Primer for UV curable coat agent

A primer with acid-modified polyolefin resin, urethane resin, and ethylene glycol in specific ratios provides effective adhesion and flexibility on thermoplastic resin base materials, overcoming high-temperature drying requirements and film rigidity issues.

JP2024137791APending Publication Date: 2024-10-07UNITIKA LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024037681
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-22
Filing Date
2024-03-12
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing primers for UV-curable coating agents on thermoplastic resin base materials, particularly polyester and polyolefin resins, require high-temperature drying, leading to poor adhesion and flexibility issues, especially when forming a coating film during UV curing.

Method used

A primer composition containing acid-modified polyolefin resin, urethane resin, and ethylene glycol in specific ratios, allowing for adhesion and flexibility even at low drying temperatures, forming a flexible coating film on thermoplastic resin base materials.

Benefits of technology

The primer achieves good adhesion and flexibility of the coating film on polyester and polyolefin resin base materials, even when dried at low temperatures, addressing the limitations of existing primers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137791000001
    Figure 2024137791000001
  • Figure 2024137791000002
    Figure 2024137791000002
Patent Text Reader

Abstract

To provide a primer coated onto a thermoplastic resin base material which is excellent in adhesion between a base material and a UV curable resin even in low temperature drying, and enables formation of a coating film having flexibility.SOLUTION: A primer for a UV curable coat agent contains 100 pts.mass of an acid modified polyolefin resin (A), 20 to 50 pts.mass of an urethane resin (B), 0.3 to 3 pts.mass of ethylene glycol (C), and an aqueous medium.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a primer for UV-curable coating agents, which contains an acid-modified polyolefin resin, a urethane resin, and ethylene glycol in specific ratios. [Background technology]

[0002] Traditionally, floors, walls, etc. have often been covered with resin to protect them and maintain their beauty. In particular, there is a demand for highly durable resins that can maintain their appearance for a long period of time, and UV-curable coating agents are often used because of their ease of application. In recent years, as the required performance has become more diverse and sophisticated, studies are being conducted on applying a UV-curable coating agent to a thermoplastic resin substrate, particularly a polyester resin substrate or a polyolefin resin substrate. When applying a UV-curable coating agent to a substrate, a primer is often used, and for example, Cited Document 1 discloses a polyolefin / polyester mixed primer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-229737 A Summary of the Invention [Problem to be solved by the invention]

[0004] The primer described in Reference 1 has good adhesion to substrates such as polyolefin resins, but in order to improve adhesion, it is necessary to dry it at a high temperature, which poses an issue in terms of workability. In addition, the coating film formed from the primer has poor flexibility and may not be able to withstand shrinkage during UV curing. An object of the present invention is to provide a primer to be applied to a thermoplastic resin substrate, particularly a polyester resin substrate or a polyolefin resin substrate, which has excellent adhesion between the substrate and a UV-curable resin even during drying at low temperature and can form a coating film having flexibility. [Means for solving the problem]

[0005] Means for Solving the Problems The present inventors conducted extensive research to solve the above problems and discovered that a primer containing an acid-modified polyolefin resin, a urethane resin, and ethylene glycol in specific ratios has excellent adhesion to a UV-curable coating layer, and also has excellent adhesion to polyester resin substrates and polyolefin resin substrates and to a UV-curable coating layer even when dried at low temperature, and the resulting coating film has flexibility, thereby arriving at the present invention.

[0006] That is, the gist of the present invention is as follows. (1) A primer for a UV-curable coating agent, comprising: 100 parts by mass of an acid-modified polyolefin resin (A); 20 to 50 parts by mass of a urethane resin (B); 0.3 to 3 parts by mass of ethylene glycol (C); and an aqueous medium. (2) A primer for UV-curable coating agents according to (1), characterized in that the urethane resin (B) is a polyether-type polyurethane. (3) The primer for UV-curable coating agents according to (1) or (2), wherein the acid-modified polyolefin resin (A) has a melting point of 60 to 110°C. (4) A coating film formed from the primer described in (1) or (2) above. (5) A laminate comprising a thermoplastic resin substrate, the coating film according to (4), and a UV-curable coating layer laminated in this order. (6) The laminate according to (5), wherein the thermoplastic resin substrate is a polyester substrate or a polyolefin substrate. Effect of the Invention

[0007] According to the primer for UV-curable coating agent of the present invention, a primer layer having good adhesion to a thermoplastic resin substrate and a UV-curable coating layer can be obtained. In particular, even when dried at low temperature on a polyester resin substrate or a polyolefin resin substrate, which have been difficult to apply in the past, a primer layer having good adhesion to a UV-curable coating layer and flexibility can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in detail below. The primer for a UV-curable coating material of the present invention contains an acid-modified polyolefin resin (A), a urethane resin (B), ethylene glycol (C), and an aqueous medium.

[0009] <Acid-modified polyolefin resin (A)> Examples of the olefin component constituting the acid-modified polyolefin resin (A) include alkenes such as ethylene, propylene, isobutylene, 1-butene, 1-pentene, 1-hexene, and 1-octene, and cycloalkenes such as norbornene, and mixtures thereof can also be used. Among these, alkenes having 2 to 6 carbon atoms such as ethylene, propylene, isobutylene, 1-butene, 1-pentene, and 1-hexene are preferred, and alkenes having 2 to 4 carbon atoms such as ethylene, propylene, isobutylene, and 1-butene are particularly preferred. In addition, two or more kinds of olefin components may be copolymerized. The content of the olefin component in the acid-modified polyolefin resin (A) is preferably 50% by mass or more, more preferably 70% by mass or more. If the content of the olefin component is less than 50% by mass, the properties derived from the polyolefin resin, such as adhesion to substrates, may be lost.

[0010] The acid-modified polyolefin resin (A) must contain an unsaturated carboxylic acid component and be acid-modified in order to make the resin water-soluble (liquefied) and to improve the adhesion between the resulting coating film and the substrate. The content of the unsaturated carboxylic acid component in the acid-modified polyolefin resin (A) must be 0.1 to 25% by mass, preferably 0.5 to 15% by mass, more preferably 1 to 8% by mass, and even more preferably 1 to 5% by mass. Examples of the unsaturated carboxylic acid component include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, crotonic acid, etc., as well as half esters and half amides of unsaturated dicarboxylic acids, etc. Among these, acrylic acid, methacrylic acid, maleic acid, and maleic anhydride are preferred, and acrylic acid and maleic anhydride are more preferred. The unsaturated carboxylic acid component may be copolymerized in the polyolefin resin in any form, and examples of the form include random copolymerization, block copolymerization, and graft copolymerization.

[0011] The acid-modified polyolefin resin (A) preferably contains a (meth)acrylic acid ester component for the reason of improving adhesion to thermoplastic resin substrates, particularly polyolefin resin substrates such as polyethylene and polypropylene. The content of the (meth)acrylic acid ester component in the acid-modified polyolefin resin (A) is preferably 40% by mass or less, more preferably 35% by mass or less, even more preferably 30% by mass or less, and most preferably 25% by mass or less in order to provide good adhesion to various thermoplastic resin film substrates. If the content of the (meth)acrylic acid ester component in the acid-modified polyolefin resin (A) exceeds 40% by mass, the properties of the olefin-derived resin are lost, and the resulting coating film may have reduced adhesion to the substrate. Examples of the (meth)acrylic acid ester component include esters of (meth)acrylic acid and alcohols having 1 to 30 carbon atoms, and among these, from the viewpoint of easy availability, esters of (meth)acrylic acid and alcohols having 1 to 20 carbon atoms are preferred. Specific examples of such compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate. A mixture of these may also be used. Among these, from the viewpoint of adhesion to the base film, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl acrylate, and octyl acrylate are more preferred, ethyl acrylate and butyl acrylate are more preferred, and ethyl acrylate is particularly preferred. (Note that "(meth)acrylic acid" means "acrylic acid or methacrylic acid.")

[0012] In addition to the above components, other components may be contained in an amount of about 10 mass% or less of the acid-modified polyolefin resin (A). Examples of other components include dienes, maleic acid esters such as dimethyl maleate, diethyl maleate, and dibutyl maleate, (meth)acrylic acid amides, alkyl vinyl ethers such as methyl vinyl ether and ethyl vinyl ether, vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, vinyl pivalate, and vinyl versatate, as well as vinyl alcohols obtained by saponifying vinyl esters with a basic compound, vinyl halides, vinylidene halides, 2-hydroxyethyl acrylate, glycidyl (meth)acrylate, (meth)acrylonitrile, styrene, substituted styrene, carbon monoxide, and sulfur dioxide, and mixtures thereof may also be used.

[0013] Specific examples of the acid-modified polyolefin resin (A) include ethylene-acrylic acid ester-maleic anhydride copolymer, ethylene-propylene-maleic anhydride copolymer, ethylene-butene-maleic anhydride copolymer, propylene-butene-maleic anhydride copolymer, ethylene-propylene-butene-maleic anhydride copolymer, ethylene-propylene-acrylic acid ester-maleic anhydride copolymer, ethylene-butene-acrylic acid ester-maleic anhydride copolymer, propylene-butene-acrylic acid ester-maleic anhydride copolymer, ethylene-propylene-butene-acrylic acid ester-maleic anhydride copolymer, propylene-maleic anhydride copolymer, and the like, among which ethylene-acrylic acid ester-maleic anhydride copolymer, propylene-butene-maleic anhydride copolymer, and ethylene-propylene-butene-maleic anhydride copolymer are most preferred. These acid-modified polyolefin resins (A) may be used in combination of two or more kinds, for example, a combination of an ethylene-acrylic acid ester-maleic anhydride copolymer and a propylene-butene-maleic anhydride copolymer, or a combination of an ethylene-acrylic acid ester-maleic anhydride copolymer and an ethylene-propylene-butene-maleic anhydride copolymer may be mentioned.

[0014] When the acid-modified polyolefin resin (A) is an ethylene (a1)-acrylic acid ester (a4)-maleic anhydride (a5) copolymer, the mass ratio (a1 / a4 / a5) is preferably from 95 / 4 / 1 to 55 / 40 / 5, more preferably from 94 / 5 / 1 to 60 / 36 / 4, and particularly preferably from 92 / 7 / 1 to 62 / 35 / 3. In the case of a propylene (a2)-butene (a3)-maleic anhydride (a5) copolymer, the mass ratio (a2 / a3 / a5) is preferably from 95 / 4 / 1 to 53 / 40 / 7, more preferably from 94 / 5 / 1 to 60 / 34 / 6, and particularly preferably from 92 / 7 / 1 to 62 / 33 / 5. In the case of a propylene (a2)-ethylene (a1)-butene (a3)-maleic anhydride (a5) copolymer, the mass ratio (a2 / a1 / a3 / a5) is preferably 95 / 3 / 1 / 1 to 50 / 15 / 28 / 7.

[0015] The acid-modified polyolefin resin (A) preferably has a melt flow rate of 0.01 to 500 g / 10 min at 190° C. under a load of 2160 g, which is an index of molecular weight, more preferably 0.1 to 400 g / 10 min, even more preferably 1 to 300 g / 10 min, and particularly preferably 5 to 200 g / 10 min. If the acid-modified polyolefin resin (A) has a melt flow rate of less than 0.01 g / 10 min, it may be difficult to make the resin water-based. On the other hand, if the acid-modified polyolefin resin (A) has a melt flow rate of more than 500 g / 10 min, the resulting coating film tends to be hard and brittle, and the flexibility of the coating film may decrease.

[0016] The melting point of the acid-modified polyolefin resin (A) is preferably 60 to 110° C., more preferably 62 to 105° C., and even more preferably 65 to 100° C. If the melting point is below the above range, the cohesive force is weak and the resulting coating film may have poor adhesion. If the melting point exceeds the above range, the film-forming ability is reduced, and the resulting coating film may have poor adhesion.

[0017] <Urethane resin (B)> The urethane resin (B) is a polymer containing a urethane bond in the main chain, and examples thereof include those obtained by reacting a polyol compound with a polyisocyanate compound. The urethane resin (B) in the present invention is not particularly limited, but is preferably a polyether-type polyurethane resin because of its excellent adhesion to UV resins. The polyether type polyurethane resin contains a polyether polyol as a polyol component constituting polyurethane. Examples of the polyether polyol include polyoxyethylene polyols such as polyethylene glycol, polyoxypropylene polyols such as polypropylene glycol, and polyoxyethylene / propylene polyols such as polytetramethylene ether glycol. Among them, polyether diols such as polyethylene glycol and polytetramethylene glycol are preferred because they are easily available, and polytetramethylene glycol is more preferred because it improves adhesion. The molecular weight of the polyether diol is not particularly limited, but is preferably in the range of 1000 to 10000, and particularly preferably 1000 to 5000. As polyols other than polyether polyols, 1,3-butanediol, 1,4-butanediol, 1,2-propanediol, 1,3-propanediol, 1,6-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, methyl-1,5-pentanediol, 1,8-octanediol, 2-ethyl-1,3-hexanediol, and the like may be used as long as the effects of the present invention are not impaired.

[0018] The polyisocyanate component constituting the urethane resin (B) may be one or a mixture of two or more of known aromatic, aliphatic and alicyclic diisocyanates. Specific examples of diisocyanates include tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 1,3-phenylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, 1,5-naphthalene diisocyanate, isophorone diisocyanate, dimethyl diisocyanate, lysine diisocyanate, hydrogenated 4,4'-diphenylmethane diisocyanate, hydrogenated tolylene diisocyanate, dimer diisocyanate in which the carboxyl group of dimer acid is converted to an isocyanate group, and their adducts, biurets and isocyanurates.

[0019] The content of the urethane resin (B) relative to 100 parts by mass of the acid-modified polyolefin resin (A) must be 20 to 50 parts by mass, and from the viewpoints of adhesion to a UV-curable coating agent and coating film flexibility, it is preferably 22 to 45 parts by mass, and more preferably 25 to 40 parts by mass. If the content of the urethane resin (B) relative to 100 parts by mass of the acid-modified polyolefin resin (A) is less than 20 parts by mass, the resulting coating film will have reduced adhesion to a UV-curable coating agent, and if it exceeds 50 parts by mass, the resulting coating film may have reduced adhesion to a polyolefin substrate.

[0020] <Ethylene glycol> The primer of the present invention contains ethylene glycol (C), and the content thereof must be 0.3 to 3 parts by mass relative to 100 parts by mass of the acid-modified polyolefin resin (A), and from the viewpoint of adhesion to a UV-curable coating agent, it is preferably 0.4 to 2.5 parts by mass, and more preferably 0.5 to 2 parts by mass. If the content of ethylene glycol (C) relative to 100 parts by mass of the acid-modified polyolefin resin (A) is less than 0.3 parts by mass, the resulting coating film will have reduced adhesion to a UV-curable coating agent, and if it exceeds 3 parts by mass, the resulting coating film will tend to have reduced flexibility.

[0021] <Aqueous medium> The primer for UV-curable coating agents of the present invention contains an aqueous medium. The content of the aqueous medium in the primer is preferably 60 to 95% by mass, and more preferably 65 to 90% by mass. If the content of the aqueous medium in the primer is less than 60% by mass, the stability may decrease, and if it exceeds 95% by mass, the drying property may be poor. From the viewpoint of safety for workers and the working environment, the aqueous medium is most preferably water. However, for the purpose of making the acid-modified polyolefin resin (A) or the urethane resin (B) aqueous-based, reducing the drying load, or the like, the aqueous medium may contain a hydrophilic organic solvent other than water within a range that does not deviate from the characteristics of the aqueous medium. Examples of hydrophilic organic solvents include ketones such as methyl ethyl ketone, acetone, and diethyl ketone; alcohols such as propanol, butanol, methanol, and ethanol; cyclic ethers such as tetrahydrofuran and dioxane; and glycol derivatives such as ethylene glycol monobutyl ether. The content of these organic solvents in the aqueous medium is preferably 40% by mass or less, more preferably 20% by mass or less, and even more preferably 5% by mass or less. In addition, the aqueous medium may contain a basic compound that is added when the acid-modified polyolefin resin (A) is made aqueous, as described below.

[0022] The primer of the present invention may contain a non-volatile water-based auxiliary such as an emulsifier, but from the viewpoint of the water resistance and adhesion of the resulting coating film, it is preferable that the amount is 5% by mass or less of the primer, and it is most preferable that the primer does not contain any. Note that, if the manufacturing method described below is used, an aqueous dispersion containing fine and stable acid-modified polyolefin resin (A) particles can be obtained without adding a non-volatile water-based auxiliary, and the primer of the present invention can be prepared using this. Note that, examples of non-volatile water-based auxiliary include emulsifiers, compounds having protective colloid action, modified waxes, acid-modified compounds with high acid values, water-soluble polymers, etc., which are described below.

[0023] The emulsifier may be a cationic emulsifier, an anionic emulsifier, a nonionic emulsifier, or an amphoteric emulsifier, and may include surfactants in addition to those generally used in emulsion polymerization.For example, the anionic emulsifier may be a sulfate salt of higher alcohol, a higher alkyl sulfonate, a higher carboxylate, an alkylbenzene sulfonate, a polyoxyethylene alkyl sulfate salt, a polyoxyethylene alkyl phenyl ether sulfate salt, or a vinyl sulfosuccinate, etc., the nonionic emulsifier may be a compound having a polyoxyethylene structure such as polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, polyethylene glycol fatty acid ester, ethylene oxide propylene oxide block copolymer, polyoxyethylene fatty acid amide, or ethylene oxide-propylene oxide copolymer, or a sorbitan derivative such as polyoxyethylene sorbitan fatty acid ester, etc., and the amphoteric emulsifier may be lauryl betaine, lauryl dimethylamine oxide, etc. Examples of compounds having a protective colloid effect, modified waxes, acid-modified compounds with a high acid value, and water-soluble polymers include polyvinyl alcohol, carboxyl group-modified polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, modified starch, polyvinylpyrrolidone, polyacrylic acid and its salts, acid-modified polyolefin waxes and their salts having a number average molecular weight of usually 5000 or less, such as carboxyl group-containing polyethylene wax, carboxyl group-containing polypropylene wax, and carboxyl group-containing polyethylene-propylene wax, carboxyl group-containing polymers and their salts having an unsaturated carboxylic acid content of 10 mass% or more, such as acrylic acid-maleic anhydride copolymers and their salts, styrene-(meth)acrylic acid copolymers, ethylene-(meth)acrylic acid copolymers, isobutylene-maleic anhydride alternating copolymers, and (meth)acrylic acid-(meth)acrylic acid ester copolymers, polyitaconic acid and its salts, water-soluble acrylic copolymers having amino groups, gelatin, gum arabic, and casein, which are generally used as dispersion stabilizers for fine particles.

[0024] <Method for Producing Primer for UV-Curable Coating Agent> Next, a method for producing a primer for a UV-curable coating agent of the present invention will be described. As a method for producing the primer of the present invention, there is no particular limitation as long as the acid-modified polyolefin resin (A), the urethane resin (B), and the ethylene glycol (C) are uniformly mixed in an aqueous medium and can be dispersed or dissolved therein. For example, the following methods can be mentioned. (A) A method of mixing an aqueous dispersion of the acid-modified polyolefin resin (A) prepared in advance, an aqueous dispersion of the urethane resin (B) prepared in advance, and ethylene glycol (C), (a) A method of simultaneously aqueous-dispersing the acid-modified polyolefin resin (A), the urethane resin (B), and ethylene glycol (C). Among these, the method (a) can more easily prepare an aqueous dispersion composed of various combinations of the acid-modified polyolefin resin (A), the urethane resin (B), and ethylene glycol (C).

[0025] Next, a method for producing an aqueous dispersion of the acid-modified polyolefin resin (A) will be described. The method for obtaining the aqueous dispersion of the acid-modified polyolefin resin (A) is not particularly limited. For example, a method of heating and stirring the acid-modified polyolefin resin (A) and the aqueous medium in a sealable container can be adopted. At this time, the shape of the resin used for aqueous conversion is not particularly limited, but from the viewpoint of increasing the aqueous conversion rate, it is preferable to use granular or powdery ones with a particle diameter of 1 cm or less, preferably 0.8 cm or less.

[0026] The container only needs to be equipped with a tank into which a liquid can be introduced and can appropriately stir the mixture of the aqueous medium and the resin introduced into the tank. As such a device, a known solid / liquid stirring device or emulsifier can be used, and a device capable of applying a pressure of 0.1 MPa or more is preferable. The method of stirring and the rotational speed of stirring are not particularly limited.

[0027] After each raw material is charged into the tank of this device, it is stirred and mixed at a temperature of preferably 40°C or less. Next, while maintaining the temperature in the tank at 50 to 200°C, preferably 60 to 200°C, stirring is continued for 5 to 120 minutes to sufficiently make the resin aqueous, and then the resin is cooled to 40°C or less while stirring to obtain an aqueous dispersion. If the temperature in the tank is less than 50°C, it is difficult to make the resin aqueous. If the temperature in the tank exceeds 200°C, the molecular weight of the resin may decrease.

[0028] It is preferable to add a basic compound to the acid-modified polyolefin resin (A) when it is made aqueous. The unsaturated carboxylic acid component is anionized by the basic compound, and aggregation between fine particles is prevented by electrical repulsion, imparting stability to the aqueous dispersion. The amount of the basic compound added is preferably 0.5 to 3.0 times equivalent to the carboxyl group in the acid-modified polyolefin resin (A) (1 mole of acid anhydride group is considered as 2 moles of carboxyl group), more preferably 0.8 to 2.5 times equivalent, and even more preferably 1.0 to 2.0 times equivalent. If the amount of the basic compound added is less than 0.5 times equivalent, the effect of adding the basic compound is not observed, and if it exceeds 3.0 times equivalent, the drying time during coating film formation may be extended or the aqueous dispersion may become colored.

[0029] From the viewpoint of the water resistance of the resulting coating film, the basic compound is preferably a compound that volatilizes during coating film formation, and is preferably ammonia or various organic amine compounds. The organic amine compound preferably has a boiling point of 250° C. or less. If the organic amine compound has a boiling point exceeding 250° C., it becomes difficult to remove the organic amine compound from the resin coating film by drying, and the water resistance of the coating film may decrease. Specific examples of the organic amine compound include triethylamine, N,N-dimethylethanolamine, aminoethanolamine, N-methyl-N,N-diethanolamine, isopropylamine, iminobispropylamine, ethylamine, diethylamine, 3-ethoxypropylamine, 3-diethylaminopropylamine, sec-butylamine, propylamine, methylaminopropylamine, methyliminobispropylamine, 3-methoxypropylamine, monoethanolamine, diethanolamine, triethanolamine, morpholine, N-methylmorpholine, and N-ethylmorpholine.

[0030] When the acid-modified polyolefin resin (A) is made water-based, it is preferable to add an organic solvent in order to improve the water-based conversion rate and to reduce the particle size of the resin particles. The amount of the organic solvent added is preferably 1 to 40% by mass, more preferably 2 to 30% by mass, and even more preferably 3 to 20% by mass in the aqueous dispersion of the acid-modified polyolefin resin (A). The organic solvent can be partially removed (stripped) from the system by heating the aqueous dispersion under normal or reduced pressure while stirring, and the amount of the organic solvent in the aqueous dispersion of the acid-modified polyolefin resin (A) can be reduced to 1% by mass or less. Specific examples of organic solvents include ethanol, n-propanol, isopropanol, n-butanol, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, dioxane, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether. Ethanol, isopropanol, and n-propanol are particularly preferred because they allow drying to be performed at lower temperatures.

[0031] The number average particle size of the acid-modified polyolefin resin (A) particles in the aqueous dispersion is preferably 0.5 μm or less, more preferably 0.3 μm or less, even more preferably 0.2 μm or less, and particularly preferably 0.15 μm or less, from the viewpoints of the stability of the aqueous dispersion, the surface smoothness when applied, and the transparency and adhesion of the resulting coating film. The weight average particle size is also preferably 0.5 μm or less, more preferably 0.3 μm or less.

[0032] Methods for producing an aqueous dispersion or solution of the urethane resin (B) include (1) a method in which the urethane resin is dissolved in an organic solvent and water is added to the urethane resin solution to obtain an aqueous dispersion, and (2) a method in which the urethane resin is dissolved in a mixed solvent of an organic solvent and water.

[0033] By the above-mentioned method, an aqueous dispersion or solution of the acid-modified polyolefin resin (A) or the urethane resin (B) can be produced, but commercially available products may also be used. Examples of aqueous dispersions of acid-modified polyolefin resins (A) include the "Zaixen" series manufactured by Sumitomo Seika Chemicals Co., Ltd. and the "Chemipearl" series manufactured by Mitsui Chemicals, Inc. Examples of aqueous dispersions of urethane resins (B) include the "Neolet's" series manufactured by Kusumoto Chemicals Co., Ltd. and the "Takelac" series manufactured by Mitsui Chemicals, Inc.

[0034] <Coating film> The primer of the present invention can be applied to a thermoplastic resin substrate, and then the aqueous medium can be removed to form a primer layer having good adhesion to the substrate as a coating film. In addition, a UV-curable coating layer can be laminated on the primer layer. The coating film formed from the primer of the present invention has excellent blocking resistance, and even when the coating films are brought into contact with each other, they can be easily peeled off without blocking.

[0035] Examples of substrates to which the primer of the present invention is applied include thermoplastic resin substrates such as polyester resins and polyolefin resins, and metal substrates such as aluminum. Examples of the shape of the thermoplastic resin substrate include, but are not limited to, films, sheets, injection molded articles, etc. The film may be an unstretched film or a stretched film, and its manufacturing method is also not limited. Further, the thickness of the film is not particularly limited, but usually, it may be 1 to 500 μm. Furthermore, a so-called in-line coat may be performed by applying the primer of the present invention to an unstretched film and then stretching the coated film to form a primer layer.

[0036] The method of applying the primer of the present invention to the substrate is not particularly limited, and methods such as gravure roll coating, reverse roll coating, wire bar coating, lip coating, air knife coating, curtain flow coating, spray coating, dip coating, and brush coating can be adopted. The coating amount of the primer may be appropriately determined depending on the substrate. When the substrate is a thermoplastic resin film, the thickness of the coating film is preferably 0.1 μm or more, more preferably 0.1 to 10 μm, still more preferably 0.2 to 8 μm, and particularly preferably 0.3 to 7 μm in order to sufficiently enhance the adhesion.

[0037] After coating the thermoplastic resin substrate, the drying temperature for removing the aqueous medium of the primer is not particularly limited and may be appropriately determined depending on the heat resistance temperature of the substrate, workability, etc. Usually, it is preferably 100°C or lower, more preferably 80°C or lower, still more preferably 65°C or lower, and particularly preferably 50°C or lower. If the drying temperature exceeds 100°C, the working environment may need to be selected.

[0038] <UV curable coating layer> Resins constituting the UV-curable coating layer include vinyl chloride resin, urethane resin, polyester resin, acrylic resin, etc., and are not particularly limited as long as they are UV-curable. A UV-curable coating layer can be formed by applying various UV-curable coating agents onto the primer layer formed as a coating film and irradiating it with UV. The UV-curable coating agent can also be dissolved or dispersed in an aqueous medium or an organic solvent.

[0039] The use of the primer of the present invention is not particularly limited, but it can be used, for example, as a floor coating for protecting floors and walls of buildings such as restaurants, hotels, hospitals, nursing homes, nurseries, and other public facilities. EXAMPLES

[0040] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these. The various characteristics were measured or evaluated by the following methods.

[0041] 1. Characteristics of acid-modified polyolefin resin (1) Composition 1 The molecular weight was determined by H-NMR analysis (Varian, 300 MHz) at 120°C using orthodichlorobenzene (d4) as a solvent.

[0042] (2) Melting point A 10 mg sample of the resin was measured using a DSC (differential scanning calorimetry) device (PerkinElmer, DSC7) at a temperature rise rate of 10° C. / min, and the melting point was determined from the obtained temperature rise curve.

[0043] (3) Melt flow rate Measurement was performed according to the method described in JIS K6730 (190°C, 2160g load).

[0044] 2. Characteristics of aqueous dispersion of acid-modified polyolefin resin (1) Solid content concentration An appropriate amount of the aqueous dispersion was weighed and heated at 150° C. until the mass of the remaining matter (solid content) reached a constant weight, and the solid content concentration was determined.

[0045] (2) Average particle size of acid-modified polyolefin resin particles The number average particle size (mn) and weight average particle size (mw) were determined using a Microtrac particle size distribution analyzer UPA150 (MODEL No. 9340, dynamic light scattering method) manufactured by Nikkiso Co., Ltd. Here, the refractive index of the resin used for calculating the particle size was set to 1.50.

[0046] 3. Coating film characteristics In the evaluation of the following properties, a polyethylene terephthalate resin film (manufactured by Unitika Ltd., Emblet, thickness 25 μm, hereinafter referred to as PET film) and a stretched polypropylene film (manufactured by Tocello Co., Ltd., thickness 20 μm, hereinafter referred to as OPP film) were used as substrates.

[0047] (1) Adhesion to substrate (tape peel test) The primer was applied to the corona-treated surfaces of the PET film and OPP film using a Mayer bar so that the dried film thickness would be 1 μm, and then dried at 80° C. for 1 minute. The resulting laminated film was left at room temperature for 1 day, after which cellophane tape (TF-12, manufactured by Nichiban Co., Ltd.) was applied to the coating surface, and the degree of peeling when the tape was peeled off in one go was visually observed to evaluate adhesion according to the following criteria. Those with an evaluation of △ or higher were deemed to have passed. ○: No peeling at all △: Partially peeled off ×: All peeled off

[0048] (2) Adhesion to UV-curable coating layers The primer was applied to the corona-treated surface of the PET film using a Mayer bar so that the film thickness after drying would be 1 μm, and then dried at 60° C. or 25° C. for 3 hours. The coating film of the obtained laminated film was used as a primer layer, and a UV ink (Raycure CPO 6300, manufactured by Jujo Chemical Co., Ltd.) was applied to the surface of the primer layer to a thickness of 3 μm as a UV-curable coating agent. The surface was then irradiated with UV light with a cumulative irradiation dose of 300 mJ using a UV irradiator to form a UV-cured coating layer, thereby obtaining a laminate consisting of a base film, a primer layer, and a UV-cured coating layer. The adhesion of the coating surface of the laminate was tested according to the method of JIS K5400 8.5.2. The coating was cut to create 1 mm x 1 mm x 100 grids, which were peeled off with adhesive tape, and the number of grids that remained unpeeled was counted and the adhesion of the coating was evaluated according to the following criteria. ◎:100 ○:97~99 △:90~96 ×:89 or less

[0049] (3) Blocking resistance The laminated films obtained by drying at 25° C. for 3 hours as described in (2) above were brought into contact with each other with the primer layer surfaces, and left to stand for 1 day in an atmosphere at 25° C. under a load of 1 MPa. Thereafter, the sample was peeled off, and the blocking resistance was evaluated according to the following criteria. ○: No blocking (no force required for peeling) △: Requires force to peel off (not adhered) ×: Adhered

[0050] (4)Flexibility Regarding the laminated film obtained by drying at 25°C for 3 hours as described in (2) above, a steel ball punch was pressed to a predetermined indentation depth using an Erichsen tester (Yasuda Seiki Seisakusho Co., Ltd. No. 5755) based on JIS Z2247 onto the laminate on which a UV-cured coating layer was formed by the method described in (2) above, and the Erichsen value was obtained (the indentation depth at which no breakage, cracks, or peeling occurred was determined). The Erichsen value was measured every 0.5 mm, and the flexibility of the coating film was evaluated according to the following criteria. ◎: Erichsen value is 7mm or more ○: Erichsen value is 5mm or more and less than 7mm △: Erichsen value is 3mm or more and less than 5mm ×: Erichsen value is less than 3 mm

[0051] The acid-modified polyolefin resin (A), the urethane resin (B) and their aqueous dispersions were produced by the following methods.

[0052] 1. Preparation of aqueous dispersion (E) of acid-modified polyolefin resin (A) (1) Aqueous dispersion (E-1) of acid-modified polyolefin resin (A-1) Using a stirrer equipped with a sealable pressure-resistant 1-liter glass container with a heater, 60.0 g of acid-modified polyolefin resin (A-1) (Arkema, Bondine HX-8290, ethylene / ethyl acrylate / maleic anhydride = 80 / 18 / 2 mass%), 60.0 g of isopropanol, 4.5 g (1.8 times equivalent to the carboxyl group of maleic anhydride in the resin) of triethylamine and 175.5 g of distilled water were charged into the glass container, and the stirring blade rotation speed was set to 300 rpm. No precipitation of resin particles was observed at the bottom of the container, and it was confirmed that the resin particles were in a floating state. Therefore, while maintaining this state, the heater was turned on after 10 minutes and heated. Then, the temperature in the system was kept at 140 to 145 ° C and stirred for another 20 minutes. The mixture was then placed in a water bath and cooled to room temperature (approximately 25°C) while stirring at a rotation speed of 300 rpm. It was then subjected to pressure filtration (air pressure 0.2 MPa) using a 300 mesh stainless steel filter (wire diameter 0.035 mm, plain weave) to obtain a milky white, uniform aqueous dispersion (E-1) of acid-modified polyolefin resin (A-1).

[0053] (2) Aqueous dispersion (E-2) of acid-modified polyolefin resin (A-2) An aqueous dispersion (E-2) of acid-modified polyolefin resin (A-2) was obtained in the same manner as in (E-1) above, except that acid-modified polyolefin resin (A-2) (Bondine TX-8030, manufactured by Arkema) was used as the acid-modified polyolefin resin.

[0054] (3) Aqueous dispersion (E-3) of acid-modified polyolefin resin (A-3) An aqueous dispersion (E-3) of acid-modified polyolefin resin (A-3) was obtained in the same manner as in (E-1) above, except that acid-modified polyolefin resin (A-3) (Bondine HX-8210, manufactured by Arkema) was used as the acid-modified polyolefin resin.

[0055] (4) Aqueous dispersion (E-4) of acid-modified polyolefin resin (A-4) 280g of propylene-butene copolymer (propylene / 1-butene=80 / 20% by mass) was dissolved in 470g of xylene under nitrogen atmosphere in a four-neck flask, and then 40.0g of maleic anhydride as an unsaturated carboxylic acid and 28.0g of dicumyl peroxide as a radical generator were added over 2 hours while stirring while maintaining the temperature in the system at 140°C, and the mixture was allowed to react for 6 hours. After the reaction was completed, the reaction product was poured into a large amount of acetone to precipitate a resin. This precipitated resin was washed once with a solution of triethylamine in acetone (mass ratio: triethylamine / acetone = 1 / 4), and then washed with acetone to remove unreacted maleic anhydride, and then dried under reduced pressure in a vacuum dryer to obtain an acid-modified polypropylene resin (A-4). Using a stirrer equipped with a sealable pressure-resistant 1L glass container with a heater, 60.0g of acid-modified polyolefin resin A-4 (propylene / butene / maleic anhydride = 80.0 / 20.0 / 4.5 (mass ratio)), 45.0g of ethylene glycol-n-butyl ether, 8.0g of N,N-dimethylethanolamine (DMEA) and 137.0g of distilled water were charged into the glass container, and the stirring blade rotation speed was set to 300 rpm. No resin precipitation was observed at the bottom of the container, and it was confirmed that the resin was in a floating state. Therefore, while maintaining this state, the heater was turned on after 10 minutes and heated. Then, the temperature in the system was kept at 160 ° C and stirred for another 60 minutes. Then, the container was cooled by air until the internal temperature reached 80° C., and the container was opened, and 45.0 g of tetrahydrofuran, 5.0 g of DMEA, and 30.0 g of distilled water were added thereto. The container was then sealed, and the internal temperature was kept at 140° C. with the stirring blade rotation speed at 300 rpm for an additional 60 minutes of stirring. Then, the mixture was cooled to room temperature (about 25°C) while stirring at a rotation speed of 300 rpm by air cooling, and then filtered under pressure (air pressure 0.2 MPa) with a 300 mesh stainless steel filter (wire diameter 0.035 mm, plain weave) to obtain a slightly cloudy aqueous dispersion (E-4) of acid-modified polyolefin resin (A-4). At this time, almost no resin remained on the filter.

[0056] (5) Aqueous dispersion (E-5) of acid-modified polyolefin resin (A-5) An acid-modified polypropylene resin (A-5) was obtained in the same manner as in the above (A-4), except that a propylene-butene-ethylene copolymer (propylene / butene / ethylene=68 / 19 / 13% by mass) was used. An aqueous dispersion (E-5) of acid-modified polyolefin resin (A-5) was obtained in the same manner as in the above (E-4), except that the acid-modified polyolefin resin (A-4) was replaced with (A-5).

[0057] Table 1 shows the characteristics of the resulting acid-modified polyolefin resin aqueous dispersion and the characteristics of the acid-modified polyolefin resin used in its production.

[0058] [Table 1]

[0059] 2. Urethane resin (B) aqueous dispersion (U) (1) Urethane resin (B-1) Aqueous dispersion (U-1) Aqueous dispersion of polyether polyurethane (B-1) (Kusumoto Chemicals, NeoRez R-600, solids concentration 33%) (2) Urethane resin (B-2) aqueous dispersion (U-2) Aqueous dispersion of polycarbonate-type polyurethane (B-2) (Mitsui Chemicals, Takelac W-6010, solids concentration 30%)

[0060] Example 1 The aqueous dispersion (E-1) of the acid-modified polyolefin resin (A-1) and the aqueous dispersion (U-1) of the urethane resin (B-1) were mixed at room temperature with stirring (100 rpm) using a mechanical stirrer so that the amount of the urethane resin (B-1) was 30 parts by mass per 100 parts by mass of the acid-modified polyolefin resin (A-1), and ethylene glycol (C) was further mixed in so that the amount was 0.5 parts by mass per 100 parts by mass of the acid-modified polyolefin resin (A-1) to prepare a primer for a UV-curable coating agent.

[0061] Examples 2 to 17, Comparative Examples 1 to 9 A primer for a UV-curable coating agent was obtained by performing the same operation as in Example 1, except that the types of acid-modified polyolefin resin (A) and urethane resin (B) and the parts by mass of urethane resin (B) and ethylene glycol (C) were changed as shown in Table 2. In Examples 16 and 17, a mixture of two types of acid-modified polyolefin resins, each of which was 50 parts by mass, was used as the aqueous dispersion of the acid-modified polyolefin resin.

[0062] Table 2 shows the compositions and properties of the primers for UV-curable coating agents obtained in Examples 1 to 17 and Comparative Examples 1 to 9.

[0063] [Table 2]

[0064] In Examples 1 to 17, the coating film (primer layer) obtained from the primer had good adhesion to polyester resin substrates and polyolefin resin substrates, and even when dried at low temperature, the adhesion between the substrate and UV ink was good, and the flexibility of the coating film was also excellent.

[0065] In Comparative Examples 1 to 9, when ethylene glycol (C) was not included or the blended amount was small or large, adhesion to UV ink tended to decrease. When the blended amount of urethane resin (B) was small, adhesion to UV ink decreased and the flexibility of the coating film was low, and when the blended amount of urethane resin (B) was large, adhesion to olefin substrates tended to decrease.

Claims

1. A primer for a UV-curable coating agent, comprising: 100 parts by mass of an acid-modified polyolefin resin (A); 20 to 50 parts by mass of a urethane resin (B); 0.3 to 3 parts by mass of ethylene glycol (C); and an aqueous medium.

2. 2. The primer for UV-curable coating agents according to claim 1, wherein the urethane resin (B) is a polyether polyurethane.

3. 3. The primer for UV-curable coating agents according to claim 1, wherein the melting point of the acid-modified polyolefin resin (A) is 60 to 110°C.

4. A coating film formed from the primer according to claim 1 or 2.

5. A laminate comprising a thermoplastic resin substrate, the coating film according to claim 4, and a UV-curable coating layer laminated in this order.

6. 6. The laminate according to claim 5, wherein the thermoplastic resin substrate is a polyester substrate or a polyolefin substrate.

Citation Information