recovery), and the increase rate of the recovery rate relative to Comparative Example 2 was calculated according to the following Equation 2, and the results are shown in Table 5 below. [Formula 2] Increase rate of capacity recovery rate relative to Comparative Example 2={(capacity recovery rate) / (capacity recovery rate of Comparative Example 2)}*100

[0154] Evaluation 3: Gas generation measurement after high temperature storage The lithium secondary batteries according to Examples 1 to 6 and Comparative Examples 1 to 4 were left at 60° C. for 30 days, and the amount of gas generated (ml) on the 10th and 30th days was measured using a refinery gas analyzer (RGA). The reduction rate of the amount of gas generated relative to Comparative Example 2 was calculated according to the following formula 3, and the results are shown in Table 4 below. [Formula 3] Gas generation reduction rate relative to Comparative Example 2={(Gas generation amount on 30th day)−(Gas generation amount on 30th day of Comparative Example 2)} / (Gas generation amount on 30th day of Comparative Example 2)

[0155] [Table 2]

[0156] [Table 3]

[0157] [Table 4]

[0158] [Table 5]

[0159] [Table 6]

[0160] Referring to Tables 2 to 6, it can be seen that the DC-IR increase rate is reduced and the high temperature storage characteristics and high temperature charge / discharge characteristics are all improved when the electrolyte according to the present invention is combined with a cobalt-free positive electrode active material.

[0161] Also, it can be seen that the amount of gas generated after high temperature storage of the lithium secondary batteries according to the embodiments was significantly reduced.

[0162] Although the above describes a preferred embodiment of the present invention, the present invention is not limited thereto, and various modifications and variations can be made within the scope of the claims, the detailed description of the invention, and the accompanying drawings, which of course also fall within the scope of the present invention. [Explanation of symbols]

[0163] 100: Lithium secondary battery 112: Negative electrode 113: Separator 114: Positive electrode 120:Battery container 140: Enclosure

Claims

1. an electrolyte solution comprising a non-aqueous organic solvent, a lithium salt and an additive; a positive electrode comprising a positive electrode active material; and a negative electrode including a negative electrode active material; The non-aqueous organic solvent contains ethylene carbonate in an amount of less than 5% by weight based on the total weight of the non-aqueous organic solvent; The positive electrode active material includes a lithium nickel manganese oxide, The additive comprises a compound represented by the following formula 1: [Formula 1] In the above chemical formula 1, X 1 and X 2 each independently represents O, S, or CR a R b and X 1 and X 2 At least one of is O; R a , R b , and R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 3 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 50 carbon atoms, a substituted or unsubstituted alkylaryl group having 7 to 50 carbon atoms, or a substituted or unsubstituted heteroaryl group having 6 to 50 carbon atoms, n is an integer of 1 or 2.

2. 2. The lithium secondary battery according to claim 1, wherein the non-aqueous organic solvent consists solely of a chain carbonate.

3. The lithium secondary battery according to claim 2, wherein the chain carbonate is represented by the following chemical formula 2: [Case 2] In the above chemical formula 2, R 5 and R 6 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.

4. 2. The lithium secondary battery according to claim 1, wherein the non-aqueous organic solvent is a mixed solvent of at least two of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and ethyl methyl carbonate (EMC).

5. 2. The lithium secondary battery according to claim 1, wherein the non-aqueous organic solvent comprises ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 0:100 to 50:

50.

6. 2. The lithium secondary battery of claim 1, wherein the formula 1 is represented by the following formula 1A or 1B: [C3] In the above Chemical Formula 1A and Chemical Formula 1B, R a , R b , R 1 ~R 4 and n is as defined in claim 1.

7. R of Formula 1 a , R b , and R 1 ~R 4 and each independently represent a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.

8. 2. The lithium secondary battery of claim 1, wherein n in Formula 1 is 1.

9. 2. The lithium secondary battery of claim 1, wherein the compound represented by Chemical Formula 1 is one selected from the compounds listed in Group 1 below: [C4] .

10. The compound represented by Chemical Formula 1 is included in an amount of 0.05 to 5.0 parts by weight based on 100 parts by weight of the total amount (lithium salt + non-aqueous organic solvent) excluding the additive in the electrolyte for lithium secondary batteries. The lithium secondary battery of claim 1.

11. The electrolyte may be any of vinylene carbonate (VC), fluoroethylene carbonate (FEC), difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, vinylethylene carbonate (VEC), adiponitrile (AN), succinonitrile (SN), 1,3,6-hexanetricyanide (HTCN), propene sultone (PST), propane sultone (PS), lithium tetrafluoroborate (LiBF 4 ), lithium difluorophosphate (LiPO 2 F 2 2. The lithium secondary battery of claim 1, further comprising at least one other additive selected from the group consisting of 2-fluorobiphenyl (2-FBP) and 2-fluorobiphenyl (2-FBP).

12. 2. The lithium secondary battery of claim 1, wherein the lithium nickel manganese-based oxide comprises a cobalt-free lithium composite oxide represented by the following formula 4: [Chemical formula 4] Li a Ni x Mn y M 1 z M 2 w O 2±b X c In the above chemical formula 4, 0.5≦a<1.8, 0≦b≦0.1, 0≦c≦0.1, 0≦w<0.1, 0.6≦x<1.0, 0<y<0.4, 0<z<0.1, and w+x+y+z=1; M 1 and M. 2 are each independently one or more elements selected from Al, Mg, Ti, Zr, Sr, V, B, W, Mo, Si, Ba, Ca, Ce, Cr, Fe, and Nb, and X is one or more elements selected from S, F, P, and Cl.

13. The lithium secondary battery according to claim 12, wherein the chemical formula 4 is represented by the following chemical formula 4-1: [Chemical formula 4-1] Li a Ni x1 Mn y1 A z1 M 2 w1 O 2±b X c In the above chemical formula 4-1, 0.5≦a<1.8, 0≦b≦0.1, 0≦c≦0.1, 0≦w1<0.1, 0.6≦x1<1.0, 0<y1<0.4, 0<z1<0.1, and w1+x1+y1+z1=1, M 2 is one or more elements selected from Mg, Ti, Zr, Sr, V, B, W, Mo, Si, Ba, Ca, Ce, Cr, Fe, and Nb, and X is one or more elements selected from S, F, P, and Cl.

14. 14. The lithium secondary battery according to claim 13, wherein, in the chemical formula 4-1, x1 is 0.6≦x1≦0.79, y1 is 0.2≦y1≦0.39, and z1 is 0.01≦z1<0.

1.

15. The lithium secondary battery according to claim 1 , wherein the negative electrode active material comprises at least one of graphite and a Si composite.

16. 2. The lithium secondary battery according to claim 1, wherein the upper limit charging voltage of the lithium secondary battery is 4.35 V or higher.

Citation Information

Patent Citations

  • Cobalt-free positive electrode material of high-voltage lithium ion battery and preparation method thereof

    CN113517424A

  • Nonaqueous electrolyte secondary battery

    JP2006344390A

  • Non-aqueous electrolyte composition containing cyclic sulfate and lithium borate

    JP2017520100A

  • Lithium ion secondary battery

    JP2018085221A

  • Lithium ion secondary battery

    JP2018125090A