Insulating material-coated soft magnetic powder, dust core, magnetic element, and electronic device
The insulator-coated soft magnetic powder with controlled particle size and hydrophobic coating addresses the challenge of maintaining density and strength in magnetic particles, enhancing magnetic performance and reducing core loss.
Patent Information
- Application Number
- JP2023220619
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-07
AI Technical Summary
Existing soft magnetic particles face challenges in achieving both high density and mechanical strength while maintaining a large specific surface area, leading to decreased magnetic properties and increased core loss due to the use of binders.
The insulator-coated soft magnetic powder features a specific particle size, surface area, and oxygen content, combined with a hydrophobic functional group-containing insulating coating, to enhance adhesion and filling properties, thereby improving mechanical strength and magnetic performance.
The solution results in a powder compact with enhanced density, mechanical strength, and reduced core loss, allowing for high-performance magnetic elements and devices.
Smart Images

Figure 2024137690000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulator-coated soft magnetic powder, a dust core, a magnetic element, and an electronic device. [Background technology]
[0002] Patent Document 1 discloses a soft magnetic material that includes first soft magnetic particles and second soft magnetic particles having a larger average particle size, and uses particles having a non-polar hydrocarbon group or a hydrocarbon group having a linear chain portion with 6 or more carbon atoms on the surface as the first soft magnetic particles. Examples of non-polar hydrocarbon groups include cyclic hydrocarbon groups such as aryl groups and phenyl groups. In such a soft magnetic material, the interaction between the first soft magnetic particles and the binder that binds the soft magnetic material can be reduced, and the fluidity of the soft magnetic particles is improved during pressure molding. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-95629 Summary of the Invention [Problem to be solved by the invention]
[0004] In the soft magnetic particles described in Patent Document 1, by introducing a non-polar hydrocarbon group or a hydrocarbon group having a straight chain portion with 6 or more carbon atoms, the interaction with the binder is reduced and the flowability during pressure molding is improved. In magnetic elements using soft magnetic powder, low iron loss is required, and as part of this, the diameter of soft magnetic particles is being reduced. When the diameter of soft magnetic particles is reduced, the specific surface area increases, so it is necessary to increase the amount of binder used during pressure molding. However, when the amount of binder used increases, the space factor of the soft magnetic particles decreases relatively. As a result, the density of the green compact decreases and the magnetic properties decrease. On the other hand, when the amount of binder used is reduced, the mechanical strength of the green compact decreases.
[0005] Therefore, it is an issue to realize an insulator-coated soft magnetic powder that can achieve both high density and mechanical strength of the green compact even when the specific surface area of the soft magnetic powder is large. [Means for solving the problem]
[0006] The insulator-coated soft magnetic powder according to the application example of the present invention is A soft magnetic powder; an insulating coating that coats the particle surfaces of the soft magnetic powder and contains a compound having a hydrophobic functional group derived from a coupling agent; Equipped with The average particle size of the soft magnetic powder is 2.0 μm or more and 25.0 μm or less, The specific surface area of the soft magnetic powder is 0.05 m 2 / g or more 0.60m 2 / g or less, The specific surface area is defined as S [m 2 / g] and the oxygen content in the soft magnetic powder is A [ppm], the ratio A / S is 3,000 or more and 20,000 or less.
[0007] The powder magnetic core according to the application example of the present invention is The present invention includes an insulating-coated soft magnetic powder according to an embodiment of the present invention.
[0008] The magnetic element according to the application example of the present invention includes: The present invention is provided with a powder magnetic core according to an application example of the present invention.
[0009] The electronic device according to the application example of the present invention includes: The magnetic element according to the application example of the present invention is provided. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a cross-sectional view showing a schematic diagram of one particle of the insulator-coated soft magnetic powder according to the embodiment. [Diagram 2] FIG. 2 is a process diagram for explaining a method for producing an insulator-coated soft magnetic powder. [Diagram 3] FIG. 2 is a plan view illustrating a schematic diagram of a toroidal type coil component. [Figure 4] FIG. 2 is a see-through perspective view that typically illustrates a closed magnetic circuit type coil component. [Diagram 5] FIG. 1 is a perspective view showing a mobile personal computer, which is an electronic device including a magnetic element according to an embodiment. [Figure 6] FIG. 1 is a plan view showing a smartphone, which is an electronic device including a magnetic element according to an embodiment. [Figure 7] FIG. 1 is a perspective view showing a digital still camera, which is an electronic device including a magnetic element according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The insulator-coated soft magnetic powder, the dust core, the magnetic element, and the electronic device of the present invention will be described in detail below with reference to preferred embodiments shown in the accompanying drawings.
[0012] 1.Insulator coated soft magnetic powder First, the insulated soft magnetic powder according to the embodiment will be described. Fig. 1 is a cross-sectional view showing a schematic diagram of one particle of the insulated soft magnetic powder 1 according to the embodiment. In the following description, one particle of the insulated soft magnetic powder 1 is also referred to as an "insulated soft magnetic particle 4."
[0013] The insulator-coated soft magnetic particles 4 shown in FIG. 1 have soft magnetic particles 2 and an insulating coating 3 provided on the surface of the soft magnetic particles 2. Of these, the soft magnetic particles 2 contain a soft magnetic material described below. The insulating coating 3 is provided so as to cover the surface of the soft magnetic particles 2, and has insulating properties. In this specification, the term "coating" refers to a state in which the entire surface of the soft magnetic particles 2 is covered, as well as a state in which part of the surface is covered. In the following description, the aggregate of the soft magnetic particles 2 is also referred to as "soft magnetic powder."
[0014] As described later, the insulator-coated soft magnetic particles 4 have excellent moisture resistance and are prevented from decreasing in insulation and fluidity due to moisture absorption. Therefore, in a compact obtained by compressing the insulator-coated soft magnetic powder 1, the insulation between the insulator-coated soft magnetic particles 4 is good even when moisture is absorbed, and high packing is obtained, resulting in a high compact density. This allows for a dust core with good voltage resistance and magnetic properties to be obtained.
[0015] 1.1. Soft magnetic particles 1.1.1. Composition of soft magnetic materials The soft magnetic particles 2 are made of a soft magnetic material. Examples of the soft magnetic material include materials that contain at least one of Fe, Ni, and Co as the main component, that is, materials that contain these elements at 50% or more in terms of atomic ratio. In addition to these main components, the soft magnetic material may contain at least one selected from the group consisting of Cr, Nb, Cu, Al, Mn, Mo, Si, Sn, B, C, P, Ti, and Zr depending on the target characteristics. In addition, the soft magnetic material may contain unavoidable impurities within a range that does not impair the effects of this embodiment. The unavoidable impurities are impurities that are unintentionally mixed into the raw materials or during production. The unavoidable impurities include all elements other than the above-mentioned elements, and examples thereof include O, N, S, Na, Mg, K, and the like.
[0016] Specific examples of soft magnetic materials include Fe-Si based alloys such as silicon steel, Fe-Si-Al based alloys such as sendust, as well as various alloys such as Fe-Ni based, Fe-Co based, Fe-Ni-Co based, Fe-Si-B based, Fe-Si-BC based, Fe-Si-B-Cr-C based, Fe-Si-Cr based, Fe-B based, Fe-PC based, Fe-Co-Si-B based, Fe-Si-B-Nb based, Fe-Si-B-Nb-Cu based, Fe-Zr-B based, Fe-Cr based, and Fe-Cr-Al based Fe-based alloys, Ni-based alloys such as Ni-Si-B based and Ni-PB based alloys, and Co-based alloys such as Co-Si-B based alloys.
[0017] By using a soft magnetic material having such a composition, it is possible to obtain insulator-coated soft magnetic particles 4 having high magnetic properties such as magnetic permeability and magnetic flux density, and low coercive force.
[0018] The content of the main component in the soft magnetic material is preferably 50% or more, more preferably 70% or more, in terms of atomic ratio, which can particularly enhance the magnetic properties such as magnetic permeability and magnetic flux density of the insulator-coated soft magnetic particles 4.
[0019] The structure constituting the soft magnetic material is not particularly limited, and may be any of a crystalline structure, an amorphous structure, or a microcrystalline structure. Of these, it is preferable that the soft magnetic material contains an amorphous structure or a microcrystalline structure. By containing these, the coercive force becomes small, which contributes to reducing the hysteresis loss of the magnetic element. Note that the soft magnetic material may contain a mixture of structures with different crystallinity.
[0020] Examples of amorphous and microcrystalline materials include Fe-based alloys such as Fe-Si-B, Fe-Si-BC, Fe-Si-B-Cr-C, Fe-Si-Cr, Fe-B, Fe-PC, Fe-Co-Si-B, Fe-Si-B-Nb, Fe-Si-B-Nb-Cu, and Fe-Zr-B, Ni-based alloys such as Ni-Si-B and Ni-PB, and Co-based alloys such as Co-Si-B.
[0021] The composition of the soft magnetic material is specified by the following analytical method. Examples of analytical methods include iron and steel-atomic absorption spectrometry specified in JIS G 1257:2000, iron and steel-inductively coupled plasma atomic emission spectrometry specified in JIS G 1258:2007, iron and steel-spark discharge atomic emission spectrometry specified in JIS G 1253:2002, iron and steel-fluorescent X-ray analysis specified in JIS G 1256:1997, and gravimetry, titration, and absorptiometry specified in JIS G 1211 to G 1237.
[0022] Specific examples include a solid-state optical emission spectrometer manufactured by SPECTRO, in particular a spark discharge optical emission spectrometer, model: SPECTROLAB, type: LAVMB08A, and an ICP device, CIROS120 type manufactured by Rigaku Corporation.
[0023] In particular, when specifying C (carbon) and S (sulfur), the oxygen flow combustion (high-frequency induction heating furnace combustion)-infrared absorption method specified in JIS G 1211:2 011 is also used. Specifically, the LECO carbon / sulfur analyzer, CS-200, can be used.
[0024] In particular, when specifying N (nitrogen) and O (oxygen), the nitrogen determination method for iron and steel specified in JIS G 1228:1997 and the general method for oxygen determination for metallic materials specified in JIS Z 2613:2006 are also used. Specifically, the LECO oxygen / nitrogen analyzer, TC-300 / EF-300, can be mentioned.
[0025] 1.1.2.Particle size distribution In the particle size distribution of the soft magnetic powder on a volume basis, when the particle size at which the cumulative frequency is 50% is defined as the average particle size, the average particle size of the soft magnetic powder is preferably 2.0 μm or more and 25.0 μm or less, more preferably 3.0 μm or more and 15.0 μm or less, and even more preferably 4.0 μm or more and 10.0 μm or less.
[0026] When the average particle size of the soft magnetic powder is within the above range, the path of eddy currents within the soft magnetic particles 2 is shortened, making it possible to sufficiently reduce eddy current loss in the magnetic element in the high frequency range. In addition, when the average particle size of the soft magnetic powder is within the above range, the filling property during compaction is improved, making it possible to improve magnetic properties such as magnetic permeability, saturation magnetic flux density, as well as density and mechanical strength of the compact.
[0027] If the average particle size of the soft magnetic powder is below the lower limit, aggregation is likely to occur, making it difficult to form the insulating coating 3 and reducing the packing property during compaction, resulting in reduced density, mechanical strength, magnetic properties, etc. of the compact. On the other hand, if the average particle size of the soft magnetic powder is above the upper limit, the path of the eddy current in the particle becomes longer, increasing eddy current loss due to the eddy current in the particle. Also, the density and mechanical strength of the compact are likely to decrease.
[0028] The volumetric particle size distribution of the soft magnetic powder can be obtained, for example, by using a laser diffraction particle size distribution measuring device.
[0029] 1.1.3.Specific surface area The specific surface area of the soft magnetic powder is 0.05 [m 2 / g] or more 0.60[m 2 / g] or less, preferably 0.10 [m 2 / g] or more 0.50[m 2 / g] or less, and more preferably 0.15 [m 2 / g] or more 0.40[m 2 / g] or less. If the specific surface area is within this range, the filling property of the soft magnetic powder during compaction is improved, and the occupancy rate of the insulating coating 3 in the compact can be optimized. As a result, the density and mechanical strength of the compact can be increased, and the magnetic permeability of the compact can be increased.
[0030] If the specific surface area is below the lower limit, the contact area between the soft magnetic powder and the binder decreases, and the mechanical strength of the green compact decreases, whereas if the specific surface area is above the upper limit, the packing property during green compaction decreases, and the density, mechanical strength, magnetic properties, etc. of the green compact decrease.
[0031] The specific surface area of the soft magnetic powder is obtained by the BET method. For example, a specific surface area measuring device such as BET type specific surface area measuring device HM1201-010 manufactured by Mountec Co., Ltd. is used, and the amount of the sample is 5 g.
[0032] 1.1.4.Average circularity The average circularity of the soft magnetic powder is preferably 0.75 to 1, more preferably 0.80 to 1, and even more preferably 0.85 to 1. This allows the particles to roll easily even if the particle size of the soft magnetic powder is small, and allows the packed state to approach close packing. In addition, the mechanical strength of the powder compact can be ensured even if the amount of insulating coating 3 used is reduced, making it easier to increase the density and magnetic permeability of the powder compact.
[0033] If the average circularity is below the lower limit, the flowability of the soft magnetic powder decreases and the packing rate decreases.
[0034] The average circularity of the soft magnetic powder is measured as follows. First, an image (secondary electron image) of the soft magnetic powder is taken with a scanning electron microscope (SEM). Next, the obtained image is loaded into image processing software. For example, image analysis type particle size distribution measurement software "Mac-View" manufactured by Mountech Co., Ltd. is used as the image processing software. The imaging magnification is adjusted so that 50 to 100 particles are captured in one image. Then, multiple images are acquired so that a total of 300 or more particle images are obtained.
[0035] Next, the circularity of 300 or more particle images is calculated using software, and the average value is obtained. The obtained average value is the average circularity of the soft magnetic powder. Note that when the circularity is e, the area of the particle image is s, and the perimeter of the particle image is L, the circularity e can be calculated using the following formula. e=4πs / L2
[0036] 1.1.5.Oxygen content The oxygen content of the soft magnetic powder is preferably 200 ppm or more and 5000 ppm or less, more preferably 400 ppm or more and 4000 ppm or less, and even more preferably 800 ppm or more and 3500 ppm or less, by mass ratio. If the oxygen content is within the above range, the adhesion between the soft magnetic particles 2 and the insulating coating 3 can be increased. Since the insulating coating 3 contains a compound derived from a coupling agent, if the oxygen content of the soft magnetic particles 2 is within the above range, the binding between the coupling agent and the surface of the soft magnetic particles 2 can be increased. As a result, even if the coverage rate of the insulating coating 3 is low, the affinity between the insulator-coated soft magnetic powder 1 and the binder can be increased, and the mechanical strength of the green compact can be increased.
[0037] If the oxygen content falls below the lower limit, the oxide film on the surface of the soft magnetic particles 2 becomes thin, weakening the bond between the soft magnetic particles 2 and the insulating coating 3, which may reduce the mechanical strength of the green compact. On the other hand, if the oxygen content exceeds the upper limit, the oxide film becomes thick, which may reduce the occupancy rate of the soft magnetic particles 2 in the green compact, which may reduce the magnetic properties such as magnetic permeability.
[0038] The oxygen content of the soft magnetic powder is measured, for example, in accordance with the general rules for determining oxygen content of metallic materials as defined in JIS Z 2613: 2006. Specifically, the oxygen content can be measured using a LECO oxygen / nitrogen analyzer, TC-300 / EF-300, a LECO oxygen / nitrogen / hydrogen analyzer, ONH836, or the like.
[0039] 1.1.6. Oxygen content A relative to specific surface area S The oxygen content of the soft magnetic powder is A, and the specific surface area is S. The ratio A / S of the oxygen content A to the specific surface area S of the soft magnetic powder is 3000 or more and 20000 or less, preferably 4000 or more and 15000 or less, and more preferably 5000 or more and 13000 or less. If the ratio A / S is within the above range, the density, mechanical strength, and magnetic permeability of the green compact can be optimized. In particular, even if the specific surface area S of the soft magnetic powder is large, the mechanical strength of the green compact can be increased. This is because the oxygen content A is optimized with respect to the specific surface area S, and the binding force between the soft magnetic particles 2 and the insulating coating 3 can be ensured.
[0040] If the ratio A / S is below the lower limit, the oxygen content A relative to the specific surface area S is too low, weakening the bond between the soft magnetic particles 2 and the insulating coating 3 and reducing the mechanical strength of the green compact. On the other hand, if the ratio A / S is above the upper limit, the oxygen content A relative to the specific surface area S is too high, reducing the occupancy rate of the soft magnetic powder in the green compact and reducing the density and magnetic permeability.
[0041] 1.2.Insulating Coating The insulating coating 3 covers the surfaces of the soft magnetic particles 2. The insulating coating 3 shown in Fig. 1 contains a compound derived from a coupling agent having a hydrophobic functional group.
[0042] 1.2.1.Constituent Materials The insulating coating 3 is formed by reacting a coupling agent having a hydrophobic functional group with the surface of the soft magnetic particles 2. Therefore, the insulating coating 3 contains a compound derived from the coupling agent having a hydrophobic functional group, and exhibits properties derived from the hydrophobic functional group.
[0043] Examples of the hydrophobic functional group include those containing a saturated hydrocarbon group, a group containing a cyclic structure, a fluoroalkyl group, a fluoroaryl group, a nitro group, an acyl group, a cyano group, etc. These impart good hydrophobicity to the insulating coating 3.
[0044] Among these, the hydrophobic functional group is preferably a hydrocarbon group, more preferably a saturated hydrocarbon group, and even more preferably a linear alkyl group having 1 to 6 carbon atoms. This can impart particularly high hydrophobicity to the insulating coating 3. As a result, an insulator-coated soft magnetic powder 1 is obtained that has excellent flowability and good packing properties when compressed even in a humid environment. If the carbon number exceeds the upper limit, it becomes difficult to form a state in which adjacent long-chain alkyl groups are regularly arranged. In other words, the arrangement of adjacent long-chain alkyl groups may be disrupted. This may result in a decrease in the hydrophobicity of the insulating coating 3.
[0045] The hydrophobic functional group may be a cyclic structure-containing group. The cyclic structure-containing group has a cyclic structure and imparts particularly high hydrophobicity to the insulating coating 3. In addition, since the cyclic structure is highly stable, good hydrophobicity can be maintained even after heating. For this reason, an insulator-coated soft magnetic powder 1 having excellent flowability and good packing properties during compaction can be obtained even in a humid environment.
[0046] Examples of the cyclic structure-containing group include an aromatic hydrocarbon group, an alicyclic hydrocarbon group, and a cyclic ether group.
[0047] The aromatic hydrocarbon group is a residue obtained by removing hydrogen atoms from an aromatic hydrocarbon, and preferably has 6 to 20 carbon atoms. Examples of the aromatic hydrocarbon group include an aryl group, an alkylaryl group, an aminoaryl group, and a halogenated aryl group. Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and an indenyl group. Examples of the alkylaryl group include a benzyl group, a methylbenzyl group, a phenethyl group, a methylphenethyl group, and a phenylbenzyl group. The aromatic hydrocarbon group may be substituted with a substituent such as an alkyl group having 1 to 3 carbon atoms.
[0048] The alicyclic hydrocarbon group is a residue obtained by removing a hydrogen atom from an alicyclic hydrocarbon, and preferably has 3 to 20 carbon atoms. Examples of the alicyclic hydrocarbon group include a cycloalkyl group and a cycloalkylalkyl group. Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. Examples of the cycloalkylalkyl group include a cyclopentylmethyl group and a cyclohexylmethyl group. The alicyclic hydrocarbon group may be substituted with a substituent such as an alkyl group having 1 to 3 carbon atoms.
[0049] Examples of the cyclic ether group include an epoxy group, a 3,4-epoxycyclohexyl group, an oxetanyl group, etc. The cyclic ether group may be substituted with a substituent such as an alkyl group having 1 to 3 carbon atoms.
[0050] The hydrocarbon group and the cyclic structure-containing group have good affinity with the binder used during powder compaction. This increases the binding force between the insulator-coated soft magnetic powder 1 and the binder, thereby increasing the mechanical strength of the compact. In addition, the amount of binder used can be reduced while maintaining the mechanical strength of the compact, thereby increasing the occupancy rate of the soft magnetic powder in the compact.
[0051] The hydrophobic functional group may be a fluoroalkyl group or a fluoroaryl group. These groups impart particularly high hydrophobicity to the insulating coating 3. Fluorine-containing fluoroalkyl groups and fluoroaryl groups have low surface tension due to the fluorine atoms, and therefore have particularly excellent hydrophobicity. For this reason, an insulator-coated soft magnetic powder 1 can be obtained that has excellent flowability and good packing properties during compaction even in a humid environment.
[0052] The fluoroalkyl group is an alkyl group having from 1 to 16 carbon atoms, which is substituted with one or more fluorine atoms, or a cycloalkyl group having from 3 to 16 carbon atoms. In particular, the fluoroalkyl group is preferably a perfluoroalkyl group.
[0053] The fluoroaryl group is an aryl group substituted with one or more fluorine atoms and having from 6 to 20 carbon atoms. In particular, the fluoroaryl group is preferably a perfluoroaryl group.
[0054] 1.2.2.Average thickness The average thickness of the insulating coating 3 is not particularly limited, but is preferably 0.1 nm to 50 nm, more preferably 0.5 nm to 30 nm, and even more preferably 1 nm to 20 nm. This ensures a film thickness necessary to maintain the insulating coating 3, and the above-mentioned effects can be sufficiently obtained, while preventing the occupancy rate of the insulating coating 3 in the insulation-coated soft magnetic powder 1 from becoming high.
[0055] The average thickness of the insulating coating 3 can be determined by, for example, qualitative and quantitative analysis in the depth direction using a combination of X-ray photoelectron spectroscopy and ion sputtering. Specifically, the concentration of the component derived from the coupling agent is examined in the depth direction. The region where the concentration of the component derived from the coupling agent is relatively high is then determined as the average thickness of the insulating coating 3. Specifically, when the concentration changes near the boundary between the insulating coating 3 and the soft magnetic particles 2, half of the amount of change in concentration, that is, the position corresponding to the midpoint between the concentration on the insulating coating 3 side and the concentration on the soft magnetic particle 2 side, is regarded as the boundary, and the thickness on the surface side of the boundary is determined as the average thickness of the insulating coating 3.
[0056] Coverage The coverage of the insulating coating 3 is the ratio of the area covered by the insulating coating 3 to the entire surface of the soft magnetic particle 2. The coverage of the insulating coating 3 is preferably 20% or more and 120% or less, more preferably 30% or more and 110% or less, and even more preferably 40% or more and 100% or less. This ensures sufficient insulation between the soft magnetic particles 2 by the insulating coating 3, and reduces the iron loss of the green compact. In addition, the affinity between the insulator-coated soft magnetic powder 1 and the binder can be further increased, and the mechanical strength of the green compact can be increased or the amount of the binder used can be reduced while maintaining the mechanical strength of the green compact. A coverage rate of more than 100% means that two or more molecules of the compound derived from the coupling agent overlap on a part of the surface of the soft magnetic particle 2.
[0057] If the coverage rate of the insulating coating 3 is below the lower limit, the mechanical strength of the green compact may decrease. On the other hand, if the coverage rate of the insulating coating 3 is above the upper limit, compounds derived from the coupling agent may become excessive, which may decrease the density and magnetic permeability of the green compact.
[0058] The coverage of the insulating coating 3 can be calculated from the amount of compound contained in the insulating-material-coated soft magnetic powder 1, the amount of the soft magnetic powder, the minimum coverage area of the coupling agent, and the specific surface area of the soft magnetic powder.
[0059] 1.3.Moisture content The moisture content of the insulator-coated soft magnetic powder 1 is not particularly limited, but is preferably 30 ppm or more and 500 ppm or less, more preferably 40 ppm or more and 300 ppm or less, and even more preferably 50 ppm or more and 200 ppm or less. If the moisture content of the insulator-coated soft magnetic powder 1 is within the above range, the decrease in fluidity due to the adsorption of moisture is suppressed. Therefore, the insulator-coated soft magnetic powder 1 having excellent fluidity can be obtained. In addition, if the moisture content is within the above range, the chargeability of the insulator-coated soft magnetic powder 1 can be controlled within an appropriate range, and the decrease in fluidity due to charging can be suppressed. Furthermore, if the moisture content is within the above range, rusting of the soft magnetic particles 2 due to moisture can be suppressed, and the decrease in magnetic properties of the compact can also be suppressed.
[0060] If the moisture content is below the lower limit, the insulator-coated soft magnetic powder 1 may be easily charged and the fluidity may decrease. On the other hand, if the moisture content is above the upper limit, the moisture content of the insulator-coated soft magnetic powder 1 may be too high, resulting in a decrease in fluidity and causing rusting of the soft magnetic particles 2.
[0061] The moisture content of the insulator-coated soft magnetic powder 1 is measured by leaving the insulator-coated soft magnetic powder 1 to be measured in an environment of 25° C. temperature and 50% relative humidity for 1 hour or more, and then measuring the moisture content at 250° C. by the Karl Fischer method. For example, a moisture measuring device CA-310 manufactured by Nitto Seiko Analytech Co., Ltd. is used for the measurement.
[0062] 1.4.Ring crushing strength The insulator-coated soft magnetic powder 1 was mixed with 2% by mass of epoxy resin and dried at 50°C for 1 hour to obtain a granulated powder. The obtained granulated powder was then compressed under a pressure of 294.2 MPa (3 t / cm 2 ) and then heated at 150°C for 30 minutes to harden the epoxy resin, the resulting molded article preferably has a radial crushing strength of 10 MPa or more, more preferably 20 MPa or more, and even more preferably 30 MPa or more. This makes it possible to realize a magnetic element with high mechanical strength and high reliability. The upper limit does not need to be set in particular, but from the viewpoint of reducing manufacturing variations, it is preferably 60 MPa or less, and more preferably 50 MPa or less.
[0063] The shape of the molded body is annular with an outer diameter of 14 mm, an inner diameter of 8 mm, and a thickness of 3 mm. The method for measuring the radial crushing strength is in accordance with the radial crushing strength test method specified in JIS Z 2507:2000. Specifically, when the radial crushing strength is K, the outer diameter is D, the radial thickness (half the difference between the outer diameter and the inner diameter) is t, the thickness is L, and the breaking load is F, the radial crushing strength K can be calculated as K=F(Dt) / (Lt2).
[0064] 2. Manufacturing method of insulator-coated soft magnetic powder Next, a method for producing the insulator-coated soft magnetic powder 1 will be described. FIG. 2 is a process diagram illustrating a method for producing the insulator-coated soft magnetic powder 1. As shown in FIG.
[0065] The method for producing an insulating-material-coated soft magnetic powder shown in FIG. 2 includes a preparation step S102 and an insulating coating forming step S104.
[0066] 2.1. Preparation process In the preparation step S102, soft magnetic powder is prepared. The soft magnetic powder may be a powder produced by any method. Examples of the production method include various atomization methods such as water atomization, gas atomization, and rotary water flow atomization, as well as reduction, carbonyl, and pulverization. Among these, the atomization method is preferably used. That is, the soft magnetic powder is preferably an atomized powder. Atomized powder is fine, has high sphericity, and has high production efficiency. In particular, water atomized powder or rotary water flow atomized powder has a thin oxide film on the surface because it is produced by contacting molten metal with water. This oxide film can be the base of the insulating coating 3. For this reason, the soft magnetic particles 2 and the insulating coating 3 have excellent adhesion, and finally, the insulator-coated soft magnetic particles 4 having particularly high insulation between the particles are obtained. In addition, since the cooling rate is fast, it is also possible to produce soft magnetic powder including an amorphous structure or a microcrystalline structure.
[0067] 2.2. Insulating film formation process In the insulating coating formation step S104, a coupling agent having a hydrophobic functional group is reacted with the soft magnetic particles 2. As a result, the coupling agent is attached to the surface of the soft magnetic particles 2.
[0068] Examples of this operation include the following three operations. The first operation includes an operation of putting both the soft magnetic particles 2 and the coupling agent into a chamber, and then heating the inside of the chamber.
[0069] The second operation includes an operation of putting the soft magnetic particles 2 into a chamber, and then spraying a coupling agent into the chamber while stirring the soft magnetic particles 2.
[0070] The third operation includes adding water, a coupling agent, an alkaline solution such as ammonia or sodium hydroxide, and the soft magnetic particles 2 to a primary alcohol such as methanol, ethanol, or isopropyl alcohol, stirring the mixture, filtering, and then drying.
[0071] Examples of the coupling agent include a silane coupling agent, a titanium coupling agent, and a zirconium coupling agent. The following chemical formula is an example of the molecular structure of a silane coupling agent.
[0072] [ka]
[0073] In the above formula, X is a functional group, Y is a spacer, and OR is a hydrolyzable group, and R is, for example, a methyl group or an ethyl group.
[0074] Examples of the spacer include an alkylene group, an arylene group, an aralkylene group, and an alkylene ether group.
[0075] The hydrolyzable group is, for example, an alkoxy group, a halogen atom, a cyano group, an acetoxy group, an isocyanate group, etc., and among these, in the case of an alkoxy group, a silanol is generated by hydrolysis. This silanol reacts with the hydroxyl group generated on the surface of the soft magnetic particle 2, and the coupling agent adheres to the surface of the soft magnetic particle 2.
[0076] The coupling agent may contain at least one such hydrolyzable group, but preferably contains two or more, and more preferably contains three hydrolyzable groups as shown in the above formula. For example, a coupling agent whose hydrolyzable group is an alkoxy group preferably contains a dialkoxy group, and more preferably contains a trialkoxy group. A coupling agent containing a trialkoxy group reacts with three hydroxyl groups generated on the surface of the soft magnetic particles 2. For this reason, it has good adhesion to the soft magnetic particles 2. In addition, a coupling agent containing a trialkoxy group is also excellent in film-forming properties, so that an insulating coating 3 with excellent continuity can be obtained. Such an insulating coating 3 contributes to further increasing the fluidity of the insulator-coated soft magnetic powder 1.
[0077] Furthermore, in the case of a coupling agent containing a trialkoxy group, even if the hydrophobic functional group is thermally decomposed after the insulating coating 3 is formed, the remainder can continue to cover the surfaces of the soft magnetic particles 2. This makes it possible to suppress a decrease in hydrophobicity.
[0078] Here, examples of coupling agents having a hydrophobic functional group are given. Examples of coupling agents having an aromatic hydrocarbon group include, for example, Phenyltrimethoxysilane represented by the following formula (A-1):
[0079] [ka]
[0080] Phenyltriethoxysilane represented by the following formula (A-2):
[0081] [ka]
[0082] Dimethoxydiphenylsilane represented by the following formula (A-3):
[0083] [ka]
[0084] 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane represented by the following formula (A-4):
[0085] [ka]
[0086] 3-phenoxypropyltrichlorosilane represented by the following formula (A-11):
[0087] [ka]
[0088] Phenyltriacetoxysilane represented by the following formula (A-12):
[0089] [ka]
[0090] Triethoxy(p-tolyl)silane represented by the following formula (A-13):
[0091] [ka]
[0092] p-aminophenyltrimethoxysilane represented by the following formula (A-14):
[0093] [ka]
[0094] m-aminophenyltrimethoxysilane represented by the following formula (A-15):
[0095] [ka]
[0096] ((chloromethyl)phenylethyl)trimethoxysilane represented by the following formula (A-16):
[0097] [ka] etc.
[0098] Examples of coupling agents having a cyclic ether group include: 3-glycidoxypropylmethyldimethoxysilane represented by the following formula (A-5):
[0099] [ka]
[0100] 3-glycidoxypropyltrimethoxysilane represented by the following formula (A-6):
[0101] [ka]
[0102] 3-glycidoxypropylmethyldiethoxysilane represented by the following formula (A-7):
[0103] [ka]
[0104] 3-glycidoxypropyltriethoxysilane represented by the following formula (A-8):
[0105] [ka] etc.
[0106] Examples of coupling agents having a fluoroalkyl group include: Trimethoxy(3,3,3-trifluoropropyl)silane represented by the following formula (B-1):
[0107] [ka]
[0108] Trimethoxy(1H,1H,2H,2H-tridecafluoro-n-octyl)silane represented by the following formula (B-2):
[0109] [ka]
[0110] Trimethoxy(1H,1H,2H,2H-nonafluorohexyl)silane represented by the following formula (B-3):
[0111] [ka] etc.
[0112] Examples of coupling agents having a fluoroaryl group include: Trimethoxy(11-pentafluorophenoxyundecyl)silane represented by the following formula (C-1):
[0113] [ka]
[0114] Pentafluorophenyldimethylchlorosilane represented by the following formula (C-2):
[0115] [ka] etc.
[0116] The amount of the coupling agent added is not particularly limited, but is preferably 0.01% by mass to 1.00% by mass, and more preferably 0.05% by mass to 0.50% by mass, relative to the soft magnetic particles 2.
[0117] The coupling agent is supplied by being left stationary in the chamber or by being sprayed into the chamber.
[0118] Thereafter, the soft magnetic particles 2 to which the coupling agent is attached are heated. As a result, an insulating coating 3 is formed on the surface of the soft magnetic particles 2, and an insulator-coated soft magnetic powder 1 is obtained. In addition, unreacted coupling agent can be removed by heating.
[0119] The heating temperature of the soft magnetic particles 2 to which the coupling agent is attached is not particularly limited, but is preferably 50° C. to 300° C., and more preferably 100° C. to 250° C. The heating time is preferably 10 minutes to 24 hours, and more preferably 30 minutes to 10 hours. Examples of the atmosphere for the heat treatment include air and inert gas.
[0120] 3. Powder cores and magnetic components Next, the powder magnetic core and the magnetic element according to the embodiment will be described.
[0121] The magnetic element according to the embodiment can be applied to various magnetic elements having a magnetic core, such as a choke coil, an inductor, a noise filter, a reactor, a transformer, a motor, an actuator, an electromagnetic valve, a generator, etc. Furthermore, the powder magnetic core according to the embodiment can be applied to the magnetic cores included in these magnetic elements.
[0122] Two types of coil components will be described below as representative examples of the magnetic element. 3.1.Toroidal type First, a toroidal type coil component, which is an example of a magnetic element according to the embodiment, will be described. FIG. 3 is a plan view that illustrates a schematic diagram of a toroidal type coil component.
[0123] 3 has a ring-shaped powder core 11 and a conductive wire 12 wound around this powder core 11. Such a coil component 10 is generally called a toroidal coil.
[0124] The powder magnetic core 11 is obtained by mixing the insulator-coated soft magnetic powder according to the embodiment with a binder, supplying the mixture to a molding die, and pressing and molding it. Since the powder magnetic core 11 is a compact containing the insulator-coated soft magnetic powder according to the embodiment, it is possible to realize a coil component 10 that has both magnetic properties and mechanical strength. Therefore, when the coil component 10 is mounted on an electronic device or the like, it is possible to improve the performance and reduce the size of the electronic device or the like.
[0125] Examples of the binder material used to manufacture the powder magnetic core 11 include organic materials such as silicone resins, epoxy resins, phenol resins, polyamide resins, polyimide resins, and polyphenylene sulfide resins, and inorganic materials such as phosphates such as magnesium phosphate, calcium phosphate, zinc phosphate, manganese phosphate, and cadmium phosphate, and silicates such as sodium silicate. Thermosetting polyimide or epoxy resins are particularly preferred. These resin materials are easily cured by heating and have excellent heat resistance. This can improve the ease of manufacture and heat resistance of the powder magnetic core 11.
[0126] The ratio of the binder to the insulator-coated soft magnetic powder varies slightly depending on the desired magnetic properties, mechanical properties, allowable eddy current loss, etc. of the powder core 11 to be produced, but is preferably about 0.3% by mass to 5.0% by mass, more preferably about 0.5% by mass to 3.0% by mass, and even more preferably about 0.7% by mass to 2.0% by mass. This allows the particles of the insulator-coated soft magnetic powder to be sufficiently bound together, while providing a coil component 10 with excellent magnetic properties. If necessary, various additives may be added to the mixture for any purpose.
[0127] Examples of materials constituting the conductor 12 include highly conductive materials, such as metal materials including Cu, Al, Ag, Au, Ni, etc. Furthermore, an insulating film may be provided on the surface of the conductor 12 as necessary.
[0128] The shape of the powder magnetic core 11 is not limited to the ring shape shown in FIG. 3, but may be, for example, a ring shape in which part of the ring is missing, a shape in which the longitudinal direction is linear, or a sheet or film shape.
[0129] The dust core 11 may contain soft magnetic powder other than the insulator-coated soft magnetic powder according to the embodiment described above, or non-magnetic powder, as necessary.
[0130] 3.2.Closed magnetic circuit type Next, a closed magnetic circuit type coil component, which is an example of a magnetic element according to the embodiment, will be described. FIG. 4 is a see-through perspective view that typically shows a closed magnetic circuit type coil component.
[0131] The closed magnetic circuit type coil component will be described below, but in the following description, the differences from the toroidal type coil component will be mainly described, and a description of similar points will be omitted.
[0132] 4, the coil component 20 according to this embodiment is formed by embedding a conductor wire 22 formed into a coil shape inside a powder magnetic core 21. That is, the coil component 20, which is a magnetic element, includes a powder magnetic core 21 containing the above-mentioned insulator-coated soft magnetic powder, and is formed by molding the conductor wire 22 with the powder magnetic core 21. This powder magnetic core 21 has a similar configuration to the above-mentioned powder magnetic core 11. This makes it possible to realize a coil component 20 with high magnetic properties and mechanical strength.
[0133] Moreover, the coil component 20 having such a configuration can be made relatively small in size. Therefore, when the coil component 20 is mounted in an electronic device or the like, the electronic device or the like can be made smaller and with higher performance.
[0134] Furthermore, because the conductive wire 22 is embedded inside the powder core 21, a gap is unlikely to occur between the conductive wire 22 and the powder core 21. This makes it possible to suppress vibrations caused by magnetostriction of the powder core 21, and also to suppress the generation of noise associated with this vibration.
[0135] The shape of the powder magnetic core 21 is not limited to the shape shown in FIG. 4, and may be a sheet, a film, or the like.
[0136] Furthermore, the dust core 21 may contain soft magnetic powder other than the insulator-coated soft magnetic powder according to the embodiment described above, or non-magnetic powder, as necessary.
[0137] 4.Electronic equipment Next, an electronic device including the magnetic element according to the embodiment will be described with reference to FIGS.
[0138] Fig. 5 is a perspective view showing a mobile personal computer, which is an electronic device including a magnetic element according to an embodiment. The personal computer 1100 shown in Fig. 5 includes a main body 1104 including a keyboard 1102, and a display unit 1106 including a display unit 100. The display unit 1106 is rotatably supported by the main body 1104 via a hinge structure. Such a personal computer 1100 includes a magnetic element 1000, such as a choke coil or inductor for a switching power supply, or a motor.
[0139] Fig. 6 is a plan view showing a smartphone, which is an electronic device including the magnetic element according to the embodiment. The smartphone 1200 shown in Fig. 6 includes a plurality of operation buttons 1202, an earpiece 1204, and a mouthpiece 1206. A display unit 100 is disposed between the operation buttons 1202 and the earpiece 1204. Such a smartphone 1200 includes a magnetic element 1000, such as an inductor, a noise filter, or a motor.
[0140] 7 is a perspective view showing a digital still camera, which is an electronic device including the magnetic element according to the embodiment. The digital still camera 1300 photoelectrically converts an optical image of a subject using an imaging element such as a CCD (Charge Coupled Device) to generate an imaging signal.
[0141] 7 includes a display unit 100 provided on the back of a case 1302. The display unit 100 functions as a viewfinder that displays a subject as an electronic image. In addition, a light receiving unit 1304 including an optical lens, a CCD, etc. is provided on the front side of the case 1302, i.e., on the back side in the figure.
[0142] When the photographer checks the subject image displayed on the display unit 100 and presses the shutter button 1306, the image signal of the CCD at that time is transferred to and stored in memory 1308. Such a digital still camera 1300 also has a built-in magnetic element 1000, such as an inductor or a noise filter.
[0143] Examples of electronic devices according to the embodiments include the personal computer of FIG. 5, the smartphone of FIG. 6, and the digital still camera of FIG. 7, as well as mobile phones, tablet terminals, watches, inkjet discharge devices such as inkjet printers, laptop personal computers, televisions, video cameras, video tape recorders, car navigation devices, pagers, electronic organizers, electronic dictionaries, calculators, electronic game devices, word processors, workstations, videophones, security television monitors, electronic binoculars, POS terminals, medical devices such as electronic thermometers, blood pressure monitors, blood glucose meters, electrocardiogram measuring devices, ultrasonic diagnostic devices, and electronic endoscopes, fish finders, various measuring devices, instruments for vehicles, aircraft, and ships, mobile object control devices such as automobile control devices, aircraft control devices, railway vehicle control devices, and ship control devices, and flight simulators.
[0144] As described above, such electronic devices include the magnetic element according to the embodiment, which provides both magnetic properties and mechanical strength, and thus allows the electronic devices to have high performance and be compact.
[0145] 5. Advantages of the above embodiment As described above, the insulating material-coated soft magnetic powder 1 according to this embodiment includes a soft magnetic powder and an insulating coating 3. The insulating coating 3 coats the surfaces of the soft magnetic particles 2 (particle surfaces of the soft magnetic powder) and contains a compound having a hydrophobic functional group derived from a coupling agent. The soft magnetic powder has an average particle size of 2.0 μm or more and 25.0 μm or less, and a specific surface area of 0.05 m 2 / g or more 0.60m 2 / g or less. In addition, the specific surface area of the soft magnetic powder is S[m 2 / g] and the oxygen content in the soft magnetic powder is A [ppm], the ratio A / S is 3,000 or more and 20,000 or less.
[0146] According to this configuration, even when the specific surface area of the soft magnetic powder is large, it is possible to obtain the insulator-coated soft magnetic powder 1 that can achieve both high density and mechanical strength of the powder compact.
[0147] The oxygen content A in the soft magnetic powder is preferably 200 ppm or more and 5000 ppm or less.
[0148] This configuration can improve the adhesion between the soft magnetic particles 2 and the insulating coating 3. This can increase the affinity between the insulator-coated soft magnetic powder 1 and the binder, thereby increasing the mechanical strength of the green compact.
[0149] The hydrophobic functional group is preferably a hydrocarbon group. This configuration can impart particularly high hydrophobicity to the insulating coating 3. As a result, the insulating material-coated soft magnetic powder 1 has excellent flowability even in a humid environment and good packing properties when compressed.
[0150] The hydrocarbon group is preferably a linear alkyl group having 1 to 6 carbon atoms.
[0151] This configuration can impart particularly high hydrophobicity to the insulating coating 3. As a result, the insulating material-coated soft magnetic powder 1 has excellent flowability even in a humid environment and good packing properties when compressed.
[0152] The hydrophobic functional group may also be a group containing a cyclic structure. The cyclic structure-containing group has a cyclic structure and imparts particularly high hydrophobicity to the insulating coating 3 . In addition, the ring structure is highly stable and can maintain good hydrophobicity even after heating, which allows the insulation-coated soft magnetic powder 1 to be obtained that has excellent flowability and good packing properties during compaction even in a humid environment.
[0153] Moreover, the coverage of the insulating coating 3 is preferably not less than 20% and not more than 120%. With this configuration, the insulation between the soft magnetic particles 2 by the insulating coating 3 can be sufficiently ensured, and the iron loss of the green compact can be reduced. Also, the affinity between the insulator-coated soft magnetic powder 1 and the binder can be further increased, and the mechanical strength of the green compact can be increased or the amount of binder used can be reduced while maintaining the mechanical strength of the green compact.
[0154] In addition, it is preferable that the epoxy resin is mixed with 2 mass % of the epoxy resin, the resulting mixture is press-molded at a pressure of 294.2 MPa, and then heated at 150°C for 30 minutes to harden the epoxy resin, resulting in a molded article having a radial crushing strength of 10 MPa or more.
[0155] According to this configuration, it is possible to obtain the insulator-coated soft magnetic powder 1 that can realize a magnetic element having high mechanical strength and high reliability.
[0156] In addition, the water content measured at 250° C. by the Karl Fischer method is preferably 30 ppm or more and 500 ppm or less.
[0157] According to this configuration, the decrease in fluidity due to the adsorption of moisture is suppressed, and the excellent fluidity of the insulator-coated soft magnetic powder 1 can be obtained. In addition, the chargeability of the insulator-coated soft magnetic powder 1 can be controlled within an appropriate range, and the decrease in fluidity due to charging can be suppressed.
[0158] Moreover, the powder magnetic core according to the embodiment contains the insulator-coated soft magnetic powder according to the embodiment, thereby obtaining a powder magnetic core capable of realizing a magnetic element that achieves both magnetic properties and mechanical strength.
[0159] Moreover, the magnetic element according to the embodiment includes the powder magnetic core according to the embodiment, thereby obtaining a magnetic element that has both excellent magnetic properties and excellent mechanical strength.
[0160] Moreover, the electronic device according to the embodiment includes the magnetic element according to the embodiment, thereby providing an electronic device with high performance and small size.
[0161] The insulator-coated soft magnetic powder, the dust core, the magnetic element, and the electronic device of the present invention have been described above based on the preferred embodiments, but the present invention is not limited thereto.
[0162] For example, in the above embodiment, the application example of the insulator-coated soft magnetic powder of the present invention has been described with reference to a dust core, but the application example is not limited thereto and may be, for example, a magnetic device such as a magnetic fluid, a magnetic head, a magnetic shielding sheet, etc. Furthermore, the shapes of the dust core and the magnetic element are not limited to those shown in the drawings and may be any shape.
[0163] Moreover, the powder magnetic core and magnetic element according to the present invention may be configured in such a manner that any desired component is added to the above-described embodiment. EXAMPLES
[0164] Next, specific examples of the present invention will be described. 6. Preparation of insulator-coated soft magnetic powder 6.1. Sample No. 1 First, soft magnetic powder composed of the soft magnetic material shown in Table 1 was produced by an atomization method. The composition of the soft magnetic material is as shown in Table 1. The average particle size, specific surface area, oxygen content, average circularity, etc. of the soft magnetic powder are as shown in Table 2.
[0165] Next, an insulating film was formed on the surface of the soft magnetic powder particles. The hydrophobic functional group of the coupling agent used to form the insulating film, the number of carbon atoms when the hydrophobic functional group is an alkyl group, and the coverage rate of the insulating film are as shown in Table 2.
[0166] In this manner, an insulator-coated soft magnetic powder was obtained as sample No. 1. Thereafter, the moisture content of the obtained insulator-coated soft magnetic powder was measured. The measurement results are shown in Table 2.
[0167] 6.2. Samples No. 2 to 26 Except for changing the composition of the insulator-coated soft magnetic powder as shown in Tables 1 and 2, the insulator-coated soft magnetic powders of Samples Nos. 2 to 26 were obtained in the same manner as Sample No. 1.
[0168] [Table 1]
[0169] In Table 2 shown later, among the insulator-coated soft magnetic powders of each sample number, those that correspond to the present invention are labeled "Examples", and those that do not correspond to the present invention are labeled "Comparative Examples".
[0170] In addition, the chemical formula symbols shown in Table 2 correspond to the following compounds. A-1: Phenyltrimethoxysilane A-6: 3-glycidoxypropyltrimethoxysilane B-1: Trimethoxy(3,3,3-trifluoropropyl)silane C-1: Trimethoxy(11-pentafluorophenoxyundecyl)silane D-1: Methyltrimethoxysilane D-2: Propyltrimethoxysilane D-3: Hexyltrimethoxysilane D-4: Octyltrimethoxysilane
[0171] 7. Evaluation of insulator-coated soft magnetic powder 7.1. Relative density of green body First, each of the insulator-coated soft magnetic powders was mixed with an epoxy resin as a binder and toluene as an organic solvent to obtain a mixture. The amount of the epoxy resin added was 2 parts by mass per 100 parts by mass of the insulator-coated soft magnetic powder.
[0172] Next, the obtained mixture was stirred and then dried at 50° C. for 1 hour in an air atmosphere to obtain a lump-shaped dried product, which was then sieved through a sieve with a mesh size of 400 μm and pulverized to obtain a granulated powder.
[0173] Next, the obtained granulated powder was filled into a molding die, and a green compact was obtained based on the following molding conditions.
[0174] Molding method: Press molding Shape of molding: Ring -Dimensions of molded body: Outer diameter 14mm, inner diameter 8mm, thickness 3mm ·Molding pressure: 3t / cm 2 (294.2MPa)
[0175] Next, the green compact was heated at 150° C. for 30 minutes in an air atmosphere to harden the binder, thereby obtaining a ring-shaped compact.
[0176] Next, the density of the green compact was measured. Next, the density of the green compact was divided by the true density of the soft magnetic powder to calculate the relative density. The calculated relative density was then evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2.
[0177] A: Relative density is 67% or more B: Relative density is 66% or more and less than 67% C: Relative density is 65% or more and less than 66% D: Relative density is 64% or more but less than 65% E: Relative density is 63% or more and less than 64% F: Relative density is less than 63%
[0178] 7.2. Radial crushing strength of compact The radial crushing strength of the molded bodies prepared in the same manner as in 7.1 was measured according to the radial crushing strength test method specified in JIS Z 2507:2000. The radial crushing strength was evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2.
[0179] A: Radial crushing strength is 50 MPa or more B: Radial crushing strength is 45 MPa or more and less than 50 MPa C: Radial crushing strength is 40 MPa or more and less than 45 MPa D: The radial crushing strength is 35 MPa or more and less than 40 MPa. E: Radial crushing strength is 30 MPa or more and less than 35 MPa F: The radial crushing strength is less than 30 MPa.
[0180] 7.3. Magnetic permeability of compact The magnetic permeability of the compact produced in the same manner as in 7.1 was measured. The magnetic permeability of the compact is the relative magnetic permeability, i.e., effective magnetic permeability, found from the self-inductance of a closed magnetic circuit magnetic core coil produced in the compact described above. The magnetic permeability was measured using an impedance analyzer at a measurement frequency of 100 kHz. The number of turns of the winding was 7, and the wire diameter of the winding was 0.6 mm.
[0181] The measured magnetic permeability was evaluated in accordance with the following evaluation criteria. The evaluation results are shown in Table 2. The reference values in the following evaluation criteria are values set for each soft magnetic material, and are the magnetic permeability of a compact made using the soft magnetic powder of sample No. 21 for the crystalline material, the soft magnetic powder of sample No. 25 for the amorphous material 1, and the soft magnetic powder of sample No. 26 for the amorphous material 2.
[0182] A: The measured magnetic permeability is 115% or more of the standard value. B: The measured magnetic permeability is 110% or more but less than 115% of the standard value. C: The measured permeability is 105% or more but less than 110% of the standard value. D: The measured magnetic permeability is 100% or more but less than 105% of the standard value. E: The measured magnetic permeability is 95% or more but less than 100% of the standard value. F: The measured permeability is less than 95% of the standard value.
[0183] 7.4. Core loss of compact The iron loss of the compacts prepared in the same manner as in 7.1 was measured under the following conditions:
[0184] Measurement equipment: BH analyzer, Iwasaki Electric Co., Ltd. SY-8258 Measurement frequency: 900kHz Number of turns of winding: 36 turns on the primary side, 36 turns on the secondary side Winding wire diameter: 0.5mm Maximum magnetic flux density: 50mT
[0185] Next, the measured iron loss was evaluated in accordance with the following evaluation criteria. The evaluation results are shown in Table 2. The reference values in the following evaluation criteria are values set for each soft magnetic material, and are the iron loss of compacts made using soft magnetic powder sample No. 21 for crystalline material, soft magnetic powder sample No. 25 for amorphous material 1, and soft magnetic powder sample No. 26 for amorphous material 2.
[0186] A: The measured iron loss value is less than 85% of the standard value. B: The measured iron loss value is between 85% and 90% of the standard value. C: The measured iron loss value is 90% or more but less than 95% of the standard value. D: The measured iron loss value is 95% or more but less than 100% of the standard value. E: The measured iron loss value is 100% or more but less than 105% of the standard value. F: The measured iron loss value is 105% or more of the reference value.
[0187] [Table 2]
[0188] As shown in Table 2, it was found that the insulator-coated soft magnetic powder of each Example can produce a compact with higher density, radial crushing strength, and magnetic permeability than the insulator-coated soft magnetic powder of the comparative example. In particular, it was found that even when the specific surface area S is large, the radial crushing strength can be increased by optimizing the ratio of the oxygen content A to the specific surface area S. It was also found that the use of the insulator-coated soft magnetic powder of each Example can produce a compact with low iron loss. [Explanation of symbols]
[0189] Reference Signs List 1...insulating material-coated soft magnetic powder, 2...soft magnetic particles, 3...insulating coating, 4...insulating material-coated soft magnetic particles, 10...coil component, 11...powder core, 12...conductor, 20...coil component, 21...powder core, 22...conductor, 100...display unit, 1000...magnetic element, 1100...personal computer, 1102...keyboard, 1104...main body, 1106...display unit, 1200...smartphone, 1202...operation buttons, 1204...earpiece, 1206...mouthpiece, 1300...digital still camera, 1302...case, 1304...light-receiving unit, 1306...shutter button, 1308...memory, S102...preparation process, S104...inorganic insulating film formation process.
Claims
1. A soft magnetic powder; an insulating coating that coats the particle surfaces of the soft magnetic powder and contains a compound having a hydrophobic functional group derived from a coupling agent; Equipped with The average particle size of the soft magnetic powder is 2.0 μm or more and 25.0 μm or less, The specific surface area of the soft magnetic powder is 0.05 m 2 / g or more 0.60m 2 / g or less, The specific surface area is defined as S [m 2 / g] and the oxygen content in the soft magnetic powder is A [ppm], the ratio A / S is 3,000 or more and 20,000 or less.
2. 2. The insulator-coated soft magnetic powder according to claim 1, wherein the oxygen content A in the soft magnetic powder is 200 ppm or more and 5000 ppm or less.
3. 3. The insulator-coated soft magnetic powder according to claim 1, wherein the hydrophobic functional group is a hydrocarbon group.
4. 4. The insulator-coated soft magnetic powder according to claim 3, wherein the hydrocarbon group is a linear alkyl group having 1 to 6 carbon atoms.
5. 3. The insulator-coated soft magnetic powder according to claim 1, wherein the hydrophobic functional group is a group containing a cyclic structure.
6. 3. The insulator-coated soft magnetic powder according to claim 1, wherein the insulating coating has a coverage rate of 20% or more and 120% or less.
7. 3. The insulator-coated soft magnetic powder according to claim 1 or 2, which is mixed with 2 mass% of an epoxy resin, the resulting mixture is press-molded at a pressure of 294.2 MPa, and then heated at 150°C for 30 minutes to harden the epoxy resin, resulting in a molded product having a radial crushing strength of 10 MPa or more.
8. 3. The insulator-coated soft magnetic powder according to claim 1, wherein the moisture content measured at 250° C. by the Karl Fischer method is 30 ppm or more and 500 ppm or less.
9. A dust core comprising the insulator-coated soft magnetic powder according to claim 1 or 2.
10. A magnetic element comprising the powder magnetic core according to claim 9.
11. An electronic device comprising the magnetic element according to claim 10.
Citation Information
Patent Citations
Soft magnetic material and green compact
JP2021095629A