All-solid battery
By integrating a chlorine-based gas trapping agent in all-solid-state batteries, the issue of exterior body corrosion from acidic gases is mitigated, ensuring sustained battery performance and longevity.
Patent Information
- Application Number
- JP2024037915
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-07
AI Technical Summary
All-solid-state batteries using chlorine-containing solid electrolytes experience corrosion of the exterior body due to the generation of acidic gases during charge/discharge cycles, leading to a decrease in battery capacity and shortened lifespan.
Incorporation of a chlorine-based gas trapping agent, such as hydrotalcite or carbonates, within the exterior body to adsorb and neutralize acidic gases generated during cycling, thereby preventing corrosion.
The chlorine-based gas trapping agent effectively suppresses corrosion of the exterior body, maintaining battery capacity and extending the lifespan by continuously adsorbing acidic gases within the sealed environment.
Smart Images

Figure 2024137794000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state battery. [Background technology]
[0002] In recent years, electronics technology has made remarkable progress, and efforts are being made to make portable electronic devices smaller, lighter, thinner, and more multifunctional. Accordingly, there is a strong demand for batteries, which serve as the power source for such electronic devices, to be smaller, lighter, thinner, and more reliable.
[0003] For example, Patent Document 1 discloses a lithium ion secondary battery having a non-aqueous electrolyte solution containing a fluorine-based electrolyte. It is disclosed that in a lithium ion secondary battery having a non-aqueous electrolyte solution containing a fluorine-based electrolyte, when a trace amount of moisture contained in the non-aqueous electrolyte reacts with the fluorine-based electrolyte, hydrogen fluoride and phosphorus trifluoride are generated, and further, a reaction that generates organic fluorophosphoric acid occurs in a chain reaction. It is believed that the above reaction increases the internal pressure of the battery. In addition, phosphorus pentafluoride generated as a by-product of the above reaction quickly reacts with the trace amount of moisture in the battery, generating a gas mainly composed of hydrogen fluoride. It is believed that this hydrogen fluoride further increases the internal pressure of the battery.
[0004] When the internal pressure of the battery increases, the risk of the battery exploding or leaking increases. Patent Document 1 discloses that in order to suppress such risks, the negative electrode surface is coated with a polymer gel having a fluoride ion trapping function.
[0005] From the viewpoint of safety, which suppresses explosion and leakage of batteries, attention is being paid to all-solid-state batteries that use solid electrolytes as the electrolyte of the battery. Known solid electrolytes include oxide-based solid electrolytes, sulfide-based solid electrolytes, complex hydride-based solid electrolytes, and halide-based solid electrolytes. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-54462 A Summary of the Invention [Problem to be solved by the invention]
[0007] In the case of an all-solid-state battery, when a chlorine-containing solid electrolyte containing chlorine element is used as the solid electrolyte, acid gas may be generated during the charge / discharge cycle, and the metal layer and resin film of the exterior body that seals the power generation element of the all-solid-state battery may be corroded. The generation of hydrogen fluoride as in Patent Document 1 is a problem that occurs during the initial SEI formation, and is not a problem if the gas is removed before carrying out the process, but the generation of acid gas as described above is a problem that occurs during the charge / discharge cycle, and is a problem that continues even after the battery cell is sealed. If the corrosion of the exterior body progresses due to the generation of acid gas, it may lead to a decrease in battery capacity and a shortened battery life. The exterior body is formed, for example, by folding a foil-like material and sealing the outer periphery. The folded part is subjected to force, and the sealed part is more likely to corrode than other parts.
[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide an all-solid-state battery that can suppress corrosion of an exterior body due to acid gas during charge-discharge cycles, even in the case of using a chlorine-containing solid electrolyte. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides the following means.
[0010] [1] An all-solid-state battery according to one embodiment of the present invention includes a power generating element in which a positive electrode containing a positive electrode active material, a solid electrolyte layer, and a negative electrode containing a negative electrode active material are stacked in this order, and an exterior body that seals the power generating element, wherein one or more of the positive electrode, the negative electrode, and the solid electrolyte layer have a solid electrolyte containing elemental chlorine, and a chlorine-based gas trapping agent is sealed within the exterior body.
[0011] [2] In the all-solid-state battery of [1] above, the chlorine-based gas trapping agent may contain hydrotalcite represented by formula (1). M1 2+ 8-x M2 3+ x (OH) - 16 CO 3 2- nH 2 O···(1) [In formula (1), M1 2+ is Mg 2+ ,Fe 2+ ,Zn 2+ ,Ca 2+ ,Li 2+ ,Ni 2+ ,Co 2+ and Cu 2+ The compound is one or more selected from the group consisting of: M2 3+ Al 3+ and Fe 3+ and Mn 3+ The compound is one or more selected from the group consisting of: 2≦x≦5, 0≦n
[0012] [3] In the all-solid-state battery according to [1] or [2] above, the chlorine-based gas trapping agent may be a carbonate of an alkali metal element or an alkaline earth metal element.
[0013] [4] In the all-solid-state batteries according to the above [1] to [3], the chlorine-based gas trapping agent may be supported by a support made of a porous material in an amount of 5 wt % to 20 wt %.
[0014] [5] In the all-solid-state battery according to [3] above, the chlorine-based gas trapping agent may be potassium carbonate or calcium carbonate.
[0015] [6] In the all-solid-state batteries according to the above [1] to [5], the solid electrolyte may be a halide-based solid electrolyte represented by formula (2). A a E b G c Xd (2) In formula (2), A is at least one element selected from the group consisting of Li, K, and Na. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. G is OH, BO 2 , B.O. 3 , B.O. 4 , B 3 O 6 , B 4 O 7 , CO 3 , NO 3 , AlO 2 , SiO 3 , SiO 4 , Si 2 O 7 , Si 3 O 9 , Si 4 O 11 , Si 6 O 18 , P.O. 3 , P.O. 4 , P 2 O 7 , P 3 O 10 , S.O. 3 , S.O. 4 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 , B.F. 4 , P.F. 6 , BOB, COO 2 , N, AlCl 4 , C.F. 3 SO 3 , C.H. 3 COO, CF 3 COO, P 2 O 5and O. X includes a Cl element or a Cl element and at least one element selected from the group consisting of F, Br, and I. 0.5≦a<6, 0 <b<2、0≦c≦6、0<d≦6.1である。〕
[0016] [7] In the all-solid-state batteries according to any one of [1] to [6] above, the exterior body may be an aluminum laminate, and the chlorine-based gas trapping agent may be disposed in a sealed portion or a folded portion located outside the power generating element in a plan view.
[0017] [8] In the all-solid-state batteries according to the above [1] to [7], the positive electrode has a positive electrode current collector and a positive electrode mixture layer provided between the positive electrode current collector and the solid electrolyte layer, and the negative electrode has a negative electrode current collector and a negative electrode mixture layer provided between the negative electrode current collector and the solid electrolyte layer, the positive electrode current collector and the negative electrode current collector are larger than the positive electrode mixture layer and the negative electrode mixture layer in a planar view, and the chlorine-based gas trapping agent may be formed in a region outside the positive electrode mixture layer and the negative electrode mixture layer and between the positive electrode current collector and the negative electrode current collector. Effect of the Invention
[0018] According to the present invention, even when a chlorine-containing solid electrolyte is used, it is possible to provide an all-solid-state battery capable of suppressing corrosion of an exterior body due to acid gas during charge-discharge cycles. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a perspective view showing an example of a configuration of an all-solid-state battery according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the all-solid-state battery of FIG. 1. [Diagram 3] FIG. 3 is a plan view of the all-solid-state battery of FIG. 2. [Figure 4] FIG. 4 is a plan view showing a modified example of the all-solid-state battery in FIG. [Diagram 5] FIG. 3 is a cross-sectional view showing a modified example of the all-solid-state battery in FIG. [Figure 6] FIG. 6 is a plan view of the all-solid-state battery of FIG. 5. [Figure 7] 3 is a cross-sectional view showing another modified example of the all-solid-state battery in FIG. 2. [Figure 8] FIG. 8 is a plan view of the all-solid-state battery of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be appropriately modified and implemented within the scope of the present invention.
[0021] [All-solid battery] Fig. 1 is a perspective view showing an example of the configuration of an all-solid-state battery according to one embodiment of the present invention. Fig. 2 is a cross-sectional view of the all-solid-state battery of Fig. 1. Fig. 3 is a plan view of the all-solid-state battery of Fig. 2. Although a laminated type battery is shown in Figs. 1 to 3, a wound type battery may also be used.
[0022] The all-solid-state battery 100 shown in FIGS. 1 to 3 includes a power generating element in which a positive electrode containing a positive electrode active material, a solid electrolyte layer, and a negative electrode containing a negative electrode active material are laminated in this order, and an exterior body that seals the power generating element, in which one or more of the positive electrode, the negative electrode, and the solid electrolyte layer have a solid electrolyte containing elemental chlorine, and a chlorine-based gas trapping agent is sealed within the exterior body.
[0023] As shown in Fig. 1, the all-solid-state battery 100 includes an exterior body 50 and a power generating element 40 accommodated in an accommodation space K within the exterior body 50. For ease of understanding, Fig. 1 illustrates a state immediately before the power generating element 40 is accommodated in the exterior body 50. The exterior body 50 covers the periphery of the power generating element 40. The power generating element 40 is connected to the outside via a pair of connected terminals 62, 64. The all-solid-state battery 100 is used, for example, in laminate batteries, square batteries, cylindrical batteries, coin batteries, button batteries, and the like.
[0024] {Power generation element} The power generating element 40 includes a solid electrolyte layer 10, a positive electrode 20, and a negative electrode 30. The power generating element 40 is charged or discharged by the exchange of ions between the positive electrode 20 and the negative electrode 30 via the solid electrolyte layer 10 and the exchange of electrons via an external circuit. The power generating element 40 has a laminate 45 in which, for example, the positive electrode mixture layer 24, the solid electrolyte layer 10, and the negative electrode mixture layer 34 are laminated in this order.
[0025] (Solid electrolyte layer) The solid electrolyte layer 10 is sandwiched between a positive electrode 20 and a negative electrode 30. The solid electrolyte layer 10 includes a solid electrolyte that can move ions by an externally applied voltage. For example, the solid electrolyte conducts lithium ions and inhibits the movement of electrons.
[0026] The solid electrolyte constituting the solid electrolyte layer 10 contains, for example, lithium. The solid electrolyte is, for example, a sulfide-based solid electrolyte, a halide-based solid electrolyte, or a complex hydride-based solid electrolyte, and is preferably composed of one or both of a sulfide-based solid electrolyte and a halide-based solid electrolyte.
[0027] As a sulfide-based solid electrolyte, for example, Li 6 P.S. 5 Cl, Li 6 P.S. 5 Br, Li 6 P.S. 5 I, xLi 2 S-(1-x)P 2 S 5 , xLi 2 S-(1-x)GeS2 , xLi 2 S-yGeS 2 -(1-xy)P 2 S 5 , xLi 4 GeS 4 -(1-x)Li 3 P.S. 4 , Li 9.54 S 1.74 P 1.44 S 11.7 C l0.3 , Li 4 SnS 4 , Li 3 P.S. 4 , xLi 2 S-(1-x)P 2 S 5 , xLi 2 S-yP 2 S 5 -(1-xy)Li 3 N, Li 5 B 7 S 13 , Li 3 B.S. 3 , Li 2 B 2 S 5 etc.
[0028] As the halide-based solid electrolyte, for example, a solid electrolyte represented by the following formula (2) can be used. A a E b G c X d (2) (In formula (2), A is at least one element selected from the group consisting of Li, K, Cs, and Na. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Sn, Hf, and lanthanides. G is O, OH, BO 2 , B.O. 3 , B.O. 4 , B 3 O 6 , B 4 O 7 , CO 3 , NO 3 , AlO 2、SiO 3 、SiO 4 、Si 2 O 7 、Si 3 O 9 、Si 4 O 11 、Si 6 O 18 、PO 3 、PO 4 、P 2 O 7 、P 3 O 10 、SO 3 、SO 4 、SO 5 、S 2 O 3 、S 2 O 4 、S 2 O 5 、S 2 O 6 、S 2 O 7 、S 2 O 8 、BF 4 、PF 6 、BOB、(COO) 2 、N、AlCl 4 、CF 3 SO 3 、CH 3 COO、CF 3 COO、OOC-(CH 2 ) 2 -COO、OOC-CH 2 -COO、OOC-CH(OH)-CH(OH)-COO、OOC-CH(OH)-CH 2 -COO、C 6 H 5 SO 3 、OOC-CH=CH-COO、OOC-CH=CH-COO、C(OH)(CH 2 COOH) 2 COO、AsO 4 、BiO 4 、CrO 4 、MnO 4 、PtF 6 、PtCl 6 、PtBr 6 、PtI 6 、SbO 4 、SeO4 、TeO 4 、HCOO, CN, SCN, NO 3 、P 2 O 5 and is at least one group selected from the group consisting of X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5 ≦ a < 6, 0 < b < 2, 0 ≦ c ≦ 6, 0 < d ≦ 6.1 are satisfied.) In the above (2), A is preferably at least one element selected from the group consisting of Li, K, and Na, and G is OH, BO 2 、BO 3 、BO 4 、B 3 O 6 、B 4 O 7 、CO 3 、NO 3 、AlO 2 、SiO 3 、SiO 4 、Si 2 O 7 、Si 3 O 9 、Si 4 O 11 、Si 6 O 18 、PO 3 、PO 4 、P 2 O 7 、P 3 O 10 、SO 3 、SO 4 、SO 5 、S 2 O 3 、S 2 O 4 、S 2 O 5 、S 2 O 6 、S 2 O 7 、S 2 O 8 、BF 4 、PF 6 、BOB, (COO) 2 、N, AlCl 4 、CF 3 SO3 , C.H. 3 COO, CF 3 COO, P 2 O 5 and O.
[0029] The halide-based solid electrolyte represented by formula (2) is, for example, Li 2 ZrSO 4 Cl 4 (LZSOC), Li 2 ZrOCl 4 (LZOC), Li 2 ZrCl 6 (LZC), Li 2 ZrBr 6 (LZBr), Li 2 ZrBO 2 Cl 5 , Li 2 ZrBF 4 Cl 5 , Li 3 YSO 4 Cl 4 , Li 3 YCO 3 Cl 4 , Li 3 YBO 2 Cl 5 , Li 3 YBF 4 Cl 5 , Li 2 ZrSO 4 (P 2 O 5 ) 0.1 Cl 4 , Li 2 Zr 0.5 Al 0.5 Cl 3.5 Examples include O.
[0030] Here, when neither the positive electrode 20 nor the negative electrode 30 has a solid electrolyte containing a chlorine element, the solid electrolyte layer 10 has a solid electrolyte containing a chlorine element. Even when at least one of the positive electrode 20 and the negative electrode 30 contains a solid electrolyte containing a chlorine element, the solid electrolyte layer 10 may have a solid electrolyte containing a chlorine element. In such a case, since the amount of acid gas generated during the charge / discharge cycle increases, the effect of the present invention in which the acid gas is adsorbed by a chlorine-based gas trapping agent can be further enhanced.
[0031] As a solid electrolyte containing chlorine, for example, Li 6 P.S. 5 A sulfur-based solid electrolyte such as Cl(LPSC) or a halide-based solid electrolyte that satisfies the following condition in the above formula (2) can be used. The following condition is the above condition in which the condition of the X site in formula (2) is not adjusted. In this embodiment, such a solid electrolyte containing chlorine element may be referred to as a chlorine-containing solid electrolyte. (In formula (2), A is at least one element selected from the group consisting of Li, K, Cs, and Na. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanides. G is OH, BO 2 , B.O. 3 , B.O. 4 , B 3 O 6 , B 4 O 7 , CO 3 , NO 3 , AlO 2 , SiO 3 , SiO 4 , Si 2 O 7 , Si 3 O 9 , Si 4 O 11 , Si 6 O 18 , P.O. 3 , P.O. 4 , P 2 O 7 , P 3 O 10, S.O. 3 , S.O. 4 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 , B.F. 4 , P.F. 6 , BOB, (COO) 2 , N, AlCl 4 , C.F. 3 SO 3 , C.H. 3 COO, CF 3 COO, OOC-(CH 2 ) 2 -COO, OOC-CH 2 -COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH 2 -COO, C 6 H 5 SO 3 , OOC-CH=CH-COO, OOC-CH=CH-COO, C(OH)(CH 2 COOH) 2 COO, AsO 4 , BiO 4 , CrO 4 , MnO 4 , PtF 6 , PtCl 6 , PtBr 6 , PtI 6 , SbO 4 , SeO 4 , TeO 4 , HCO, CN, SCN, NO 3 , P 2 is at least one group selected from the group consisting of O and O. X consists of Cl element alone, or contains Cl element and at least one element selected from the group consisting of F, Br and I. 0.5≦a<6, 0 <b<2、0≦c≦6、0<d≦6.1である。)
[0032] That is, among the examples of the above-mentioned halide-based solid electrolytes, the chlorine-containing solid electrolyte is Li 2 ZrSO 4 Cl 4 (LZSOC), Li 2 ZrOCl 4 (LZOC), Li 2 ZrCl 6 (LZC), Li 2 ZrBO 2 Cl 5 , Li 2 ZrBF 4 Cl 5 , Li 3 YSO 4 Cl 4 , Li 3 YCO 3 Cl 4 , Li 3 YBO 2 Cl 5 , Li 3 YBF 4 Cl 5 , Li 2 ZrSO 4 (P 2 O 5 ) 0.1 Cl 4 , Li 2 Zr 0.5 Al 0.5 Cl 3.5 It is O.
[0033] [Positive electrode] The positive electrode 20 has, for example, a plate-shaped (foil-shaped) positive electrode current collector 22 and a positive electrode mixture layer 24. The positive electrode mixture layer 24 is formed so as to be in contact with at least one surface of the positive electrode current collector 22, for example.
[0034] (Positive electrode current collector) The positive electrode current collector 22 may be made of any electronically conductive material that can withstand oxidation during charging and is not easily corroded. The positive electrode current collector 22 may be made of, for example, a metal such as aluminum, stainless steel, nickel, or titanium, or an electronically conductive resin. The positive electrode current collector 22 may be in the form of a powder, a foil, a punched piece, or an expanded piece.
[0035] (Positive electrode mixture layer) The positive electrode mixture layer 24 includes a positive electrode active material. The positive electrode mixture layer 24 may further include one or more of a solid electrolyte, a conductive assistant, and a binder, as necessary. For example, the positive electrode mixture layer 24 is composed of a positive electrode active material layer, a solid electrolyte, and a conductive assistant.
[0036] The positive electrode active material is not particularly limited as long as it is capable of reversibly absorbing and releasing lithium ions and inserting and extracting them (intercalation and deintercalation), and any positive electrode active material used in known lithium ion secondary batteries can be used. Examples of the positive electrode active material include lithium-containing metal oxides and lithium-containing metal phosphates.
[0037] The lithium-containing metal oxide is, for example, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), Lithium Manganese Spinel (LiMn 2 O 4 ), and general formula: LiNi x Co y Mn z O 2 The complex metal oxide represented by (x+y+z=1), lithium vanadium compound (LiVOPO 4 , Li 3 V 2 (PO 4 ) 3 ), olivine type LiMPO 4 (wherein M represents at least one selected from Co, Ni, Mn, and Fe), lithium titanate (Li 4 Ti 5 O 12 ) etc.
[0038] The positive electrode active material does not have to contain lithium. Examples of such a positive electrode active material include MnO 2 , V 2 O 5 Lithium-free metal oxides such as MoS 2 Lithium-free metal sulfides such as FeF 3 , V.F. 3When using a positive electrode active material that does not contain lithium, the negative electrode is doped with lithium ions in advance, or a negative electrode containing lithium ions is used.
[0039] The solid electrolyte contained in the positive electrode mixture layer 24 is, for example, a sulfide-based solid electrolyte, a halide-based solid electrolyte, or a complex hydride-based solid electrolyte, and is preferably composed of one or both of a sulfide-based solid electrolyte and a halide-based solid electrolyte. The above-mentioned solid electrolytes can be used as such a solid electrolyte. Here, when neither the solid electrolyte layer 10 nor the negative electrode 30 has a chlorine-containing solid electrolyte, the positive electrode 20 has a chlorine-containing solid electrolyte. In addition, even when at least one of the solid electrolyte layer 10 and the negative electrode 30 contains a solid electrolyte containing a chlorine element, the positive electrode 20 may have a solid electrolyte containing a chlorine element. In such a case, the amount of acid gas generated during the charge / discharge cycle increases, so that the effect of the present invention in which the acid gas is adsorbed by a chlorine-based gas trapping agent can be further increased.
[0040] The content of the solid electrolyte in the positive electrode mixture layer 24 is not particularly limited, but is preferably 1 mass % to 50 mass %, and more preferably 5 mass % to 30 mass %, based on the total mass of the positive electrode active material, the solid electrolyte, the conductive assistant, and the binder.
[0041] The conductive assistant improves the electronic conductivity of the positive electrode mixture layer 24. Known conductive assistants can be used. Examples of the conductive assistant include carbon materials such as carbon black, graphite, carbon nanotubes, and graphene, metals such as aluminum, copper, nickel, stainless steel, iron, and amorphous metals, conductive oxides such as ITO, and mixtures thereof. The conductive assistant may be in the form of powder or fiber.
[0042] There is no particular limitation on the content of the conductive assistant in the positive electrode mixture layer 24. When the conductive assistant is added, the mass ratio of the conductive assistant is preferably 0.5 mass % to 20 mass %, and more preferably 1 mass % to 5 mass %, based on the total mass of the positive electrode active material, solid electrolyte, conductive assistant, and binder.
[0043] The binder bonds the positive electrode active material, the solid electrolyte, and the conductive assistant to one another in the positive electrode mixture layer 24, and also firmly bonds the positive electrode mixture layer 24 to the positive electrode current collector 22. The binder preferably has oxidation resistance and good adhesiveness.
[0044] In the case where the positive electrode mixture layer 24 contains a binder, examples of the binder include polyvinylidene fluoride (PVDF) or a copolymer thereof, polytetrafluoroethylene (PTFE), polyamide (PA), polyimide (PI), polyamideimide (PAI), polybenzimidazole (PBI), polyethersulfone (PES), polyacrylic acid (PAA) and a copolymer thereof, a metal ion crosslinked product of polyacrylic acid (PAA) and a copolymer thereof, polypropylene (PP) grafted with maleic anhydride, polyethylene (PE) grafted with maleic anhydride, and mixtures thereof.
[0045] When the positive electrode mixture layer 24 contains a binder, the content of the binder is not particularly limited, but may be up to 15 mass %, or may be 1 mass % to 5 mass %, based on the total mass of the positive electrode active material, the solid electrolyte, the conductive assistant, and the binder.
[0046] [Negative electrode] The negative electrode 30 has a negative electrode current collector 32 and a negative electrode mixture layer 34. The negative electrode mixture layer 34 is in contact with the negative electrode current collector 32.
[0047] The negative electrode current collector 32 may have electronic conductivity. The negative electrode current collector 32 is made of, for example, a metal such as copper, aluminum, nickel, stainless steel, or iron, or a conductive resin. The negative electrode current collector 32 may be in the form of a powder, a foil, a punching, or an expandable material.
[0048] The negative electrode mixture layer 34 includes a negative electrode active material. The negative electrode mixture layer 34 may further include one or more of a solid electrolyte, a conductive assistant, and a binder, as necessary. For example, the negative electrode mixture layer 34 is composed of a negative electrode active material layer, a solid electrolyte, and a conductive assistant.
[0049] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions and insert and detach lithium ions. The negative electrode active material is a compound that exhibits a lower potential than the positive electrode active material. As the negative electrode active material, a material used in a known lithium ion secondary battery can be used, and a material similar to the positive electrode active material may be used. The negative electrode active material and the positive electrode active material used in the all-solid-state battery 100 are determined in consideration of the potential of the negative electrode active material and the potential of the positive electrode active material.
[0050] Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, and organic compound sintered bodies, Si, SiO x Metals that can combine with lithium, such as Sn and aluminum, their alloys, composites of these metals and carbon materials, lithium titanate (Li 4 Ti 5 O 12 ), SnO 2 and the like, and metallic lithium.
[0051] The solid electrolyte contained in the negative electrode mixture layer 34 is, for example, a sulfide-based solid electrolyte, a halide-based solid electrolyte, or a complex hydride-based solid electrolyte, and is preferably composed of one or both of a sulfide-based solid electrolyte and a halide-based solid electrolyte. As such a solid electrolyte, the above-mentioned solid electrolytes can be used. Here, when neither the solid electrolyte layer 10 nor the positive electrode 20 has a chlorine-containing solid electrolyte, the negative electrode 30 has a chlorine-containing solid electrolyte. In addition, even when at least one of the solid electrolyte layer 10 and the positive electrode 20 contains a solid electrolyte containing a chlorine element, the negative electrode 30 may have a solid electrolyte containing a chlorine element. In such a case, the amount of acid gas generated during the charge / discharge cycle increases, so that the effect of the present invention in which the acid gas is adsorbed by a chlorine-based gas trapping agent can be further increased.
[0052] The types and amounts of the binder and conductive assistant contained in the negative electrode 30 are similar to those of the binder and conductive assistant contained in the positive electrode 20, and one or both of the binder and the conductive assistant may not be included.
[0053] <Terminal> As shown in FIG. 2, the terminals 62, 64 are connected to the positive electrode collector 22 of the positive electrode 20 and the negative electrode collector 32 of the negative electrode 30, respectively. The terminal 62 connected to the positive electrode 20 is a positive electrode terminal. The terminal 64 connected to the negative electrode 30 is a negative electrode terminal. The terminals 62, 64 are responsible for electrical connection with the outside. The terminals 62, 64 are formed of a conductive material such as aluminum, nickel, or copper. The terminals 62, 64 may be electrically connected to the positive electrode collector 22 of the positive electrode 20 or the negative electrode collector 32 of the negative electrode 30 by welding or screwing. The terminals 62, 62 are preferably protected with insulating tape to prevent short circuits.
[0054] {Exterior body} The exterior body 50 has, for example, a metal foil 52 and a resin layer 54 laminated on both sides of the metal foil 52 (see FIG. 2). The exterior body 50 is a metal laminate film in which the metal foil 52 is coated on both sides with a polymer film (resin layer). The metal foil 52 is, for example, an aluminum foil. The resin layer 54 is, for example, a polymer film such as polypropylene. The resin layer 54 may be different between the inside and the outside. For example, a polymer having a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), may be used as the outside resin layer, and a resin having high heat resistance, oxidation resistance, and reduction resistance, such as polyethylene (PE) or polypropylene (PP), may be used as the inside resin layer. In this embodiment, the metal foil 52 is an aluminum foil and the resin layer 54 is formed on it, which is referred to as an aluminum laminate. That is, the exterior body 50 is, for example, made of an aluminum laminate.
[0055] The exterior body 50 is, for example, formed by folding the laminate film in half and sealing the power generating element 40. As shown in FIG. 3, when viewed in a plan view, the exterior body 50 is defined by a first side S1, a second side S2, a third side S3, and a fourth side S4. The first side S1 is a side that is generated by folding the laminate film in half and is not sealed. The first side S1 is formed at a position corresponding to a line that bisects the laminate film. The second side S2, the third side S3, and the fourth side S4 are formed at positions where the laminate film is folded in half and overlaps. The second side S2 and the third side S3 face each other. The fourth side S4 is formed at a position that overlaps the terminals 62 and 64. The first side S1 is formed at a position that faces the fourth side S4 that overlaps the terminals 62 and 64.
[0056] The power generating element 40 is formed inside a region surrounded by a first side S1, a second side S2, a third side S3, and a fourth side S4 in a plan view, and is sealed by the exterior body 50. In this embodiment, in a plan view, a region between the first side S1 of the exterior body 50 and the power generating element 40 is referred to as a folded portion. In addition, a region between the second side S2 and the power generating element 40, a region between the third side S3 and the power generating element 40, and a region between the fourth side S4 and the power generating element 40 are referred to as a sealed portion. In particular, the region between the second side S2 and the power generating element 40 is referred to as a first sealed portion, a region between the third side S3 and the power generating element 40 is referred to as a second sealed portion, and a region between the fourth side S4 and the power generating element 40 is referred to as a third sealed portion. Both the folded portion and the sealed portion are located outside the power generating element in a plan view.
[0057] {Chlorine-based gas trap} The all-solid-state battery 100 further includes a chlorine-based gas trapping agent 1. The chlorine-based gas trapping agent 1 is sealed in an exterior body 50 together with the power generating element 40. The chlorine-based gas trapping agent 1 is formed, for example, in a region outside the power generating element 40 in a plan view. The chlorine-based gas trapping agent 1 is disposed in a bent portion, for example, as shown in FIG. 3. The first side S1 close to the bent portion is the part of the exterior body that is most susceptible to corrosion. Therefore, by providing the chlorine-based gas trapping agent 1 in the bent portion, acidic gas, which causes corrosion, is easily adsorbed by the chlorine-based gas trapping agent 1.
[0058] The chlorine-based gas trapping agent 1 is an adsorbent capable of adsorbing HCl. The chlorine-based gas trapping agent 1 is, for example, hydrotalcite. Hydrotalcite is a double hydroxide represented by the following formula (2). M1 2+ 1-Y M2 3+ Y (OH) - 2 A Y / m m- nH 2 O···(2)
[0059] Hydrotalcite is a layered inorganic compound consisting of alternating positively charged base layers and negatively charged intermediate layers. The base layers are, for example, M1 2+ , M2 3+ , O.H. - and A m- The intermediate layer is, for example, A m- and H 2 It is made up of O.
[0060] When the chlorine-based gas trapping agent 1 is a hydrotalcite represented by the above formula (2), the chlorine-based gas trapping agent 1 may be composed of hydrotalcite.
[0061] In the above formula (2), M1 2+ is Mg 2+ ,Fe 2+ ,Zn 2+ ,Ca 2+ ,Li 2+ ,Ni 2+ ,Co 2+ and Cu 2+ In the above formula (2), M1 is one or more selected from the group consisting of divalent metal ions. 2+ is Mg 2+ and Ni 2+ It is preferable that the compound is one or more of the above.
[0062] In the above formula (2), M2 3+ Al 3+ , Fe 3+ , Mn 3+ and Cr 3+ In the above formula (2), M2 is one or more selected from the group consisting of trivalent metal ions. 3+ is Mn 2+ ,Fe 2+ and Al 2+ It is preferable that the epoxy resin is one or more selected from the group consisting of:
[0063] In the above formula (2), A m- CO 3 2- , F - , Cl - , Br - , S.O.4 2- and NO 3 - It is one or more selected from an m-valent anion group consisting of
[0064] In the above formula (2), Y satisfies, for example, 0 < Y ≤ 0.33.
[0065] Specific examples of the hydrotalcite represented by the above formula (2) include the hydrotalcite represented by the following formula (1). In the following formula (1), M1 and M2 are the same as M1 and M2 in the above formula (2). M1 2+ 8-x M2 3+ x (OH) - 16 CO 3 2- ·nH 2 O···(1)
[0066] In the above formula (1), x satisfies, for example, 1 ≤ x ≤ 5, and preferably satisfies 2 ≤ x ≤ 5. If x is too large in formula (1), the ion exchange capacity may decrease, and if x is too small, M1 2+ may elute as a hydroxide. In the above formula (1), n satisfies 0 ≤ n, and preferably satisfies 1 ≤ n.
[0067] Examples of such hydrotalcite include Mg 6 Mn 2 (CO 3 )(OH) 16 ·4H 2 O, Mg 6 Fe 2 (OH) 16 Cl 2 ·4H 2 O, Mg 6 Al 2 (CO 3 )(OH) 16 ·4H 2 O, Mg 6 Fe 2 (CO 3 )(OH)16 4H 2 O, Mg 6 Fe 2 (CO 3 )(OH) 16 4H 2 O, Ni 6 Al 2 (CO 3 )(OH) 16 4H 2 O, Mg 5 CaAl 2 (SO 4 ) 2 (OH) 18 12H 2 O, Zn 4 Al 4 (CO 3 )(OH) 12 3H 2 Examples include O.
[0068] The chlorine-based gas trapping agent 1 may be one or both of a carbonate of an alkali metal element or an alkaline earth metal element and an acetate of an alkali metal element or an alkaline earth metal element. The chlorine-based gas trapping agent 1 is preferably a carbonate of an alkali metal element or an alkaline earth metal element. These chlorine-based gas trapping agents 1 undergo a neutralization reaction when an acid gas is generated.
[0069] The carbonate of an alkali metal element or an alkaline earth metal element used as the chlorine-based gas trapping agent 1 is preferably one or more selected from the group consisting of potassium carbonate, calcium carbonate, lithium carbonate, and sodium carbonate, and more preferably one or both of potassium carbonate and calcium carbonate.
[0070] The acetate salt of an alkali metal element or an alkaline earth metal element used as the chlorine-based gas trapping agent 1 is preferably one or more selected from the group consisting of potassium acetate, calcium acetate, lithium acetate, and sodium acetate, and more preferably one or both of potassium acetate and calcium acetate.
[0071] When one or both of a carbonate of an alkali metal element or an alkaline earth metal element and an acetate of an alkali metal element or an alkaline earth metal element are used as the chlorine-based gas trapping agent 1, they may be supported on another material and sealed in an exterior body. In this embodiment, the material on which the chlorine-based gas trapping agent 1 is supported is called a support material.
[0072] As the support material, for example, a porous material can be used. As the support material, for example, a microporous material (pore diameter (hereinafter, pore diameter) less than 2 nm), a mesoporous material (pore diameter 2 nm or more and less than 50 nm), or a macroporous material (pore diameter 50 nm or more) can be used, and it is preferable to use a microporous material or a mesoporous material. As such a porous material, for example, activated carbon, alumina, zeolite, silica, titania, pumice, etc. can be used, and among these, it is preferable to use one or more of activated carbon, alumina, zeolite, silica, and titania, and it is particularly preferable to use activated carbon. In addition, as the support material, it is preferable to use one with a pore diameter of 50 nm or less, more preferably 5 nm or more and 25 nm or less, and more preferably 10 nm or more and 20 nm or less. It is considered that the pore diameter of the support material is small enough to prevent the chlorine-based gas trapping agent from forming a lump, and the contact area between the chlorine-based gas trapping agent and the acid gas can be increased, and the pore diameter of the activated carbon is large enough to disperse the chlorine-based gas trapping agent inside the pores of the support material, thereby enhancing reactivity. The pore diameter is calculated by the BJH method conforming to JISZ8831-2:2010, or the DFT method conforming to JISZ8831-3:2010. Since the BJH method can accurately measure pore diameters, particularly those of 2 to 50 nm, the pore diameters in this range are calculated by the BJH method, and the pore diameters outside this range are calculated by the DFT method. That is, when the pore diameter is calculated to be less than 2 nm or greater than 50 nm by the BJH method, the pore diameter is calculated by the DFT method.
[0073] The chlorine-based gas trapping agent 1 is supported on the support material in an amount of, for example, 0.1 wt% to 50 wt%, preferably 1 wt% to 30 wt%, and more preferably 5 wt% to 20 wt%. By supporting the chlorine-based gas trapping agent 1 on a support material made of a porous material, the surface area of the chlorine-based gas trapping agent in the atmosphere can be increased. In addition, since water generated by the neutralization reaction between the acid gas and the carbonate or acetate of an alkaline earth metal element remains in the support material, the effect on the charge / discharge cycle of the all-solid-state battery is considered to be minimized.
[0074] [Manufacturing method of all-solid-state batteries] Next, a method for manufacturing the all-solid-state battery according to the present embodiment will be described. The all-solid-state battery according to the present embodiment is manufactured, for example, by using a powder molding method. The powder molding method is carried out in an environment with a dew point of -20°C or less and -90°C or more. The powder formation method is preferably carried out in an environment with a dew point of -30°C or less and -85°C or more. The powder formation method is carried out, for example, by adjusting the dew point in a glove box by the following method.
[0075] First, a solid electrolyte is prepared. The solid electrolyte can be produced, for example, by mixing raw material powders containing predetermined elements in a predetermined molar ratio and allowing them to undergo a mechanochemical reaction. The solid electrolyte is pressed using a pellet-making jig that includes a cylindrical holder (die) and an upper punch and a lower punch that can be inserted into the cylindrical holder, thereby forming a pellet-shaped solid electrolyte layer.
[0076] In the powder molding method, a positive electrode mixture disposed on one surface of a solid electrolyte layer and a negative electrode mixture disposed on the other surface are pressed using a pellet preparation tool having a cylindrical holder (die) and an upper punch and a lower punch that can be inserted into the cylindrical holder, thereby forming a pellet-shaped positive electrode mixture layer 24 and a negative electrode mixture layer 34. Specifically, a solid electrolyte layer is first inserted into a cylindrical holder. Next, a negative electrode mixture is poured onto one surface of the solid electrolyte, and a lower punch is inserted onto the negative electrode mixture layer. At this time, the negative electrode mixture may be provisionally pressed. Next, the orientation of the solid electrolyte is reversed, a positive electrode mixture is poured onto the other surface of the solid electrolyte, and an upper punch is inserted onto the positive electrode mixture. At this time, the positive electrode mixture may be provisionally pressed. Then, the pellet preparation tool is placed on a press machine, and the lower punch and the upper punch are pressed to produce a pellet-shaped positive electrode mixture layer 24 and a negative electrode mixture layer 34.
[0077] Here, the positive electrode mixture inserted into the cylindrical holder is obtained by mixing the positive electrode active material with other materials in a predetermined ratio using a mortar, etc. Similarly, the negative electrode mixture inserted into the cylindrical holder is obtained by mixing the negative electrode active material with other materials in a predetermined ratio using a mortar, etc.
[0078] In this way, a laminate is obtained in which the positive electrode mixture layer 24, the solid electrolyte layer 10, and the negative electrode mixture layer 34 are laminated in this order. The positive electrode current collector 22 is pressure-bonded to the surface of the positive electrode mixture layer 24 of the obtained laminate, and the negative electrode current collector 32 is pressure-bonded to the surface of the negative electrode mixture layer 34, respectively, to obtain a power generation element 40 in which the positive electrode 20, the solid electrolyte layer 10, and the negative electrode 30 are laminated in this order. The power generation element 40 can be produced by using the powder molding method as described above.
[0079] Next, external terminals are welded to the positive electrode current collector 22 of the positive electrode 20 and the negative electrode current collector 32 of the negative electrode 30, which form the laminate, by a known method, respectively, to electrically connect the positive electrode current collector 22 or the negative electrode current collector 32 to the external terminal. Thereafter, the power generating element 40 connected to the external terminal and the chlorine-based gas trapping agent 1 are housed in an exterior body 50, and the opening of the exterior body 50 is sealed by heat sealing. The chlorine-based gas trapping agent 1 may be one supported in a predetermined amount on a support material. Through the above steps, the all-solid-state battery 100 of this embodiment is obtained.
[0080] When using a chlorine-based gas trapping agent supported on a support material, a pretreatment is required. The pretreatment may be performed, for example, by the following method. First, the chlorine-based gas trapping agent is mixed and stirred in water to prepare a solution. Next, the support material is mixed into this solution. Next, the solution containing the support material is heated to evaporate the water, thereby preparing a chlorine-based gas trapping agent supported on the support material. The amount of the chlorine-based gas trapping agent supported can be adjusted by adjusting the amount of carbonate mixed in water and the amount of the support material.
[0081] Alternatively, raw material powders containing predetermined elements in a predetermined molar ratio may be mixed, molded, and sintered in a vacuum or in an inert gas atmosphere to form a solid electrolyte made of a sintered body.
[0082] In the all-solid-state battery 100 according to the present embodiment, the power generating element 40 contains a chlorine-containing solid electrolyte, and acidic gas such as hydrochloric acid is generated during charge / discharge cycles. However, since the chlorine-based gas trapping agent 1 is sealed in the exterior body 50, the acidic gas in the exterior body 50 can be adsorbed by the chlorine-based gas trapping agent 1. Therefore, the exterior body 50 can be continuously prevented from being corroded by the acidic gas that is continuously generated during charge / discharge cycles after the cell is sealed. Therefore, the all-solid-state battery 100 according to the present embodiment exhibits high cycle characteristics. Since the interior of the exterior body 50 is a closed space, the amount of acidic gas in the atmosphere in the exterior body 50 can be reduced by providing the chlorine-based gas trapping agent 1 in any region in the exterior body 50.
[0083] Although an embodiment of the present invention has been described above in detail with reference to the drawings, each configuration and their combination in each embodiment is merely an example, and addition, omission, substitution, and other modifications of the configuration are possible within the scope of the present invention. For example, the all-solid-state battery according to one embodiment of the present invention may have a modified configuration as shown below. In the all-solid-state battery according to the modified embodiment, the same configuration as that of the all-solid-state battery according to the above embodiment may be denoted by the same reference numerals, and the description thereof may be omitted.
[0084] Fig. 4 is a plan view showing a modified example of the all-solid-state battery of Fig. 3. The all-solid-state battery 100A shown in Fig. 4 has a chlorine-based gas trapping agent 1 at multiple locations. In the all-solid-state battery 100A, the chlorine-based gas trapping agent 1 is provided not only at the folded portion but also at the first sealed portion, the second sealed portion, and the second sealed portion.
[0085] Not only the first side S1 where the laminate film is folded back, but also the second side S2, third side S3, and fourth side S4 which are heat sealed are more susceptible to corrosion than other areas, so if the chlorine-based gas trapping agent 1 is provided in at least one of the first sealed portion, the second sealed portion, and the third sealed portion which are close to these areas, corrosion of the exterior body 50 in these areas is suppressed. As described above, since the interior of the exterior body 50 is a closed space, the amount of acid gas in the atmosphere inside the exterior body 50 can be suppressed regardless of where the chlorine-based gas trapping agent 1 is provided. From the viewpoint of reducing the amount of acid gas in the atmosphere inside the exterior body 50, it is preferable that the chlorine-based gas trapping agent 1 is provided in multiple locations among the folded portion and the three sealed portions.
[0086] Moreover, the all-solid-state battery according to one embodiment of the present invention may have a configuration as shown in Fig. 5 and Fig. 6. Fig. 5 is a cross-sectional view showing a modified example of the all-solid-state battery of Fig. 2, and Fig. 6 is a plan view of the all-solid-state battery of Fig. 5. In the all-solid-state battery 100B shown in Fig. 5 and Fig. 6, the size of the laminate 45B in plan view is smaller than that of the laminate 45, and the chlorine-based gas trapping agent 1 is provided between the positive electrode current collector 22 and the negative electrode current collector 32 in the outer region of the laminate 45B.
[0087] That is, in the all-solid-state battery 100B, the positive electrode current collector 22 and the negative electrode current collector 32 are larger than the positive electrode mixture layer 24 and the negative electrode mixture layer 34 in a plan view, and the chlorine-based gas trapping agent 1 is formed in a region between the positive electrode current collector 22 and the negative electrode current collector 32, which is an area outside the positive electrode mixture layer 24 and the negative electrode mixture layer 34. In this way, the chlorine-based gas trapping agent 1 may be provided on the positive electrode current collector 22 and the negative electrode current collector 32 outside the laminate 45B in a plan view. Although an example in which the chlorine-based gas trapping agent 1 is formed on the side closer to the first side S1 of the laminate 45B is shown in FIG. 5 and FIG. 6, the present invention is not limited to this example. The chlorine-based gas trapping agent 1 may be formed on the side closer to the second side S2 of the laminate 45B, on the side closer to the third side S3, on the side closer to the fourth side S4, or in a plurality of places.
[0088] In the all-solid-state battery 100B, the chlorine-based gas trapping agent 1 is formed at a position closer to the laminate 45B, which is a source of acidic gas, and can adsorb acidic gas in the region between the positive electrode current collector 22 and the negative electrode current collector 32. Therefore, the amount of acidic gas flowing out to the outside of the positive electrode current collector 22 and the negative electrode current collector 32 in plan view can be reduced.
[0089] Moreover, the all-solid-state battery according to an embodiment of the present invention may have a configuration as shown in FIG. 7 and FIG. 8. FIG. 7 is a cross-sectional view showing another modified example of the all-solid-state battery of FIG. 2, and FIG. 8 is a plan view of the all-solid-state battery of FIG. 7. In the all-solid-state battery 100C shown in FIG. 7 and FIG. 8, the chlorine-based gas trapping agent 1 is formed so as to surround the outer periphery of the laminate 45B. That is, in the all-solid-state battery 100C, the chlorine-based gas trapping agent 1 is formed over the entire outer periphery of the laminate 45B. The distance of the chlorine-based gas trapping agent 1 from the laminate 45B can be set arbitrarily as long as it is between the positive electrode current collector 22 and the negative electrode current collector 32.
[0090] The all-solid-state battery 100C can provide the same effect as the all-solid-state battery 100B. In the all-solid-state battery 100C, the chlorine-based gas trapping agent 1 is formed so as to surround the outer periphery of the laminate 45B, so that the chlorine-based gas trapping agent 1 is always located midway between the laminate 45B and the exterior body 50 in plan view. EXAMPLES
[0091] EXAMPLES Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0092] [Example 1] (Preparation of positive electrode mixture) The positive electrode mixture is made of powdered positive electrode active material LCO (LiCoO 2 ), solid electrolyte LZSOC(Li 2 ZrSO 4 Cl 4 ), and VGCF as a conductive additive were prepared, and were weighed and mixed so as to have a ratio of 63 mass %: 35 mass %: 2 mass % (positive electrode active material: solid electrolyte: conductive additive), respectively.
[0093] (Preparation of negative electrode mixture) The negative electrode mixture is made of powdered negative electrode active material LTO (Li 4 Ti 5 O 12 ), solid electrolyte LZSOC(Li 2 ZrSO 4 Cl 4 ), and VGCF as a conductive additive were prepared, and were weighed and mixed so as to have a ratio of 60 mass %: 35 mass %: 5 mass % (negative electrode active material: solid electrolyte: conductive additive), respectively.
[0094] (Preparation of Molded Body) A resin holder with a through hole of 10 mm diameter in the center, and a lower punch and an upper punch of 9.99 mm diameter made of SKD11 were prepared. The lower punch was inserted from below the through hole of the resin holder, and the powdered materials, the positive electrode mixture, the solid electrolyte LZSOC, and the negative electrode mixture were added in that order from the opening side of the resin holder.
[0095] Next, an upper punch was inserted on top of the added powdered material, and the unit having the upper punch, a resin holder for containing the powdered material, and the lower punch was placed in a press and pressed at a pressure of 20 kN to produce a molded body.
[0096] Next, a positive electrode current collector made of aluminum foil with a diameter of 15 mm and a thickness of 20 μm was placed on the positive electrode active material. Also, a negative electrode current collector made of aluminum foil with a diameter of 15 mm and a thickness of 20 μm was placed under the negative electrode active material layer. Through the above procedure, a laminated structure was obtained in which the positive electrode current collector / positive electrode mixture layer / solid electrolyte layer / negative electrode mixture layer / negative electrode current collector were laminated in this order.
[0097] Next, external terminals were welded to the positive electrode current collector of the positive electrode layer and the negative electrode current collector of the negative electrode layer constituting the laminated structure, respectively, to electrically connect the positive electrode current collector and the negative electrode current collector to the external terminals, thereby forming a power generating element.
[0098] Then, a power generating element was placed on the aluminum laminate, and Mg was placed next to the power generating element as a chlorine gas trap. 6 Mn 2 (CO 3 )(OH) 16 4H 2 5 mg of O was placed on the battery. The aluminum laminate was folded in half from the side where the chlorine-based gas trapping agent was placed, and the power generation element and the chlorine-based gas trapping agent were housed in an exterior body made of aluminum laminate material. Finally, the opening of the exterior body was sealed by heat sealing. In this way, the power generation element and the chlorine-based gas trapping agent were sealed in the exterior body, and an all-solid-state battery was produced in which the power generation element and the chlorine-based gas trapping agent were surrounded by the first side, the second side, the third side, and the fourth side in a plan view, and the chlorine-based gas trapping agent was formed in the folded portion.
[0099] [Examples 2 to 8] An all-solid-state battery was produced in the same manner as in Example 1, except that the chlorine-based gas trapping agent was changed to another hydrotalcite. In Examples 2 to 8, the following chlorine-based gas trapping agents were used. Example 2: Mg6 Al 2 (CO 3 )(OH) 16 4H 2 O, Example 3: Mg 6 Fe 2 (OH) 16 Cl 2 4H 2 O, Example 4: Mg 6 Fe 2 (CO 3 )(OH) 16 4H 2 O, Example 5: Mg 6 Fe 2 (CO 3 )(OH) 16 4H 2 O, Example 6: Ni 6 Al 2 (CO 3 )(OH) 16 4H 2 O, Example 7: Mg 5 CaAl 2 (SO 4 ) 2 (OH) 18 12H 2 O, Example 8: Zn 4 Al 4 (CO 3 )(OH) 12 3H 2 O
[0100] [Examples 9 and 10] All solid electrolytes used in the production of power generation elements are Li 2 ZrSO 4 (P 2 O 5 ) 0.1 Cl 4 Except for the above change, an all-solid-state battery was produced in the same manner as in Example 1 and Example 2.
[0101] [Examples 11 and 12] All solid electrolytes used in the production of power generation elements are Li 2 Zr 0.5 Al 0.5 Cl 3.5An all-solid-state battery was fabricated in the same manner as in Examples 1 and 2, except that Li was used instead of LiO. 2 Zr 0.5 Al 0.5 Cl 3.5 O is produced using ZrCl as a raw material. 4 , AlCl 3 and Li 2 This is a composition that uses O, and has Li at the A site, Zr and Al at the E site, O at the G site, and Cl at the X site in the above formula (2).
[0102] [Examples 13 to 19] The chlorine gas trap agent is potassium carbonate (KCO) supported on activated carbon (Kuraray Chemical, Kuraray Coal GG, pore size 20 nm) as a support material. 2 CO 3 An all-solid-state battery was produced in the same manner as in Example 1, except that the above-mentioned step was changed to the above-mentioned step. In the following examples in which the chlorine-based gas trapping agent is supported on a support material, the total weight of the chlorine-based gas trapping agent and the support material is 5 mg. The weight of the chlorine-based gas trapping agent (supported amount) relative to the total weight of the chlorine-based gas trapping agent and the support material is shown in Table 2. In the following examples, the total weight of the chlorine-based gas trapping agent and the support material was not adjusted, but the supported amount was adjusted by adjusting the ratio between them.
[0103] When a chlorine-based gas trapping agent is supported on a support material, first, carbonate is mixed into water and stirred to prepare a solution. Then, activated carbon, which serves as the support material, is mixed into this solution. Next, the solution containing the support material is heated to evaporate the water, and a chlorine-based gas trapping agent supported on the support material is prepared. The amount of the chlorine-based gas trapping agent supported was adjusted by adjusting the amount of carbonate mixed in water and the amount of the support material. In the other examples below, examples in which carbonate or acetate is supported on a support material use those prepared by the same method.
[0104] [Example 20] All solid electrolytes used in the production of power generation elements are Li 2 ZrSO 4 (P 2O 5 ) 0.1 Cl 4 An all-solid-state battery was produced in the same manner as in Example 16, except for the above change.
[0105] [Example 21] All solid electrolytes used in the production of power generation elements are Li 2 Zr 0.5 Al 0.5 Cl 3.5 An all-solid-state battery was produced in the same manner as in Example 16, except that O was used.
[0106] [Examples 22 to 28] All-solid-state batteries were produced in the same manner as in Examples 13 to 19, except that the support material was changed to alumina (manufactured by Sumitomo Chemical, product number: pore diameter 6.6 nm).
[0107] [Example 29] Except for using potassium carbonate as a chlorine-based gas trapping agent without supporting it on a support material, an all-solid-state battery was produced in the same manner as in Example 13. The amount of the chlorine-based gas trapping agent in Example 29 was 5 mg.
[0108] [Examples 30 to 36] Chlorine gas trapping agent is calcium carbonate (CaCO 3 ), all-solid-state batteries were produced in the same manner as in Examples 13 to 19.
[0109] [Example 37] All solid electrolytes used in the production of power generation elements are Li 2 ZrSO 4 (P 2 O 5 ) 0.1 Cl 4 An all-solid-state battery was produced in the same manner as in Example 33, except for the above change.
[0110] [Example 38] All solid electrolytes used in the production of power generation elements are Li 2 Zr 0.5 Al 0.5 Cl3.5 An all-solid-state battery was produced in the same manner as in Example 33, except that O was used.
[0111] [Examples 39 to 45] Chlorine gas trapping agent is calcium carbonate (CaCO 3 ), all-solid-state batteries were produced in the same manner as in Examples 22 to 28.
[0112] [Example 46] An all-solid-state battery was produced in the same manner as in Example 30, except that calcium carbonate was used as a chlorine-based gas trapping agent without being supported on a support material.
[0113] [Example 47 and Example 48] In Example 47, the chlorine-based gas trapping agent was replaced with lithium carbonate (Li 2 CO 3 An all-solid-state battery was produced in the same manner as in Example 33, except that the above-mentioned was changed to the above-mentioned. In Example 48, the chlorine gas trap was replaced with sodium carbonate (Na 2 CO 3 ), an all-solid-state battery was produced in the same manner as in Example 33. The amount of the chlorine-based gas trapping agent supported on the chlorine-based gas trapping agent and the support material in Example 48 was 9.8 wt %.
[0114] [Examples 49 to 52] In Example 49, all the solid electrolytes used to prepare the power generating element were LPSC (Li 6 P.S. 5 An all-solid-state battery was produced in the same manner as in Example 1, except that the electrolyte was changed to HCl. In Example 50, an all-solid-state battery was produced in the same manner as in Example 2, except that all the solid electrolytes used in producing the power generating element were changed to LPSC. In Example 51, an all-solid-state battery was produced in the same manner as in Example 16, except that all the solid electrolytes used in producing the power generating element were changed to LPSC. In Example 52, an all-solid-state battery was produced in the same manner as in Example 33, except that all the solid electrolytes used in producing the power generating element were changed to LPSC.
[0115] [Example 53 to Example 56] An all-solid-state battery was produced in the same manner as in Example 16, except that the chlorine-based gas trapping agent was changed. In Example 54, calcium acetate Ca(CH 3 COO) 2 The amount of the chlorine-based gas trapping agent supported on the support material was 10.2 wt %. In Example 55, lithium acetate CH was used as a chlorine gas trap. 3 COOLi was used, and the amount of the chlorine-based gas trapping agent supported on the support material was set to 10.2 wt%. In Example 56, potassium acetate CH was used as a chlorine gas trap. 3 COONa was used, and the amount of the chlorine-based gas trapping agent supported on the support material was 10.4 wt%.
[0116] [Examples 57 to 68] In Examples 57 to 68, all-solid-state batteries were fabricated in the same manner as in Example 1, Example 2, Example 9, Example 10, Example 11, Example 12, Example 51, Example 52, Example 53, Example 54, Example 55, and Example 56, respectively, except that larger positive electrode current collectors and negative electrode current collectors (20 mm × 30 mm) were used and a chlorine-based gas trap was formed in the region between the positive electrode current collector and the negative electrode current collector, which was the outer region in plan view of the laminate composed of the positive electrode mixture layer, the solid electrolyte layer, and the negative electrode mixture layer (change in the all-solid-state battery layout).
[0117] [Comparative Example 1] Except for not using a chlorine-based gas trapping agent, an all-solid-state battery was produced in the same manner as in Example 1. That is, in Comparative Example 1, a power generating element containing LZSOC as a solid electrolyte was sealed in an exterior body.
[0118] [Comparative Example 2 and Comparative Example 3] All the solid electrolytes used in the production of the power generation element are Li 2 ZrSO 4 (P 2 O 5 ) 0.1 Cl 4 ,Li 2 Zr 0.5 Al 0.5 Cl 3.5 An all-solid-state battery was produced in the same manner as in Comparative Example 1, except that O was used.
[0119] [Comparative Example 4] Except for not using a chlorine-based gas trapping agent, an all-solid-state battery was produced in the same manner as in Example 49. That is, in Comparative Example 1, a power generating element containing LPSC as a solid electrolyte was sealed in an exterior body.
[0120] [Comparative Example 5] Except for not using a chlorine-based gas trapping agent, an all-solid-state battery was produced in the same manner as in Example 13. That is, in Comparative Example 5, a power generating element containing LZSOC as a solid electrolyte was sealed in an exterior body together with activated carbon not supporting a chlorine-based gas trapping agent.
[0121] [Comparative Example 6 and Comparative Example 7] All the solid electrolytes used in the production of the power generation element are Li 2 ZrSO 4 (P 2 O 5 ) 0.1 Cl 4 ,Li 2 Zr 0.5 Al 0.5 Cl 3.5 An all-solid-state battery was produced in the same manner as in Comparative Example 5, except that O was used.
[0122] [Comparative Example 8] Except for not using a chlorine-based gas trapping agent, an all-solid-state battery was produced in the same manner as in Example 63. That is, in Comparative Example 5, a power generating element containing LPSC as a solid electrolyte was sealed in an exterior body together with activated carbon not supporting a chlorine-based gas trapping agent.
[0123] [Comparative Example 9] Except for not using a chlorine-based gas trapping agent, an all-solid-state battery was produced in the same manner as in Example 22. That is, in Comparative Example 9, a power generating element containing LZSOC as a solid electrolyte was sealed in an exterior body together with alumina not supporting a chlorine-based gas trapping agent.
[0124] [Comparative Examples 10 and 11] All the solid electrolytes used in the production of the power generation element are Li 2 ZrSO 4 (P 2 O 5 ) 0.1 Cl 4 ,Li 2 Zr 0.5 Al 0.5 Cl 3.5 An all-solid-state battery was produced in the same manner as in Comparative Example 9, except that O was used.
[0125] [Comparative Example 12] In Comparative Example 12, a power generating element containing LPSC as a solid electrolyte was sealed in an exterior body together with alumina that did not support a chlorine-based gas trapping agent.
[0126] {Cycle characteristic test} The cycle characteristics were measured for the all-solid-state batteries of Examples 1 to 68 and Comparative Examples 1 to 12. The cycle characteristics were measured using a secondary battery charge / discharge tester (manufactured by Hokuto Denko Corporation) by the following method.
[0127] The cycle characteristics were measured using a CC-CV charge-CC discharge format. Specifically, first, a constant current charge was performed at a charge rate of 1C up to a charging upper limit voltage of 2.7V, and then a constant voltage charge was performed up to 2.7V in constant voltage mode (2.7V). After that, the battery was discharged at a constant current discharge rate of 1C until the battery voltage reached 1.3V. The discharge capacity after the end of charge and discharge was detected, and the battery capacity Q before the cycle test was calculated. 1 asked for.
[0128] Next, constant current charging was performed at a charge rate of 1C up to a charging upper limit voltage of 2.7V, and further constant voltage charging was performed in constant voltage mode (2.7V) up to 2.7V. After that, discharging was performed at a constant current discharge rate of 1C until the battery voltage reached 1.3V, and the battery capacity was measured. The above charge and discharge were counted as one cycle, and the battery capacity was measured when the battery capacity was half the battery capacity before the cycle test (Q 1 A cycle test was conducted up to 500 cycles until the fatigue life of the specimen reached 1 / 2.
[0129] The outline of the configuration of the all-solid-state batteries of Examples 1 to 8 and the results of the cycle characteristic test are summarized in Table 1. The outline of the configuration of the all-solid-state batteries of Examples 13 to 56 and the results of the cycle characteristic test are summarized in Table 2. The outline of the configuration of the all-solid-state batteries of Examples 57 to 68 and the results of the cycle characteristic test are summarized in Table 3. The outline of the configuration of the all-solid-state batteries of Comparative Examples 1 to 12 and the results of the cycle characteristic test are summarized in Table 4.
[0130] In the following Tables 1 to 4, "LZSOC" in the solid electrolyte column indicates that the solid electrolyte is Li. 2 ZrSO 4 Cl 4 The "LPSC" uses Li as a solid electrolyte. 6 P.S. 5 The column for "50% capacity cycle" in the table shows the battery capacity (Q 1 / 2), and the battery capacity after 500 cycles is still (Q 1 For those that exceed the 50% cycle capacity (500+), "500+" is written in the 50% cycle capacity column.
[0131] [Table 1]
[0132] [Table 2]
[0133] [Table 3]
[0134] [Table 4]
[0135] As shown in Tables 1 to 4, it was confirmed that the all-solid-state batteries in which the chlorine-based gas trapping agents of Examples 1 to 68 were sealed in the exterior body together with the power generating element exhibited superior cycle characteristics compared to Comparative Examples 1 to 12 in which the chlorine-based gas trapping agent was not sealed in the exterior body. Among these, the all-solid-state battery including the hydrotalcite represented by the above formula (1) as the chlorine-based gas trapping agent exhibited particularly excellent cycle characteristics.
[0136] In the examples in which the chlorine-based gas trapping agent is a carbonate of an alkali metal element or an alkaline earth metal element, it was confirmed that the agent supported on either activated carbon or alumina showed superior cycle characteristics compared to the agent not supported on a support material, and it was confirmed that the agent showed particularly superior cycle characteristics when the support material was activated carbon. It was also confirmed that the agent showed particularly superior cycle characteristics when the amount of support was 5 wt% or more and 20 wt% or less. [Explanation of symbols]
[0137] 1...chlorine-based gas trapping agent, 10...solid electrolyte layer, 20...positive electrode, 22...positive electrode current collector, 24...positive electrode mixture layer, 30...negative electrode, 32...negative electrode current collector, 34...negative electrode mixture layer, 40...power generating element, 45...laminated body, 50...exterior body, 52...metal foil, 54...resin layer, 62, 64...terminal, 100...all-solid-state battery
Claims
1. a power generating element in which a positive electrode including a positive electrode active material, a solid electrolyte layer, and a negative electrode including a negative electrode active material are laminated in this order, and an exterior body that seals the power generating element, one or more of the positive electrode, the negative electrode, and the solid electrolyte layer have a solid electrolyte containing elemental chlorine; A chlorine-based gas trapping agent is sealed within the exterior body of the all-solid-state battery.
2. The all-solid-state battery according to claim 1, wherein the chlorine-based gas trapping agent is a hydrotalcite represented by formula (1): M1 2+ 8-x M2 3+ x (OH) - 16 CO 3 2- ・nH 2 O・・・(1) (In formula (1), M1 2+ is Mg 2+ , Fe 2+ , Zn 2+ , Ca 2+ , Li 2+ , Ni 2+ , Co 2+ and Cu 2+ The compound is one or more selected from the group consisting of: M2 3+ is Al 3+ and Fe 3+ and Mn 3+ The compound is one or more selected from the group consisting of: 2≦x≦5, 0≦n).
3. The all-solid-state battery according to claim 1 , wherein the chlorine-based gas trapping agent is a carbonate of an alkali metal element or an alkaline earth metal element.
4. 4. The all-solid-state battery according to claim 3, wherein the chlorine-based gas trapping agent is supported by a support made of a porous material in an amount of 5 wt % to 20 wt %.
5. The all-solid-state battery according to claim 3 , wherein the chlorine-based gas trapping agent is potassium carbonate or calcium carbonate.
6. 2. The all-solid-state battery according to claim 1, wherein the solid electrolyte is a halide-based solid electrolyte represented by formula (2): A a E b G c X d ・・・(2) (In formula (2), A is at least one element selected from the group consisting of Li, K, and Na. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanides. G is OH, BO 2 , B.O. 3 , B.O. 4 , B 3 O 6 , B 4 O 7 , CO 3 , NO 3 , AlO 2 , SiO 3 , SiO 4 , Si 2 O 7 , Si 3 O 9 , Si 4 O 11 , Si 6 O 18 , P.O. 3 , P.O. 4 , P 2 O 7 , P 3 O 10 , S.O. 3 , S.O. 4 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 , B.F. 4 , P.F. 6 ,BOB,(COO) 2 , N, AlCl 4 , C.F. 3 SO 3 , C.H. 3 COO, CF 3 COO, P 2 O 5 and at least one group selected from the group consisting of O. X contains a Cl element or a Cl element and at least one element selected from the group consisting of F, Br and I. 0.5≦a<6, 0<b<2, 0≦c≦6, 0<d≦6.
1.
7. The exterior body is an aluminum laminate, The all-solid-state battery according to claim 1 , wherein the chlorine-based gas trapping agent is disposed in a sealed portion or a folded portion located outside the power generating element in a plan view.
8. the positive electrode has a positive electrode current collector and a positive electrode mixture layer provided between the positive electrode current collector and the solid electrolyte layer, the negative electrode has a negative electrode current collector and a negative electrode mixture layer provided between the negative electrode current collector and the solid electrolyte layer, When viewed from above, the positive electrode current collector and the negative electrode current collector are larger than the positive electrode mixture layer and the negative electrode mixture layer, 2. The all-solid-state battery according to claim 1, wherein the chlorine-based gas trapping agent is formed in a region outside the positive electrode mixture layer and the negative electrode mixture layer, the region being between the positive electrode current collector and the negative electrode current collector.
Citation Information
Patent Citations
Lithium-ion secondary battery
JP2009054462A
Cited By
Solid electrolyte membrane and preparation method therefor, all-solid-state lithium ion battery, and electronic device
JP2026081137A
Solid electrolyte membrane and preparation method thereof, all-solid-state lithium ion battery, and electronic device
JP2026081138A
Acid chloride solid electrolytes, methods for producing the same, and their applications
JP2026114946A
Solid electrolyte membrane and method for preparing the same, all-solid-state lithium-ion battery, and electronic device
JP7904970B2
Solid electrolyte membrane and its preparation method, all-solid-state lithium-ion battery and electronic device
JP7904971B2