Polyester-based elastomer composition, molding and laminate
A blended polyester elastomer composition with a styrene elastomer and specific rubber softener improves thermal adhesion and reduces smoke generation, addressing the limitations of existing compositions by enhancing rubber elasticity and weight reduction.
Patent Information
- Application Number
- JP2024005478
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-22
- Filing Date
- 2024-01-17
- Publication Date
- 2024-10-07
AI Technical Summary
Existing polyester elastomer compositions do not adequately address issues of thermal adhesion to polar hard resins, rubber elasticity, weight reduction, and smoke generation during molding.
A polyester elastomer composition is formulated by blending a polyester elastomer with a styrene elastomer and a specific rubber softener, characterized by a weight average molecular weight of 800 to 1,200 and a dispersity index of less than 1.10, which enhances thermal adhesion to polar hard resins and reduces smoke generation.
The composition achieves high thermal adhesion, excellent rubber elasticity, and lightweight properties while minimizing smoke emission during molding, making it suitable for applications requiring flexibility and soft texture.
Smart Images

Figure 2024137706000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester elastomer composition, specifically to a polyester elastomer composition that has excellent heat fusion properties with polar hard resins such as polycarbonate resins (PC resin and bio-PC resin) and acrylonitrile-butadiene copolymer resins (ABS resin), emits little smoke during injection or extrusion molding, has excellent rubber elasticity (compression set), has a soft texture, and can be made lightweight, and to a molded article and a laminate using the polyester elastomer composition. [Background technology]
[0002] Polyester-based elastomers have excellent mechanical properties such as strength, impact resistance, rubber elasticity, flexibility, oil resistance, and abrasion resistance, as well as excellent low- and high-temperature properties. In addition, they can be heat-fused to hard resins such as polycarbonate resin (PC resin) and acrylonitrile-butadiene copolymer resin (ABS resin), which is why they are widely used in fields such as automobiles, electrical and electronic parts, and various consumer goods.
[0003] In recent years, polyester elastomers that have been softened with a rubber polymer and a plasticizer have been considered for use in grips or packings for cameras, power tools, bicycles, etc., due to their soft feel, rubber elasticity, low density, oil resistance, and abrasion resistance, and have been put to practical use.
[0004] Patent Document 1 discloses a thermoplastic elastomer composition consisting of a polyester-based elastomer, a styrene-based elastomer, and a hydrocarbon-based rubber softener, which is said to have excellent oil resistance, rubber elasticity (compression set), and heat resistance, as well as good flexibility, mechanical strength, and impact resistance. It is also said to be free of defects such as delamination when injection molded, and to have excellent injection molded appearance.
[0005] Patent Document 2 discloses a thermoplastic elastomer composition that contains a thermoplastic styrene-based elastomer, a softener, and a thermoplastic polyester-based elastomer, and that is excellent in flexibility and fusion-adhesion to polar resins, suppresses surface stickiness, and can provide a molded article that is also excellent in abrasion resistance. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-7878 [Patent Document 2] JP 2019-218561 A Summary of the Invention [Problem to be solved by the invention]
[0007] Although Patent Document 1 describes the molded appearance such as suppressing delamination of the injection molded body, it does not mention smoke generation during molding. Although Patent Document 2 describes the fusion adhesion to polar resins, it makes no mention of rubber elasticity, weight reduction, and smoke generation during molding.
[0008] In view of the above-mentioned problems in the prior art, an object of the present invention is to provide a polyester-based elastomer composition which has excellent thermal adhesion to polar hard resins, has a soft feel, excellent rubber elasticity, can be made lightweight, and generates little smoke during molding, and a molded article and laminate thereof. [Means for solving the problem]
[0009] As a result of intensive research conducted by the present inventors to solve the above problems, it has been discovered that by blending a specific rubber softener with a polyester-based elastomer and a styrene-based elastomer, it is possible to obtain a polyester-based elastomer composition which has excellent thermal adhesion to polar hard resins, is excellent in flexibility and rubber elasticity (compression set), is lightweight, and generates little smoke during molding. That is, the gist of the present invention lies in the following.
[0010] [1] A polyester-based elastomer composition comprising the following components (A), (B) and (C): Component (A): Polyester elastomer Component (B): Styrene-based elastomer Component (C): A rubber softener having a weight average molecular weight (Mw) of 800 to 1,200 and a polydispersity index (PDI) expressed as weight average molecular weight (Mw) / number average molecular weight (Mn) of less than 1.10 as measured by gel permeation chromatography (GPC).
[0011] [2] The polyester-based elastomer composition according to [1], wherein the rubber softener of component (C) is an isoalkane mixture.
[0012] [3] The polyester-based elastomer composition according to [1] or [2], wherein the contents of components (B) and (C) are each less than 100 parts by mass when the content of component (A) is 100 parts by mass.
[0013] [4] The polyester-based elastomer composition according to any one of [1] to [3], wherein the component (A) has a hard segment and a soft segment, and the soft segment is a polyalkylene glycol.
[0014] [5] The polyester-based elastomer composition according to [4], wherein the content of the soft segment in the component (A) is 10% by mass or more and 95% by mass or less.
[0015] [6] The polyester-based elastomer composition according to [4] or [5], wherein the polyalkylene glycol is polytetramethylene glycol.
[0016] [7] The polyester-based elastomer composition according to any one of [1] to [6], having a Duro A hardness according to ISO 7619-1 of 40 or more and 90 or less.
[0017] [8] The polyester-based elastomer composition according to any one of [1] to [7], wherein the component (C) is derived from a biomass material.
[0018] [9] The polyester-based elastomer composition according to [8], having a biomass content of 1% or more and 100% or less according to ASTM D6866-22.
[0019]
[10] A molded article made of the polyester-based elastomer composition according to any one of [1] to [9].
[0020]
[11] A laminate comprising a layer made of the polyester elastomer composition according to any one of [1] to [9] and a layer made of a hard resin having polarity. Effect of the Invention
[0021] According to the present invention, there are provided a polyester-based elastomer composition which has high thermal adhesion to polar hard resins, has a soft feel, is excellent in flexibility and rubber elasticity, can be made lightweight, and generates little smoke during molding, and a molded article and a laminate using this polyester-based elastomer composition. Because of such excellent properties, the polyester elastomer composition of the present invention is expected to be suitable for use in applications such as grips or packings for cameras, power tools, bicycles, stationery, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments. The present invention is not limited to the following description, and can be modified in any manner without departing from the spirit and scope of the present invention. In this specification, when "~" is used to express a numerical value or a physical property value, the values before and after the "~" are included.
[0023] [Polyester-based elastomer composition] The polyester-based elastomer composition of the present invention is characterized by comprising component (A): a polyester-based elastomer, component (B): a styrene-based elastomer, and component (C): a specific rubber softener.
[0024] [mechanism] According to the polyester elastomer composition of the present invention, it is possible to obtain a molded article which has high heat fusion property to a hard resin having polarity, has a soft touch, is excellent in flexibility and rubber elasticity, can be made lightweight, and generates little smoke during molding. Although the details of why the polyester elastomer composition of the present invention exhibits such effects are not clear, it is presumed as follows.
[0025] The polyester-based elastomer composition of the present invention contains, as component (C), a rubber softener having a weight average molecular weight (Mw) of 800 to 1,200 as measured by gel permeation chromatography (GPC) and a polydispersity index (PDI) expressed as weight average molecular weight (Mw) / number average molecular weight (Mn) of less than 1.10. This rubber softener has a sharp molecular weight distribution and contains a small amount of low molecular weight components. As a result, it is presumed that the polyester-based elastomer composition can obtain molded products that have high thermal adhesion to polar hard resins and generate little smoke during molding. A low content of low molecular weight components means that the minimum molecular weight detected on the low molecular weight side in GPC measurement is large, and it is presumed that this results in high thermal adhesion to polar hard resins and low smoke generation during molding. Furthermore, when the rubber softener of component (C) is an isoalkane mixture, it is presumed that the affinity between the elastomer and the isoalkane is increased due to the entanglement of the elastomers of components (A) and (B) with the isoalkane of component (C). As a result, it is presumed that the plasticization of the elastomers of components (A) and (B) is promoted, and a molded product having high heat fusion properties with polar hard resins, soft touch, flexibility, and rubber elasticity, as well as low smoke generation during molding, can be obtained. In addition, the isoalkane mixture of component (C) is an alkane and therefore has a low specific gravity, making it possible to reduce the weight of the polyester elastomer composition.
[0026] [Component (A)] The polyester elastomer of component (A) is usually a block copolymer having a hard segment having crystallinity and a soft segment having flexibility.
[0027] (1. Hardware Segment) The hard segment may be a hard segment made of a cyclic polyester (hereinafter, may be referred to as a "cyclic polyester unit"), etc. In the present invention, the term "cyclic polyester" refers to a raw material dicarboxylic acid or its alkyl ester containing a dicarboxylic acid or its alkyl ester having a cyclic structure in the main chain or side chain.
[0028] Examples of the cyclic polyester unit include a hard segment made of an aromatic polyester (hereinafter, may be referred to as an "aromatic polyester unit"), a hard segment made of an alicyclic polyester (hereinafter, may be referred to as an "alicyclic polyester unit"), and the like.
[0029] (1.1 Aromatic polyester unit) The aromatic polyester unit may be an aromatic polyester obtained from an aromatic dicarboxylic acid and an alicyclic diol or polyalkylene glycol as raw materials.
[0030] Examples of the aromatic dicarboxylic acid raw material used in the aromatic polyester unit include aromatic dicarboxylic acids or their alkyl esters. Examples of the aromatic dicarboxylic acid or its alkyl ester include terephthalic acid and its lower alkyl ester (in this specification, "lower" means carbon number 4 or less), as well as isophthalic acid, phthalic acid, 2,5-norbornene dicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and their lower alkyl esters. These aromatic dicarboxylic acids or their alkyl esters may be used alone or in combination of two or more. Among these, terephthalic acid and isophthalic acid are preferred, and terephthalic acid is more preferred.
[0031] Examples of the alicyclic diols and polyalkylene glycols include 1,4-cyclohexene glycol, 1,4-cyclohexanedimethanol, ethylene glycol, 1,4-butanediol, etc. These alicyclic diols and polyalkylene glycols may be used alone or in combination of two or more.
[0032] Among these, it is preferable that the aromatic polyester unit contains polybutylene terephthalate.
[0033] (1.2 Alicyclic polyester unit) The alicyclic polyester unit may be an alicyclic polyester obtained from an alicyclic dicarboxylic acid, an alicyclic diol, and a polyalkylene glycol as raw materials. In this specification, the term "alicyclic dicarboxylic acid" refers to a compound in which two carboxyl groups are directly bonded to a cyclic aliphatic hydrocarbon.
[0034] The raw material of the alicyclic dicarboxylic acid used in the alicyclic polyester unit may be alicyclic dicarboxylic acid or its alkyl ester. The alicyclic dicarboxylic acid or its alkyl ester may be one generally used as a raw material for polyester, such as cyclohexane dicarboxylic acid and its lower alkyl ester, cyclopentane dicarboxylic acid and its lower alkyl ester, etc. Among these, cyclohexane dicarboxylic acid and its lower alkyl ester are preferred, and cyclohexane dicarboxylic acid is particularly preferred. These alicyclic dicarboxylic acids or their alkyl esters may be used alone or in combination of two or more.
[0035] Examples of the alicyclic diol include 1,4-cyclohexene glycol and 1,4-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol is preferred. These alicyclic diols may be used alone or in combination of two or more.
[0036] Among these, the alicyclic polyester unit preferably contains an alicyclic polyester unit obtained using cyclohexanedicarboxylic acid and 1,4-cyclohexanedimethanol as raw materials.
[0037] (2. Software Segment) Examples of the soft segment include a soft segment made of polyalkylene glycol (hereinafter, sometimes referred to as a "polyalkylene glycol unit"), a soft segment made of a chain aliphatic polyester (hereinafter, sometimes referred to as a "chain aliphatic polyester unit"), etc. In the present invention, the term "chain aliphatic polyester" refers to a dicarboxylic acid or its alkyl ester, which is a raw material, having only a chain structure.
[0038] (2.1 Polyalkylene glycol unit) The polyalkylene ether glycol unit is preferably used as a soft segment having flexibility.The polyalkylene ether glycol constituting this polyalkylene ether glycol unit includes, for example, polymethylene glycol, polyethylene glycol, poly(1,2- and 1,3-)propylene glycol, polytetramethylene glycol such as polytetramethylene ether glycol, polyhexamethylene glycol, etc., and their linear and branched aliphatic ethers, as well as homopolymers or copolymers of alicyclic ethers such as condensates of cyclohexanediol and condensates of cyclohexanedimethanol. In addition, it may be a random copolymer within these ether units. In addition, a block copolymer having a polyalkylene glycol unit may also be used. In addition, it may be a random copolymer within these ether units. Among these, preferred are linear and branched aliphatic ether glycols such as polymethylene glycol, polyethylene glycol, poly(1,2- and 1,3-)propylene glycol, polytetramethylene glycol, and polyhexamethylene glycol, more preferred are polymethylene glycol, polyethylene glycol, poly(1,2- and 1,3-)propylene glycol, and polytetramethylene glycol, and particularly preferred is polytetramethylene glycol.
[0039] For example, when the polyester-based elastomer is a cyclic polyester-polyalkylene glycol block copolymer, the cyclic polyester-polyalkylene glycol block copolymer may contain only one type of polyalkylene glycol unit, or may contain two or more types of units having different number average molecular weights or constituent components.
[0040] This polyalkylene glycol unit preferably contains a soft segment made from polytetramethylene glycol such as polytetramethylene ether glycol (hereinafter, sometimes referred to as "polytetramethylene glycol unit").
[0041] (2.2 Linear Aliphatic Polyester Unit) Examples of the chain aliphatic polyester constituting the chain aliphatic polyester unit include polyesters obtained from chain aliphatic dicarboxylic acids having 4 to 10 carbon atoms, such as sebacic acid and adipic acid, and chain aliphatic diols.
[0042] Examples of the chain aliphatic diol include ethylene glycol, propylene glycol, trimethylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, and 1,6-hexene glycol. These may be used alone or in combination of two or more. Among them, 1,4-butylene glycol is preferred as the chain aliphatic diol.
[0043] (3. Block Copolymers) Examples of the combination of the hard segment and the soft segment, that is, the polyester-based elastomer, include a block copolymer having a cyclic polyester unit and a polyalkylene glycol unit (hereinafter, sometimes referred to as a "cyclic polyester-polyalkylene glycol block copolymer"), a block copolymer having a cyclic polyester unit and a linear aliphatic polyester unit (hereinafter, sometimes referred to as a "cyclic polyester-linear aliphatic polyester block copolymer"), etc. Among these, the cyclic polyester-polyalkylene glycol block copolymer is preferred because of its easy availability.
[0044] (3.1 Cyclic polyester-polyalkylene glycol block copolymer) Examples of the cyclic polyester-polyalkylene glycol block copolymer include a copolymer having an aromatic polyester unit and a polyalkylene glycol unit (hereinafter, sometimes referred to as an "aromatic polyester-polyalkylene glycol block copolymer"), a block copolymer having an alicyclic polyester unit and a polyalkylene glycol unit (hereinafter, sometimes referred to as an "alicyclic polyester-polyalkylene glycol block copolymer"), etc. Among these, aromatic polyester-polyalkylene glycol block copolymers are preferred in terms of heat resistance.
[0045] The number average molecular weight of the polyalkylene glycol unit contained in the cyclic polyester-polyalkylene glycol block copolymer is preferably 600 to 4,000, more preferably 800 to 2,500, and even more preferably 900 to 2,100. The number average molecular weight of the polyalkylene glycol unit herein refers to a polystyrene-equivalent value measured by GPC.
[0046] The respective contents of the cyclic polyester unit and the polyalkylene glycol unit in the cyclic polyester-polyalkylene glycol block copolymer are not limited, but are usually within the following ranges taking into account the balance between the crystallinity of the hard segment and the flexibility of the soft segment.
[0047] That is, the lower limit of the content of the cyclic polyester unit in the cyclic polyester-polyalkylene glycol block copolymer is usually 10% by mass or more, preferably 20% by mass or more, and the upper limit of the content of the cyclic polyester unit is usually 95% by mass or less, preferably 90% by mass or less, more preferably 80% by mass or less.
[0048] The lower limit of the content of the polyalkylene glycol unit in the cyclic polyester-polyalkylene glycol block copolymer is usually 5% by mass or more, preferably 10% by mass or more, more preferably 20% by mass or more. The upper limit of the content of the polyalkylene glycol unit is usually 90% by mass or less, preferably 80% by mass or less.
[0049] The content of the cyclic polyester unit in the block copolymer having the cyclic polyester unit can be calculated based on the chemical shift and content of the hydrogen atom by using nuclear magnetic resonance spectroscopy (hereinafter sometimes abbreviated as NMR).Similarly, the content of the polyalkylene glycol unit in the block copolymer having the polyalkylene glycol unit can be calculated based on the chemical shift and content of the hydrogen atom by using NMR.
[0050] The cyclic polyester-polyalkylene glycol block copolymer can also be obtained as a commercially available product, such as "KEYFLEX (registered trademark)" (manufactured by LG Chemical Co., Ltd.), "TEFABLOCK (registered trademark)" (manufactured by Mitsubishi Chemical Corporation), "Pelprene (registered trademark)" (manufactured by Toyobo Co., Ltd.), "Hytrel (registered trademark)" (manufactured by Toray Celanese Co., Ltd.), and "Hetroflex (registered trademark)" (manufactured by Hetron Co., Ltd.).
[0051] The polyester-based thermoplastic elastomers such as cyclic polyester-polyalkylene glycol block copolymers may be used alone or in combination of two or more kinds.
[0052] (3.1.1 Aromatic polyester-polyalkylene glycol block copolymer) The aromatic polyester-polyalkylene glycol block copolymer is a known thermoplastic elastomer as described in JP-A-10-130451 and the like, and each block may be a homopolymer or a copolymer as long as it is a polymer containing a polyalkylene glycol unit.
[0053] As the aromatic polyester-polyalkylene glycol block copolymer, a polybutylene terephthalate-polyalkylene glycol block copolymer is preferable because it has a particularly fast crystallization rate and excellent moldability. Here, the number of carbon atoms in the alkylene group of the polyalkylene glycol unit is preferably 2 to 12, more preferably 2 to 8, even more preferably 2 to 5, and particularly preferably 4.
[0054] In addition, in the cyclic polyester-polyalkylene glycol block copolymer represented by the aromatic polyester-polyalkylene glycol block copolymer according to the present invention, in addition to the above-mentioned components, a small amount of one or more of trifunctional alcohols and tricarboxylic acids and / or esters thereof may be copolymerized, and further, a chain aliphatic dicarboxylic acid such as adipic acid or a dialkyl ester thereof may be introduced as a copolymerization component.
[0055] (3.1.2 Alicyclic polyester-polyalkylene glycol block copolymer) A representative example of the alicyclic polyester-polyalkylene glycol block copolymer is a block copolymer consisting of an alicyclic polyester unit using the alicyclic dicarboxylic acid, an alicyclic diol, and a polyalkylene glycol, and a polyalkylene glycol unit. In the polyester elastomer according to the present invention, when the polyester elastomer contains a polyalkylene glycol unit, each of the blocks may be a homopolymer or a copolymer.
[0056] (3.2 Cyclic polyester-linear aliphatic polyester block copolymer) Examples of the cyclic polyester-linear aliphatic polyester block copolymer include a block copolymer having a hard segment made of an aromatic polyester and a soft segment made of a linear aliphatic polyester (hereinafter, sometimes referred to as an "aromatic polyester-linear aliphatic polyester block copolymer"), and a block copolymer having a hard segment made of an alicyclic polyester and a soft segment made of a linear aliphatic polyester (hereinafter, sometimes referred to as an "alicyclic polyester-linear aliphatic polyester block copolymer"). Among these, aromatic polyester-linear aliphatic polyester block copolymers are preferred. As the aromatic polyester-linear aliphatic polyester block copolymer, a polybutylene terephthalate-linear aliphatic polyester block copolymer in which the aromatic polyester unit is made of polybutylene terephthalate is more preferred.
[0057] (3.3 Preferred polyester elastomers) As the polyester elastomer used in the present invention, a polybutylene terephthalate-polyalkylene glycol block copolymer is preferred, and a polybutylene terephthalate-polytetramethylene glycol block copolymer is particularly preferred.
[0058] (4. Method for producing polyester elastomer) The method for producing the polyester-based elastomer is not particularly limited. For example, among cyclic polyester-polyalkylene glycol block copolymers, an aromatic polyester-polyalkylene glycol block copolymer using an aromatic polyester and a polyalkylene ether glycol can be obtained by condensing an oligomer obtained by an esterification reaction or a transesterification reaction using a chain aliphatic and / or alicyclic diol having 2 to 12 carbon atoms, an aromatic dicarboxylic acid or an alkyl ester thereof, and a polyalkylene ether glycol as raw materials.
[0059] As the chain aliphatic and / or alicyclic diol having 2 to 12 carbon atoms, those generally used as raw materials for polyesters can be used. As examples of the chain aliphatic diol and alicyclic diol, the above-mentioned compounds can be used. These chain aliphatic and / or alicyclic diols having 2 to 12 carbon atoms may be used alone or in combination of two or more. As the aromatic dicarboxylic acid or alkyl ester thereof, those generally used as raw materials for polyesters can be used, for example, the above-mentioned compounds can be used. These aromatic dicarboxylic acids or alkyl esters thereof may also be used alone or in combination of two or more. As the polyalkylene ether glycol, for example, the above-mentioned compounds can be used. These may be used alone or in combination of two or more.
[0060] In addition, when producing an alicyclic polyester-polyalkylene glycol block copolymer, an alicyclic dicarboxylic acid or an alkyl ester thereof may be used instead of the aromatic dicarboxylic acid or an alkyl ester thereof used as a raw material in producing the aromatic polyester-polyalkylene glycol block copolymer. That is, the alicyclic polyester-polyalkylene glycol block copolymer can be obtained by polycondensing an oligomer obtained by an esterification reaction or an ester exchange reaction using a chain aliphatic and / or alicyclic diol having 2 to 12 carbon atoms, an alicyclic dicarboxylic acid or an alkyl ester thereof, and a polyalkylene ether glycol as raw materials.
[0061] (5. Melt flow rate of polyester elastomer) The melt flow rate (MFR) of the polyester elastomer of component (A) used in the present invention is preferably 1 to 50 g / 10 min, more preferably 10 to 30 g / 10 min, as measured at 230° C. and a load of 2.16 kgf in accordance with ISO 1133. When the MFR of the polyester elastomer of component (A) is within the above range, the raw materials tend to be easily mixed uniformly when melt-kneaded, and variation in performance can be suppressed.
[0062] The polyester elastomer of component (A) may be used alone or in combination of two or more types having different hard and soft segments, different compositions, different physical properties, etc. The polyester elastomer of component (A) may be a biopolyester elastomer using plant-derived raw materials as at least a part of the raw materials.
[0063] <Ingredient (B)> As the component (B): styrene-based elastomer contained in the polyester-based elastomer composition of the present invention, from the viewpoints of heat resistance and flexibility, a hydrogenated copolymer of styrene (which may be a derivative of styrene) and a conjugated diene block represented by the following formula (1) and / or formula (2) is preferred.
[0064] S-(DS)m …(1) (SD)n …(2) (In the formula, S represents a polymer block composed of styrene units, D represents a polymer block composed of conjugated diene units, and m and n represent integers of 1 to 5.)
[0065] The block copolymers described above may be linear, branched and / or radial.
[0066] Examples of the monomer constituting the polymer block of S include styrene and styrene derivatives such as α-methylstyrene. The conjugated diene monomer constituting the polymer block of D is preferably butadiene and / or isoprene.
[0067] Larger m and n are better in terms of lowering the order-disorder transition temperature, but smaller m and n are better in terms of ease of production and cost. As the hydrogenated product of the styrene-conjugated diene block copolymer, the hydrogenated product of the block copolymer represented by formula (1) is more preferable than the block copolymer represented by formula (2) because of its excellent rubber elasticity, the hydrogenated product of the block copolymer represented by formula (1) in which m is 3 or less is more preferable, and the hydrogenated product of the block copolymer represented by formula (1) in which m is 2 or less is particularly preferable.
[0068] In addition, the proportion of the "S polymer block" in the block copolymer represented by formula (1) and / or formula (2) is preferably high from the viewpoints of mechanical strength and heat fusion strength of the resulting polyester elastomer composition, while being low from the viewpoints of flexibility, moldability, and resistance to bleed-out. Specifically, the proportion of the "S polymer block" in the block copolymer represented by formula (1) and / or formula (2) is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, and is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less.
[0069] The weight average molecular weight of the styrene-based elastomer used in the present invention is preferably large in terms of mechanical strength, but is preferably small in terms of molded appearance and fluidity. Specifically, the weight average molecular weight of the styrene-based elastomer is preferably 10,000 or more, more preferably 30,000 or more, and is preferably 450,000 or less, more preferably 400,000 or less, and particularly preferably 250,000 or less. Here, the weight average molecular weight is the weight average molecular weight in terms of polystyrene measured by GPC under the following conditions.
[0070] (Measurement conditions) Equipment: "150C ALC / GPC" manufactured by Nihon Millipore Column: Showa Denko "AD80M / S" x 3 Detector: FOXBORO infrared spectrophotometer "MIRANIA" Wavelength: 3.42μm Temperature: 140℃ Flow rate: 1cm 3 / min Injection volume: 200 microliters Concentration: 2mg / cm 3 0.2% by mass of 2,6-di-t-butyl-p-phenol was added as an antioxidant.
[0071] The content of the styrene polymer block in the styrene elastomer is preferably high from the viewpoint of mechanical strength of the polyester thermoplastic elastomer composition, while being low from the viewpoints of flexibility, injection moldability, and resistance to bleed-out. The content of the styrene polymer block is preferably 10% by mass or more, more preferably 15% by mass or more, and particularly preferably 20% by mass or more. On the other hand, it is preferably 50% by mass or less, more preferably 45% by mass or less, and particularly preferably 40% by mass or less.
[0072] The above-mentioned styrene-based elastomer may be produced by any method as long as the above-mentioned structure and physical properties are obtained, and any known production method can be used.
[0073] As such a styrene-based elastomer, commercially available products can be used, specifically, Kraton (registered trademark) G manufactured by Kraton Polymers, Septon (registered trademark) and Septon (registered trademark) Bio manufactured by Kuraray Co., Ltd., Tuftec (registered trademark) and SOE (registered trademark) manufactured by Asahi Kasei Corporation, TAIPOL (registered trademark) manufactured by TSRC, and GLOBALPRENE manufactured by LCY.
[0074] The styrene-based elastomer of component (B) may be used alone or in combination of two or more types having different block structures, types of conjugated dienes, physical properties, etc.
[0075] <Component (C)> Component (C): a rubber softener contained in the polyester elastomer composition of the present invention is effective in improving the heat fusion properties of the polyester elastomer composition of the present invention to hard resins such as polycarbonate resin (PC resin) and acrylonitrile-butadiene copolymer resin (ABS resin), imparting excellent flexibility and rubber elasticity, and reducing smoke generation during molding.
[0076] The component (C): rubber softener is characterized by having a weight average molecular weight (Mw) of 800 to 1,200 and a polydispersity index (PDI) expressed by weight average molecular weight (Mw) / number average molecular weight (Mn) of less than 1.10 in GPC measurement. By including such a component (C): rubber softener, the polyester-based elastomer composition of the present invention has excellent heat fusion properties with hard resins such as polycarbonate resin (PC resin) and acrylonitrile-butadiene copolymer resin (ABS resin), flexibility and rubber elasticity, and exhibits low smoke generation performance during molding. From this viewpoint, the component (C): rubber softener is preferably characterized by having a weight average molecular weight (Mw) of 1000 to 1200 and a polydispersity index (PDI) expressed by weight average molecular weight (Mw) / number average molecular weight (Mn) of 1.07 or less in GPC measurement. The lower limit of the polydispersity index (PDI) is 1.00. Furthermore, from the viewpoint of satisfying the above polydispersity index (PDI), the component (C): rubber softener used in the present invention preferably has a minimum molecular weight detected by GPC measurement of 200 or more, and more preferably 300 or more.
[0077] Here, the number average molecular weight (Mn) and the weight average molecular weight (Mw) are values measured by GPC under the following conditions and converted into polystyrene equivalent values.
[0078] (Measurement conditions) Equipment: "Tosoh HLC-8220 / GPC" manufactured by Nihon Millipore Column: Showa Denko PL3μm Mixed-E (7.8mmI.D.×30cmL) x 2 Detector: FOXBORO infrared spectrophotometer "RI (built-in)" measurement Column temperature: 40℃ Flow velocity: 0.7cm 3 / min Injection volume: 100 microliters
[0079] The polyester elastomer composition of the present invention preferably contains an isoalkane mixture as component (C). Isoalkane refers to an alkane having a terminal isomethyl group and does not contain a double bond or a cyclic substituent. The term "isoalkane mixture" refers to a mixture of isoalkanes and hydrocarbons not having an isoalkane structure. The "isoalkane" according to the present invention may be any alkane having an isomethyl group at a terminal, and may be either an isoalkane having no side chain other than the terminal isomethyl group, or an isoalkane having an alkyl group as a side chain other than the terminal isomethyl group in the main chain of the alkane (in the present invention, this alkyl group is referred to as a "side chain alkyl group"). As described above, from the viewpoint of the entanglement effect between the elastomers of components (A) and (B) and the isoalkane, an isoalkane having a side chain alkyl group is preferred. Since isoalkanes are generally commercially available as isoalkane mixtures, in the present invention they are referred to as "isoalkane mixtures", but component (C) may be a single isoalkane substance.
[0080] Examples of the side chain alkyl group contained in the isoalkane mixture as component (C): a rubber softener, include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, etc. Among these, an alkyl group having 1 to 18 carbon atoms is more preferable, an alkyl group having 1 to 3 carbon atoms is even more preferable, and a methyl group is particularly preferable.
[0081] The side chain alkyl group of the isoalkane mixture as component (C) rubber softener is an alkyl chain that branches off from the main chain, which is the longest linear alkyl chain, and the number of side chain alkyl groups in one molecule is not limited to one, but may be two or more. The number of side chain alkyl groups in the isoalkane is preferably 2 to 16, more preferably 4 to 12, and even more preferably 4 to 8.
[0082] Component (C): the isoalkane mixture as a rubber softener preferably has side chain alkyl groups in a content of 1 to 80% in the molecule, more preferably 5 to 70%, further preferably 10 to 60%, and particularly preferably 15 to 50%. From the viewpoints of bleed-out resistance and rubber elasticity, the higher the side chain alkyl group content, the better, and from the viewpoint of moldability, the lower the side chain alkyl group content. Here, the content of the side chain alkyl group refers to the ratio (percentage) of the molecular weight of the side chain alkyl group (when a plurality of side chain alkyl groups are present, the total molecular weight) to the molecular weight of the entire isoalkane.
[0083] Component (C): isoalkane mixture as a rubber softener is measured by gas chromatography mass spectrometry (GC / MS) under the measurement conditions shown below, and the amount of heated gas generated is measured under the heat extraction conditions of 250°C for 10 minutes. In a comparison of retention times using a standard sample of a mixed n-alkane standard solution (carbon number 16 to 34) with a known molecular weight, the amount of heated gas generated corresponding to carbon number 26 or less is 500 ppm or less in n-eicosane equivalent. The amount of components with carbon number 26 or less is calculated by comparing the peak areas of GC / MS measurement using n-eicosane with a known molecular weight as a standard reagent. On the other hand, the same measurement of typical hydrocarbon oils showed that the amount of heated gases equivalent to carbon numbers of 26 or less was more than 2,000 ppm, indicating that the isoalkane mixture generates significantly fewer low molecular weight components when heated than typical hydrocarbon oils.
[0084] (Measurement conditions) Heat extraction device: Gestell "TDU2" Equipment: Agilent Technologies "Agilent 7890GC / Agilent 5977AMSD" Column: Agilent Technologies "DB-5MSUI 30mL x 250μm x 0.25μm" Sample size: 0.1 mg Heat extraction temperature: 250℃ x 10 minutes GC oven temperature: 40℃ 5 min → 10℃ / min → 300℃ (20 min) Carrier gas: Helium Gas flow rate: 1.0mL / min
[0085] The rubber softener of component (C), such as an isoalkane mixture, preferably has a kinematic viscosity at 40° C. of 20 cSt or more and 8,000 cSt or less, and from the viewpoints of bleed-out resistance and rubber elasticity, preferably 20 cSt or more, and more preferably 25 cSt or more, while from the viewpoints of processability and moldability, it is preferably 8000 cSt or less, more preferably 3000 cSt or less, and even more preferably 1000 cSt or less. Here, the kinetic viscosity is a kinetic viscosity at 40° C. measured by a method in accordance with JIS K2283.
[0086] From the viewpoint of safety during processing, the flash point (COC method) of the rubber softener of component (C), such as an isoalkane mixture, is preferably equal to or higher than the processing temperature of the elastomers of components (A) and (B), and is preferably 150°C or higher, more preferably 180°C or higher, even more preferably 200°C or higher, and particularly preferably 250°C or higher.
[0087] The pour point (measured by ASTM D97) of the rubber softener of component (C) such as an isoalkane mixture is preferably -60°C or higher, more preferably -50°C or higher, and even more preferably -40°C or higher, since the lower the pour point, the higher the molecular mobility and the poorer the bleed-out resistance. On the other hand, from the viewpoint of handleability during processing, it is preferably 0°C or lower, more preferably -10°C or lower, even more preferably -20°C or lower, and particularly preferably -25°C or lower.
[0088] The rubber softener of component (C), such as an isoalkane mixture, usually has a naphthenic carbon percentage (%CN) by ring analysis of 20% or less, preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less. Also, the aromatic carbon percentage (%CA) by ring analysis is preferably 5% or less, more preferably 1% or less. Specifically, the ring analysis can be carried out by the ndM method defined in ASTM D2140 or ASTM D3238. By setting the naphthenic carbon ratio and the aromatic carbon ratio within the above ranges, the composition has excellent heat resistance and resistance to discoloration due to light.
[0089] The rubber softener of component (C), such as the isoalkane mixture, may include those derived from biomass materials or derived from biomass. The biomass degree of component (C) is calculated based on the 14C content according to ASTM D6866-22. From the viewpoint of reducing the environmental load, the biomass degree of component (C) is preferably 1% or more, more preferably 10% or more, even more preferably 20% or more, and particularly preferably 30% or more. There is no particular upper limit for the biomass degree of component (C), and it is 100% or less.
[0090] The isoalkane mixture used as component (C) may be a commercially available product. Examples of commercially available isoalkane mixtures include the "VIVA-B-FIX" series manufactured by H&R Corporation, and any of these may be appropriately selected and used.
[0091] Component (C): Rubber softeners may be used alone or in any combination and ratio of two or more kinds. They may also be used in combination with general hydrocarbon rubber softeners that do not satisfy the above weight average molecular weight (Mw) and polydispersity (PID).
[0092] Common hydrocarbon-based rubber softeners include mineral oil-based softeners and synthetic resin-based softeners, and mineral oil-based softeners are particularly preferred. Mineral oil-based softeners are generally mixtures of aromatic hydrocarbons, naphthenic hydrocarbons, and paraffinic hydrocarbons, and those in which 50% or more of the total carbon atoms are paraffinic hydrocarbons are called paraffinic oils, those in which 30-45% of the total carbon atoms are naphthenic hydrocarbons are called naphthenic oils, and those in which 35% or more of the total carbon atoms are aromatic hydrocarbons are called aromatic oils. Among these, paraffinic oils are preferred.
[0093] The kinetic viscosity (JIS K2283) of the hydrocarbon rubber softener at 40°C is preferably 20 cSt or more, more preferably 50 cSt or more, while it is preferably 800 cSt or less, more preferably 600 cSt or less. The flash point (COC method) of the hydrocarbon rubber softener is preferably 200°C or more, more preferably 250°C or more.
[0094] The hydrocarbon rubber softener may be a commercially available product, such as the "Nippon Oil Polybutene (registered trademark) HV" series manufactured by JX Nippon Oil & Energy Corporation and the "Diana (registered trademark) Process Oil PW" series manufactured by Idemitsu Kosan Co., Ltd., and may be appropriately selected from these.
[0095] The hydrocarbon-based rubber softeners may be used alone or in any combination and ratio of two or more kinds.
[0096] <Content of Components (A) to (C)> The content of component (A) in the polyester elastomer composition of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more. On the other hand, it is preferably 90% by mass or less, more preferably 70% by mass or less. If the content of component (A) in the polyester elastomer composition is above the above lower limit, the composition will have excellent heat fusion properties, impact resistance, oil resistance, abrasion resistance, and low-temperature and high-temperature properties with respect to hard resins such as polycarbonate resin (PC resin) and acrylonitrile-butadiene copolymer resin (ABS resin). If the content of component (A) is below the above upper limit, the necessary amounts of components (B) and (C) can be secured, and the composition will have excellent flexibility, softness, rubber elasticity, weight reduction, and low smoke generation during molding.
[0097] The content of component (B) in the polyester elastomer composition of the present invention is preferably 5% by mass or more, particularly 20% by mass or more, and 50% by mass or less, particularly 40% by mass or less. If the content of component (B) in the polyester elastomer composition is above the above lower limit, the composition will have excellent flexibility, softness, and rubber elasticity due to component (B). If the content of component (B) is below the above upper limit, the necessary amounts of components (A) and (C) can be secured, and the composition will have excellent heat fusion properties, impact resistance, oil resistance, abrasion resistance, low-temperature and high-temperature properties, weight reduction, and low smoke generation during molding with respect to hard resins such as polycarbonate resin (PC resin) and acrylonitrile-butadiene copolymer resin (ABS resin).
[0098] The content of component (C) in the polyester elastomer composition of the present invention is preferably 1% by mass or more, particularly 10% by mass or more, and 50% by mass or less, particularly 40% by mass or less. If the content of component (C) in the polyester elastomer composition is above the above lower limit, the composition will have excellent flexibility, softness, rubber elasticity, weight reduction, and low smoke generation during molding due to component (C). If the content of component (C) is below the above upper limit, the necessary amounts of components (A) and (B) can be secured, and the composition will have excellent heat fusion properties, impact resistance, oil resistance, abrasion resistance, low and high temperature properties, flexibility, softness, and rubber elasticity with respect to hard resins such as polycarbonate resin (PC resin) and acrylonitrile-butadiene copolymer resin (ABS resin).
[0099] In addition, in the polyester elastomer composition of the present invention, the contents of components (B) and (C) are preferably less than 100 parts by mass, respectively, per 100 parts by mass of the content of component (A). If the contents of components (B) and (C) are less than the above upper limit, the effect of heat fusion properties of component (A) with respect to hard resins such as polycarbonate resin (PC resin) and acrylonitrile-butadiene copolymer resin (ABS resin) can be sufficiently obtained. From this viewpoint, the content of component (B) is more preferably 90 parts by mass or less, and more preferably 80 parts by mass or less, per 100 parts by mass of the content of component (A). On the other hand, in order to effectively obtain the effect of softening and the like due to the inclusion of component (B), the content of component (B) is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more, per 100 parts by mass of component (A). From the same viewpoint, the content of component (C) is more preferably 90 parts by mass or less, and preferably 80 parts by mass or less, per 100 parts by mass of the content of component (A). On the other hand, in order to effectively obtain the effects of flexibility and soft texture due to the inclusion of component (C), the content of component (C) is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, per 100 parts by mass of component (A).
[0100] When the polyester-based elastomer composition of the present invention contains the above-mentioned hydrocarbon-based rubber softener together with component (C), the content of the hydrocarbon-based rubber softener is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, per 100 parts by mass of component (A) from the viewpoints of weight reduction, low smoke generation during molding, and good moldability. Also, it is preferable to use the component (C) and the hydrocarbon-based rubber softener so that the total content falls within the above-mentioned content range of component (C).
[0101] In this case, the content of component (C) relative to the total amount of component (C) and the hydrocarbon-based rubber softener is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. When the content of component (C) relative to the total amount of component (C) and the hydrocarbon-based rubber softener is equal to or more than the above lower limit, the above-mentioned effects of using component (C) can be effectively obtained.
[0102] <Other ingredients> The polyester elastomer composition of the present invention may contain other components, such as various additives and fillers, as required, within the scope of not impairing the object of the present invention.
[0103] Examples of additives include antioxidants, acidic compounds and derivatives thereof, lubricants, ultraviolet absorbers, light stabilizers, nucleating agents, flame retardants, impact resistance improvers, foaming agents, colorants, organic peroxides, etc. These may be used alone or in combination of two or more.
[0104] Examples of the filler include inorganic fillers such as talc, calcium carbonate, zinc carbonate, wollastonite, silica, alumina, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, sodium aluminosilicate, magnesium silicate, glass balloons, cut glass fibers, milled glass fibers, glass flakes, glass powder, silicon carbide, silicon nitride, gypsum, gypsum whiskers, calcined kaolin, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, metal fibers, metal whiskers, metal powder, ceramic whiskers, potassium titanate, boron nitride, graphite, and carbon fibers; and organic fillers such as naturally derived polymers such as starch, cellulose fine particles, wood flour, soybean pulp, rice husks, and bran, and modified products thereof. These may be used alone or in combination of two or more.
[0105] When a filler is blended into the polyester elastomer composition of the present invention, the blending amount is usually 50% by mass or less, and preferably 30% by mass or less, of all the components.
[0106] <Method of producing polyester elastomer composition> The polyester-based elastomer composition of the present invention can be produced by mechanically mixing the components (A) to (C) and other additives and fillers used as necessary using a known method, for example, a Henschel mixer, a V blender, a tumbler blender, etc., and then mechanically melt-kneading the components using a known method. For the mechanical melt-kneading, a general melt-kneading machine such as a Banbury mixer, various kneaders, or a single-screw or twin-screw extruder can be used.
[0107] <Physical properties of polyester elastomer composition> The polyester elastomer composition of the present invention is usually required to have excellent moldability such as injection molding in its applications, so that the melt flow rate (MFR) measured at 230°C and a load of 2.16 kgf according to ISO 1133 is preferably 30 g / 10 min or less, more preferably 20 g / 10 min or less, and even more preferably 10 g / 10 min or less. If the MFR exceeds the upper limit, flash is likely to occur during injection molding, and a molded product with good appearance may not be obtained. The lower limit of the MFR of the polyester elastomer composition of the present invention is usually 1 g / 10 min or more from the viewpoint of production stability by melt kneading.
[0108] Since the polyester elastomer composition of the present invention is required to have a soft touch in its applications, the Duro A hardness according to ISO 7619-1 is preferably 90 or less, more preferably 80 or less. On the other hand, from the viewpoint of practical material strength, it is preferably 30 or more, more preferably 40 or more.
[0109] The methods for evaluating the above MFR and Duro A hardness will be specifically described in the Examples section.
[0110] [Molded article of polyester-based elastomer composition] The molded article of the present invention is one molded using the polyester elastomer composition of the present invention.
[0111] The polyester-based elastomer composition of the present invention can be molded by various molding methods such as injection molding, extrusion molding, and blow molding, and can also be applied to a molding method that combines a plurality of molding processing techniques, such as injection blow molding, which combines injection molding and blow molding.
[0112] The molded article produced from the polyester elastomer composition of the present invention has a soft texture and excellent heat fusion properties with polar hard resins such as polycarbonate resins (PC resins and bio-PC resins made from plant-derived raw materials) and acrylonitrile-butadiene copolymer resins (ABS resins). Therefore, it can be suitably used for various applications such as stationery, toys, sporting goods, covers for mobile phones and smartphones, parts such as grips, school teaching materials, home appliances, repair parts for OA equipment, various parts for automobiles, motorcycles, bicycles, etc., and building materials. In particular, it can be suitably used for the laminate of the present invention including a layer made of the polyester elastomer composition of the present invention described below and a layer made of a polar hard resin such as polycarbonate resins (PC resins and bio-PC resins) and acrylonitrile-butadiene copolymer resins (ABS resins).
[0113] [Laminate] The laminate of the present invention is a laminate comprising a layer made of the polyester-based elastomer composition of the present invention and a layer made of a polar hard resin such as polycarbonate resin (PC resin and bio-PC resin) or acrylonitrile-butadiene copolymer resin (ABS resin). By laminating and integrating the hard resin layer made of PC resin or ABS resin, which has excellent chemical resistance and heat resistance, and the soft resin layer made of the polyester-based elastomer composition of the present invention by thermal fusion, a product that combines rigidity and softness can be obtained.
[0114] Preferred examples of polar hard resins include polycarbonate resins (PC resin and bio-PC resin), polyester resins, poly(meth)acrylate resins such as polymethyl methacrylate, polyethylene oxide resins, polypropylene oxide resins, polyvinyl acetate resins, polyamide resins, polyurethane resins, polystyrene resins such as acrylonitrile-butadiene copolymer resin (ABS resin), polyvinyl ether resins, polyvinyl alcohol resins, polyphenylene ether resins, polyphenylene sulfide resins, polysulfone resins, polyetherimide resins, polyether ketone resins, polyether ether ketone resins, LCP (liquid crystal polymer), ionomers, and other polar resins, as well as mixtures of two or more of these. Among these, PC resin, bio-PC resin, and ABS resin are preferred from the viewpoints of high fusion strength with polyester-based elastomers, moldability, and cost efficiency.
[0115] Commercially available hard resins having such polarity include "Iupilon (registered trademark)" manufactured by Mitsubishi Engineering Plastics Corporation as a PC resin and a bio-PC resin, "Durabio (registered trademark)" manufactured by Mitsubishi Chemical Corporation as a bio-PC resin, and "Toyolac (registered trademark)" manufactured by Toray Industries, Inc. as an ABS resin.
[0116] There is no particular limitation on the method for producing the laminate of the present invention having a layer made of the polyester-based thermoplastic elastomer composition of the present invention and a layer made of a polar hard resin. The laminate can be produced by insert injection molding in which the polyester-based thermoplastic elastomer composition of the present invention is injected into a molded product such as a sheet of a polar hard resin such as a polycarbonate resin (PC resin and bio-PC resin) or an acrylonitrile-butadiene copolymer resin (ABS resin) that has been previously prepared, or by a co-extrusion molding method, inflation molding method, blow molding method, or the like. The laminate of the present invention can be obtained by integrating a layer of a polar hard resin such as an acrylonitrile-butadiene copolymer resin (ABS resin) and the polyester-based elastomer composition of the present invention by heat fusing them together. EXAMPLES
[0117] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values between the examples.
[0118] [Raw materials] <Component (A): Polyester-based elastomer> A-1: Polybutylene terephthalate-polytetramethylene glycol block copolymer Number average molecular weight of polytetramethylene glycol unit: 1,700 Polybutylene terephthalate unit content: 27% by mass Polytetramethylene glycol unit content: 73% by mass MFR (230℃, load 2.16kgf): 20g / 10min A-2: Polybutylene terephthalate-polytetramethylene glycol block copolymer Number average molecular weight of polytetramethylene glycol unit: 1,800 Polybutylene terephthalate unit content: 29% by mass Polytetramethylene glycol unit content: 71% by mass MFR (230℃, load 2.16kgf): 16g / 10min A-3: Polybutylene terephthalate-polytrimethylene glycol block copolymer Number average molecular weight of polytrimethylene glycol unit: 1,800 Polybutylene terephthalate unit content: 35% by mass Polytrimethylene glycol unit content: 65% by mass MFR (230℃, load 2.16kgf): 30g / 10min Biomass content: 65%
[0119] <Component (B): Styrene-based elastomer> B-1: Kraton (registered trademark) G1641HU manufactured by Kraton Polymers Styrene-Ethylene / Butylene-Styrene Block Copolymer Styrene polymer block content: 32% by mass Weight average molecular weight: 2.2×10 5 MFR (230℃, load 2.16kgf): 1g / 10min
[0120] <Component (C): Rubber softener> C-1: Isoalkane mixture H&R "VIVASPES 10227" Kinematic viscosity at 40℃: 56cSt Flash point: 280℃ Pour point: -27℃ Mw: 1,110 Mn: 1,070 Molecular weight dispersity (PDI): 1.04 Minimum molecular weight detected by GPC: 390 Biomass content: 100% C-2: Hydrocarbon oil Idemitsu Kosan Co., Ltd. Diana (registered trademark) "Process Oil PW-90" Kinematic viscosity at 40℃: 95cSt Flash point: 272℃ Pour point: -17℃ Mw:730 Mn;630 Molecular weight dispersity (PDI): 1.16 Minimum molecular weight detected by GPC: 60 Biomass content: 0% C-3: Hydrocarbon oil Idemitsu Kosan Co., Ltd. Diana (registered trademark) "Process Oil PW-380" Kinematic viscosity at 40℃: 409cSt Flash point: 300℃ Pour point: -15℃ Mw: 1,230 Mn:1,090 Molecular weight dispersity (PDI): 1.13 Minimum molecular weight detected by GPC: 160 Biomass content: 0%
[0121] [Examples 1 to 4, Comparative Examples 1 to 4] <Production of Polyester-Based Elastomer Composition> The components shown in the compounding composition in Table 1 were melt-kneaded (cylinder temperature: 220° C.) in a twin-screw kneader to produce pellets of a polyester-based elastomer composition.
[0122] <Creating molded bodies for evaluating physical properties> The polyester elastomer composition pellets were injection molded using an injection molding machine (Japan Steel Works, Ltd., "J110AD", mold clamping force 110T) at a mold temperature of 40°C and a cylinder temperature of 200 to 230°C to obtain molded bodies of 100 mm x 100 mm x 2 mm (thickness). Hereinafter, each of these molded bodies is referred to as "molded bodies for physical property evaluation."
[0123] <Preparation of molded body for evaluating heat fusion property> The pellets of the polyester-based elastomer composition were molded using an injection molding machine (Japan Steel Works, Ltd., "J110AD", mold clamping force 110T) to form a polycarbonate resin (Mitsubishi Engineering Plastics Corporation, "Iupilon (registered trademark) H3000", PC resin I) sheet (thickness 2 mm), a polycarbonate resin (Mitsubishi Chemical Corporation, "Durabio (registered trademark) D6350R", bio-PC resin II obtained from plant-derived isosorbide as the main raw material) sheet ( A sheet (thickness 2 mm) made of polycarbonate resin (PC resin I), bio-polycarbonate resin (bio-PC resin II) or acrylonitrile-butadiene copolymer resin (ABS resin), a thickness of 2 mm, was injection molded at a mold temperature of 80°C and a cylinder temperature of 220°C to obtain a laminated molded article having a substrate layer of polycarbonate resin (PC resin I), bio-polycarbonate resin (bio-PC resin II) or acrylonitrile-butadiene copolymer resin (ABS resin) and a surface layer of the polyester elastomer composition, the dimensions of which were 100 mm x 100 mm x 4 mm (thickness). Hereinafter, these are referred to as "molded articles for evaluating thermal adhesion."
[0124] [Evaluation method] The pellets, molded articles for evaluating physical properties, and molded articles for evaluating heat fusion properties of the polyester-based thermal elastomer compositions of Examples 1 to 4 and Comparative Examples 1 to 4 shown in Table 1 were evaluated by the following methods. The results are shown in Table 1.
[0125] <mfr> The pellets of the polyester elastomer composition were measured for MFR (based on ISO 1133 (230° C., load 2.16 kgf)).
[0126] <Duro A hardness> The Duro A hardness of the molded products for evaluating physical properties prepared above was measured in accordance with ISO 7619-1.
[0127] <density> The density of the molded article for evaluating physical properties prepared above was measured in accordance with ISO 1183. From the viewpoint of light weight, this density is preferably 1.00 g / cm 3 The lower limit is usually 0.90 g / cm 3 It is.
[0128] <Compression set (CS)> The compression set (CS) of the molded article for evaluating physical properties prepared above was measured in accordance with ISO 815. The smaller the compression set (CS), the better the rubber elasticity.
[0129] <Thermal adhesiveness> A rectangular test piece 25 mm wide and 100 mm long was cut out from the molded product for evaluating heat fusion properties prepared above, and the surface layer was pulled at an angle of 90 degrees to the base layer at a pulling speed of 200 mm / min to measure the peel strength between the two layers. The higher the peel strength, the better the heat fusion properties.
[0130] <Smoke generation during molding> Pellets of the polyester elastomer composition were injection molded using an injection molding machine (Japan Steel Works, Ltd., "J110AD", mold clamping force 110T) at a cylinder temperature of 240°C, and the smoke generation of the sample (purged mass) was visually confirmed. The smoke generation was visually evaluated relatively as "+", "++", or "+++". The more "+" the more preferable, since it means less smoke generation.
[0131] <Biomass ratio> For the pellets of polyester elastomer composition obtained in the examples and comparative examples, the 14C concentration was measured using a tandem accelerator-based C-AMS dedicated device (manufactured by NEC Corporation), and then the biomass degree was calculated according to ASTM D6866-22. In Table 1 below, "-" in the column of biomass degree indicates that the biomass degree was not measured.
[0132] [Table 1]
[0133] [Consideration] From Table 1, we can see the following: The evaluation of the Examples and Comparative Examples is performed by comparing Examples 1 and 3 with Comparative Examples 1 and 2, and Examples 2 and 4 with Comparative Examples 3 and 4, respectively, according to the type of component (A). It was found that, compared with Comparative Examples 1 to 4, Examples 1 to 4 had superior thermal fusion bonding properties with polycarbonate resin (PC resin I and Bio-PC resin II) and acrylonitrile-butadiene copolymer resin (ABS resin) at 220°C. It was found that, compared with Comparative Examples 1 to 4, Examples 1 and 2 had lower densities and could be made lighter in weight. It was found that Examples 1 to 4 had smaller compression set (CS) and improved rubber elasticity than Comparative Examples 1 to 4. It was found that Examples 1 to 4 had reduced smoke generation during molding compared to Comparative Examples 1 to 4, and had the effect of reducing smoke generation during molding.
[0134] As described above, according to the present invention, by using a rubber softener characterized by a weight average molecular weight (Mw) of 800 to 1,200 and a polydispersity index (PDI) expressed by weight average molecular weight (Mw) / number average molecular weight (Mn) of less than 1.10 as measured by gel permeation chromatography (GPC), it is possible to provide a polyester-based elastomer composition having excellent heat fusion properties with polar hard resins such as polycarbonate resins (PC resins and bio-PC resins) and acrylonitrile-butadiene copolymer resins (ABS resins). Furthermore, it is found that the rubber elasticity is improved, the weight is reduced, and there is an effect of less smoke generation during molding. [Industrial Applicability]
[0135] According to the present invention, it is possible to provide molded articles and laminates which can be heat fused to polar hard resins such as polycarbonate resins (PC resin and bio-PC resin) and acrylonitrile-butadiene copolymer resins (ABS resins), and which have improved rubber elasticity, reduced weight, and a soft texture with low smoke generation during molding. The molded article and laminate produced according to the present invention can be suitably used for applications such as stationery, toys, sporting goods, covers for mobile phones and smartphones, parts such as grips, school teaching materials, home appliances, repair parts for office automation equipment, various parts for automobiles, motorcycles, bicycles, etc., and building materials, etc.< / mfr>
Claims
1. A polyester-based elastomer composition comprising the following components (A), (B) and (C): Component (A): Polyester-based elastomer Component (B): Styrene-based elastomer Component (C): A rubber softener having a weight average molecular weight (Mw) of 800 to 1,200 and a polydispersity index (PDI) expressed as weight average molecular weight (Mw) / number average molecular weight (Mn) of less than 1.10 as measured by gel permeation chromatography (GPC).
2. 2. The polyester elastomer composition according to claim 1, wherein the rubber softener of component (C) is an isoalkane mixture.
3. 3. The polyester-based elastomer composition according to claim 1, wherein the contents of the components (B) and (C) are each less than 100 parts by mass when the content of the component (A) is taken as 100 parts by mass.
4. 3. The polyester-based elastomer composition according to claim 1, wherein the component (A) has a hard segment and a soft segment, and the soft segment is a polyalkylene glycol.
5. The polyester-based elastomer composition according to claim 4 , wherein the content of the soft segment in the component (A) is 10% by mass or more and 95% by mass or less.
6. The polyester-based elastomer composition according to claim 4, wherein the polyalkylene glycol is polytetramethylene glycol.
7. 3. The polyester elastomer composition according to claim 1, having a Duro A hardness according to ISO 7619-1 of 40 or more and 90 or less.
8. The polyester-based elastomer composition according to claim 1 or 2, wherein the component (C) is derived from a biomass material.
9. The polyester elastomer composition according to claim 8, wherein the biomass content according to ASTM D6866-22 is 1% or more and 100% or less.
10. A molded article comprising the polyester elastomer composition according to claim 1 or 2.
11. A laminate comprising a layer made of the polyester elastomer composition according to claim 1 or 2 and a layer made of a hard resin having polarity.
Citation Information
Patent Citations
Thermoplastic elastomer molded product
JP1998007878A
Thermoplastic elastomer composition
JP2019218561A