Heat exchanger and method for suppressing swelling of gasket
By increasing the compression ratio of gaskets in heat exchangers to 25.0% to 27.0% and applying a coating with elastic deformation followability, gasket swelling is suppressed, reducing maintenance frequency and equipment downtime.
Patent Information
- Application Number
- JP2024006774
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2044-01-19
AI Technical Summary
Conventional methods for suppressing gasket swelling in heat exchangers are not cost-effective and fail to adequately reduce the volumetric expansion coefficient, leading to frequent gasket replacement and equipment downtime, especially when dealing with aromatic hydrocarbons.
A plate-type heat exchanger with increased compression ratios of 25.0% to 27.0% and a coating film on the gasket surface with elastic deformation followability and benzene resistance, using a rubber gasket between heat transfer plates to suppress swelling.
The solution effectively reduces gasket swelling and extends the replacement cycle by half a year, minimizing equipment downtime and repair costs while maintaining heat transfer plate integrity.
Smart Images

Figure 2024137708000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat exchanger and a method for suppressing swelling of a gasket. [Background technology]
[0002] It has been known that when a liquid containing aromatic hydrocarbons is introduced into a plate-type heat exchanger in which multiple heat transfer plates are stacked, the gasket provided between adjacent heat transfer plates absorbs the aromatic hydrocarbons and expands in volume. This volume expansion of the gasket is generally called swelling, and causes the gasket to soften and deteriorate. When the gasket swells in this way, not only does the sealing performance deteriorate, but the components of the heat exchanger, especially the plates, are compressed. If the swelling of the gasket continues, the heat transfer plate undergoes plastic deformation, causing liquid leakage from the heat exchanger. In the technology disclosed in Patent Document 1, an attempt is made to change the material of the gasket. In addition, Patent Document 2 discloses a technology for suppressing excessive swelling of the gasket by immersing the gasket in oil in advance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-132754 A [Patent Document 2] Japanese Patent Application Publication No. 7-292140 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the technology disclosed in Patent Document 1 does not demonstrate cost-effectiveness, and from that perspective, it is unclear whether it is suitable for practical use. In addition, the technology disclosed in Patent Document 2 could not shorten the time it takes for the gasket to swell or reduce the volume expansion rate in an equilibrium state.
[0005] In addition, even if an emulsion breaker (surfactant), which is a chemical used to separate water (ammonia water) and oil (aromatic hydrocarbons such as tar), is added to the ammonia water upstream of the heat exchanger in an attempt to separate the aromatic hydrocarbons, it is difficult to separate them completely and gasket swelling will occur.
[0006] In conventional heat exchangers, the gasket was compressed at a compression rate of 23.1% to 24.0%, but gasket swelling occurred. Although swelling can be suppressed by increasing the compression rate of the gasket, the plate may be deformed and damaged by the repulsive force from the gasket at a compression rate of more than 24.0%, so conventionally, the gasket was compressed at 24.0% or less. For this reason, conventionally, inexpensive gaskets were used, and the heat exchanger was disassembled after a certain period of time and the gasket was replaced with a new one, assuming that gasket swelling could occur. In actual fact, gaskets need to be replaced once every six months, and since many heat exchangers are installed in coal chemical plants, the cost of gasket replacement and the impact of equipment shutdown (heat loss) were considered to be problems. Therefore, if gasket swelling can be suppressed, it can lead to a reduction in gasket replacement costs and the impact of equipment shutdown (heat loss).
[0007] The present invention has been made in consideration of the above-mentioned problems, and its object is to provide a heat exchanger and a method for suppressing gasket swelling that can suppress gasket swelling while preventing damage to heat transfer plates. [Means for solving the problem]
[0008] In order to solve the above-mentioned problems and achieve the object, the heat exchanger of the present invention is a plate-type heat exchanger in which a plurality of heat transfer plates are stacked with a rubber gasket interposed between adjacent heat transfer plates, and a space is formed between adjacent heat transfer plates through which a liquid containing aromatic hydrocarbons flows, characterized in that a coating film having elastic deformation followability and benzene resistance is formed on the surface of the gasket, and fastening members are provided for fastening the plurality of heat transfer plates so as to compress the gasket at a compression rate of 25.0[%] to 27.0[%].
[0009] The heat exchanger according to the present invention is a plate-type heat exchanger for recovering low-temperature waste heat from circulating ammonia water circulating between a coke oven and a tar decanter, and is a bottom heat exchanger connected to the bottom of a reduced-pressure ammonia stripper for distilling excess ammonia water.
[0010] Furthermore, the method for suppressing gasket swelling according to the present invention is a method for suppressing gasket swelling in a plate-type heat exchanger in which a plurality of heat transfer plates are stacked between adjacent heat transfer plates with a rubber gasket interposed therebetween, and a space is formed between the adjacent heat transfer plates through which a liquid containing aromatic hydrocarbons flows, characterized in that a coating having elastic deformation followability and benzene resistance is applied to the surface of the gasket, the plurality of heat transfer plates are fastened together with fastening members, and the gasket is compressed at a compression rate of 25.0% to 27.0%. Effect of the Invention
[0011] The heat exchanger and the method for suppressing swelling of a gasket according to the present invention have the advantage of being able to suppress swelling of the gasket while preventing damage to the heat transfer plate. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram showing an example of an ammonia water treatment system according to an embodiment. [Diagram 2]FIG. 2 is a perspective view that illustrates a heat exchanger according to the embodiment. [Diagram 3] FIG. 3 is a perspective view that illustrates a schematic exploded view of the heat exchanger according to the embodiment. [Figure 4] FIG. 4 is a side view that illustrates a schematic exploded view of the heat exchanger according to the embodiment. [Diagram 5] FIG. 5 is a diagram showing an example of the structure of a coating film formed on the surface of a gasket. [Figure 6] FIG. 6 is a diagram showing a compression mechanism for the gasket test piece used in Example 1. [Figure 7] FIG. 7 is a graph showing the time transition of the mass change rate of the gasket test piece. [Figure 8] FIG. 8 is a graph showing the change in hardness of the gasket test piece over time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of a method for suppressing swelling of a heat exchanger and a gasket according to the present invention will be described. Note that the present invention is not limited to this embodiment.
[0014] FIG. 1 is a schematic diagram showing an example of an ammonia water treatment system using a heat exchanger according to an embodiment.
[0015] In the ammonia distillation system according to the embodiment, a part of the excess ammonia distillation solution generated in the coke oven 2 is supplied to a reduced pressure ammonia stripper 4 for distilling the excess ammonia distillation solution. The excess ammonia distillation solution supplied to the ammonia stripper 4 is sent from the bottom of the ammonia stripper 4 to the heat exchanger 1, where it is heated by heat exchange in the heat exchanger 1, and then returned to the bottom of the ammonia stripper 4. As a result, the heated excess ammonia distillation solution becomes ammonia-containing steam under reduced pressure and reaches the top of the ammonia stripper 4. As a result, ammonia is removed from the excess ammonia distillation solution. Deammonia distillation solution, which is the excess ammonia distillation solution from which the ammonia has been removed, is discharged from the bottom of the ammonia stripper 4. As a heat source for the heat exchanger 1, circulating ammonia distillation solution circulating between the coke oven 2 and the tar decanter 3 is introduced into the heat exchanger 1 and used.
[0016] Fig. 2 is a perspective view showing a heat exchanger according to an embodiment. Fig. 3 is a perspective view showing a heat exchanger according to an embodiment in an exploded state. Fig. 4 is a side view showing a heat exchanger according to an embodiment in an exploded state.
[0017] The heat exchanger 1 according to the embodiment is a plate-type heat exchanger for recovering low-temperature waste heat from circulating ammonia water circulating between a coke oven 2 and a tar decanter 3, and is a bottom heat exchanger connected to the bottom of a reduced-pressure ammonia stripper 4 for distilling excess ammonia water. The heat exchanger 1 according to the embodiment is composed of a pair of nameplates 11a, 11b, a plurality of heat transfer plates 12 arranged between the nameplates 11a, 11b, a plurality of gaskets 13 arranged between adjacent heat transfer plates 12, a plurality of bolts 14, a plurality of nuts 15, and the like.
[0018] The heat exchanger 1 performs heat exchange by stacking a plurality of heat transfer plates 12 side by side, forming a first space forming a flow path for a high-temperature medium between adjacent heat transfer plates 12, and a second space forming a flow path for a low-temperature medium between the first space and the second space. A gasket 13, which is a sealing member that maintains liquid-tightness, is disposed between adjacent heat transfer plates 12 to maintain the liquid-tight state.
[0019] The heat transfer plates 12 are integrated by being sandwiched between the pair of nameplates 11a, 11b. To sandwich the heat transfer plates 12 between the pair of nameplates 11a, 11b, a plurality of fastening members, namely a plurality of bolts 14 and a plurality of nuts 15, are provided at predetermined intervals around each of the pair of nameplates 11a, 11b. Note that the bolts 14 and nuts 15 are not shown in Figs. 2 and 3.
[0020] 3, reference numeral 111 denotes a supply pipe for supplying the circulating ammonia water, which is a high-temperature medium, to the heat exchanger 1, reference numeral 112 denotes a discharge pipe for discharging the circulating ammonia water from the heat exchanger 1, reference numeral 113 denotes a supply pipe for supplying excess ammonia water, which is a low-temperature medium, to the heat exchanger 1, and reference numeral 114 denotes a discharge pipe for discharging the excess ammonia water from the heat exchanger 1. In the heat exchanger 1 having such a configuration, the circulating ammonia water supplied from the supply pipe 111 passes through a flow path 121 for flowing a high-temperature medium, a first space, a flow path 122, etc. of the heat exchanger 1, and is discharged from the discharge pipe 112. On the other hand, the excess ammonia water supplied from the supply pipe 113 passes through a flow path 123 for flowing a low-temperature medium, a second space, a flow path 124, etc. of the heat exchanger 1, and is discharged from the discharge pipe 114. As a result, heat exchange is performed between the circulating ammonia water (high-temperature medium) and the excess ammonia water (low-temperature medium) via the multiple heat transfer plates 12.
[0021] The heat exchanger 1 according to the embodiment has a structure in which heat transfer plates 12 and gaskets 13 are alternately arranged and sandwiched. The heat exchanger 1 prevents leakage of liquid introduced into the heat exchanger by compressing the gaskets 13 in the grooves of the heat transfer plates 12 so that they are tightly attached. However, conventionally, compression is only for sealing purposes, not for the purpose of preventing swelling, and compression is performed to 24.0% or less.
[0022] In the heat exchanger 1 according to the embodiment, the compression ratio of the gasket 13 is increased in order to prevent the swelling of the gasket 13. For example, when the distance L between the pair of nameplates 11a and 11b is 1817 mm, the width Lp of the heat transfer plate 12 is 4.16 mm, and the number N of the heat transfer plates 12 is 395, the total width of the gasket 13 is expressed as LN×Lp. By increasing the compression ratio of the gasket 13 from 23.1% to 25.0%, the distance L between the pair of nameplates 11a and 11b is reduced by 2.1 mm. In addition, by increasing the compression ratio of the gasket 13 from 23.1% to 27.0%, the distance L between the pair of nameplates 11a and 11b is reduced by 5.0 mm. Furthermore, by increasing the compression rate of the gasket 13 from 23.1% to 30.0%, the distance L between the pair of nameplates 11a and 11b is reduced by 7.5 mm.
[0023] As described above, by sandwiching the gasket 13 between the heat transfer plates 12 and increasing the compressive force, it is easy to obtain the effect of suppressing the swelling of the gasket 13. However, care must be taken because if the compressive force is increased too much, the repulsive force of the gasket 13 may become too large, which may hasten the deformation of the heat transfer plates 12.
[0024] In the heat exchanger 1 according to the embodiment, examples of the material that can be used for the gasket 13 (rubber base material 131 described below) include EPDM (ethylene propylene rubber), IIR (butyl) rubber, and fluororubber.
[0025] Here, it is possible to set the compression rate of the gasket 13 to 24.0[%] to 33.0[%] in terms of the structure of the heat exchanger 1. On the other hand, if the compression rate of the gasket 13 is 24.0[%] or more, there is a concern that the swelling of the gasket 13 may cause deformation of the heat transfer plate 12, and even damage to the heat transfer plate 12. Therefore, in the heat exchanger 1 according to the embodiment, a coating for suppressing swelling is applied to the surface of the gasket 13.
[0026] FIG. 5 is a diagram showing an example of the structure of a coating film formed on the surface of the gasket 13. As shown in FIG.
[0027] As shown in FIG. 5, the gasket 13 is formed by coating a rubber base material 131 with paint made of a binder 133 containing a scaly filler 132, and a coating film is formed on the surface of the gasket 13. After the coating film is formed, it forms a flexible and transparent thin film, and has adhesion to the rubber base material 131 and elastic deformation followability. Furthermore, the coating film has a barrier property against chemicals such as benzene resistance because the binder 133 contains the scaly filler 132 having high barrier properties such as silica-based scaly filler or metal-based scaly filler as a filler. The thickness of the coating film is preferably 90 μm or more and 110 μm or less, and is preferably 100 μm.
[0028] The scaly filler 132 may be, for example, scaly silica powder or scaly metal powder.
[0029] As the binder 133, for example, a fluorine-containing resin is preferably used. As the fluorine-containing resin, for example, a solvent-based paint made of a copolymer of TFE (Tetrafluoroethylene), isobutylene, and hydroxybutyl vinyl ether can be mentioned. As the fluorine-containing resin, for example, a solvent-based paint made of a copolymer of TFE, vinyl versatate, and hydroxybutyl vinyl ether can be mentioned. As the fluorine-containing resin, for example, a solvent-based paint made of a copolymer of CTFE (Chloro Tri Fluoro Ethylene) and hydroxybutyl vinyl ether can be mentioned. As the fluorine-containing resin, for example, a solvent-based paint made of a copolymer of TFE, vinylidene fluoride, and hydroxybutyl vinyl ether can be mentioned.
[0030] A curing agent appropriate for the functional group of the fluorine-containing resin can be selected and added to the binder 133. For example, when a fluorine-containing resin having a hydroxyl group is used for the binder 133, a polyisocyanate compound, a melamine curing agent, a urea resin curing agent, a silicate compound, an isocyanate group-containing silane compound, and a polybasic acid curing agent can be used. Among these, a polyisocyanate compound is preferred because it provides an excellent balance of physical properties of the cured film.
[0031] The method of applying the paint (binder 133 containing scaly filler 132) to the surface of rubber substrate 131 is not particularly limited, and for example, it can be applied using a known application device such as an air spray coating device. After applying the paint (binder 133 containing scaly filler 132) to rubber substrate 131, a drying process is performed to form a coating layer on the surface of rubber substrate 131. The drying conditions at this time are not particularly limited, and for example, from the viewpoint of promoting the crosslinking reaction and protecting the urethane layer, it is preferable that the drying temperature is 60[°C] to 150[°C]. The drying time may be appropriately set until the curing of the paint (binder 133) is completed.
[0032] In this embodiment, in the heat exchanger 1 into which a liquid (ammonia) containing aromatic hydrocarbons is introduced, the gasket 13 is painted, and a paint film having elastic deformation followability and benzene resistance is formed on the surface of the gasket 13. Furthermore, in the heat exchanger 1 according to the embodiment, the heat transfer plates 12 are fastened by the fastening members, the bolts 14 and the nuts 15, so that the gasket 13 is compressed at a compression rate of 25.0% to 27.0%. As a result, in the heat exchanger 1 according to the embodiment, a remarkable swelling suppression effect of the gasket 13 is obtained. That is, there is a concern that the deformation of the heat transfer plate 12 may occur due to an increase in the repulsive force of the gasket 13 caused by an increase in the fastening force. However, in the heat exchanger 1 according to the embodiment, due to the swelling suppression effect by the painting of the gasket 13, it is possible to increase the compression rate of the gasket 13 while suppressing the deformation of the heat transfer plate 12 up to a compression rate of 27.0%. And, due to the compression of the gasket 13 and the swelling suppression effect by painting, the period until leakage of the liquid (ammonia water) introduced into the heat exchanger 1 can be extended by half a year when the compression rate of the gasket 13 is 25.0[%] to 27.0[%] compared to the case where the compression rate is 23.1[%]. As a result, in the heat exchanger 1 according to the embodiment, it is possible to reduce repair costs by extending the replacement period of the gasket 13 and reduce the effect of equipment stoppage (heat loss). As described above, in order to obtain a sufficient swelling suppression effect while suppressing the deformation of the heat transfer plate 12 due to compression, the compression rate of the gasket 13 is set to 25[%] or more and 27[%] or less, more preferably 25.1[%] or more and 26.9[%] or less.
[0033] Example 1 Hereinafter, the configuration of the present invention will be described in detail based on an embodiment in which the present invention is applied to a gasket test piece made of EPDM (ethylene propylene rubber) for a plate-type heat exchanger.
[0034] FIG. 6 is a diagram showing a compression mechanism for the gasket test piece 201 used in Example 1. As shown in FIG.
[0035] In Example 1, the structure of a plate-type heat exchanger was simulated, and a pair of steel plates 202a, 202b sandwiching an EPDM gasket test piece 201 was fastened using a plurality of bolts 203 and a plurality of nuts 204. The compression ratios of the gasket test piece 201 were set to 23.1[%] and 24.0[%], which are equivalent to the actual machine set values, and 25.0[%], 27.0[%], 30.0[%], and 33.0[%], which exceed the actual machine set values.
[0036] In Example 1, the gasket test piece 201, which was sandwiched between a pair of plates 202a and 202b and compressed, was immersed in a liquid having the same composition as the liquid (ammonia water) introduced into the heat exchanger 1. Then, the mass change rate and hardness change of the gasket test piece 201 were measured 7 days after the start of immersion, 14 days after the start of immersion, and 21 days after the start of immersion. The compression rate of the gasket test piece 201 was obtained by dividing the thickness change amount of the gasket test piece 201 before and after compression by the thickness of the gasket test piece before compression. The mass change rate was obtained by dividing the mass change amount of the gasket test piece 201 before and after the immersion test by the mass of the gasket test piece 201 before immersion. The hardness of the gasket test piece 201 was measured by a measurement method conforming to JIS K 6253, and the hardness change before and after the immersion test was obtained.
[0037] The immersion liquid in which the gasket test piece 201 is immersed contains 1000 [ppm] to 4000 [ppm] of ammonia and 0 [ppm] to 1500 [ppm] of benzene, simulating the ammonia solution that is the liquid introduced into the heat exchanger 1. The gasket test piece 201 is prepared by cutting an EPDM gasket into a length of about 5 [mm] and compressing it by sandwiching it with the compression mechanism shown in Fig. 6. When neither compression nor sandwiching between the heat transfer plates 12 is performed, the mass increase rate and hardness change of the gasket test piece 201 reach an equilibrium state in about 7 days.
[0038] FIG. 7 is a graph showing the time course of the mass change rate of the gasket test piece 201. FIG. 8 is a graph showing the time course of the hardness change of the gasket test piece 201. In FIG. 7 and FIG. 8, "coated" indicates that the surface of the gasket test piece 201 is coated with the paint described in the above embodiment, and a coating film having elastic deformation followability and benzene resistance is formed on the surface of the gasket test piece 20. The thickness of the coating film is set to 100 [μm]. In FIG. 7 and FIG. 8, "no coating" indicates that there is no coating film on the surface of the gasket test piece 201.
[0039] As shown in FIG. 7 and FIG. 8, it was confirmed that by increasing the compression ratio of the gasket test piece 201, both the mass change rate and the hardness change of the gasket test piece 201 were reduced.
[0040] Example 2 In Example 2, based on the results of Example 1, a gasket with and without coating was applied to an actual heat exchanger with five different compression ratios: 24.0% (%), 25.0% (%), 27.0% (%), 30.0% (%), and 33.0% (%). The coating material used for coating the surface of the gasket was the same as that described in the above embodiment. These heat exchangers were used to exchange heat between liquids containing aromatic hydrocarbons for two years, and the deformation of the heat transfer plate and the presence or absence of leakage of the introduced liquid were observed. Table 1 shows the observation results after two years. In Table 1, "◯" indicates no leakage, "△" indicates leakage but no damage to the heat transfer plate, and "×" indicates leakage and damage to the heat transfer plate.
[0041] [Table 1]
[0042] As can be seen from Table 1, in the heat exchanger using an unpainted gasket, damage to the heat transfer plate and leakage occurred at all compression rates. On the other hand, in the heat exchanger using a painted gasket, the heat transfer plate deformed and liquid leaked at a compression rate of 24.0%. In the heat exchanger using a painted gasket, no leakage occurred at compression rates of 25.0% and 27.0%. In the heat exchanger using a painted gasket, the heat transfer plate deformed and liquid leaked at a compression rate of 30.0%. In the heat exchanger using a painted gasket, the heat transfer plate broke and leakage occurred at a compression rate of 33.0%.
[0043] Thus, with an unpainted gasket, increasing the compression rate above 24.0% would damage the heat transfer plate, and no swelling suppression effect could be achieved. On the other hand, with a painted gasket, leakage could be suppressed without damaging the heat transfer plate at a compression rate of 25.0% to 27.0%. This shows that compressing a painted gasket at a compression rate of 25.0% to 27.0% would achieve a significant swelling suppression effect, and could extend the gasket's lifespan by six months. [Explanation of symbols]
[0044] 1 heat exchanger 2. Coke ovens 3 Tar Decanter 4. Ammonia Stripper 11a, 11b Nameplate 12 Heat transfer plate 13 Gasket 14 Volts 15 Nut 111,113 Supply pipe 112,114 Discharge pipe 121,122,123,124 Distribution Channels 131 Rubber base material 132 Scaly Filler 133 Binder 201 Gasket test piece 202a, 202b Plate 203 Volts 204 Nut
Claims
1. A plate-type heat exchanger in which a plurality of heat transfer plates are stacked with a rubber gasket between adjacent heat transfer plates, and a space through which a liquid containing aromatic hydrocarbons flows is formed between adjacent heat transfer plates, A coating film having elastic deformation followability and benzene resistance is formed on the surface of the gasket, A heat exchanger comprising fastening members for fastening the heat transfer plates together so as to compress the gasket at a compression rate of 25.0% to 27.0%.
2. A plate-type heat exchanger for recovering low-temperature waste heat from circulating ammonia water between a coke oven and a tar decanter, comprising:
2. The heat exchanger according to claim 1, which is a bottom heat exchanger connected to the bottom of a reduced-pressure ammonia stripper for distilling excess ammonia water.
3. A method for suppressing swelling of a gasket in a plate-type heat exchanger in which a plurality of heat transfer plates are stacked with a rubber gasket interposed between adjacent heat transfer plates, and a space through which a liquid containing aromatic hydrocarbons flows is formed between adjacent heat transfer plates, comprising: A coating having elastic deformation followability and benzene resistance is applied to the surface of the gasket; A method for suppressing swelling of a gasket, comprising fastening a plurality of the heat transfer plates with fastening members and compressing the gasket at a compression rate of 25.0% to 27.0%.
Citation Information
Patent Citations
Method for treating excess ammoniacal liquor
JP2016112516A
Elastomeric Gasket
US20110284194A1
Sealing product made of synthetic rubber and adjusting treatment for its excessive swelling
JP1995292140A
Seal member for rolling bearing, molded article and method for preventing or reducing curing or swelling of molded article by urea compound
JP2016132754A